Ash fusion properties and mineral transformation behavior of gasified semi-char at high temperature under oxidizing atmosphere Yukui Zhang, Qiangqiang Ren, Hongxiang Deng, and Qinggang Lyu Energy Fuels, Just Accepted Manuscript • DOI: 10.1021/acs.energyfuels.7b02756 • Publication Date (Web): 28 Nov 2017 Downloaded from http://pubs.acs.org on November 29, 2017

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

Energy & Fuels is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 29

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Energy & Fuels

1

2

Ash fusion properties and mineral transformation behavior of gasified

3

semi-char at high temperature under oxidizing atmosphere

4

Yukui Zhang1,2, Qiangqiang Ren*,1,2, Hongxiang Deng1,2, Qinggang Lyu1,2

5

6

1

Institute of Engineering Thermophysics, Chinese Academy of Sciences, Beijing 100190, People’s Republic of China

7

8

2

University of Chinese Academy of Sciences, Beijing 100049, People’s Republic of China

1 ACS Paragon Plus Environment

Energy & Fuels

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 29

1

ABSTRACT

2

The carbon conversion of fluidized bed gasification has been restricted by the entrainment of semi-chars

3

with high carbon content. Recently, the disposal of the semi-char has become an intractable problem. In this

4

study, the ash fusion properties and mineral transformation behavior at high temperature of the semi-char

5

from an industrial circulating fluidized bed (CFB) gasifier were investigated under oxidizing condition. In

6

comparison with the raw coal, the total base content increases from 27.92 to 29.45 after partial gasification,

7

which results in a decrease in the ash fusion temperatures (AFTs) of the semi-char. Kaolinite decomposed

8

into quartz, alumina and water via dihydroxylation reaction and anhydrite was transformed into oldhamite in

9

the CFB gasifier. As the particle size increases, the AFTs of the semi-char decrease first and then remain

10

almost unchanged, which coincides with the variations in acid/base ratio; however, the disparity is relatively

11

small, which favors its melting utilization. Quartz, anorthite, pyroxene and hematite are the main crystalline

12

phases of the semi-char ash at high temperature and the major molten phase turns out as anorthite. The

13

liquidus temperature (1325 °C) predicted by FactSage is slightly higher than the flow temperature (1310 °C)

14

of the semi-char ash due to kinetic limits and mass transfer. In-situ observation of the semi-char ash melting

15

process indicates that low-melting-point minerals first fuse and flow between the adjacent particles; as the

16

temperature increases, high-melting-point minerals then start to melt, the molten phase content increases and

17

the flow behavior accelerates.

2 ACS Paragon Plus Environment

Page 3 of 29

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

1 2

Energy & Fuels

1. Introduction Gasification, which converts carbon-rich solid fuels (coal, biomass and semi-coke, etc.) into gaseous [1, 2]

3

products, e.g., syngas (H2 and CO), CH4 and CO2 with the presence of air, steam and oxygen

, has been

4

considered one of the most significant technologies for power generation, chemical synthesis and IGCC

5

systems. Despite the availability of diverse techniques, fluidized bed gasification has attracted substantial

6

interests because of its feedstock flexibility, low-cost operation and high environmental performance

7

However, large amounts of carbon-containing semi-chars are entrained out by crude gas, which reduces

8

carbon conversion of the gasification system (< 90%). As byproducts from gasification, the semi-chars are

9

generally considered as solid wastes; and serious environmental problems would occur if improperly

10

disposed [5]. Besides, the semi-chars always contain large quantities of unburned carbon (30-70%) compared

11

with combustion fly ash. Thus, it would be considered feasible if the semi-chars are reclaimed and reused for

12

further utilization.

[3, 4]

.

13

Currently, considerable studies have been carried out to explore effective methods for the semi-char

14

utilization. Semi-char re-injection could increase the carbon concentration of dense phase and improve the

15

carbon conversion

16

residence time

17

entrained flow gasification. However, complete conversion of the semi-char is impossible to achieve in

18

consideration of the fact that the fly ash from entrained flow gasifiers also contain certain amounts of

19

unburned carbon (30-50%) [10]. Fluidized bed combustion has proven to be an effective way to fully recover

20

residual carbons in the semi-char

21

aggravate atmospheric pollution problems, such as acid rain and photochemical smog. Furthermore, the

22

combusted fly ashes are of low density as with the semi-char, and thus volume reduction could not be

23

attained. Therefore, it is necessary to develop new techniques to obtain clean and efficient conversion of the

[8]

[6, 7]

, whereas the benefit is restricted by kinetic limits at given temperature and solids

. Wu et al.

[9]

proposed the integrated gasification concept, i.e., fluidized bed coupled with

[11]

. Nevertheless, the NOx and SO2 emitted from combustion would

3 ACS Paragon Plus Environment

Energy & Fuels

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

1

Page 4 of 29

semi-char.

2

Considering the above situations, we proposed the concept of fluidized bed gasification combined with

3

combustion melting system to make effective use of the residual carbon in the semi-char. Coal was fed into

4

the fluidized bed gasifier and the generated semi-chars were reclaimed and reused as fuel of the melting

5

furnace. The organic material in the semi-char was completely combusted and the high temperature flue gas

6

was guided directly into the gasifier to elevate the temperature of dilute zone and accelerate the gasification

7

reactions. As a result, the residual carbon was extracted from the semi-char to increase total carbon

8

conversion, and the heat released during combustion was recovered to enhance the cold gas efficiency. The

9

NOx and SO2 were converted into N2, NH3 and H2S under reducing atmosphere and removed downstream to

10

avoid air pollution. Simultaneously, the mineral matters in the semi-char were transformed into liquid slags

11

at high temperature and volume reduction was achieved. However, preliminary tests indicated that severe

12

slagging problem occurred at high temperature and long-term operation of the melting furnace was impeded.

13

Therefore, investigations on the fusion properties of the semi-char are essential for the research and

14

development of the integrated system.

15

In recent years, the fusion characteristics of coal ashes and slags from entrained flow gasifiers have been

16

extensively investigated. van Dyk [12] concluded that the addition of acid components, e.g., SiO2, Al2O3 and

17

TiO2, could raise the ash fusion temperatures (AFTs) of South African coal. The AFTs of coal ashes were

18

found to decrease first, reach a minimum and increase again when the contents of CaO, Fe2O3 and MgO

19

increased

20

reported that iron presented as iron oxides in Ar atmosphere, which was reduced to metallic iron in H2

21

atmosphere, resulting in a decrease in AFTs. The fusibility and flow properties of coal ash and slag from

22

Shell gasifier were compared and the results indicated that the AFTs and viscosity of coal ash were higher

23

than those of slag [16]. Kong et al. [17] evaluated the effect of CaCO3 on the flow properties of slag and found

[13]

; while it decreased continuously with an increase in SiO2/Al2O3 ratio

4 ACS Paragon Plus Environment

[14]

. Song et al.

[15]

Page 5 of 29

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Energy & Fuels

1

that the slag viscosity changed notably with the addition of CaCO3 owing to the difference in formation

2

route of solid phase. Song et al. [18] explored the rheology of slag from Texaco gasifiers and obtained that the

3

slag behaved as non-Newtonian fluid below its liquidus temperature because of the increase in solid content.

4

Furthermore, the fusion behavior of coal ashes are closely related to the transformation mechanism of

5

minerals at high temperature

6

Indian coals and correlated them to the AFTs. Bai et al.

7

low-temperature ash under reducing atmosphere and found that the residence time had major influence on

8

the mineral compositions at high temperature. The amounts of crystalline phases and glassy materials in

9

coarse gasification ash were determined to predict its melting behavior

[19]

. Chakravarty et al.

[20]

analyzed the mineralogical compositions of three [21]

characterized the fusion behavior of

[22]

. van Dyk et al.

[23]

investigated

10

the mineral transformation mechanism and slagging behavior of coal resources at high temperature during

11

Sasol-Lurgi fixed bed gasification. With reference to the characteristics of the semi-char from fluidized bed

12

gasification, lots of literatures

13

However, little work has been reported concerning the fusion properties and mineral transformation

14

behavior of the semi-char at high temperature, despite the fact that these characteristics are crucial for the

15

design and operation of the melting furnace.

[24-27]

regarding its physical and chemical properties have been published.

16

In this study, the basic properties and fusion characteristics of the semi-char from an industrial circulating

17

fluidized bed (CFB) gasifier were analyzed. Meanwhile, the transformation behavior of minerals at high

18

temperature

19

thermogravimetric-differential thermal analysis (TG-DTG-DTA), X-ray diffraction (XRD) and FactSage

20

simulation. Moreover, in-situ melting and crystallization of the semi-char ash were observed by using a

21

heating stage microscopy. This work aims to get a thorough understanding of the ash fusion behavior and

22

mineral transformation mechanism of the semi-char at high temperature and provide valuable information

23

for its melting utilization.

under

oxidizing

atmosphere

was

investigated

5 ACS Paragon Plus Environment

by

thermogravimetric-differential

Energy & Fuels

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

1

Page 6 of 29

2. Experimental section

2

2.1. Raw materials. The semi-char was obtained from an industrial CFB gasifier, the flowsheet of which

3

has been elaborated elsewhere [28]. The gasifier, located in Liaocheng city of Shandong province, China, was

4

established to provide clean fuel gas for alumina calcination. The feed coal is a bituminous coal, and the

5

gasifying agents are the mixture of air and steam. Generally, the gasifier operates at 950 °C under

6

atmospheric pressure and the gas-producing capacity is approximately 40,000 Nm3/h. The high-temperature

7

semi-char is separated by the cyclone separator and transported directly back into the riser via a loop seal.

8

The semi-char sample was derived from the bag dust collector, and the feed coal was collected from the coal

9

bunker. The conventional properties of the raw coal and semi-char, including proximate and ultimate

10

analyses, ash compositions and AFTs under an oxidizing atmosphere (21:79 O2/N2, volume ratio) are

11

presented in Table 1.

12

Table 1. Conventional properties of the raw coal and gasified semi-char.

Item

Raw coal

Semi-char

Proximate analysis (wt. %, ar) Moisture

12.48

0.31

Volatile matter

29.06

3.86

Fixed carbon

47.23

75.67

Ash

11.23

20.16

Ultimate analysis (wt. %, ar) Carbon

61.73

76.66

Hydrogen

3.27

0.58

Oxygen

9.88

0.00

Nitrogen

0.44

0.57

6 ACS Paragon Plus Environment

Page 7 of 29

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Energy & Fuels

Sulfur

0.98

1.72

Ash fusion temperatures (°C) DT

1255

1180

ST

1290

1250

HT

1320

1290

FT

1345

1310

SiO2

51.10

50.59

Al2O3

17.95

18.13

Fe2O3

9.26

6.80

CaO

8.93

9.36

MgO

2.13

2.30

SO3

5.35

8.70

TiO2

0.64

0.81

P2O5

1.89

0.42

K2O

1.10

0.98

Na2O

1.15

1.31

Ash compositions (wt. %)

a

Abbreviations: ar, as received basis; DT, deformation

temperature; ST, sphere temperature; HT, hemisphere temperature; FT, flow temperature. 1

2.2. Samples preparation.

2

2.2.1. Preparation of the semi-char sample of various particle sizes. The particle size distribution of the

3

semi-char was analyzed by a laser diffractometer (Mastersizer 2000, Malvern, Britain). The semi-char was 7 ACS Paragon Plus Environment

Energy & Fuels

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 29

1

divided into five groups with different particle sizes, namely, 45 µm, via sieving method.

3

2.2.2. Ash preparation. The raw coal (less than 100 µm), gasified semi-char and the semi-char of various

4

particle sizes were ashed at 815 °C in a muffle furnace according to Chinese standard GB/T 1574-2007.

5

Briefly, the furnace was first heated from ambient temperature to 500 °C within 30 min, and then held for

6

another 30 min. Subsequently, the furnace was raised to 815 °C and remained at this temperature for

7

approximately 120 min. The resultant ash samples were preserved in a desiccator for further treatment and

8

analysis.

9

2.2.3. High temperature treatment of the semi-char ash. The semi-char ash prepared previously was retreated

10

at higher temperatures (1100 °C, 1150 °C, 1200 °C, 1250 °C, 1300 °C and 1350 °C) under an oxidizing

11

atmosphere (21:79 O2/N2, volume ratio). The schematic diagram of the horizontal tube furnace is illustrated

12

in Figure 1. The treatment procedure was designed as follows. First, the alumina crucible loaded with 1 g ash

13

samples was pushed into the reaction zone by a pushing rod. Then, the tube furnace was heated to the

14

prescribed temperature at 15 °C/min and stayed for 5 min. Consequently, the samples after treatment were

15

withdrawn from the tube furnace and quenched in ice water to prevent phase transformation and crystal

16

segregation. The quenched samples were dried at 105 °C, ground to a size of Ca>Mg>Fe>Na [34, 35]. Thus, the augmented sulfur content should be responsible for the decrease in AFTs

10

[32]

. The B value, which represents the total amounts

[33]

. The B value of the raw coal is 27.92, which increases to 29.45 for the semi-char, resulting in a

of the semi-char.

11

3.1.3. Mineral transformation during gasification. The mineralogical properties of the raw coal and

12

gasified semi-char were determined by powder XRD and the crystalline phases were identified and labeled

13

in Figure 3. Clearly, A broad hump is observed between 20° and 35° (2θ) for both samples, which is mainly

14

due to the presence of organic matter

15

(Al4(OH)8(Si4O10)), anhydrite (CaSO4) and hematite (Fe2O3). After gasification, the peak representing quartz

16

ascended, while kaolinite was not identified. This was caused by dehydroxylation of kaolinite at high

17

temperature: Al4Si4O10(OH)8(s) → 2Al2O3(s) + 4SiO2(s) + 4H2O(g)

18

amounts of oldhamite (CaS) present in the semi-char, while anhydrite vanished. This indicated that anhydrite

19

was transformed into oldhamite under reducing atmosphere in the CFB gasifier according to: CaSO4(s) +

20

4CO(g) → CaS(s) + 4CO2(g) [38].

[36]

. The main minerals in coal are quartz (SiO2), kaolinite

[37]

12 ACS Paragon Plus Environment

. Moreover, there are considerable

Page 13 of 29

1 Raw coal Semi-char Relative intensity (CPS)

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Energy & Fuels

1 5 1

2

23

10

1 1 1 51 1

4

1

1

4

1

1

1 2

20

3

3 11 1 1 1

30

40

1 50

60

70

80

2θ(°)

1 2

1-quartz (SiO2); 2-Kaolinite (Al4(OH)8(Si4O10)); 3-anhydrite (CaSO4);

3

4-hematite (Fe2O3); 5-oldhamite (CaS).

4

Figure 3. XRD patterns of the raw coal and gasified semi-char.

5

The SEM micrographs of the raw coal and gasified semi-char are displayed in Figure 4. The surface of the

6

raw coal appears clean and smooth, with few fragments stacked. Scarcely any pore structure is found. In

7

contrast, the semi-char comprises many fine, irregular particles. The surface seems rough and loose, with

8

clear pore texture being visible. The morphology differences are closely related to the drastic coal

9

devolatilization process occurred in the gasifier

10

[39]

. Particularly, no agglomerates are observed on the

surface of the semi-char.

11

Raw coal 12

Gasified semi-char

Figure 4. SEM micrographs (×500) of the raw coal and gasified semi-char. 13 ACS Paragon Plus Environment

Energy & Fuels

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 14 of 29

1

3.2. AFTs variation with particle size. Investigators have reported that elemental compositions of the

2

gasified semi-char were greatly affected by its particle size due to different processes the inorganic matters

3

experienced during coal gasification [27, 40]. Thus, the ash fusion properties of the semi-char might vary with

4

its particle size, causing difficulties in operation of the melting furnace. Therefore, the semi-char were

5

sieved into five groups according to its particle size distribution and the AFTs of the semi-char with various

6

particle sizes are illustrated in Figure 5. As the particle size increases, the AFTs first decrease and then

7

remain almost unchanged. The chemical compositions of the semi-char with different particle sizes were

8

determined by XRF analysis and shown in Figure 6. Clearly, the major mineral elements in the semi-char are

9

Si, Al, Ca, Fe and S. The fractions of SiO2 and SO3 increase when the particle size is less than 45 µm, and

10

then decrease; the inverse trend is observed for Al2O3 and Fe2O3. However, none of these compounds

11

exhibits the same variation tendency as the AFTs. This implies that the variation in AFTs is not controlled

12

by a certain compound. The acid/base (A/B) ratio [41], which is developed to predict the ash fusion behavior

13

of coal ashes, is defined as below:

A/B ratio=

14

SiO2 +Al2O3 +TiO2 CaO+MgO+Fe2O3 +Na 2O+K 2O+SO3

15

where the chemical formulas represent the mass fraction of the compounds in the ash. The A/B ratios of the

16

semi-char of various particle sizes are calculated and also depicted in Figure 7. Notably, the variation trend

17

of A/B ratio is similar to that of the AFTs. It has been acknowledged that the AFTs of coal ashes increase as

18

the A/B ratio increases

19

particle sizes.

[41]

, which explains the variation trend of the AFTs of the semi-char of various

14 ACS Paragon Plus Environment

Page 15 of 29

1320

DT HT

ST FT

Temperature (°C)

1280

1240

1200

45

Particle size (µm)

1 2

Figure 5. The variations of AFTs with particle size. 60 45µm

50

Ash composition (%)

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Energy & Fuels

40

30

20

10

0 Na2O MgO Al2O3 SiO2 P2O5

SO3

K2O

CaO

TiO2 Fe2O3

3 4

Figure 6. The variations of ash compositions with particle size.

15 ACS Paragon Plus Environment

Energy & Fuels

2.74 2.72 2.70

A/B ratio (%/%)

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 16 of 29

2.68 2.66 2.64 2.62 2.60 45

Particle size (µm)

1

Figure 7. The variations of A/B ratio with particle size.

2 3

Despite the fact that the AFTs of the semi-char vary with its particle size, the disparity is not remarkable,

4

e.g., the FTs falls between 1285 °C and 1320 °C. Li et al. [27] evaluated the influence of particle sizes on the

5

AFTs of Shenmu and Jincheng fine chars separated from a pilot-scale ash-agglomerated fluidized bed (AFB)

6

gasifier. The FTs vary within the range of 1220-1310 °C and 1380-1500 °C for Shenmu and Jincheng

7

semi-char, respectively. The temperature intervals (90 °C and 120 °C) are noticeably larger than our results

8

(35 °C). This is directly relevant to the variations of chemical compositions of the semi-char with different

9

particle sizes and further attributable to the type and structure of reactors and operational parameters of the

10

gasifier [42]. In our study, the gasifier is a CFB reactor with a superficial velocity of about 4 m/s. The larger

11

particles are mostly collected by the cyclone separator and delivered into the riser for multi-circulated

12

gasification. As a result, the semi-chars entrained out by crude gas are of ultrafine particle size characterized

13

by a narrow distribution (Figure 2); thus, the elemental contents of the semi-char differ slightly with its

14

particle size. Accordingly, the discrepancy of the AFTs is relatively small. In contrast, the AFB gasifier

15

emerges as optimization and upgrading of bubbling fluidized bed reactor and the superficial velocity is low