Aging of Silicon Nanocrystals on Elastomer Substrates

Dec 2, 2016 - Yaozhong Zhang , Daniel C. Ratchford , Rebecca J. Anthony ... Sun , Chenxi Qian , Annabelle P. Y. Wong , Laura M. Reyes , Geoffrey A. Oz...
0 downloads 0 Views 5MB Size
Subscriber access provided by Olson Library | Northern Michigan University

Article

Aging of Silicon Nanocrystals on Elastomer Substrates: Photoluminescence Effects Rajib Mandal, and Rebecca Joy Anthony ACS Appl. Mater. Interfaces, Just Accepted Manuscript • DOI: 10.1021/acsami.6b10155 • Publication Date (Web): 02 Dec 2016 Downloaded from http://pubs.acs.org on December 9, 2016

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

ACS Applied Materials & Interfaces is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 23

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

Aging of Silicon Nanocrystals on Elastomer Substrates: Photoluminescence Effects Rajib Mandal and Rebecca J. Anthony* Department of Mechanical Engineering, Michigan State University, East Lansing, MI 48824, United States KEYWORDS: Silicon, Nanocrystals, PDMS, Photoluminescence, Plasma.

ABSTRACT: Nanocrystalline silicon is widely known as an efficient and tunable optical emitter and is attracting great interest for applications such as light-emitting devices (LEDs), electronic displays, sensors and solar-photovoltaics. To date, however, luminescent silicon nanocrystals have been used exclusively in traditional rigid devices, leaving a gap in knowledge regarding how they behave on elastomeric substrates. The present study shows how the optical and structural/morphological properties of plasma-synthesized silicon nanocrystals (SiNCs) change when they are deposited on stretchable substrates made from polydimethylsiloxane (PDMS). Our results indicate that SiNCs deposited directly from the gas-phase onto PDMS exhibit morphological changes, as well as modified aging characteristics due to enhanced oxidation. These results begin to fill the knowledge gap, and point to the potential of using luminescent SiNC layers for flexible and stretchable electronics such as LEDs, displays and sensors.

ACS Paragon Plus Environment

1

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 23

1. INTRODUCTION Silicon (Si) is one of the most commonly-used semiconductor materials and offers advantages over some other semiconductors in that it is inexpensive, nontoxic, abundant, and has benefitted from decades of experience in purification, growth and device fabrication. Bulk Si is a major contributor in today’s microelectronics,1–3 photonics4–6 and solar-photovoltaics industries.7–10 In addition, new properties and functionalities arise for nanoscale Si, which exhibits efficient and tunable luminescence due to quantum size effects.11–14 Si nanocrystals (SiNCs) have opened the way for new and interesting applications in photovoltaics, photonics, microelectronics and nanobiotech industries.15–17 Additionally, emerging applications involving stretchable and flexible electronics for optoelectronic applications such as in-situ health monitoring, display technology, and inexpensive, versatile LEDs and solar cells are not feasible using bulk semiconductors. Hence, SiNCs offer a huge technological and scientific interest in these areas. In any NC-based application, incorporating the nanocrystals into the device architectures presents a novel challenge, particularly when deformable substrates for flexible/stretchable devices are required. Some groups have had success creating SiNC/elastomer mixed materials starting from the liquid phase, including combining SiNCs and PDMS, to make bulk hybrid NC/elastomers.18,19 When it comes to creating thin layers of NCs on top of substrates, many deposition schemes involve solvent processing (spin- or drop-casting) or high temperatures, which can dissolve or thermally decompose polymer substrates, precluding deposition directly onto elastomers like PDMS. Gas-phase inertial impaction, however, can sidestep many of these issues by allowing NCs to directly impinge upon substrates from the vapor phase, eliminating solvents and high temperatures.20–22 This inertial impaction opens the door to creating next-

ACS Paragon Plus Environment

2

Page 3 of 23

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

generation stretchable and flexible devices using the exciting tunable properties of NCs. Here, we present results on inertial impaction of plasma-produced SiNCs onto elastomer substrates, and the effects of aging on the photoluminescence properties of the resulting SiNC films. This research is the first investigation to our knowledge of inertial impaction of nanomaterials onto elastomeric substrates. 2. EXPERIMENTAL DETAILS Plasma reactor: SiNCs were synthesized using a nonthermal plasma reactor, as has been demonstrated for SiNCs as well as for NCs of other materials including germanium and zinc oxide.11,23–26 A schematic diagram of the plasma reactor is shown in Figure 1. The flow-through reactor consists of a Pyrex tube with an outer diameter (O.D.) of 1.27cm in the top portion and 2.54cm in the bottom portion. The tube is 30.5cm long and the expansion area is 17.8cm from the top. Argon (Ar) and silane (SiH4, 1% in Ar) were flown through the Pyrex tube, and 13.56 MHz radiofrequency (rf) power was supplied via dual ring electrodes encircling the upper portion of the tube. The gas flowrates for Ar and SiH4/Ar were 5-30 sccm and 50-80 sccm respectively. The pressure in the reactor was kept at 1.85-2.7 Torr using a slit-shaped nozzle orifice, and was 160-300 mTorr downstream of the orifice. The slit-shaped orifice at the reactor base accelerated the SiNCs and they inertially impacted onto the substrates underneath.20–22 The described conditions led to the synthesis of crystalline SiNCs of diameter 4-5 nm, as confirmed using transmission electron microscopy (TEM), x-ray diffraction (XRD), and Raman spectroscopy (Figure 1). Sample deposition and storage: SiNCs were deposited via inertial impaction onto polydimethylsiloxane (PDMS) films and bulk silicon wafers. The deposition was performed by

ACS Paragon Plus Environment

3

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 23

rastering the substrates beneath the orifice at a standoff distance of ~3mm. Following synthesis, the samples were stored in air. PDMS preparation: PDMS was prepared in the lab using Sylgard 184 (Dow Corning Corp.). The prepolymer base (PDMS monomer) and the cross linking agent were vigorously mixed in a 10:1 weight ratio, then degassed in a vacuum desiccator for 20-25 minutes until all the air bubbles were removed from the mixture. Pre-measured amounts of the mixture were cast into plastic petri dishes, leading to film thicknesses of ~ 0.5 mm. The PDMS was then heat-cured using a hot plate at 60ºC for 2-3 hrs. The PDMS was cooled at room temperature and cut into small substrates of dimensions 28mm × 12mm. Photoluminescence Measurements: Photoluminescence (PL) measurements were performed using an Ocean Optics, Inc. USB spectrometer and optical fiber. The PL was excited using a UV/blue LED (peak at 395nm). The measurements were performed in air.

ACS Paragon Plus Environment

4

Page 5 of 23

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

Figure 1. (a) Schematic of the Plasma Reactor with (b) TEM image of SiNCs (circles indicate nanocrystallites), (c) XRD pattern, and (d) Raman analysis. The Raman peak is shifted to lower wavenumbers compared to the bulk silicon value (520 cm-1)27 due to the small nanocrystal size. 3. RESULTS AND DISCUSSION We deposited ~1µm layers of SiNCs onto relaxed PDMS substrates as well as silicon wafer substrates to compare the appearance and photoluminescence of the resulting films. For some cases, we also pre-stretched the PDMS substrates using a house-built stretching stage (Figure 2). For our measurements using pre-stretched PDMS, we deposited the SiNCs while the PDMS was stretched and then allowed the PDMS and SiNC films to relax before performing any measurements. Henceforth, we refer to samples produced on prestretched PDMS according to the applied strain during SiNC deposition, meaning the ratio of the length of the PDMS during

ACS Paragon Plus Environment

5

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 6 of 23

the stretching/deposition to its length when relaxed. We produced SiNCs on silicon wafer, relaxed PDMS (0% pre-strain), and PDMS at pre-strain conditions of 10%, 20%, and 40%.

Figure 2. Flowchart showing different steps for PDMS and wafer substrates. The SiNCs as-produced have a nontrivial surface defect density and thus photoluminescence quantum yields of only several percent immediately after deposition.23 Thus, to measure their photoluminescence, we waited 2 days after deposition to allow ambient-air oxidation to begin to cap the defects and increase the samples' PL intensities: as such, oxidation of these SiNC films was our default passivation method. Despite using exactly the same recipe for synthesis, the PL from SiNCs on relaxed (0% prestrain) PDMS was significantly blueshifted in comparison to the PL from SiNCs on silicon wafer (up to 80 nm) (Figure 3a). The PL peak should, in principle, depend on the SiNCs themselves and not their substrate. We also found that the PL peak for the SiNCs on prestretched PDMS actually redshifted back towards the peak position for SiNCs on silicon wafer.

ACS Paragon Plus Environment

6

Page 7 of 23

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

Figure 3. Photoluminescence spectra for (a) SiNCs on relaxed (0%) PDMS and on silicon wafer, (b) SiNCs on PDMS with different pre-strain conditions, and (c) SiNC layers with different thicknesses of SiNCs on relaxed (0%) PDMS films. As the SiNC synthesis recipe was the same for all these samples, we expected the PL peak to remain constant regardless of substrate. Visual analysis via both top-down and cross-sectional

ACS Paragon Plus Environment

7

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 23

SEM images (Figure 4) showed that the Si NC layers on relaxed (0%) PDMS were more densely packed compared to layers on silicon wafer.

Figure 4. SEM images of gas-phase-impacted SiNC films on Si wafer (a, c) and relaxed PDMS (0% strain) (b, d). As a next step, we deposited films of varying thickness on PDMS to investigate any whether the observed PL shift was dependent on layer thickness. Our initial measurements had been made on fairly thick layers (~1µm) which required 100 deposition rastering cycles. We deposited SiNCs on relaxed PDMS with 10 cycles, 50 cycles, and 100 cycles (corresponding to ~100nm, 500nm, and 1µm). PL measurements taken after 2 days showed that the thinner films exhibited even more blueshifting compared to the thicker films. (see Figure 3 c). Again, as the SiNCs are the

ACS Paragon Plus Environment

8

Page 9 of 23

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

same before deposition, this indicated a change that occurred for the NCs as a result of the PDMS substrate and film properties, possibly as a result of modified aging characteristics. Aging is important for SiNCs because they are susceptible to oxidation in ambient conditions. Oxidation of SiNCs causes an SiOx layer to grow at the NC surface, corresponding to a core size shrinkage and blueshifting photoluminescence.28 Increasing the fractional volume of oxidized SiNC films on PDMS compared to on silicon wafer would explain the difference in peak PL wavelength, and would also explain the thickness dependence (thinner films oxidize more rapidly). In order to test this, we needed to eliminate oxygen-exposure and compare the results for the as-produced and air-shielded samples with the results from samples that were aged in air. We made two sets of SiNC films on relaxed (0%) and 20% pre-strained PDMS as well as on Si wafers: one set was stored in a nitrogen-purged glove bag immediately after removal from the reactor, and the second set of films was stored in air. PL from all samples was measured immediately after synthesis and after 2 days of aging to observe whether the oxygen-free environment affected the peak luminescence. The results are shown in Figure 5. For samples stored in the glove bag, the PL peaks overlap on the first day and on subsequent days. For samples stored in air, the peaks began to shift from one another (blueshifting for the samples on PDMS) within a day of synthesis. This confirmed the hypothesis that oxidation is enhanced for SiNC films on PDMS. The air-permeability of PDMS has been demonstrated by previous groups, and thus the SiNC films on PDMS were oxidizing not only from the top but also through the bottom of the films.27,28 The PL measurements are ensemble measurements, collecting light from the entirety of the film thickness – thus, additional oxidation at the back of the films would

ACS Paragon Plus Environment

9

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 10 of 23

lead to blueshifting compared to the films on silicon wafer, which were only oxidizing from the top.

Figure 5. Photoluminescence spectra from oxidation dependence experiment for samples stored in N2-purged glove bag (a and b) and stored in air (c and d). The dependence on pre-strain can be explained by examining the surface of a SiNC film on prestretched PDMS before and after relaxing the substrate. To do this, we deposited SiNCs on a PDMS substrate pre-stretched to 40% of its initial length, and left the substrate and SiNC film in place on the stretching stage while imaging in the scanning electron microscope (SEM). The SEM image shows a fairly flat layer of nanocrystals. Then, we removed the stage and relaxed the film of SiNCs to image it again. After relaxing the substrate, the SiNC film developed wrinkles across its surface. Due to the very thin nature of the SiNC film in comparison with the elastomer

ACS Paragon Plus Environment

10

Page 11 of 23

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

substrate, these instabilities are limited to the surface of the SiNC film as described by Bigoni.31 The surface instabilities cause the SiNC film to be thicker in some places compared to the same thickness SiNC film on relaxed PDMS or on silicon wafer. The increased thickness would result in reduced fraction of SiNCs that are oxidized, compared to the entirety of the film. This explains why increasing stretching ratio causes reduced blueshifting of the PL peak. Figure 6 shows a cartoon of this process.

Figure 6. (a) SEM image showing surface instability formation. (b) Proposed stages of oxidation for samples on PDMS vs. Si wafer.

ACS Paragon Plus Environment

11

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 12 of 23

4. CONCLUSION In conclusion, we have demonstrated the first all-gas-phase deposition of luminescent nanocrystals onto elastomeric substrates. The films showed wrinkling in response to pre-stretch of the PDMS substrates, as well as structural changes compared to SiNCs deposited on Si wafers. The SiNCs on relaxed PDMS exhibited blueshifted luminescence compared to SiNCs on Si wafer, with decreased blueshifting observed for the wrinkled SiNC films which had been deposited on prestretched PDMS. Our experiments indicate that the blueshift effect is due to enhanced oxidation on PDMS, caused by the air-permeability of PDMS and thus oxidation of the SiNC films from all sides as opposed to the top-down-only oxidation that occurs for SiNCs on Si wafers. These results will aid ongoing and future development of stretchable and flexible luminescent NC layers for next-generation displays, LEDs, and other devices.

AUTHOR INFORMATION Corresponding Author *E‒mail: [email protected]. Author Contributions The manuscript was written through contributions of all authors. All authors have given approval to the final version of the manuscript. Funding Sources This work was supported by faculty startup funds provided by Michigan State University’s College of Engineering and Department of Mechanical Engineering. The work was also performed with partial support from NSF CMMI Grant #1561964.

ACS Paragon Plus Environment

12

Page 13 of 23

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

Notes The authors declare no competing financial interest. ACKNOWLEDGMENTS The authors would like to thank Dr. Xudong Fan from Center For Advanced Microscopy, Michigan State University, for his help with TEM analysis. We used Siemens NX 10 to create the reactor schematic (Figure 1a). The authors would also like to thank Michael Bigelow, Duncan

Kroll

and

Naomi

Carlisle

for

their

help

with

schematic

and

sample

preparation/characterization. REFERENCES (1)

Takagahara, T.; Takeda, K. Theory of the Quantum Confinement Effect on Excitons in Quantum Dots of Indirect-Gap Materials. Phys. Rev. B 1992, 46, 15578–15581.

(2)

Proot, J. P.; Delerue, C.; Allan, G. Electronic Structure and Optical Properties of Silicon Crystallites: Application to Porous Silicon. Appl. Phys. Lett. 1992, 61, 1948–1950.

(3)

Ledoux, G.; Guillois, O.; Porterat, D.; Reynaud, C.; Huisken, F.; Kohn, B.; Paillard, V. Photoluminescence Properties of Silicon Nanocrystals as a Function of Their Size. Phys. Rev. B 2000, 62, 15942–15951.

(4)

Maier-Flaig, F.; Rinck, J.; Stephan, M.; Bocksrocker, T.; Bruns, M.; Kübel, C.; Powell, A. K.; Ozin, G. a; Lemmer, U. Multicolor Silicon Light-Emitting Diodes (SiLEDs). Nano Lett. 2013, 13, 475–480.

(5)

Fujita, S.; Sugiyama, N. Visible Light-Emitting Devices with Schottky Contacts on an Ultrathin Amorphous Silicon Layer Containing Silicon Nanocrystals. Appl. Phys. Lett. 1999, 74, 308–310.

(6)

Torre, J. D. La; Souiÿ, A.; Poncet, A.; Busseret, C.; Lemiti, M.; Bremond, G. Optical Properties of Silicon Nanocrystal LEDs. Physica E 2003, 16, 326–330.

(7)

Liu, C.-Y.; Holman, Z. C.; Kortshagen, U. R. Hybrid Solar Cells from P3HT and Silicon Nanocrystals. Nano Lett. 2009, 9, 449–452.

(8)

Tian, B.; Zheng, X.; Kempa, T. J.; Fang, Y.; Yu, N.; Yu, G.; Huang, J.; Lieber, C. M. Coaxial Silicon Nanowires as Solar Cells and Nanoelectronic Power Sources. Nature 2007, 449, 885–890.

ACS Paragon Plus Environment

13

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 14 of 23

(9)

Conibeer, G.; Green, M.; Corkish, R.; Cho, Y.; Cho, E.-C.; Jiang, C.-W.; Fangsuwannarak, T.; Pink, E.; Huang, Y.; Puzzer, T.; Trupke, T.; Richards, B.; Shalav, A.; Lin, K. Silicon Nanostructures for Third Generation Photovoltaic Solar Cells. Thin Solid Films 2006, 511–512, 654–662.

(10)

Timmerman, D.; Izeddin, I.; Stallinga, P.; Yassievich, I. N.; Gregorkiewicz, T. SpaceSeparated Quantum Cutting with Silicon Nanocrystals for Photovoltaic Applications. Nat. Photonics 2008, 2, 105–109.

(11)

Mangolini, L.; Thimsen, E.; Kortshagen, U. High-Yield Plasma Synthesis of Luminescent Silicon Nanocrystals. Nano Lett. 2005, 5, 655–659.

(12)

Canham, L. T. Silicon Quantum Wire Array Fabrication by Electrochemical and Chemical Dissolution of Wafers. Appl. Phys. Lett. 1990, 57, 1046–1048.

(13)

Mangolini, L.; Jurbergs, D.; Rogojina, E.; Kortshagen, U. Plasma Synthesis and LiquidPhase Surface Passivation of Brightly Luminescent Si Nanocrystals. J. Lumin. 2006, 121, 327–334.

(14)

Sangghaleh, F.; Sychugov, I.; Yang, Z.; Veinot, J. G. C.; Linnros, J. Near-Unity Internal Quantum Efficiency of Luminescent Silicon Nanocrystals with Ligand Passivation. ACS Nano 2015, 9, 7097–7104.

(15)

O ’Farrell, N.; Houlton, A.; Horrocks, B. R. Silicon Nanoparticles: Applications in Cell Biology and Medicine. Int. J. Nanomed. 2006, 1, 451–472.

(16)

Fenollosa, R.; Garcia-Rico, E.; Alvarez, S.; Alvarez, R.; Yu, X.; Rodriguez, I.; CarregalRomero, S.; Villanueva, C.; Garcia-Algar, M.; Rivera-Gil, P.; de Lera, A. R.; Parak, W. J.; Meseguer, F.; Alvarez-Puebla, R. A. Silicon Particles as Trojan Horses for Potential Cancer Therapy. J. Nanobiotechnol. 2014, 12, 1–10.

(17)

Timoshenko, V. Y.; Kudryavtsev, A. A.; Osminkina, L. A.; Vorontsov, A. S.; Ryabchikov, Y. V.; Belogorokhov, I. A.; Kovalev, D.; Kashkarov, P. K. Silicon Nanocrystals as Photosensitizers of Active Oxygen for Biomedical Applications. JETP Lett. 2006, 83, 423–426.

(18)

Van Sickle, A. R.; Miller, J. B.; Moore, C.; Anthony, R. J.; Kortshagen, U. R.; Hobbie, E. K. Temperature Dependent Photoluminescence of Size-Purified Silicon Nanocrystals. ACS Appl. Mater. Interfaces 2013, 5, 4233–4238.

(19)

Hohlein, I. M. D.; Werz, P. D. L.; Veinot, J. G. C.; Rieger, B. Photoluminescent Silicon Nanocrystal-Polymer Hybrid Materials via Surface Initiated Reversible AdditionFragmentation Chain Transfer (RAFT) Polymerization. Nanoscale 2015, 7, 7811–7818.

(20)

Di Fonzo, F.; Gidwani, A.; Fan, M. H.; Neumann, D.; Iordanoglou, D. I.; Heberlein, J. V. R.; McMurry, P. H.; Girshick, S. L.; Tymiak, N.; Gerberich, W. W.; Rao, N. P. Focused Nanoparticle-Beam Deposition of Patterned Microstructures. Appl. Phys. Lett. 2000, 77, 910.

ACS Paragon Plus Environment

14

Page 15 of 23

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

(21)

Holman, Z. C.; Kortshagen, U. R. A Flexible Method for Depositing Dense Nanocrystal Thin Films: Impaction of Germanium Nanocrystals. Nanotechnology 2010, 21, 335302.

(22)

Anthony, R. J.; Cheng, K.-Y.; Holman, Z. C.; Holmes, R. J.; Kortshagen, U. R. An AllGas-Phase Approach for the Fabrication of Silicon Nanocrystal Light-Emitting Devices. Nano Lett. 2012, 12, 2822–2825.

(23)

Anthony, R. J.; Rowe, D. J.; Stein, M.; Yang, J.; Kortshagen, U. Routes to Achieving High Quantum Yield Luminescence from Gas-Phase-Produced Silicon Nanocrystals. Adv. Funct. Mater. 2011, 21, 4042–4046.

(24)

Cernetti, P.; Gresback, R.; Campbell, S. A.; Kortshagen, U. Nonthermal Plasma Synthesis of Faceted Germanium Nanocrystals. Chem. Vap. Deposition 2007, 13, 345–350.

(25)

Felbier, P.; Yang, J.; Theis, J.; Liptak, R. W.; Wagner, A.; Lorke, A.; Bacher, G.; Kortshagen, U. Highly Luminescent ZnO Quantum Dots Made in a Nonthermal Plasma. Adv. Funct. Mater. 2014, 24, 1988–1993.

(26)

Jariwala, B. N.; Kramer, N. J.; Petcu, M. C.; Bobela, D. C.; Sanden, M. C. M. Van De; Stradins, P.; Ciobanu, C. V.; Agarwal, S. Surface Hydride Composition of PlasmaSynthesized Si Nanoparticles. J. Phys. Chem. C 2011, 115, 20375–20379.

(27)

Tan, D.; Ma, Z.; Xu, B.; Dai, Y.; Ma, G.; He, M.; Jin, Z.; Qiu, J. Surface Passivated Silicon Nanocrystals with Stable Luminescence Synthesized by Femtosecond Laser Ablation in Solution. Phys. Chem. Chem. Phys. 2011, 13, 20255–20261.

(28)

Liptak, R. W.; Kortshagen, U.; Campbell, S. A. Surface Chemistry Dependence of Native Oxidation Formation on Silicon Nanocrystals. J. Appl. Phys. 2009, 106, 064313-1–5.

(29)

Shiku, H.; Saito, T.; Wu, C.-C.; Yasukawa, T.; Yokoo, M.; Abe, H.; Matsue, T.; Yamada, H. Oxygen Permeability of Surface-Modified Poly(dimethylsiloxane) Characterized by Scanning Electrochemical Microscopy. Chem. Lett. 2006, 35, 234–235.

(30)

Lamberti, A.; Marasso, S. L.; Cocuzza, M. PDMS Membranes with Tunable Gas Permeability for Microfluidic Applications. RSC Adv. 2014, 4, 61415–61419.

(31)

Bigoni, D. Nonlinear Solid Mechanics: Bifurcation Theory and Material Instability, 1st ed.; Cambridge University Press: New York, 2012; 363-365.

ACS Paragon Plus Environment

15

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 16 of 23

TABLE OF CONTENTS GRAPHIC

ACS Paragon Plus Environment

16

Page ACS 17 of Applied 23 Materials & Interfaces

1 2 3 4 5 6 7 8

ACS Paragon Plus Environment

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27

ACS Paragon Plus Environment

Page 18 of 23

Page 19 of 23

1 2 3 4 5 6 7 8 9 10 11 12

ACS Applied Materials & Interfaces

ACS Paragon Plus Environment

ACS Applied Materials & Interfaces Page 20 of 23

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41

ACS Paragon Plus Environment

Page 21 of 23

a

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26

c

ACS Applied Materials & Interfaces

b

d

ACS Paragon Plus Environment

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26

ACS Paragon Plus Environment

Page 22 of 23

Page 23 of 23

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33

ACS Applied Materials & Interfaces

ACS Paragon Plus Environment