Subscriber access provided by Kaohsiung Medical University
Functional Inorganic Materials and Devices
A Highly Bendable and Durable Transparent Electromagnetic Interference Shielding Film Prepared by Wet Sintering of Silver Nanowires Dong Gyu Kim, Jong Han Choi, Duck-Kyun Choi, and Sang Woo Kim ACS Appl. Mater. Interfaces, Just Accepted Manuscript • DOI: 10.1021/acsami.8b07054 • Publication Date (Web): 14 Aug 2018 Downloaded from http://pubs.acs.org on August 14, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
A Highly Bendable and Durable Transparent Electromagnetic Interference Shielding Film Prepared by Wet Sintering of Silver Nanowires
Dong Gyu Kim,†,§ Jong Han Choi,†,∥ Duck-Kyun Choi,§ and Sang Woo Kim*†,‡
†
Clean Energy Research Center, Korea Institute of Science and Technology (KIST), Seoul
02792, Republic of Korea ‡
Division of Energy Environment Technology, KIST school, University of Science and
Technology (UST), Seoul 02792, Republic of Korea §
Division of Materials Science and Engineering, Hanyang University, Seoul 04763, Republic
of Korea ∥Department
of Chemical and Biological Engineering, Korea University, Seoul, 02841,
Republic of Korea
ABSTRACT: Electromagnetic (EM) wave emissions from wearable or flexible smart display devices can cause product malfunction and have a detrimental effect on human health. Therefore, EM shielding strategies are becoming increasingly necessary. Consequently, herein, we prepared a transparent acrylic polymer-coated/reduced graphene oxide/silver nanowire (Ag NW) (A/RGO/SANW) EM interference (EMI) shielding film via liquid-to-vapor pressure-assisted wet sintering. The film exhibited enhanced Ag NW network formation and antireflection (AR) effects. The wet-sintered Ag NW shielding film had a threshold radius of curvature (ROC) of 1
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
0.31 mm at a film thickness of 100 µm, demonstrating its high flexibility, while the conventional indium tin oxide (ITO) shielding film had a threshold ROC of ~5 mm. The EMI shielding effectiveness (SE) of the A/RGO/SANW multilayer film was approximately twice that of the ITO film at a similar relative transmittance (84%–85%). The optical relative reflectance of the Ag NW layer was reduced due to the AR effect, and the visible light transmittance was considerably improved owing to the different refractive indices in the multilayer shielding film. Because the acrylic coating layer had a high contact angle, the multilayer film exhibited high temperature and humidity durability with little change in the SE over 500 h at 85 °C and 85% relative humidity. The multilayer film comprising wetsintered Ag NW exhibited high flexibility and humidity durability, high shielding performance (more than 24 dB at a relative transmittance of 85% or more), and high mass productivity, making it highly applicable for use as a transparent shielding material for future flexible devices.
KEYWORDS: transparent electromagnetic shielding, flexible electromagnetic interference shielding film, silver nanowire, sintering, acrylic polymer, graphene oxide
2
ACS Paragon Plus Environment
Page 2 of 47
Page 3 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1. INTRODUCTION
The demand for flexible components for use in wearable devices and highly portable foldable displays has significantly increased in recent years.1–5 However, these components tend to be relatively small, indicating that electromagnetic interference (EMI) generated by each independent component can impact product function and shorten the operational lifetime.6,7 In addition, previous studies have shown that the EM waves radiated from certain devices can have harmful direct or indirect effects on human health.8–10 Accordingly, the need for appropriate shielding to suppress the harmful EM waves generated by certain electronic devices is increasing.11–13
Transparent EMI shielding films for flexible devices must exhibit high EMI shielding effectiveness (SE), high visible-light transmittance, high flexibility, ultrathin, lightweight, and excellent durability.12–14 However, EMI shielding materials that satisfy all these criteria have not yet been developed. The performance of an EMI shielding material strongly depends on its electrical conductivity, permeability, thickness, and the EM frequency of interest.15–18 Above all, to develop a superior flexible transparent shielding film, the material must have improved electrical conductivity, which is an intrinsic material characteristic, while maintaining a high degree of visible light transmittance.
To address these issues, various transparent EMI shielding materials, including transparent conducting oxides (TCOs),19,20 metal meshes,21,22 and graphene,23–24 have been investigated. Recently, hybrid EMI shielding films, which combine a metal mesh with graphene, have been studied.26,27 Indium tin oxide (ITO) is the most widely used TCO material owing to its high 3
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
transmittance and electrical conductivity. However, ITO is unsuitable for use as a transparent flexible material28,29 because it is brittle and fractures easily. Moreover, its threshold radius of curvature (ROC) is greater than 7 mm,30 which is defined as the ROC at which a 10% change in the electrical resistance is observed. Al-doped ZnO, developed as an alternative to ITO, exhibits relatively high flexibility and high optical relative transmittance (84.1%); however, it suffers from a poor shielding performance of 6.5 dB at frequencies of 0.3–1.5 GHz,20 which limits its use as a transparent shielding material. For higher EMI shielding and optical performance, metal mesh films have been studied.21,22 Metal meshes exhibit high optical transmittance and EMI shielding performance. However, they have disadvantages in that they are costly (owing to their complicated preparation) and have poor repetitive fatigue bending characteristics.31 To address the problems associated with their complicated manufacturing process, a metal mesh film fabricated by ink jet printing has been developed.21 However, its EMI SE is only 20 dB (8–12 GHz) at a relative transmittance of 88.2% and it is poorly flexible. Monolayer graphene is a promising alternative material for fabricating transparent EMI shielding films owing to its excellent optical and electronic properties. However, despite its high relative transmittance of 97%, it exhibits a low SE of 2.27 dB (2.2–7 GHz) owing to its ultralow thickness and the presence of defects.23 Multilayer graphene, which shows improved EMI shielding performance, exhibits a high SE of 19.14 dB (18–26.5 GHz) at a relative transmittance of 80.5%.25 However, its preparation is too complicated for it to be produced on a large scale.
To overcome these drawbacks, metal NWs have been reported to be promising nextgeneration transparent and flexible EMI shielding materials. Among them, silver nanowires (Ag NWs) are regarded as the most promising candidate owing to their excellent 4
ACS Paragon Plus Environment
Page 4 of 47
Page 5 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
transmittance, electrical conductivity, and mechanical flexibility.32–34 Furthermore, Ag NWs can be wet coated onto flexible substrates with continuous equipment using solutions dispersed as inks, thus enabling low-cost and high-volume production.35 Owing to these properties, Ag NWs have been studied as a highly bendable transparent EMI shielding material.36 However, despite these advantages, Ag NWs have several issues that need to be addressed if they are to be used as a shielding material. First, in the polyol synthesis process, the insulating capping agent used to promote anisotropic growth surrounds the AgNWs,37 which indicates that the electrically conducting network structure is not sufficiently formed and the contact conductance between the NWs is poor. Furthermore, Ag NWs weakly bind to substrates, are susceptible to oxidation, and reflect light, causing scattering.38
Recently, a number of methods have been proposed to enhance the electrical conductivity of Ag NWs by strengthening their network structures. These include high-temperature sintering,39–41 mechanical pressing,42,43 and light-induced welding.44,45 Another approach is to combine Ag NWs with conductive polymers to inhibit their light scattering and improve their bonding with flexible substrates.46 However, the former methods have the limitations that high temperature and/or high pressure are required, both of which are drawbacks to largescale production and can damage the polymeric components of the material. Furthermore, the light-induced welding of Ag NWs requires the usage of expensive optical equipment due to sophisticated precision control and high energy output for nanowire sintering. The use of the latter conductive polymer and Ag NWs exhibits a problem that the conductive polymer is easily deteriorated and that the conductivity of the polymer is lowered.
5
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Herein, we report on the development of a transparent multilayer EMI shielding film comprising Ag NWs arranged in a network that is reinforced by a wet sintering process assisted by liquid-to-vapor pressure (LVP). The EMI shielding performance of the multilayer film was evaluated in the frequency range 0.3–3.0 GHz, which corresponded to a quasimicrowave frequency band widely used in communication systems, such as television and radio transmissions, channel broadcasting, mobile phones, and local area networks.
2. EXPERIMENTAL SECTION 2.1. Materials An isopropyl alcohol (IPA) suspension (004c) containing Ag NWs (0.5 wt%) was purchased from N & B, Korea. The diameters and lengths of the Ag NWs in the IPA suspension were in the ranges 35–45 nm and 5–15 µm, respectively. A polyethylene terephthalate (PET) film (RX160) with a thickness of 100 µm was purchased from HSfinetech, Korea. A graphene oxide (GO) suspension (GO-A400) was purchased from Grapheneall, Korea. The GO suspension contained 0.6 wt% GO dispersed in distilled water, and the GO flakes had a single-layer thickness of 80% and a size of 0.5–5 µm. An aqueous acrylic emulsion comprising 30% solids (emulsion size = ~100 nm) was used for top coating the Ag NW films. 2.2. Fabrication of transparent EMI Ag NW films Figure 1a shows a schematic of the wet sintering process used to prepare the Ag NWs proposed herein. The pristine Ag NWs were wet coated onto the PET film using an automatic film applicator (PI-1210; Sangyo, Japan). The Ag NW films were then dried on a hot plate at 80 °C for 10 min and further dried in a constant-temperature drying chamber at 60 °C for 1 h. 6
ACS Paragon Plus Environment
Page 6 of 47
Page 7 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Figure 1. Schematic of the fabrication of silver (Ag) nanowire (NW) electromagnetic interference (EMI) shielding films: (a) overall fabrication process, (b) wet sintering process using hot rolling system, and (c) an A/RGO/SANW EMI shielding multilayer film obtained from the process.
To develop an Ag NW film with a strong network structure, the pristine Ag NW films were sprayed or coated with water or a water-based GO suspension, after which the Ag NWs were wet sintered with the aid of LVP using a roll-to-roll system at temperatures of 40 °C–140 °C and a speed of 3.2 cm/s. The sintered Ag NW (SANW) film and the GO/Ag NW (GO/SANW) film were dried in a constant-temperature drying chamber at 60 °C for 1 h. The RGO/SANW film was obtained by reduction from the GO/SANW film with hydrazine vapor and then drying.48 The acrylic microemulsion was spin coated onto the SANW and GO/SANW films at a 7
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
rotation speed of 1,000 rpm for 1 min. The acrylic polymer-coated SANW (A/SANW) film and the acrylic polymer-coated GO/SANW (A/GO/SANW) film were dried on a hot plate at 80 °C for 10 min. For complete curing, the films were dried in a constant-temperature drying chamber at 60 °C for 1 h. Figure 1b shows the photographs of the wet sintering process used to prepare the Ag NW EMI shielding film. Figure 1c shows the Ag NW EMI shielding film fabricated by the wet sintering process.
2.3. Characterizations of EMI shielding films The images of the Ag NW films were obtained using field-emission scanning electron microscopy (FESEM; Nova SEM; FEI, USA). The surface roughness of the Ag NW films was measured using atomic force microscopy (AFM; XE-100; Park Systems; Korea). The sheet resistances of the Ag NW films were measured using the four-point probe method (NCP-TFP; Mitsubishi Chemical, Japan). The optical properties of the Ag NW films were measured using a UV spectrophotometer (CM5; Scinco, Korea) in the wavelength range 350– 750 nm. Bending tests were performed using the collapsing radius test.49 The resistance changes of the Ag NW films according to the ROCs were measured using a bending tester (see Supplementary Figure S2). Silver paste was coated onto both ends of the Ag NW films for electrode formation. A DC power supply source (GPD-3303s; GW Instek, Taiwan) was connected to both sides of the Ag NW film electrodes, and the electrical current changes according to the ROC were calculated as the resistance changes of the bent state. Note that when a voltage is applied to an Ag NW film, heat is generated via joule heating.50 Therefore, voltage should be regulated so that the temperature of the Ag NW film remains below 40 °C, thereby ensuring that the resistance is not affected by the temperature. The constant temperature and humidity tests of the Ag NW films were performed by a testing agency 8
ACS Paragon Plus Environment
Page 8 of 47
Page 9 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
(KOPTRI, Korea). The electrical properties of the acrylic-layer-coated Ag NW films cannot be measured using the four-point probe equipment. Therefore, electrodes were formed at both ends of Ag NW films and the resistance changes were measured using a DC power supply source. Infrared (IR) images of the Ag NW films were obtained using an IR camera (T620; FLIR, USA). The EMI SE was measured using an RF vector network analyzer (VNA 8753ES; Agilent, USA) in the frequency range 0.03–3 GHz. A coaxial sample holder was used with a shielding effect measurement kit (S-39D-D4935, Keycom, Japan) designed according to the ASTM D4935-10 standard. For VNA calibration, SOLT calibration was performed using a well-defined short, open and load (50 Ω characteristic impedance). The size of the circular film sample for shielding effect measurement was 49 mm outside diameter. The EM transmittance (T) and reflectance (R) were calculated according to Equation 1 using the measured S-parameters of the two-port network system, which include the reflection coefficient ( or ) and transmission coefficient ( or ). When the total output of the incident EM radiation is 1, the EM absorbance A can be obtained from equation (2) by subtracting R and T (see Supplementary Figure S1). The total EMI SE (SE ) of a solid T
material with no apertures can be expressed as the sum of the three loss factors: effective reflection (SE ), effective absorption (SE ), and multiple reflections (SE R
Equation 3–6.51,52 Since SE
A
MR
MR
), as shown in
can be ignored when SE is greater than 10 dB,53,54 SE can A
T
be approximated as the sum of SE and SE . When an incident wave passes through a shield, A
R
the SE at the interface between mediums 1 (free space) and 2 (shield) is related to the R
difference in the characteristic impedances between the media, which is logarithmically proportional to the ratio of the impedance of the incident wave (ZW) and the impedance of the
9
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 47
shield (ZS), as presented in Equation 4. SE and SE are obtained using Equations 4 and 5, R
A
respectively, which can be applied to a plane wave that approaches the shield at normal incidence. Finally, SE can be calculated by Equation 6, which is the sum of Equation 4 and T
Equation 5 that are given below.
| |2 = R, | |2 = T
(1)
A=1−R−T
(2)
SE = SE + SE + SE T
R
SE = 20 log R
A
| |
| |
= SE + SE (dB)
MR
R
A
= −10 log (1 − R) (dB)
(3)
(4)
SE = −10 log (dB)
(5)
A
SE = −10 log(1 − R) − 10 log (dB)
(6)
T
3. RESULTS AND DISCUSSION 3.1. Fabrication of EMI shielding films Figures 2a–2f show the SEM and AFM images of the network structures of the Ag NW EMI shielding films. As shown in Figure 2a, the Ag NWs become electrically connected as the NWs stack; however, the contact resistance can be increased by ohmic contact owing to the weak network between the NWs. Figure 2e shows the surface roughness of the Ag NW films, which serves as a criterion to assess the electrical network between the NWs. The Ra roughness value of the pristine Ag NWs was measured to be 23.5 nm. Figure 2b shows the SEM image of the SANW layer wet sintered at 120 °C, indicating that the stacked NWs are 10
ACS Paragon Plus Environment
Page 11 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
fully networked by LVP-assisted wet sintering, thereby increasing the electrical contact between the NWs. When comparing the surface roughnesses in Figures 2e and 2f, it can be observed that the Ra roughness value decreases from 23.5 to 14.3 nm owing to the sintering effect. Figure 2c shows an SEM image of GO (0.5 wt%) coated onto SANW. The Ra roughness value is significantly reduced to 5.3 nm by the uniform coating of GO onto the sintered Ag NW film. Figures 2d and 2h show the SEM and AFM images of the acrylic polymer coated onto the GO/SANW film. The Ra roughness value increased to 13.1 nm because of the covering of the GO surface with 40−50-nm acrylic nanoparticles. The hydrophobic acrylic coating layer prevents the Ag NWs from being oxidized by moisture and oxygen in the external environment.
Figure 2. Scanning electron microscopy (SEM; 15° tilted) and atomic force microscopy (AFM) images of the Ag NW EMI shielding films fabricated via wet sintering process: (a and 11
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
e) pristine Ag NW/polyethylene terephthalate (PET) film, (b and f) SANW/PET film, (c and g) GO/SANW/PET film, and (d and h) A/GO/SANW/PET film. Ra indicates the mean surface roughness, calculated on 5 x 5 µm2 area. (a–d) scale bar = 100 nm and (e–h) scale bar = 1 µm.
3.2. Electrical and optical properties Figure 3a shows the change in the sheet resistance of the Ag NW films with the roll temperature during both wet and dry sintering processes. In the dry sintering process, the sheet resistance shows little change up to 120 °C, after which it gradually decreases with increasing temperature. The sheet resistance is reduced by ~10.5% from 38.9 to 34.8 Ω/□ at 140 °C. This result is consistent with those of the previous reports wherein the sintering of Ag NWs occurred in the temperature range 140 °C–180 °C.39 However, such a high-temperature sintering method is unsuitable for its application to flexible substrates comprising polymer materials having a low melting point of 280 °C or less.
12
ACS Paragon Plus Environment
Page 12 of 47
Page 13 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Figure 3. (a) Variation in sheet resistances of Ag NW films fabricated by dry and wet sintering processes and (b) sheet resistance vs. relative transmittance (at 550 nm) compared with Ag NWs (in this work) and previously reported Ag NWs prepared via sintering.
In the wet sintering process, the sheet resistance drastically decreases from 38.9 to 15.6 Ω/□ in the roll temperature range 20 °C–120 °C. The first step decrease in the sheet resistance is 18.3% between 40 and 80 °C. The second step decrease in the sheet resistance is a significant 13
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
reduction of 55.0% in the temperature range 80 °C–100 °C, where a phase transition from liquid to vapor occurs, unlike the case of the dry sintering process. This result indicates that the NWs are softened and sintered with the aid of LVP. The last step decrease is a slight reduction up to 59.6% in the temperature range 100 °C–120 °C, followed by a resistance increase as the temperature rises to 140 °C. Compared to the dry sintering process, the reduction in the sheet resistance in the wet sintering process is much greater, indicating that sintering is complete at a much lower temperature of 100 °C. The GO/SANW film shows almost the same sheet resistance decrease up to 120 °C but shows no change in the sheet resistance at higher temperatures. This is attributed to the fact that as GO is coated onto the SANW/PET substrate, the adhesion of the NWs to the substrate is increased so that the NWs do not peel off from the substrate under a relatively high vapor pressure at 140 °C. Figure 3b compares the sheet resistances of pristine Ag NWs, the Ag NWs prepared by wet sintering, and the Ag NWs produced using previously reported methods, including hightemperature sintering,40 mechanical pressing,42 and light-induced welding,44,45. The sheet resistances of the A/GO/SANW and A/RGO/SANW films prepared via wet sintering slightly increase as the relative transmittance increases, whereas the sheet resistances of the pristine Ag NWs and Ag NWs from previous studies tend to significantly increase at a relative transmittance that was greater than 75% (except that prepared via light-induced welding). Compared with the films prepared using the previously reported methods other than lightinduced welding, the films prepared via wet sintering are superior in terms of sheet resistance to relative transmittance. However, the wet sintering method is superior to the light-induced welding method in terms of commercialization and mass production because it may be applied to roll-to-roll processing. 14
ACS Paragon Plus Environment
Page 14 of 47
Page 15 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Figure 4a shows a plot of relative transmittance vs. the amount of GO coated onto SANW. For typical coating methods, the relative transmittance tends to decrease as the concentration of the solution increases. However, as shown in Figure 4a, the relative transmittance improves as the GO content increases. When the 0.5 wt% GO-coated SANW film was coated with the acrylic polymer, no change was observed in the relative transmittance. Thus, the acrylic polymer has high transparency and no effect on overall transmittance. However, the relative transmittance of the A/RGO (0.5 wt%)/SANW film was slightly lowered by reducing the GO layer in the A/GO (0.5 wt%)/SANW film.
Figure 4. (a) Relative transmittance values of Ag NW films with GO and acrylic polymer coatings at 550 nm, (b) Relative transmittance and reflectance values of Ag NW films, (c–g) SEM images of GO-coated Ag NW EMI shielding films with different GO contents: (c) 0%, 15
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
(d) 0.05%, (e) 0.2%, and (f and g) 0.5%. (h) SEM image of the A/GO (0.5 wt%)/SANW EMI shielding film. □ and ○ represent the relative transmittance and relative reflectance of pristine Ag NWs, respectively, in (b).
Figure 4b shows a plot of the relative transmittance and reflectance values of the films vs. GO concentration. The results show that the relative transmittance improves as the GO concentration increases. The relative transmittance improves because light loss is reduced with the commensurate decrease in relative reflectance. The relative reflectance gradually decreases depending on the GO concentration, which is confirmed by the SEM images in Figures 4c–4f. The relative transmittance of the 0.05 wt% GO-coated Ag NWs increases by 3% from that of pristine Ag NWs (79.6%) to 82.6%. As shown in Figure 4d, the fraction of the Ag NWs not covered by GO is more than 40%. In the case of the 0.2 wt% GO-covered NWs shown in Figure 4e, the relative transmittance is increased to 84.5% and the SEM image shows that the uncovered area of the sample is less than 5%. The relative transmittance of the 0.5 wt% GO-coated Ag NWs is further increased to 86.7%. The SEM images in Figures 4f, 4g, and 4f confirm that the GO and acrylic coating layers cover all the Ag NW surfaces in this sample. To suppress reflectivity, the refractive indexes of the component layers should be controlled such that the light reflected from the Ag NWs and that from the overcoat layer interfere with each other. Thus, the larger the GO coverage, which has a refractive index different from that of the Ag NWs, the higher the increase in transmittance. In addition, reflectance is also influenced by the surface roughness and the incident angle of the light. The SEM images in Figures 2d, 2h, and 4f show that the surface of the acrylic coating layer comprises 16
ACS Paragon Plus Environment
Page 16 of 47
Page 17 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
nanoparticles and is therefore not smooth. Thus, reflectance is further reduced by the acrylic coating layer. 3.3. EMI shielding performance Figures 5a–5c show the reflection loss, absorption loss, and total EMI SE of the Ag NW EMI shielding films fabricated using each method.
17
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 47
Figure 5. (a) Reflection loss, (b) absorption loss, (c) total EMI shielding effectiveness (SE) of Ag NW EMI shielding films, and (d) comparison of total EMI SE vs. optical transmittance (at 550 nm) for Ag NW films and other EMI shielding films.
In this case of a good conductor, SE and SE are approximately given by equations 7 and 8, R
A
respectively.53,54
SE ∝ 10 log " R
σ# % µ# $
(7)
SE ∝ t'σ( µ( f
(8)
A
SE
R
at the interface between two media is related to the difference in characteristic
impedances between the incident wave and the surface of the shield. Since the relative permeability µr of nonmagnetic silver is 1, SE is logarithmically proportional to the relative R
electrical conductivity σr, as shown in equation 7. SE
A
is directly proportional to the
thickness of the shield and proportional to the square root of σr, as shown in equation 8. Thus, the total EMI SE of the Ag NW film can be improved by decreasing the ohmic resistance between the NWs. For RGO or CNT containing nanocomposites51,54 that are not good conductors, the EMI shielding effectiveness should be taken into account magnetic permeability and dielectric permittivity. Figure 5a shows that the SE values of the pristine Ag NWs and A/GO/SANW before and R
after the wet sintering process increase by 2.1 times from 4.1 to 8.6 dB (at 1 GHz) at the same 18
ACS Paragon Plus Environment
Page 19 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
optical transmittance (90.3%). For GO/SANW, A/SANW, and A/GO/SANW with sintered Ag NWs coated with acrylic polymer and GO, the SE values of the coatings show little R
dependence on frequency at 0.1–3 GHz. Figure 5b shows that the SE value of SANW A
increases by approximately 1.5 times from 9.4 to 13.9 dB as compared to that of the pristine Ag NWs at the same optical transmittance (90.3%). In addition, with improved optical transmittance, the SE value for A/GO/SANW (or A/SANW) increases by approximately 1.6 A
times from 9.4 to 15.5 dB as compared to that of the pristine Ag NWs. Electrical conductivity can be calculated as shown in equation 9:
* = ,,
(9)
+
where * is the electrical conductivity (S/m), Rs is the sheet resistance (Ω/□), and t is the thickness of the sample (m). The increase in SE for the pristine Ag NWs and SANW is due A
to the decrease in sheet resistance from 39.0 to 17.3 Ω/□ and the decrease in the thickness of the Ag NWs from 115.2 to 64.1 nm by wet sintering and σ increasing significantly by 3.6 times from 3.5 × 105 to 12.6 × 105 S/m. Furthermore, as shown in Figures 4a and 4b, the optical relative reflectance increases from 60% to 80% upon wet sintering when compared to those of the pristine Ag NWs and SANW. This result is consistent with the tendency of good conductors to exhibit increased EM reflectance and decreased EM absorbance when the electrical conductivity is improved, as depicted in Supplementary Figure S1a and S1b. Figure 5c shows that the SE values of SANW, A/RGO/SANW, and A/GO/SANW increase by T
approximately 1.5, 1.7, and 1.8 times upon wet sintering as compared to that of the pristine Ag NWs at the same optical transmittance. In particular, as shown in Supplementary Figure 19
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
S3, the SET value of A/GO/SANW shows little change with frequency even at 8–18 GHz, indicating that the transparent film is applicable as a material for shielding devices at a wide range of radio frequencies.
Figure 5d and Table 1 shows the total EMI SE values of various shielding materials reported in the literature and those of the Ag NW EMI shielding films prepared herein. The total EMI SE values of the Ag NW films prepared herein are much higher than those of the other shielding materials at the same transmittance (except for that of the graphene/metal mesh with almost the same EMI SE value).
3.4. Flexibility and durability Figure 6a shows the changes in the resistance changes of Ag NW EMI shielding films with optical relative transmittance and ROC. For the pristine Ag NWs, ∆R/R0 increases as the ROC decreases and the optical relative transmittance increases. The optical relative transmittance of the Ag NWs decreases as the surface density of the NWs increases and the networking property is enhanced. Thus, as the NW density increases and the friction between the NWs increases, the stresses exerted on the NWs are dispersed and the threshold ROC is reduced. Consequently, Ag NWs with enhanced networking property have high flexibility; however, their optical transmittance is decreased.
20
ACS Paragon Plus Environment
Page 20 of 47
Page 21 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Table 1. Comparison of the total electromagnetic interference (EMI), shielding effectiveness (SE), and optical transmittance of silver (Ag) nanowire (NW) EMI shielding materials at different optical transmittance values
EMI shielding materials
Frequency (GHz)
SET (dB)
Al-doped ZnO
0.3−1.5
6.5
Relative transmittance (%) 84.2
Metal mesh
8−12
20.0
88.2
21
Triangular ring metal mesh
12−18
17−21
95
22
Monolayer graphene
2.2−7
2.3
97
23
RGO
0.5−8.5
6.4
62
24
Multi-layer graphene
18–26.5
19.1
80.5
25
Graphene/metal-mesh
12−18
14.1
90.5
26
PMMA-graphene/metal-mesh
12−18
23.6−28.9
91
27
Graphene/metal-mesh/dielectric
26.5
34.5
85
56
Ag NWs
8−12
12.5−16.0
80
34
PES/Ag NWs/PET
8−12
16
85
36
CA/Ag NW/polyurethane
8−12
20.7
92
14
ITO
0.5−3
14.0
84.1
In this study
Pristine Ag NWs
0.5−3
13.5
90.3
In this study
SANW
0.5−3
20.4
90.3
In this study
A/GO/SANW
0.5−3
24.1
90.3
In this study
A/GO/SANW
0.5−3
28.0
85.2
In this study
A/GO/SANW
0.5−3
30.1
80.3
In this study
A/RGO/SANW*
0.5−3, 8−18
23.9
84.9
In this study
A/RGO/SANW
0.5−3
24.1
82.5
In this study
Ref. 20
*: SET at 8-18 GHz is shown in Supplementary Figure S3.
21
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 6. (a and b) Resistance changes (∆R/R0) of the Ag NW EMI shielding films with radius of curvature (ROC) and optical relative transmittance (at 550 nm), (c, d, f, g, i, and j) infrared (IR) thermographs, and (e, h, and k) SEM images of each Ag NW film (90.4% at 550 nm; applied voltage = 1.5 V) before and after bending at ROC = 1.35 mm. (c–e) Pristine Ag NW film, (f–h) SANW film, and (i–k) A/GO/SANW film.
The SANW film with sintered NWs has flexibility higher than that of the pristine Ag NW film at the same optical transmittance, as shown in Figure 6b. This result is also evident in Table 2, showing that the threshold ROC decreases from 2.1 to 1.2 mm. As shown in Figure 6b and Table 2, for A/GO/SANW with enhanced adhesion to substrates with acrylic polymer and GO coatings, the threshold ROC is dramatically decreased to 0.4 mm. These results demonstrate that the decrease in the critical threshold ROC value at the same optical transmittance is due to the effect of increased thickness or the adhesion force and not the 22
ACS Paragon Plus Environment
Page 22 of 47
Page 23 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
surface density of the Ag NWs. The thickness of the acrylic polymer overcoat layer was measured to be 100–150 nm, indicating that this layer was considerably thin. Therefore, the effect of the thickness of the overcoat layer on decreasing the threshold ROC is negligible.30 Consequently, the threshold ROC reduction is attributed to an increase in adhesion between the substrate and the Ag NWs by the overlayer coating.
Table 2. Threshold radius of curvatures (ROCs) and relative transmittances of the Ag NW EMI shielding films
2.1
Relative transmittance (%) 90.4
1.7
84.5
1.4
76.5
SANW
1.2
90.2
GO/SANW
1.2
90.4
A/SANW
1
90.3
0.4
90.4
0.42
84.2
0.31
78.9
0.44
83.7
Threshold ROC (mm)
Ag NW EMI shielding film
Pristine Ag NWs
A/GO/SANW
A/RGO/SANW
The threshold ROC reduction was confirmed by the IR and SEM images that depict the image during the time at which electricity is applied after bending and restretching the film. Figures 6c and 6d show the thermal image and heat distribution, respectively, of the pristine 23
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Ag NW film after bending at an of ROC of 1.35 mm. The temperature of the bent area in the bent and restretched film was measured to be 23.3 °C (Figure 6d), whereas that of the rest of the film was measured to be below 26.5 °C (Figure 6c). Figure 6e shows that the cause of the increased resistance is that the NWs are stressed upon exceeding the threshold ROC and are fractured at the bending edge. As shown in Figure 6f, the surface temperature is ~5 °C higher than that of the pristine Ag NW film at the same optical transmittance (90.4%). This result demonstrates that the resistance of the Ag NWs is reduced by wet sintering. Joule heating is a process wherein the energy of an electric current is converted into heat as it flows through a resisting material. Therefore, when the resistance is decreased, the heating property is improved. Figure 6g shows the surface temperature of the SANW film. The temperature of the bent area was measured to be 35.5 °C, while that of the rest of the film was measured to be 35.2 °C and 34.8 °C. Figure 6h shows that the NWs were not fractured at the ROC same as that of the pristine Ag NWs (1.35 mm). This result demonstrates that the flexibility of Ag NWs is improved by wet sintering. Figure 6j shows the IR image of the A/GO/SANW film bent at an ROC of 1.35 mm. The surface temperature of the bent area of the A/GO/SANW film was measured to be 37.3 °C, while that of the rest of the film was 35.6 °C. The resistance is not changed even at the same ROC, and the A/GO/SANW film has the same temperature distribution throughout. Thus, the flexibility of Ag NW EMI SE films is dramatically improved by the NW sintering effect and enhanced adhesion to the substrate by the acrylic polymer and GO coatings. Figure 7a shows the results of the taping tests performed with 3M scotch tape, which were used to assess the adhesion between the substrate and the coating layers. The resistance of the 24
ACS Paragon Plus Environment
Page 24 of 47
Page 25 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
pristine Ag NWs increases by ~19% for the 1-N taping test, whereas that for the 5-N taping test increases by 65% for 5 N. Beyond 10 N, the resistance converges to infinity. For the SANW film, a 10% increase in resistance is observed in the 10-N taping test. This result shows that wet sintering improves adhesion to the substrate. The GO/SANW, A/SANW, and A/GO/SANW films showed no change in the resistance, even in the 10-N taping test, because the adhesion to the substrate is improved considerably by the acrylic polymer and GO coatings.
Figure 7. (a) Resistance changes (∆R/R0) of the Ag NW EMI shielding films (T = 90.3%; at 550 nm) after taping test with number of cycles (N). (b) Constant temperature and humidity (85 °C/85% RH) test results. (c) Contact angles of Ag NW EMI shielding films: (c1) Pristine Ag NWs, (c2) SANW, (c3) GO/SANW, (c4) RGO/SANW, (c5) A/SANW, and (c6) A/GO/SANW.
25
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 7b shows the changes in resistance with time for each Ag NW EMI shielding film under the same humidity and temperature conditions (85 °C/85% RH). The resistance of the pristine Ag NWs slightly decreases until 72 h and then increases by 50% at 120 h, followed by an increase to 410% at 500 h. The decrease in the resistance until 48 h is thought to be due to the effect of humidity, which reduces the contact resistance by softening the PVP, an impurity remaining in the NW.42 An interesting result is that the resistance of GO/SANW, which is expected to exhibit low water permeability, becomes almost infinite after 24 h. Conversely, the resistance of the A/GO/SANW film remains unchanged after 500 h. Furthermore, the resistance of the A/SANW film only exhibited a slight change. Figure 7c shows the water contact angles of the films, which reflect their hydrophilicities. The contact angles of the pristine Ag NW, SANW, GO/SANW, RGO/SANW, A/SANW, and A/GO/SANW films are 33.5°, 47.86°, 59.6°, 77.6°, 86.1°, and 86.3° respectively. The pristine Ag NWs have a hydrophilic PVP coating and a low contact angle because moisture can easily penetrate into the void space between the NWs. In the case of the SANW film, hydrophilic PVP is partially removed upon wet sintering and the contact angle is improved by 42%. Unlike hydrophilic GO,55 RGO is hydrophobic. Thus, GO absorbs moisture under constant humidity conditions and promotes Ag NW oxidation over 500 h. Conversely, the hydrophobic acrylic polymer coating on A/SANW and A/RGO/SANW effectively prevents Ag NW oxidation. Figure 8 shows the SE value of each Ag NW film under constant humidity conditions. Similar to the changes in resistance, the SE value of the SANW film decreases with time: the SE value reduces by 28% after 360 h and by 68% after 500 h. For the GO/SANW film, Ag NW oxidation is promoted by GO and the SE value decreases by 100% after 120 h. 26
ACS Paragon Plus Environment
Page 26 of 47
Page 27 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Conversely, the SE values of A/SANW and A/RGO/SANW remain nearly unchanged, even after 500 h, which is consistent with the results of the 85 °C/85% RH tests shown in Figure 7b.
Figure 8. Total SE change (∆SET/SET0) of the Ag NW EMI shielding films after constant temperature and humidity (85 °C/85% RH) tests.
27
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
4. CONCLUSIONS Herein, an LVP-assisted wet sintering of Ag NWs for a highly bendable, durable, and transparent EMI shielding film was presented. Using this process, the sintering temperature can be lowered to strengthen network formation between the NWs, thereby effectively reducing their contact resistance. Consequently, the electrical conductivity of the Ag NW EMI shielding film was significantly improved compared to that of pristine Ag NWs and the SE value was considerably improved from 13.5 to 24.1 dB at a transmittance of 90.3%. The threshold ROC of the Ag NW EMI shielding film was significantly reduced from 2.1 to 0.31 mm owing to the increased adhesion to the substrate imparted by the acrylic polymer and GO (or RGO) multilayer coatings. In addition, the AR effect of A/GO/SANW (or A/RGO/SANW) multilayers with different refractive indexes significantly reduced the reflectance of the Ag NW film, improving the transmittance by 7%. Owing to the water repellency of the acrylic polymer coating, the EMI SE value of the Ag NW film remained almost unchanged for 500 h under 85 °C/85% RH conditions. The Ag NW EMI SE film fabricated via LVP-assisted wet sintering can be mass produced by the roll-to-roll process and has high durability and flexibility. In addition, the Ag NW EMI shielding film has an excellent SE value and high transmittance, making it highly applicable to devices, including flexible displays, flexible touchscreen panels, and wearable devices.
28
ACS Paragon Plus Environment
Page 28 of 47
Page 29 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
ACKNOWLEDGMENTS This material is based upon work performed by the Clean Energy Research Center, supported through the Korea Institute of Science and Technology under Award Grant No. 2E28350.
ASSOCIATED CONTENT Supporting Information Figures S1, S2, and S3 provided in the Supporting Information document (.pdf file).
List of Supplementary Figures
Supplementary Figure S1. EM reflectance, absorbance, and transmittance of Ag NW EMI shielding films (T = 90.3 %; at 550 nm). Supplementary Figure S2. Image of the radius of curvature (ROC) bending tester; a schematic of ROC. Supplementary Figure S3. Total EMI SE of A/RGO/SANW EMI shielding film at 8–18 GHz.
AUTHOR INFORMATION Corresponding Author *E-mail:
[email protected]. Phone: +82-2-958-5526. Fax: +82-2-958-5219
29
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
REFERENCES (1) Chen, J.; Liu, C. T. Technology Advances in Flexible Displays and Substrates. IEEE
Access 2013, 1, 150–158. (2) Khan, Y.; Ostfeld, A. E.; Lochner, C. M.; Pierre, A.; Arias, A. C. Monitoring of Vital Signs with Flexible and Wearable Medical Devices. Adv. Mater. 2016, 28, 4373–4395. (3) Pang, H.; Rajan, K.; Silvernail, J.; Mandlik, P.; Ma, R.; Hack, M.; Brown, J. J.; Yoo, J. S.; Jung, S.-H.; Kim, Y.-C. In Recent Progress of Flexible AMOLED Displays, Advances in Display Technologies; and E-papers and Flexible Displays, International Society for Optics and Photonics, Feb 3, 2011; p 79560J. (4) Rogers, J. A.; Someya, T.; Huang, Y. Materials and Mechanics for Stretchable Electronics.
Science 2010, 327, 1603–1607. (5) Torres Alonso, E.; Karkera, G.; Jones, G. F.; Craciun, M. F.; Russo, S. Homogeneously Bright, Flexible, and Foldable Lighting Devices with Functionalized Graphene Electrodes.
ACS Appl. Mater. Interfaces 2016, 8, 16541–16545. (6) Yang, L.; Wang, S; Feng, J. Advances in electromagnetic interference modeling and noise reduction for adjustable speed motor drive systems. IEEE International Symposium on
Electromagnetic Compatibility & Signal/Power Integrity (EMCSI) 7–11 Aug 2017, 249–254. (7) Sudo, T; Sasaki, H; Masuda, N; Drewniak, J. L; Electromagnetic interference (EMI) of system-on-package (SOP). IEEE Trans. Adv. Packaging 2004, 27, 304–314. (8) Chauhan, P; Verma, H. N; Sisodia, R; Kesari K. K; Microwave radiation (2.45 GHz)induced oxidative stress: Whole-body exposure effect on histopathology of Wistar rats. J.
Electromagn. Bio. Med. 2017, 36, 20–30. 30
ACS Paragon Plus Environment
Page 30 of 47
Page 31 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
(9) Fragopoulou, A. F; Samara, A; Antonelou, M. H; Xanthopoulou, A; Papadopoulou, A; Vougas, K; Koutsogiannopoulou, E; Anastasiadou, E; Stravopodis, D. J; Tsangaris, G. Th. Margaritis, L. H; Brain proteome response following whole body exposure of mice to mobile phone or wireless DECT base radiation. J. Electromagn. Bio. Med. 2017, 31, 250–274. (10) Dasdag, S; Taş, M; Akdag M. Z; Yegin, K; Effect of long-term exposure of 2.4 GHz radiofrequency radiation emitted from Wi-Fi equipment on testes functions. J. Electromagn.
Bio. Med. 2015, 34, 37–42. (11) Chen, Z.; Xu, C.; Ma, C.; Ren, W.; Cheng, H. M. Lightweight and Flexible Graphene Foam Composites for High-performance Electromagnetic Interference Shielding. Adv. Mater. 2013, 25, 1296–1300. (12) Wen, B.; Cao, M.; Lu, M.; Cao, W.; Shi, H.; Liu, J.; Wang, X.; Jin, H.; Fang, X.; Wang, W.; Yuan, J.; Reduced Graphene Oxides: Light-Weight and High-Efficiency Electromagnetic Interference Shielding at Elevated Temperatures. Adv. Mater. 2014, 26, 3484–3489. (13) Kang, J.; Kim, D.; Kim, Y.; Choi, J.-B.; Hong, B. H.; Kim, S. W. High-performance Near-field Electromagnetic Wave Attenuation in Ultra-thin and Transparent Graphene Films.
2D Mater. 2017, 4, 025003. (14) Jia, L.-C.; Yan, D.-X.; Liu, X.; Ma, R.; Wu, H.-Y.; Li, Z.-M. Highly Efficient and Reliable Transparent Electromagnetic Interference Shielding Film. ACS Appl. Mater.
Interfaces 2018, 10(14), 11941–11949. (15) Bora, P. J.; Lakhani, G.; Ramamurthy, P. C.; Madras, G. Outstanding electromagnetic interference shielding effectiveness of polyvinylbutyral–polyaniline nanocomposite film.
RSC Adv. 2016, 6, 79058–79065. 31
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
(16) Bora, P. J.; Vinoy, K. J.; Ramamurthy, P. C.; Kishore; Madras, K. G. Electromagnetic interference shielding effectiveness of polyaniline-nickel oxide coated cenosphere composite film. Compos. Comm. 2017, 4, 37–42. (17) Kim, S. W; Lee, J. H; Kim, Y. B; Lee, K. S. Attenuation characteristics of near-field electromagnetic noise through microstrip line for magnetic absorbers with different levels of conductivity. J. Appl. Phys. 2008, 103, 07E733. (18) Kim, S. W; Lee, J. H. Estimation of high-frequency loss properties through analytical calculation for semiconducting soft magnetic films in a near-field electromagnetic wave. J.
Appl. Phys. 2009, 105, 07A529. (19) Huang, J.-L.; Yau, B.-S.; Chen, C.-Y.; Lo, W.-T.; Lii, D.-F. The Electromagnetic Shielding Effectiveness of Indium Tin Oxide Films. Ceram. Int. 2001, 27, 363–365. (20) Choi, Y.-J.; Gong, S. C.; Johnson, D. C.; Golledge, S.; Yeom, G. Y.; Park, H.-H. Characteristics of the Electromagnetic Interference Shielding Effectiveness of Al-doped ZnO Thin Films Deposited by Atomic Layer Deposition. Appl. Surf. Sci. 2013, 269, 92–97. (21) Vishwanath, S. K.; Kim, D.-G.; Kim, J. Electromagnetic Interference Shielding Effectiveness of Invisible Metal-mesh Prepared by Electrohydrodynamic Jet Printing. Jpn. J.
Appl. Phys. 2014, 53, 05HB11. (22) Wang, H.; Lu, Z.; Tan, J. Generation of Uniform Diffraction Pattern and High EMI Shielding Performance by Metallic Mesh Composed of Ring and Rotated Sub-ring Arrays.
Opt. Express 2016, 24, 22989–23000.
32
ACS Paragon Plus Environment
Page 32 of 47
Page 33 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
(23) Hong, S. K.; Kim, K. Y.; Kim, T. Y.; Kim, J. H.; Park, S. W.; Kim, J. H.; Cho, B. J. Electromagnetic
Interference
Shielding
Effectiveness
of
Monolayer
Graphene.
Nanotechnology 2012, 23, 455704. (24) Kim, S.; Oh, J.-S.; Kim, M.-G.; Jang, W.; Wang, M.; Kim, Y.; Seo, H. W.; Kim, Y. C.; Lee, J.-H.; Lee, Y. Electromagnetic Interference (EMI) Transparent Shielding of Reduced Graphene Oxide (RGO) Interleaved Structure Fabricated by Electrophoretic Deposition. ACS
Appl. Mater. Interfaces 2014, 6, 17647–17653. (25) Lu, Z.; Ma, L.; Tan, J.; Wang, H.; Ding, X. Transparent Multi-layer Graphene/Polyethylene Terephthalate Structures with Excellent Microwave Absorption and Electromagnetic Interference Shielding Performance. Nanoscale 2016, 8, 16684–16693. (26) Han, Y.; Liu, Y.; Han, L.; Lin, J.; Jin, P. High-performance Hierarchical Graphene/Metal-mesh Film for Optically Transparent Electromagnetic Interference Shielding.
Carbon 2017, 115, 34–42. (27) Ma, L.; Lu, Z.; Tan, J.; Liu, J.; Ding, X.; Black, N.; Li, T.; Gallop, J.; Hao, L. Transparent Conducting Graphene Hybrid Films to Improve Electromagnetic Interference (EMI) Shielding Performance of Graphene. ACS Appl. Mater. Interfaces 2017, 9, 34221– 34229. (28) Kumar, A.; Zhou, C. The Race to Replace Tin-doped Indium Oxide: Which Material will Win? ACS Nano 2010, 4, 11–14. (29) Leterrier, Y.; Medico, L.; Demarco, F.; Månson, J.-A.; Betz, U.; Escola, M.; Olsson, M. K.; Atamny, F. Mechanical Integrity of Transparent Conductive Oxide Films for Flexible Polymer-based Displays. Thin Solid Films 2004, 460, 156–166. 33
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
(30) Kim, D.; Kim, S.-H.; Kim, J. H.; Lee, J.-C.; Ahn, J.-P.; Kim, S. W. Failure Criterion of Silver Nanowire Electrodes on a Polymer Substrate for Highly Flexible Devices. Sci. Rep. 2017, 7, 45903. (31) Khan, A.; Lee, S.; Jang, T.; Xiong, Z.; Zhang, C.; Tang, J.; Guo, L. J.; Li, W. D. Highperformance Flexible Transparent Electrode with an Embedded Metal Mesh Fabricated by Cost-effective Solution Process. Small 2016, 12, 3021–3030. (32) Song, M.; You, D. S.; Lim, K.; Park, S.; Jung, S.; Kim, C. S.; Kim, D. H.; Kim, D. G.; Kim, J. K.; Park, J. Highly Efficient and Bendable Organic Solar Cells with Solutionprocessed Silver Nanowire Electrodes. Adv. Funct. Mater. 2013, 23, 4177–4184. (33) Lee, M.-S.; Lee, K.; Kim, S.-Y.; Lee, H.; Park, J.; Choi, K.-H.; Kim, H.-K.; Kim, D.-G.; Lee, D.-Y.; Nam, S. High-performance, Transparent, and Stretchable Electrodes Using Graphene–metal Nanowire Hybrid Structures. Nano Lett. 2013, 13, 2814–2821. (34) Jin, J.; Lee, J.; Jeong, S.; Yang, S.; Ko, J.-H.; Im, H.-G.; Baek, S.-W.; Lee, J.-Y.; Bae, B.-S. High-performance Hybrid Plastic Films: A Robust Electrode Platform for Thin-film Optoelectronics. Energy Environ. Sci. 2013, 6, 1811–1817. (35) Lee, S. J.; Kim, Y.-H.; Kim, J. K.; Baik, H.; Park, J. H.; Lee, J.; Nam, J.; Park, J. H.; Lee, T.-W.; Yi, G.-R. A Roll-to-roll Welding Process for Planarized Silver Nanowire Electrodes.
Nanoscale 2014, 6, 11828–11834. (36) Hu, M.; Gao, J.; Dong, Y.; Li, K.; Shan, G.; Yang, S.; Li, R. K.-Y. Flexible Transparent PES/Silver Nanowires/PET Sandwich-structured Film for High-efficiency Electromagnetic Interference Shielding. Langmuir 2012, 28, 7101–7106.
34
ACS Paragon Plus Environment
Page 34 of 47
Page 35 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
(37) Lee, J.; Lee, I.; Kim, T. S.; Lee, J. Y. Efficient Welding of Silver Nanowire Networks Without Post-processing. Small 2013, 9, 2887–2894. (38) Kim, S.; Kim, S. Y.; Kim, J.; Kim, J. H. Highly reliable AgNW/PEDOT:PSS hybrid films: efficient methods for enhancing transparency and lowering resistance and haziness. J.
Mater. Chem. C. 2014, 2, 5636–5643. (39) Giusti, G.; Langley, D. P.; Lagrange, M.; Collins R.; Jimenez C.; Brechet, Y.; Bellet, D. Thermal annealing effects on silver nanowire networks. Int. J. Nanotechnol. 2014, 11, 785– 795. (40) Lee, J.-Y.; Connor, S. T.; Cui, Y.; Peumans, P. Solution-processed Metal Nanowire Mesh Transparent Electrodes. Nano Lett. 2008, 8, 689–692. (41) Lee, P.; Lee, J.; Lee, H.; Yeo, J.; Hong, S.; Nam, K. H.; Lee, D.; Lee, S. S.; Ko, S. H., Highly Stretchable and Highly Conductive Metal Electrode by Very Long Metal Nanowire Percolation Network. Adv. Mater. 2012, 24, 3326–3332. (42) Hu, L.; Kim, H. S.; Lee, J.-Y.; Peumans, P.; Cui, Y. Scalable Coating and Properties of Transparent, Flexible, Silver Nanowire Electrodes. ACS Nano 2010, 4, 2955–2963. (43) Weiß, N.; Muller-Meskamp, L.; Selzer, F.; Bormann, L.; Eychmuller, A.; Leo, K.; Gaponik, N. Humidity assisted annealing technique for transparent conductive silver nanowire networks. RSC Adv. 2015, 5, 19659–19665. (44) Park, J. H.; Hwang, G. T.; Kim, S.; Seo, J.; Park, H. J.; Yu, K.; Kim, T. S.; Lee, K. J. Flash-induced Self-limited Plasmonic Welding of Silver Nanowire Network for Transparent Flexible Energy Harvester. Adv. Mater. 2017, 29.
35
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
(45) Garnett, E. C.; Cai, W.; Cha, J. J.; Mahmood, F.; Connor, S. T.; Christoforo, M. G.; Cui, Y.; McGehee, M. D.; Brongersma, M. L. Self-limited Plasmonic Welding of Silver Nanowire Junctions. Nat. Mater. 2012, 11, 241–249. (46) Gaynor, W.; Burkhard, G. F.; McGehee, M. D.; Peumans, P. Smooth Nanowire/Polymer Composite Transparent Electrodes. Adv. Mater. 2011, 23, 2905–2910. (47) Kwon, S.; Ma, R.; Kim, U.; Choi, H. R.; Baik, S. Flexible Electromagnetic Interference Shields Made of Silver Flakes, Carbon Nanotubes and Nitrile Butadiene Rubber. Carbon 2014, 68, 118–124. (48) Robinson, J. T.; Zalalutdinov, M.; Baldwin, J. W.; Snow, E. S.; Wei, Z. Q.; Sheehan P.; Houston, B. H. Wafer-scale Reduced Graphene Oxide Films for Nanomechanical Devices.
Nano Lett., 2008, 8, 3441-3445. (49) Lewis, J. Material Challenge for Flexible Organic Devices. Mater. Today 2006, 9, 38–45. (50) Hong, C.-H.; Oh, S. K.; Kim, T. K.; Cha, Y.-J.; Kwak, J. S.; Shin, J.-H.; Ju, B.-K.; Cheong, W.-S. Electron Beam Irradiated Silver Nanowires for a Highly Transparent Heater.
Sci. Rep. 2015, 5, 17716. (51) Zhang, Y.; Wang, X.; Cao, M. Confinedly implanted NiFe2O4-rGO: Cluster Tailoring and Highly Tunable Electromagnetic Properties for Selective-Frequency Microwave Absorption. Nano Res. 2018, 11, 1426–1436. (52) Zhang, C.-S.; Ni, Q.-Q.; Fu, S.-Y.; Kurashiki, K. Electromagnetic Interference Shielding Effect of Nanocomposites with Carbon Nanotube and Shape Memory Polymer. Compos. Sci.
Technol. 2007, 67, 2973–2980.
36
ACS Paragon Plus Environment
Page 36 of 47
Page 37 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
(53) Ott, H. W. Electromagnetic Compatibility Engineering. New York: John Wiley & Sons, 2009, pp. 245. (54) Saini, P.; Arora, M. Microwave Absorption and EMI Shielding Behavior of Nanocomposites Based on Intrinsically Conducting Polymers, Graphene and Carbon Nanotubes. In: De Souza Gomes, A. ed. New Polymers for Special Applications, InTech: Croatia, 2012; pp. 71–112. (55) Hu, X.; Yu, Y.; Hou, W.; Zhou, J.; Song, L. Effects of Particle Size and pH Value on the Hydrophilicity of Graphene Oxide. Appl. Surf. Sci. 2013, 273, 118–121. (56) Lu, Z.; Ma, L.; Tan, J.; Wang, H.; Ding, X. Graphene, Microscale Metallic Mesh, and Transparent Dielectric Hybrid Structure for Excellent Transparent Electromagnetic Interference Shielding and Absorbing. 2D Materials 2017, 4(2):025021.
37
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
TOC Graphic
38
ACS Paragon Plus Environment
Page 38 of 47
Page 39 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
417x154mm (300 x 300 DPI)
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 1. Schematic of the fabrication of silver (Ag) nanowire (NW) electromagnetic interference (EMI) shielding films: (a) overall fabrication process, (b) wet sintering process using hot rolling system, and (c) an A/RGO/SANW EMI shielding multilayer film obtained from the process. 80x42mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 40 of 47
Page 41 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Figure 2. Scanning electron microscopy (SEM; 15° tilted) and atomic force microscopy (AFM) images of the Ag NW EMI shielding films fabricated via wet sintering process: (a and e) pristine Ag NW/polyethylene terephthalate (PET) film, (b and f) SANW/PET film, (c and g) GO/SANW/PET film, and (d and h) A/GO/SANW/PET film. Ra indicates the mean surface roughness, calculated on 5 x 5 µm2 area. (a–d) scale bar = 100 nm and (e–h) scale bar = 1 µm. 87x50mm (300 x 300 DPI)
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 3. (a) Variation in sheet resistances of Ag NW films fabricated by dry and wet sintering processes and (b) sheet resistance vs. relative transmittance (at 550 nm) compared with Ag NWs (in this work) and previously reported Ag NWs prepared via sintering. 192x251mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 42 of 47
Page 43 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Figure 4. (a) Relative transmittance values of Ag NW films with GO and acrylic polymer coatings at 550 nm, (b) Relative transmittance and reflectance values of Ag NW films, (c–g) SEM images of GO-coated Ag NW EMI shielding films with different GO contents: (c) 0%, (d) 0.05%, (e) 0.2%, and (f and g) 0.5%. (h) SEM image of the A/GO (0.5 wt%)/SAWSANW EMI shielding film. □ and ○ represent the relative transmittance and relative reflectance of pristine Ag NWs, respectively, in (b). 103x71mm (300 x 300 DPI)
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 5. (a) Reflection loss, (b) absorption loss, (c) total EMI shielding effectiveness (SE) of Ag NW EMI shielding films, and (d) comparison of total EMI SE vs. optical transmittance (at 550 nm) for Ag NW films and other EMI shielding films. 109x81mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 44 of 47
Page 45 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Figure 6. (a and b) Resistance changes (∆R/R0) of the Ag NW EMI shielding films with radius of curvature (ROC) and optical relative transmittance (at 550 nm), (c, d, f, g, i, and j) infrared (IR) thermographs, and (e, h, and k) SEM images of each Ag NW film (90.4% at 550 nm; applied voltage = 1.5 V) before and after bending at ROC = 1.35 mm. (c–e) Pristine Ag NW film, (f–h) SANW film, and (i–k) A/GO/SANW film. 83x45mm (300 x 300 DPI)
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 7. (a) Resistance changes (∆R/R0) of the Ag NW EMI shielding films (T = 90.3%; at 550 nm) after taping test with number of cycles (N). (b) Constant temperature and humidity (85 °C/85% RH) test results. (c) Contact angles of Ag NW EMI shielding films: (c1) Pristine Ag NWs, (c2) SANW, (c3) GO/SANW, (c4) RGO/SANW, (c5) A/SANW, and (c6) A/GO/SANW. 89x44mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 46 of 47
Page 47 of 47 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Figure 8. Total SE change (∆SET/SET0) of the Ag NW EMI shielding films after constant temperature and humidity (85 °C/85% RH) tests. 106x74mm (300 x 300 DPI)
ACS Paragon Plus Environment