Article pubs.acs.org/bc
Degradable Thermoresponsive Nanogels for Protein Encapsulation and Controlled Release Neha Bhuchar,† Rajesh Sunasee,† Kazuhiko Ishihara,‡ Thomas Thundat,† and Ravin Narain*,† †
Department of Chemical and Materials Engineering, University of Alberta, Edmonton, Alberta, T6G 2G6, Canada Department of Materials Engineering and Department of Bioengineering, School of Engineering, The University of Tokyo, 7-3-1, Hongo, Bunkyo-ku, Tokyo 113-8656, Japan
‡
S Supporting Information *
ABSTRACT: Reversible addition−fragmentation chain transfer (RAFT) polymerization technique was used for the fabrication of stable core cross-linked micelles (CCL) with thermoresponsive and degradable cores. Well-defined poly(2methacryloyloxyethyl phosphorylcholine), poly(MPC) macroRAFT agent, was first synthesized with narrow molecular weight distribution via the RAFT process. These CCL micelles (termed as nanogels) with hydrophilic poly(MPC) shell and thermoresponsive core consisting of poly(methoxydiethylene glycol methacrylate) (poly(MeODEGM) and poly(2-aminoethyl methacrylamide hydrochloride) (poly(AEMA) were then obtained in a one-pot process by RAFT polymerization in the presence of an acid degradable cross-linker. These acid degradable nanogels were efficiently synthesized with tunable sizes and low polydispersities. The encapsulation efficiencies of the nanogels with different proteins such as insulin, BSA, and β-galactosidase were studied and found to be dependent of the cross-linker concentration, size of protein, and the cationic character of the nanogels imparted by the presence of AEMA in the core. The thermoresponsive nature of the synthesized nanogels plays a vital role in protein encapsulation: the hydrophilic core and shell of the nanogels at low temperature allow easy diffusion of the proteins inside out and, with an increase in temperature, the core becomes hydrophobic and the nanogels are easily separated out with entrapped protein. The release profile of insulin from nanogels at low pH was studied and results were analyzed using bicinchoninic assay (BCA). Controlled release of protein was observed over 48 h.
■
INTRODUCTION Nanogels are networks of swollen cross-linked polymers in the nanometer range. These systems are increasingly being studied for their attractive properties in drug delivery systems, biotechnology, and biomedical fields.1−6 Nanosized particles have the advantage of enhanced permeability and retention (EPR) effect7 owing to their small size. Apart from their small size, extra stability in aqueous medium, and high water retention, they can also be made to respond to changes in the external environment, such as temperature and pH. These so-called “smart” nanogels are increasingly being considered for drug delivery systems (DDS).1,8 For example, change in size of pH controlled systems helps in controlled release of encapsulated drugs.9,10 Similarly, temperature sensitive nanogels undergo a phase change from hydrophilic to hydrophobic at a transition temperature called the lower critical solution temperature (LCST). Poly(methoxydiethylene glycol methacrylate (poly(MeODEGM)) and poly(N-isopropylacrylamide) (poly(NIPAM)) are examples of thermoresponsive polymers. NIPAM has a LCST of 32 °C and can be easily copolymerized with other hydrophilic monomers to raise the LCST close to body temperature.9,11 Despite the extensive biological studies, PNIPAM based materials have not yet been approved by FDA © 2011 American Chemical Society
due to toxicity concerns. On the other hand, MeODEGM is widely used in medicine and pharmacology because of its excellent biocompatibility with an LCST of 24 °C.12−14 In order to be used as DDS, surface functionalization of nanogels with organ specific ligands can be done to target specific tissues or organs. Nanocarriers have shown very high drug loading capacity (sometimes as high as 800%, i.e., 1 mg of nanogel can load about 8.0 mg of BSA).15 The success of using such nanocarriers relies on their ability for a controlled release of encapsulated drugs. Nanogels have been synthesized using various approaches: physical self-assembly, covalent cross-linking of preformed polymers, and template supported nanofabrication.16 Emulsionfree or precipitation polymerization is an easy way to produce nanomicelles where ionic surfactants are used to stabilize these nanoparticles in water. While emulsion polymerization is carried out in an aqueous medium and the core consists of the hydrophobic monomer, the inverse mini-emulsion polymerization technique is used for hydrophilic monomers like N-vinyl Received: July 20, 2011 Revised: November 30, 2011 Published: December 15, 2011 75
dx.doi.org/10.1021/bc2003814 | Bioconjugate Chem. 2012, 23, 75−83
Bioconjugate Chemistry
Article
caprolactam.17,18 The presence of residual surfactants with the nanogels has been a major concern of toxicity and hence is not viable for in vivo studies. Also, removal of surfactants from the nanogel is not easy. Self-assembly of amphiphilic polymers is another approach which eliminates the need for surfactants in the synthesis. Wooley et al. synthesized triblock cross-linked micelles forming stabilized nanogels.19−22 Multiresponsive polymeric micelles, which respond to changes in both pH and temperature, have been synthesized by Kuckling et al.3 Various living polymerization techniques are used for the synthesis of nanogels to maintain control over molecular weights and polydispersity of the polymer units.7 These techniques include ring-opening polymerization, ring-opening metathesis polymerization, cyanoxyl-mediated free radical polymerization, atom transfer radical polymerization (ATRP), reversible addition−fragmentation chain transfer polymerization (RAFT), and nitroxide-mediated polymerization (NMP).23−26 RAFT polymerization is a suitable technique and is very popular for biological applications. Micelles containing RAFT agents are easy to cross-link and thus form core cross-linked,27−29 shell cross-linked,30,31or nexus between both.32,33 Self-assembly of the amphiphilic copolymers in water leads to the formation of micelles. However, under special conditions, like low concentration or high ionic environment, these micellar structures may not exhibit a strong amphiphilic character and hence can be unstable in aqueous solution, existing as unimers.32,34 Cross-linking of polymers can play a significant role in imparting the required stability. This technique combines self-assembly and cross-linking and provides excellent control over the “spatial distribution of polymeric chains” in an aqueous solution.16 Cross-linkers that degrade or hydrolyze under special conditions, for example, low pH, reductive environment, or the presence of dithiothreitol (DTT), are conducive for drug delivery, as their degradation causes the release of encapsulated macromolecules. Encapsulation of a drug prevents its fast clearance from body.32 Responsive nanogel systems have been shown to control the activity of biopolymers and, at the same time, control the release of a therapeutic drug.22,35,36 Previous reports have shown that nanoparticle/nanogel formation increases the stability of trapped enzymes/proteins against degradation and denaturation and modulated the release of these biomolecules at specific or targeted sites.37−40 Protein encapsulation in nanogels, microgels, nanotubes, and nanoparticles is under intense study, and these systems have shown immense potential in drug delivery systems.37,41−43 Protein encapsulation in hydrogel systems and controlled release of insulin, lysozome, calcitonin, and interleukin-2 has been studied intensively.22,44−46 The present study entails the synthesis, characterization, and application of thermoresponsive, acid degradable core crosslinked nanogels with a hydrophobic core composed of MeODEGM and AEMA cross-linked with an acid degradable cross-linker and a hydrophilic shell of poly(methacryloyloxyethyl phosphorylcholine) poly(MPC). Solubility and stability of the nanogels are attributed to the hydrophilic and zwitterionic nature of the poly(MPC) shell. The phosphorylcholine group on the methacrylate monomer resembles the polar phospholipid group present on the cell membrane. As a result, MPC based polymers show very high biocompatibility, and various copolymers of MPC are popularly
used for biomedical applications.47−49 The thermoresponsive MeODEGM core swells and shrinks with the change in temperature, which helps the entrapment of controlled encapsulation and release of therapeutic molecules. A cationic monomer, AEMA, is incorporated in the core to enhance the encapsulation of charged protein. A range of pH domains is found in the human body. While physiological pH is 7.4, pH values in endosomes and lysosomes are 5.5−6 and 4−5, respectively. The cross-linker is acid degradable, and the release of encapsulated protein was evaluated as a function of pH. Size trends and polydispersities of various nanogels synthesized by RAFT polymerization have been analyzed. Protein encapsulation and release from such nanogels have been evaluated and compared for different crosslinker concentrations.
■
EXPERIMENTAL SECTION Materials. 2-Methacryloyloxyethyl phosphorylcholine (MPC) was obtained from NOF Co (Tokyo, Japan), which was synthesized by a method reported previously.50 2Hydroxyethyl methacrylate (HEMA), 2,2-dimethoxypropane, p-toluene sulfonic acid (pTSA), triethyl amine (TEA), and 4,4′azobis-(cyanovaleric acid) (ACVA) were purchased from Sigma Aldrich (Canada) and were used as received. Methoxydiethylene glycol methacrylate (MeODEGM) was purchased from Sigma Aldrich (Canada) and was passed through a short pad of silica prior to use. Aminoethyl methacrylamide hydrochloride (AEMA)51 and 4-cyanopentanoic acid dithiobenzoate (CTP)52,53 was synthesized as described according to previous reports. 2-Propanol, HPLC grade water, acetone, hexane, and ethyl acetate were purchased from Caledon Laboratories (Canada). Micro BCA assay kit was obtained from Fisher Scientific. Gwiz β-galactosidase was purchased from Aldevron. Bovine serum albumin (BSA) was purchased from Promega Corporation. Insulin was obtained from Sigma Aldrich. The chemical structures of monomers, initiator, chain transfer agent and cross-linker used in this study are depicted in Figure 1.
Figure 1. Chemical structures of monomers (MPC, MeODEGM and AEMA), cross-linker (CL), chain transfer agent (CTP), and initiator (ACVA).
Synthesis of 2,2-Dimethacroyloxy-1-ethoxypropane (Cross-Linker). The synthesis of the cross-linker has been recently reported by Aspinwall and co-workers.54 However, their synthesis has been carried out under different conditions 76
dx.doi.org/10.1021/bc2003814 | Bioconjugate Chem. 2012, 23, 75−83
Bioconjugate Chemistry
Article
(refluxing in benzene for 20 h). A typical protocol for our synthesis is as follows. HEMA (2-hydroxyethyl methacrylate) (10 g, 76.8 mmol), 2,2-dimethoxypropane (4.0 g, 38.4 mmol), and p-TSA (66 mg, 0.34 mmol) were added to a 25 mL roundbottom flask and the mixture was stirred for 6 h at room temperature in the dark. The crude product was purified by flash column chromatography on silica gel using a mobile phase of 85:14:1 hexane/ethylacetate/TEA. Fractions containing the pure product were pooled, and the solvent was removed by rotary evaporation and dried overnight under vacuum to afford pure cross-linker as a pale yellow oil. The cross-linker was stored at 0 °C. 1 H NMR (400 MHz, CDCl3) δ 1.39 (6H, s, C(CH3)2), 1.96 (6H, s, (6H, s, (OCOCCH3CH2)2), 3.75 (4H, t, J = 10.1, 5.0 Hz, C(CH3)2(OCH2CH2O)2), 4.30 (4H, t, J = 10.0, 5.1 Hz, C(CH3)2(OCH2CH2O)2), 5.59 (2H, s, OCOCCH3CH2 − syn to methyl), 6.15 (2H, s, OCOCCH3CH2 − anti to methyl). 13C NMR (100 MHz, CDCl3) δ 17.9 (OCOCCH3CH2), 24.4 (C(CH 3 ) 2 ), 58.5 (C(CH 3 ) 2 (OCH 2 CH 2 O) 2 ), 63.6 (C(CH3)2(OCH2CH2O)2), 99.8 (C(CH3)2), 125.2 (OCOCCH 3 CH 2 ), 135.8 (OCOCCH 3 CH 2 ), 166.9 (OCOCCH3CH2). HRMS (M+Na+) for C15H24O6Na, m/z = 323.1464 observed, m/z = 323.1465 calculated. Synthesis of Poly(MPC) MacroCTA by RAFT Polymerization. MPC macroCTA was synthesized as previously reported.55 MPC (3 g, 10.2 mmol), CTP (2.8 × 10−2 g, 0.1 mmol), and ACVA (1.4 × 10−2 g, 0.051 mmol) were dissolved in 9 mL methanol in a 25 mL reactor. The solution was degassed by purging nitrogen for 30 min and then placed under stirring at a temperature of 60 °C for 6 h. The polymer was obtained by precipitating the mixture in acetone. Any remaining traces of monomer were removed by washing the solution in water/acetone (1:7). The precipitate was again washed with acetone for 3−4 times and the final powder was freeze−dried. The poly(MPC) macroCTA molecular weight and PDI were found to be 1.2 × 104 g/mol and 1.21, respectively, by GPC. General Procedure for the Synthesis of poly(MPC-b(MeODEGM-st-AEMA-st-CL)) Nanogel by RAFT Polymerization. The RAFT polymerizations were performed in water/ 2-propanol (4:1 by volume) using ACVA as initiator, Poly(MPC) as macroCTA, and 2,2-dimethacroyloxy-1-ethoxypropane as the cross-linker at 70 °C for 24 h. The molar ratio of the macroCTA and ACVA (2:1) was held constant and the molar ratio between the macroCTA and the monomers was varied in order to prepare nanogels with different chain lengths (Table 1) . A typical general procedure is as follows: Poly(MPC) macroCTA (3.9 × 10−2 g, 3.3 × 10−3 mmol), MeODEGM (0.2 g, 1.1 mmol), AEMA (4.4 × 10−2 g, 0.26 mmol), and CL (6.0 × 10−2 g, 0.19 mmol) (15 mol % with respect to total moles of MeODEGM and AEMA) were dissolved in 4 mL water and sonicated. ACVA (4.0 × 10−4 g, 1.6 × 10−3 mmol) was dissolved in 1 mL 2-propanol and added to the reaction mixture. The solution was degassed by purging with nitrogen for 30 min and the reaction was carried out at 70 °C for 24 h. Reaction was stopped by quenching in liquid nitrogen. Nanogel was centrifuged at 14 000 rpm and 40 °C. The supernatant was discarded and the precipitate was washed with distilled water 3−4 times. The final precipitate was dissolved in water and freeze−dried overnight. A white powder was recovered and stored in the refrigerator. Protein Encapsulation. Drug loading was done using incubation method. Aqueous solutions of nanogels were
Table 1. Comparison of Hydrodynamic Diameter of MPC-b(MeODEGM-st-AEMA-st CL) Nanogel with Varying CrossLinker Concentrations and MEODEGM-AEMA Chain Length nanogel
nanogel composition
NG1
MPC70-b-(MeODEGMst-AEMA-st-CL)500 MPC70-b-(MeODEGMst-AEMA-st-CL)300 MPC70-b-(MeODEGMst-AEMA-st-CL)400 MPC43-b-(MeODEGMst-AEMA-st-CL)400 MPC43-b-(MeODEGMst-AEMA-st-CL)400 MPC43-b-(MeODEGMst-AEMA-st-CL)400 MPC43-b-(MeODEGMst-AEMA-st-CL)400
NG2 NG3 NG4 NG5 NG6 NG7
crosslinker (mol %)
hydrodynamic diameter (nm)
polydispersity
7
45
0.09
10
60
0.29
10
114
0.07
15
140
0.09
20
150
0.14
25
282
0.08
35
-
-
prepared in 10 mg/mL concentrations. The nanogel solution was mixed with 1.5 × 102 μL solution of 1 mg/mL BSA solution and incubated for 24 h at 4 °C. The total amount of protein encapsulated was calculated after centrifuging the sample at 40 °C in Beckmann Coulter Centrifuge (Microfuge 22R) (14 000 rpm, 15 min). The solution was separated into a white precipitate and supernatant. The amount of protein encapsulated in the nanogel was measured by incubating with bicinchoninic acid (BCA assay) for 2 h at 37 °C and measuring the absorbance at 570 nm using TECAN Genios Pro microplate reader. The plate reader was precalibrated using varying concentrations of protein and data were analyzed using Boltzmann function to give the best sigmoidal fit. The feed amounts for encapsulation of insulin and β-galactosidase are 50 and 2 μg, respectively. The amount of protein encapsulated (D) was calculated as follows:
D=
total protein − free protein total protein
where free protein is the protein in supernatant. Release of Protein from Nanogels at Acidic pH. In order to study the release of encapsulated protein, the nanogel was precipitated and redispersed in a citrate buffer solution of pH 4.8 and 6.4. The solution was divided into 7 aliquots. At regular intervals, the nanogels aliquots were precipitated and total protein content in the supernatant (released protein) was determined using BCA assay. Activity of Protein. The activity of β-galactosidase protein encapsulated in nanogel was studied by β-galactosidase assay. The nanogel was precipitated and separated from the supernatant (solution 1). The precipitate was redispersed in 100 μL sodium phosphate buffer solution (solution 2). 150 μL O-nitrophenyl-β-D-galactopyranoside (ONPG) (4 mg/mL) was added to 100 μL solutions 1 and 2 in the presence of 4.5 μL 100× Mg solution (0.64 μL of β-mercaptoethanol in 100 μL of 0.1 M MgCl2) in a 96 well plate and was incubated for 4 h at 37 °C. The yellow color developed was detected using the TECAN Genios Pro microplate reader at 420 nm. Characterizations. Nuclear Magnetic Resonance. 1H and 13C NMR spectra of the cross-linker were recorded on a 77
dx.doi.org/10.1021/bc2003814 | Bioconjugate Chem. 2012, 23, 75−83
Bioconjugate Chemistry
Article
Scheme 1. Schematic Representation of Core Cross-Linked Micelles with Thermoresponsive and Degradable Cores
conditions, and the rate of degradation was dependent on both pH and cross-linker concentration. The acid degradable nanogels were then used to study the encapsulation efficiency and the release profile of proteins. Synthesis of 2,2-Dimethacroyloxy-1-ethoxypropane (acid degradable cross-linker). The pH in the human body varies from 7.4 (physiological pH) to 5.5−6 in endosomes and 4−5 in lysosomes. Acid degradable cross-linker was synthesized for this study, to facilitate release of encapsulated proteins at low pH. Aspinwall and co-workers54 recently reported the synthesis of the cross-linker, which involved the use of benzene as solvent under high temperature with a reaction time of 20 h. However, our synthesis proceeds under much milder conditions, namely, in the absence of organic solvent at room temperature for 6 h of reaction time. The reaction of HEMA with 2,2-dimethoxypropane in a molar ratio of 2:1 yields acid degradable cross-linker as shown in Figure S1 (Supporting Information). Excess HEMA was removed during flash column chromatography on silica gel using a small amount of triethylamine in the eluent system. The presence of triethylamine prevents the degradation of the acid sensitive crosslinker. It was observed that, if the reaction was continued for more than the specified time of 6 h, the product turned dark brown, which is possibly due to side reactions that started simultaneously. The cross-linker was stored at 0 °C to avoid these side reactions. The 1H and 13C NMR spectra of the purified cross-linker are shown in Figures S2 and S3 (Supporting Information). Synthesis of Nanogels. Core−shell nanogels were synthesized using acid degradable cross-linker, by RAFT polymerization technique. A one-pot synthesis method developed by Pan et al.,56 which involved the polymerization of cross-linker with the monomer to get stabilized core crosslinked micelles, was followed for synthesizing nanogels. Recently, our group has extended this powerful one-pot synthesis for the fabrication of fixed CCL micelles having primary amino groups on the outer coronas for further surface functionalization.58 Overall, in this RAFT polymerization process, cross-linking and polymerization happened simultaneously. The core shell nanogel comprising a temperature sensitive MeODEGM core along with a primary amine monomer AEMA, imparting an additional functionality to the core, was cross-linked by an acid degradable cross-linker (CL) and a hydrophilic shell of MPC polymer chains (Scheme 2). MPC macroCTA (Mn = 1.2 × 104 g/mol) was synthesized in methanol as discussed in previous protocol.55 The conversion
Varian 400 MHz instrument. The sample was prepared using CDCl3 as solvent. MeODEGM shows thermoresponsive behavior and undergoes coil to globule transition at a lower critical solution temperature (LCST) of 24 °C. This transition was also studied at a molecular level by NMR spectroscopy in D2O. The signal intensities of MeODEGM protons vs that of solvent protons were compared at various temperatures (below and above the LCST). To account for the chemical shift of signal intensities at elevated temperatures, 1% 4,4-dimethyl-4-silapentane-1-sulfonic acid (DSS) solution was added as a reference at 0 ppm. Mass Spectroscopy. Mass spectroscopy was carried out in Agilent Technologies 6220 orthogonal acceleration TOF (oaTOF) (Santa Clara California, USA). Gel Permeation Chromatography (GPC). The number average molecular weight (Mn) and polydispersity (Mw/Mn) of the macro CTA was studied using Viscotek conventional GPC connected to two Waters Ultrahydrogel linear WAT011545 columns (pore size: blend; exclusion limit = 7.0 × 106) and has a Viscotek model 250 dual detector. An acidic buffer of 0.50 M sodium acetate/0.50 M acetic acid was used as eluent. Calibration of GPC was done by six monodispersed poly(ethylene oxide) (PEO) standards (Mp = (1.01 × 103)−(1.01 × 105) g mol−1). Dynamic Light Scattering (DLS). Size of MeODEGM nanogels was analyzed using Viscotek DLS 802 instrument, which is equipped with a He−Ne laser at a wavelength of 632 nm and a Peltier temperature controller. The aqueous nanogel solution was filtered through a 0.45 μm pore size Millipore membrane. Data were obtained at an angle of 90° within the temperature range 25−50 °C. Omnisize software was used to record the DLS size data. 0.5 mL aliquots were drawn at 0 min, 30 min, 1 h, 2 h, 5 h, 18 h, and 24 h of reaction time. Transmission Electron Microscopy (TEM). Size and morphology of nanogels at room temperature were analyzed on a Philips transmission electron microscope operated at 80 kV and fitted with a CCD camera. A droplet of a properly diluted nanogel solution was placed on the TEM carbon coated copper grid and allowed to air-dry before it was stained with phosphotungstic acid (2 wt % aqueous solution) for 1 min. The sample was then allowed to dry overnight prior to observation.
■
RESULTS AND DISCUSSION
Nanogels (core cross-linked micelles) were successfully synthesized with a hydrophilic shell and a thermoresponsive core in a one-pot manner using the RAFT polymerization method (Scheme 1). These nanogels degraded under acidic 78
dx.doi.org/10.1021/bc2003814 | Bioconjugate Chem. 2012, 23, 75−83
Bioconjugate Chemistry
Article
amounts of cross-linker (Figure 2). It was observed that the nanogels attained a stable size within 5−6 h of reaction time
Scheme 2. RAFT Synthesis of poly(MPC-b-(MeODEGM-stAEMA-st-CL)) Core Cross-Linked Micelles with Thermoresponsive and Degradable Cores
Figure 2. Evolution of hydrodynamic diameter of reaction mixture of cross-linking nanogel and variation of size with varying cross-linker (CL) concentration.
and with increasing cross-linker concentration, the hydrodynamic size also increased (Table 1). However, for poorly degradable cross-linker concentrations (7−10 mol %), the sizes were small (45−60 nm) and increased with temperature. This may be due to the unstable micelle structures and formation of aggregates of MeODEGM polymers. On the other hand, for a high concentration of cross-linker (35 mol %), a very turbid solution was obtained. Particle precipitation was observed when the solution was left undisturbed for 10−15 min. Thus, the size of particles formed was in the micrometer range, and hence, particles were unstable in solution. Stable nanogels were obtained at an optimum cross-linker concentration of 15−20 mol % with particle sizes of 125−150 nm and low polydispersities (0.09−0.14) as determined by DLS. TEM images of these nanogels (NG4 and NG6) are depicted in Figure 3 and showed that they were
was kept low (60%) in order to prevent the formation of dead chains as a result of the termination reactions that set in toward the end of the reaction. The macroCTA was further used to copolymerize MeODEGM and AEMA in the presence of the cross-linker in water and 2-propanol using ACVA as initiator (Scheme 2). The use of ACVA as initiator is driven by two factors. First, it can be thermally decomposed and has a half-life of 10 h in aqueous solution at 69 °C, and second, it is slightly more hydrophilic than other thermally sensitive initiators like AIBN. Tao et al. observed that a hydrophobic initiator could interfere with the hydrophobic core and hence produce unstable micelles. On the contrary, ACVA, which is more hydrophilic, yields controlled and more stable nanogels.57 Micelle structures can easily dissociate after dilution, and in order to prevent dissociation of micelle structures of diblock copolymers, they are stabilized by cross-linking.58 The size and stability of nanogels depend on cross-linker concentration (molar ratio with respect to the total molar monomers concentration) (expressed in percentage). For the synthesis of uniform, fixed micelles, it is necessary to have a suitable amount of cross-linker. Branched copolymers and unstable nanostructures can be formed as a result of low cross-linker concentration.12 On the other hand, very high cross-linker concentration can result in the formation of microgel or hydrogel networks.59 To confirm this effect, cross-linker concentration was varied from 7, 10, 15, 20, 25, and 35 mol %. The particle size and their polydispersities were determined using DLS as shown in Table 1. The evolution of hydrodynamic size of the nanogel with time was studied for varying
Figure 3. TEM images of nanogels showing (A) NG4 (15 mol % CL) and (B) NG6 (25 mol % CL).
spherical in shape with a smooth surface. Both NG3 (10 mol % CL) and NG4 (15 mol % CL) (Figure S4, Supporting Information) displayed good dispersibility; however, for NG6 (25 mol % CL), the particles started to aggregate. More importantly, the TEM results indicated that the nanogel had a core−shell structure, which confirmed nanogel formation. MeODEGM is a thermoresponsive polymer and experiences a phase change from being hydrophilic at low temperatures (24 79
dx.doi.org/10.1021/bc2003814 | Bioconjugate Chem. 2012, 23, 75−83
Bioconjugate Chemistry
Article
°C) to hydrophobic at high temperatures. The MeODEGM core of the micelle, therefore, collapses at high temperatures, which is indicated by a notable decrease in size above 24 °C. Table 1 shows the variation in size of nanogels with change in MeODEGM chain length and cross-linker concentration. MeODEGM chain length has little effect on the size of nanogels, but it affects the LCST of the nanogel. Lutz et al. observed that an increase in MeODEGM levels in the nanogel raised LCST from 24 °C to as high as 84 °C.13,60 Temperature dependent DLS studies showed that nanoparticles shrunk from 147 nm at 15 °C to 115 nm at 50 °C (NG4) and 75 nm at 15 °C to 53 nm at 50 °C (NG2) as shown in Figure 4. The phase transition of MeODEGM from
Figure 5. Normalized ratio of 1H NMR signal intensity of MeODEGM protons to D2O protons vs temperature as observed for the methylene group protons of MeODEGM at 3.4 ppm and D2O for NG4.
(Figure 6). Also, the rate of degradation of the nanogels is more pronounced for low cross-linker concentration (10 mol %),
Figure 4. Decrease in mass-average hydrodynamic diameter with increase in temperature obtained for 0.5 mg/mL aqueous solution of nanogel, for varying cross-linker (CL) concentration.
hydrophilic to hydrophobic state could be seen as the solution immediately turned milky white from transparent as the temperature was raised (Figure S5, Supporting Information). The nanogels were found to be quite stable at 50 °C. The phase transition behavior of MeODEGM core was studied using VTNMR (Variable Temperature 1H NMR) as depicted in Figure S6 (Supporting Information). While disappearance of the peak for the thermoresponsive was expected at higher temperature, only a small reduction in peak intensity was observed. This shows that nanogels behave differently from homogeneous and macroscopic systems. Furthermore, Schönhoff et al. have attributed this reduction in NMR signal intensity of poly(NIPAM) to the decrease in polymer segmental mobility, which further decreases the relaxation time, T.61 The 1H NMR peak intensity of methylene group of poly(MeODEGM) at 3.4 ppm was compared with normalized solvent (D2O) peak intensity. The reduction in polymer signal intensity above phase transition is shown in Figure 5. The effect of pH on the nanogel was studied to find the rate of degradation of the cross-linker at low pH. The pH of distilled water is slightly acidic (pH 6.7). Nanogels in distilled water could be stored for 2−3 days without degradation. A comparative study of the rate of degradation at different pH (pH 4.5, 5.2, and 6.4) and varying cross-linker concentration (10 and 15 mol %) was carried out. As expected, the nanogels were found to be unstable and degrade under acidic conditions
Figure 6. Degradation profile of NG3 and NG4 at pH 4.5, 5.4, and 6.2.
which degraded within 2 h at pH 4.5 and 5.2. The nanogels were found to be very stable under neutral and alkaline pH. For higher cross-linker concentrations, however, the degradation curve shifted to the right, indicating higher stability at low pH for a longer time. Protein Encapsulation. An important application of stimuli-responsive nanogels is the encapsulation of macromolecules in their core or coronas. Cross-linking of polymers provides a stable micelle structure, which can be exploited to trap macromolecules of various sizes. However, the release of trapped drugs is only possible by the degradation of cross-linker under physiological conditions. We have used acid degradable cross-linker, which degrades at low pH, thereby releasing the encapsulated proteins. The thermoresponsive nature of the synthesized nanogels plays a vital role for protein encapsulation, since at low temperature (4 °C), the nanogel core and shell are both 80
dx.doi.org/10.1021/bc2003814 | Bioconjugate Chem. 2012, 23, 75−83
Bioconjugate Chemistry
Article
hydrophilic and, as temperature increases to 37 °C, the core of the nanogels become hydrophobic and therefore the nanogels can easily be separated out of solution by simple centrifugation. Thus, the nanogels were collapsed at 37 °C to trap the protein within the core and hence the amount of entrapped protein can easily be estimated. The protein was loaded using the incubation method. Insulin, BSA, and β-galactosidase were incubated overnight in aqueous nanogel solutions (5 mg/mL) at 4 °C. The three proteins vary largely in their sizes. Insulin is the smallest protein with size 5.81 kDa, while BSA has a molecular weight of 66.8 kDa and β-galactosidase is the largest protein of size 540 kDa. MeODEGM nanogels are hydrophobic at room temperature. The proteins were incubated at low temperature (7 °C) to ensure maximum encapsulation. The incubation method is reported to be less efficient than the encapsulation method, as per previous reports.62 However, these nanogels showed high loading probably due to the additional functionality of the core of the nanogels (presence of protonated amino groups). The cationic nature of the core has (PAEMA-pKa 8.8) has facilitated the encapsulation of negatively charged macromolecules. For example, BSA has a pI (isoelectric point or the point of zero charge) of 4.6 and therefore has a negative surface charge at neutral pH. The nanogel was precipitated at 14 000 rpm and 40 °C. Before precipitating, the gels were collapsed to trap the protein within the core. The amount of entrapped protein was estimated by calculating the difference between the amount of protein added and the amount of nonencapsulated protein in the aqueous phase of precipitated protein. It was observed that two factors that dictated the amount of protein encapsulated were the cross-linker concentration and the percentage of AEMA in the core. A comparative study of three samples is shown in Table 2. The analysis showed that 92% of insulin was encapsulated for
cross-linker decrease the pore size leading to reduced loading capacity. To study the effect of AEMA, nanogels with varying amount of cationic components were studied and compared. For the same amount of cross-linker, the AEMA component also affects the encapsulation efficiency. This may be due to the electrostatic interaction between the protein and cationic nanogel due to opposite charges of protein and MeODEGMAEMA nanogel at neutral pH. Table 2 indicates that NG4b has the optimum cross-linker concentration (15 mol %) and AEMA concentration (5 mol %) for the encapsulation of proteins. A careful analysis of data indicates that the size and properties of macromolecules also play an important role in determining the total encapsulation. Insulin showed highest percentage encapsulation in agreement with its smallest size and lowest molecular weight (5.81 kDa). β-Galactosidase, on the other hand, has a molecular weight of 540 kDa, and consequently the lowest encapsulation efficiency. The encapsulation efficiency decreased from 92% for insulin to 35% for β-galactosidase. Release Profile. The release profile of nanogels was studied at varying pH. Nanogels with 15% and 20% cross-linker concentration were incubated overnight with 50 μL insulin protein (1 mg/mL). The nanogels were precipitated and the amount of protein encapsulated was determined by BCA assay. The precipitated nanogel was redispersed in buffer solutions of pH 4.8 and 6.4. Aliquots from buffer solution were taken at regular intervals and the amount of protein released was calculated. Almost 90% protein was released over a period of 48 h at pH 4.8. Thus, the release profile of insulin from MeODEGM nanogels is slow, and no burst release was observed (Figure 7).
Table 2. Protein Encapsulation Efficiencies for Nanogels of Varying Cross-Linker Concentration and AEMA Contenta samples
protein
protein encapsulation (μg)
encapsulation (%)
NG4a
Insulin BSA β-Gal Insulin BSA β-Gal Insulin BSA β-Gal
46 54 46 90 0.7 40 40 -
92 36 92 60 35 80 27 -
NG4b
NG5
a
(A) NG4a: 15 mol % CL and 5% AEMA feed ratio. (B) NG4b: 15 mol % CL and 25% AEMA feed ratio. (C) NG 5: 20 mol % CL and 10% AEMA feed ratio. Figure 7. Cumulative release profile of insulin from NG4 and NG5 at pH 4.8 and 6.4.
nanogel with 15% feed cross-linker concentration and 25% feed ratio AEMA (NG4b). For higher cross-linker concentration, the encapsulation was reduced to 80%. A possible explanation for the strong dependence of encapsulation efficiency on the cross-linker concentration may be due to its effect on pore size of the cross-linked nanogel. A higher cross-linker concentration is expected to produce a tighter network, therefore providing a smaller pore size. Encapsulation of macromolecules is easier for a larger pore size network. While lower cross-linker concentration fails to cross-link stably, higher amounts of
To confirm the structure and activity of β-galactosidase after loading, β-galactosidase assay was conducted on the 400 μL of 5 mg/mL aqueous nanogel solution loaded with β-gal. The amount of encapsulation based on BCA assay calculation was found to be 35%. Figure S7 (Supporting Information) showed the change in color of nanogel when ONPG was hydrolyzed to o-nitrophenol (yellow) and galactose by β-galactosidase. The activity of protein in supernatant and nanogel was calculated to 81
dx.doi.org/10.1021/bc2003814 | Bioconjugate Chem. 2012, 23, 75−83
Bioconjugate Chemistry
Article
(7) Fang, J., Nakamura, H., and Maeda, H. (2011) The EPR effect: Unique features of tumor blood vessels for drug delivery, factors involved, and limitations and augmentation of the effect. Adv. Drug Delivery Rev. 63, 136−151. (8) Harris, J. M., and Chess, R. B. (2003) Effect of PEGylation on pharmaceuticals. Nat. Rev. Drug Discovery 2, 214−221. (9) Heyden, K. V., Babooram, K., Ahmed, M., and Narain, R. (2009) Protein encapsulation and release from degradable sugar based hydrogels. Eur. Polym. J. 45, 1689−1697. (10) Risbud, M. V., Hardikar, A. A., Bhat, S. V., and Bhonde, R. R. (2000) pH-sensitive freeze-dried chitosan−polyvinyl pyrrolidone hydrogels as controlled release system for antibiotic delivery. J. Controlled Release 68, 23−30. (11) Prevot, M., Déjugnat, C., Möhwald, H., and Sukhorukov, G. B. (2006) Behavior of temperature-sensitive PNIPAM confined in polyelectrolyte capsules. ChemPhysChem 7, 2497−2502. (12) Goh, C. C. E., and Stöver, D. H. (2002) Cross-linked poly(methacrylic acid-co-poly(ethylene oxide) methyl ether methacrylate) microspheres and microgels prepared by precipitation polymerization: A morphology study. Macromolecules 35, 9983−9989. (13) Lutz, J. F., Akdemir, O., and Hoth, A. (2006) Point by point comparison of two thermosensitive polymers exhibiting a similar LCST: is the age of poly(NIPAM) over? J. Am. Chem. Soc. 128, 13046−13047. (14) Hu, T., You, Y., Pan, C., and Wu, C. (2002) The coil-to-globuleto-brush transition of linear thermally sensitive poly(N-isopropylacrylamide) chains grafted on a spherical microgel. J. Phys. Chem. B 106, 6659−6662. (15) Chen, Y., Zheng, X., Qian, H., Mao, Z., Ding, D., and Jiang, X. (2010) Hollow core-porous shell structure poly(acrylic acid) nanogels with a super high capacity of drug loading. Appl. Mater. Interfaces 2, 3532−3538. (16) Tan, J. P. K., Tan, M. B. H., and Tam, M. (2010) Application of nanogel systems in the administration of local anesthetics. Local Reg. Anesth. 3, 93−100. (17) Oh, J. K., Perineau, F., and Matyjaszewski, K. (2006) Preparation of nanoparticles of well-controlled water-soluble homopolymers and block copolymers using an inverse miniemulsion ATRP. Macromolecules 39, 8003−8010. (18) Smulders, W., and Monteiro, M. J. (2004) Seeded emulsion polymerization of block copolymer core-shell nanoparticles with controlled particle size and molecular weight distribution using xanthate-based RAFT polymerization. Macromolecules 37, 4474−4483. (19) Murthy, K. S., Ma, Q., Remsen, E. E., Kowalewski, T., and Wooley, K. L. (2003) Thermal shaping of shell-crosslinked (SCK) nanoparticles, facilitated by nanoconfinement of fluid-like cores. J. Mater. Chem. 13, 2785−2795. (20) Arotçaréna, M., Heise, B., Ishaya, S., and Laschewsky, A. (2002) Preparation of shell cross-linked micelles by polyelectrolyte complexation. J. Am. Chem. Soc. 124, 3787−3793. (21) Weaver, J. V. M, Tang, Y., Liu, S., Iddon, P. D., Grigg, R., Billingham, N. C., Armes, S. P., Hunter, R., and Rannard, S. P. (2004) Switching the inside and the outside of aggregates of water-soluble block copolymers with double thermoresponsivity. Angew. Chem., Int. Ed. 116, 1413−1416. (22) Alarcon, C., de las, H., Pennadam, S., and Alexander, C. (2005) Stimuli responsive polymers for biomedical applications. Chem. Soc. Rev. 34, 276−285. (23) Sciannamea, V., Jérôme, R., and Detrembleur, C. (2008) In-situ nitroxide-mediated radical polymerization (NMP) processes: their understanding and optimization. Chem. Rev. 108, 1104−26. (24) Tsarevsky, N. V., and Matyjaszewski, K. (2007) Green atom transfer radical polymerization: from process design to preparation of well-defined environmentally friendly polymeric materials. Chem. Rev. 107, 2270−99. (25) Moad, G., Rizzardo, E., and Thang, S. H. (2008) Toward living radical polymerization. Acc. Chem. Res. 41, 1133−1142. (26) Chiefari, J., Chong, Y. K. B., Ercole, F., Krstina, J., Jeffery, J., Le, T. P. T, Mayadunne, R. T. A., Meijs, G. F., Moad, C. L., Moad, G.,
be 1384 mU/mg and 4642 mU/mg, respectively. It was therefore found that the protein was present mostly in its native form after encapsulation and likely retained its catalytic activity.
■
CONCLUSION In summary, we have successfully synthesized novel stable thermoresponsive and acid degradable poly(MeODEGMAEMA) core-cross-linked micelles via RAFT polymerization using poly(MPC) macro RAFT agent. Sizes of these nanogels can be tuned accordingly by varying the cross-linker concentration and MeODEGM chain length. AEMA provides cationic character to the nanogel core, which facilitates the encapsulation of oppositely charged proteins, for example, insulin, BSA, and β-galactosidase. The loading efficiency of these proteins largely depends on the pore size of nanogels, the cationic component, and the size of protein. The degradation profile of these proteins encapsulated in acid-degradable nanogels was studied at lower pH, and a controlled release profile of protein was observed. These MPC-b-(MeODEGM-stAEMA-st-CL) nanogels therefore have promising applications as smart carriers for targeted drug delivery systems and controlled release.
■
ASSOCIATED CONTENT
* Supporting Information S
Synthesis of acid degradable cross-linker, HNMR and CNMR spectra of cross-linker, TEM image of NG3, VT-NMR study of nanogel, digital photograph of aqueous solution of nanogel on heating above and cooling below LCST, digital photograph of β-galactosidase assay conducted on aqueous solution of nanogel. This material is available free of charge via the Internet at http://pubs.acs.org.
■
AUTHOR INFORMATION
Corresponding Author
*E-mail:
[email protected], Telephone: 1-780-492-1736, Fax: 1-780-492 2881.
■
ACKNOWLEDGMENTS The authors acknowledge support from Natural Sciences and Engineering Research Council of Canada (NSERC) for the funding of this work.
■
REFERENCES
(1) Oh, J. K., Drumright, R., Siegwart, D., and Matyjaszewski, K. (2008) The development of microgels/nanogels for drug delivery applications. Prog. Polym. Sci. 33, 448−477. (2) Graham, N. B., and Cameron, A. (1998) Nanogels and microgels: the new polymeric materials playground. Pure Appl. Chem. 70, 1271− 1275. (3) Kuckling, D., Vo, C. D., and Wohlrab, S. E. (2002) Preparation of nanogels with temperature-responsive core and pH-responsive arms by photo-cross-linking. Langmuir 18, 4263−4269. (4) Koul, V., Mohamed, R., Kuckling, D., Adler, H.J. P., and Choudhary, V. (2011) Interpenetrating polymer network (IPN) nanogels based on gelatin and poly(acrylic acid) by inverse miniemulsion technique: Synthesis and characterization. Colloids Surf., B: Biointerfaces 83, 204−213. (5) Kim, Y., Thapa, M., Hua, D. H., and Chang, K. O. (2011) Biodegradable nanogels for oral delivery of interferon for norovirus infection. Antiviral Res. 89, 165−173. (6) Sahiner, N., Godbey, W. T., McPherson, G. L., and John, V. T. (2006) Novel nanogels as drug delivery systems for poorly soluble anticancer drugs. Colloid Polym. Sci. 284, 1121−1129. 82
dx.doi.org/10.1021/bc2003814 | Bioconjugate Chem. 2012, 23, 75−83
Bioconjugate Chemistry
Article
Rizzardo, E., and Thang, S. H. (1998) Living free-radical polymerization by reversible addition-fragmentation chain transfer: the RAFT process. Macromolecules 31, 5559−5562. (27) Loppinet, B., Sigel, R., Larsen, A., Fytas, G., Vlassopoulos, D., and Liu, G. (2000) Structure and dynamics in dense suspensions of micellar nanocolloids. Langmuir 16, 6480−6484. (28) Stewart, S., and Liu, G. (1999) Hollow nanospheres from polyisoprene-block-poly(2-cinnamoylethylmethacrylate)-block-poly(tert-butylacrylate). Chem. Mater. 11, 1048−1054. (29) Saito, R., Ishizu, K., and Fukutomi, T. (1990) Cross-linking of the inner poly(methyl methacrylate) core of poly(methylstyrene-bmethyl methacrylate) micelles in selective solvent: 1. Effect of solvent selectivity. Polymer 31, 679−683. (30) Butun, V., Billingham, N. C., and Armes, S. P. (1998) Synthesis of shell-cross linked micelles with tunable hydrophilic/hydrophobic cores. J. Am. Chem. Soc. 120, 12135−12136. (31) Henselwood, F., and Liu, G. J. (1997) Water soluble nanospheres from poly(2-cinnamoylethyl methacrylate)-block-poly(acrylic acid). Macromolecules 30, 488−493. (32) Zhang, L., Liu, W., Lin, L., Chen, D., and Stenzel, M. H. (2008) Degradable disulfide core-cross-linked micelles as a drug delivery system prepared from vinyl functionalized nucleosides via the RAFT process. Biomacromolecules 9, 3321−3331. (33) Zhang, L., Bernard, J., Davis, T. P., Barner-Kowollik, C., and Stenzel, M. (2008) Acid-degradable core-crosslinked micelles prepared from thermosensitive glycopolymers synthesized via RAFT polymerization. Macromol. Rapid Commun. 28, 123−129. (34) Hales, M., Barner-Kowollik, C., Davis, T. P., and Stenzel, M. (2004) Shell-cross-linked vesicles synthesized from block copolymers of Poly(D,L-lactide) and Poly(N-isopropyl acrylamide) as thermoresponsive nanocontainers. Langmuir 20, 10809−10817. (35) Kikuchi, A., and Okano, T. (2002) Pulsatile drug release control using hydrogels. Adv. Drug Delivery Rev. 54, 53−77. (36) Kim, B., Flamme, K. L., and Peppas, N. (2003) Dynamic swelling behavior of pH-sensitive anionic hydrogels used for protein delivery. J. Appl. Polym. Sci. 89, 1606−1613. (37) Cai, C., Bakowsky, U., Rytting, E., Schaper, A. K., and Kissel, T. (2008) Charged nanoparticles as protein delivery systems: a feasibility study using lysozyme as model protein. Eur. J. Pharm. Biopharm. 69, 31−42. (38) Soppimath, K. S., Aminabhavi, T. M., Kulkarni, A. R., and Rudzinski, W. E. (2001) Biodegradable polymeric nanoparticles as drug delivery devices. J. Controlled Release 70, 1−20. (39) Panyam, J., and Labhasetwar, V. (2003) Biodegradable nanoparticles for drug and gene delivery to cells and tissue. Adv. Drug Delivery Rev. 55, 329−347. (40) Smith, M. H., South, A. B., Gaulding, J. C., and Lyon, L. A. (2010) Monitoring the erosion of hydrolytically-degradable nanogels via multiangle light scattering coupled to asymmetrical flow field-flow fractionation. Anal. Chem. 82, 523−530. (41) Kang, Y., Wang, Q., Liu, Y.-C., Shen, J. W., and Wu, T. (2010) Diameter selectivity of protein encapsulation in carbon nanotubes. J. Phys. Chem. B 114, 2869−2875. (42) Hirakura, T., Yasugi, K., Nemoto, T., Sato, M., Shimoboji, T., Aso, Y., Morimoto, N., and Akiyoshi, K. (2010) Hybrid hyaluronan hydrogel encapsulating nanogel as a protein nanocarrier: new system for sustained delivery of protein with a chaperone-like function. J. Controlled Release 142, 483−489. (43) Blanco, D., and Alonso, M. J. (1998) Protein encapsulation and release from poly(lactide-co-glycolide) microspheres: effect of the protein and polymer properties and of the co-encapsulation of surfactants. Eur. J. Pharm. Biopharm. 45, 285−294. (44) Weert, M., Hof, R., Weerd, J., Heeren, R. M. A., Posthuma, G., Hennink, W. E., and Crommelin, D. J. A. (2000) Lysozyme distribution and conformation in a biodegradable polymer matrix as determined by FTIR techniques. J. Controlled Release 68, 31−40. (45) Cadée, J., Groot, C. J., de., Jiskoot, W., Otter, W. den., and Hennink, W. E. (2002) Release of recombinant human interleukin-2 from dextran-based hydrogels. J. Controlled Release 78, 1−13.
(46) Ramkissoon-Ganorkar, C., Liu, F., Baudys, M., and Kim, S. W. (1999) Modulating insulin-release profile from pH/thermosensitive polymeric beads through polymer molecular weight. J. Controlled Release 59, 287−298. (47) Kyomoto, M., Moro, T., Takatori, Y., Kawaguchi, H., Nakamura, K., and Ishihara, K. (2010) Self-initiated surface grafting with poly(2methacryloyloxyethyl phosphorylcholine) on poly(ether-ether-ketone). Biomaterials 31, 1017−1024. (48) Nakabayashi, N., and Iwasaki, Y. (2004) Copolymers of 2methacryloyloxyethyl phosphorylcholine (MPC) as biomaterials. Biomed. Mater. Eng. 14, 345−354. (49) Katakura, O., Morimoto, N., Iwasaki, Y., Akiyoshi, K., and Kasugai, S. (2005) Original article evaluation of 2-methacryloyloxyethyl phosphorylcholine (MPC) polymer-coated dressing on surgical wounds. J. Med. Dent. Sci., 115−121. (50) Ishihara, K., Ueda, T., and Nakabayashi, N. (1990) Preparation of phospholipid polymers and their properties as polymer hydrogel membranes. Polym. J 22, 355−360. (51) Deng, Z., Bouchékif, H., Babooram, K., Housni, A., Choytun, N., and Narain, R. (2008) Facile synthesis of controlled-structure primary amine-based methacrylamide polymers via the reversible additionfragmentation chain transfer process. J. Polym. Sci., Part A: Polym. Chem. 46, 4984−4996. (52) Mitsukami, Y., Donovan, M. S., Lowe, A. B., and McCormick, C. L. (2001) Water-soluble polymers. 81. direct synthesis of hydrophilic styrenic-based homopolymers and block copolymers in aqueous solution via RAFT. Macromolecules 34, 2248−2256. (53) Lai, J. T., Filla, D., and Shea, R. (2002) Functional polymers from novel carboxyl-terminated trithiocarbonates as highly efficient RAFT agents. Macromolecules 35, 6754−6756. (54) Roberts, D. L., Ma, Y., Bowles, S. E., Janczak, C. M., Pyun, J., Saavedra, S. S., and Aspinwall, C. A. (2009) Polymer-stabilized phospholipid vesicles with a controllable, pH-dependent disassembly mechanism. Langmuir 25, 1908−1910. (55) Bhuchar, N., Deng, Z., Ishihara, K., and Narain, R. (2011) Detailed study of the reversible addition−fragmentation chain transfer polymerization and co-polymerization of 2-methacryloyloxyethyl phosphorylcholine. J. Polym. Chem. 2, 632−639. (56) Zheng, G., Zheng, Q., and Pan, C. (2006) One-pot synthesis of micelles with a cross-linked poly(acrylic acid) core. Macromol. Chem. Phys. 207, 216−223. (57) Yan, L., and Tao, W. (2010) One-step synthesis of pegylated cationic nanogels of poly(N,N′-dimethylaminoethyl methacrylate) in aqueous solution via self-stabilizing micelles using an amphiphilic macroRAFT agent. Polymer 51, 2161−2167. (58) Rapoport, N. (1999) Stabilization and activation of pluronic micelles for tumor-targeted drug delivery. Colloids Surf., B: Biointerfaces. 16, 93−111. (59) Jiang, X., Liu, S., and Narain, R. (2009) Degradable thermoresponsive core cross-linked micelles: fabrication, surface functionalization, and biorecognition. Langmuir 25, 13344−13350. (60) Fournier, D., Hoogenboom, R., Thijs, H. M. L., Paulus, R. M., and Schubert, U. S. (2007) Tunable pH- and temperature-sensitive copolymer libraries by Reversible Addition−Fragmentation Chain Transfer copolymerizations of methacrylates. Macromolecules 40, 915− 920. (61) Schönhoff, M., Larsson, A., Welzel, P. B., and Kuckling, D. (2002) Thermoreversible polymers adsorbed to colloidal silica: A 1 HNMR and DSC study of the phase transition in confined geometry. J. Phys. Chem. B 106, 7800−7808. (62) Kabanov, A. V., and Vinogradov, S. V. (2009) Nanogels as pharmaceutical carriers: finite networks of infinite capabilities. Angew. Chem., Int. Ed. 48, 5418−5429.
83
dx.doi.org/10.1021/bc2003814 | Bioconjugate Chem. 2012, 23, 75−83