Subscriber access provided by University of Winnipeg Library
Biofuels and Biobased Materials
Chitosan-sodium phytate films with a strong water barrier and antimicrobial properties via one-step consecutive stripping and layer-by-layer casting technologies Jie Yang, Liu Xiong, Man Li, and Qingjie Sun J. Agric. Food Chem., Just Accepted Manuscript • DOI: 10.1021/acs.jafc.8b01890 • Publication Date (Web): 01 Jun 2018 Downloaded from http://pubs.acs.org on June 1, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 37
Journal of Agricultural and Food Chemistry
1
Chitosan-sodium phytate films with a strong water barrier and
2
antimicrobial properties via one-step consecutive stripping and
3
layer-by-layer casting technologies
4
Jie Yang1, Liu Xiong1, Man Li, Qingjie Sun*
5
College of Food Science and Engineering, Qingdao Agricultural University (Qingdao,
6
Shandong Province, 266109, China)
7
1
8
*Correspondence author (Tel: 86-532-88030448, e-mail:
[email protected])
9
College of Food Science and Engineering, Qingdao Agricultural University, 266109, 700
Equally-contributing author
10
Changcheng Road, Chengyang District, Qingdao, China.
11
ABSTRACT: : The pursuit of sustainable functional materials requires the development of
12
materials based on renewable resources and efficient fabrication methods. Hereby, we first
13
fabricated chitosan-sodium phytate films via one-step stripping and layer-by-layer casting
14
technologies, respectively. The proposed film fabrication methods are general, facile,
15
environmentally benign, cost-effective, and easy to scale up. The resultant one-step stripping film
16
was thin (9±1 µm), soft, transparent, and strong, while the thickness of the layer-by-layer casting
17
film was 70±3 µm. FTIR analysis of the films indicated the formation of interactions between the
18
phosphoric groups in sodium phytate and the amino groups in chitosan. More importantly, the
19
water vapor permeability values of one-step stripping and casting films were 4-5 orders of
20
magnitude lower than chitosan films reported before. Layer-by-layer casting films in particular
21
exhibited high tensile strength (49.21±1.12 MPa), which were more than three times stronger than
22
that of other polyelectrolyte multilayer films. Both types of films remained stable in an acidic
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
23
environment. Meanwhile, the layer-by-layer assembly films presented greater antimicrobial
24
activity than the stripping films. The developed chitosan-sodium phytate films can enhance
25
several biomedical and environmental applications, such as packaging, drug delivery, diagnostics,
26
microfluidics, and biosensing.
27
KEYWORDS: water vapor permeability, swelling, tensile strength, stability, coating
28
INTRODUCTION
29
Due to the drawbacks of petroleum-derived bio-stable plastics, researchers have recently
30
turned utilizing different kinds of biopolymers to prepare film.1 Generally, synthetic polymers
31
were used to enhance the barrier properties of films; however, the increased use of synthetic
32
polymers has raised serious concerns on account of their serious recycling and environmental
33
challenges.2 Nowadays, it is of commercial interest to develop natural, sustainable, renewable, and
34
functional films. 3,4 In general, biopolymers derived from natural products, like polysaccharides
35
and proteins, are considered ideal candidates to replace synthetic polymers for various
36
applications because of their low cost, the renewability, biodegradability, and biocompatibility of
37
their sources, and their non-toxic, environmentally friendly processes.5 Lately, chitosan, an
38
electropositive biopolymer, has attracted widespread interest in the field of food coating and
39
wrapping materials due to its non-toxic, biocompatible, biodegradable, antimicrobial, and good
40
film-forming properties.6
41
However, the use of pure chitosan films has thus far been limited because they tend to be
42
rigid, brittle, and have poor water resistance, low mechanical strength, and so on.7 Thus, several
43
studies have been conducted, mostly in the last decade, to modify chitosan films both physically
44
and chemically. For example, many chemical crosslinkers, such as formaldehyde, glyoxal,
ACS Paragon Plus Environment
Page 2 of 37
Page 3 of 37
Journal of Agricultural and Food Chemistry
45
glutaraldehyde, and genipin, have been investigated to improve film wettability, elongation at
46
break, and thermal stability compared to pure chitosan film.8 Nevertheless, these crosslinkers are
47
evermore associated with a negative environmental impact. Porta et al.9 reported that the
48
chitosan-based edible films crosslinked with transglutaminase could create environmentally
49
friendly bioplastics. But it could not meet industrial demand due to its high cost and low efficiency.
50
Hence, developing biodegradable films with a low cost, high water vapor barrier, and enhanced
51
mechanical properties on a large scale is still a critical issue.
52
One major research direction has focused on the water vapor barrier properties and tensile
53
strength of natural chitosan-sodium phytate films, which can expand the application scope to a
54
significant extent. This study was inspired by a previous study on the preparation of
55
chitosan-sodium phytate nanoparticles through strong electrostatic and hydrogen bond interactions
56
between the phosphoric groups in sodium phytate and the amino groups in chitosan.10 Sodium
57
phytate consisted of six phosphate groups and was chosen as the negatively-charged polyanions,
58
as well as being widely used as a safe food additive extracted from natural raw materials, such as
59
plant bran and seeds. Importantly, sodium phytate shows excellent antibacterial activity and is
60
listed as a “generally recognized as safe” (GRAS) substance by the Food and Drug Administration
61
of the United States.11 Until now, only a few studies have reported that phytic acid is successfully
62
assembled into layer-by-layer films with chitosan.12 However, to the best of our knowledge,
63
sodium phytate has not previously been used to prepare chitosan films.
64
Generally, the film’s properties are closely connected with the type of preparation method
65
that is used. In this work, we prepared chitosan-sodium phytate films using two types of facile
66
methods, one-step consecutive stripping and layer-by-layer (LBL) casting technologies.
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
67
Commonly, one-step stripping film is formed at the solution interface with the key catalyst (such
68
as abundant oxygen molecules)13 or high temperature.14 Interestingly, our chitosan-sodium phytate
69
film can be prepared at room temperature without adding anything else. The LBL casting
70
technique is also a simple, easy, versatile, flexible, handling, inexpensive, and powerful tool for
71
creating stratified and versatile multilayer films with strong mechanical properties, based on
72
interactions between multivalent molecules and macromolecules.15 The technique has a number of
73
advantages, for example, the film thickness can be controlled with an almost defect-free structure;
74
Secondly, it is very versatile and can accommodate various components.16 We systematically
75
investigated the formation, physicochemical properties, stability, mechanism of film formation,
76
and antimicrobial activity of the chitosan-sodium phytate films. Such chitosan-sodium phytate
77
films may be recommended for different applications, including food, medical sciences, and drug
78
delivery.
79
MATERIALS AND METHODS
80
Materials: :Chitosan was purchased from Shanghai Ryon Biological Technique Co., Ltd.
81
(Shanghai, China). The viscosity-average molecular weights of chitosan were 1092±50 kDa and
82
the degree of chitosan deacetylation was approximately 90%. Sodium phytate was obtained from
83
Beijing Solarbio Science & Technique Co., Ltd. (Beijing, China). Urea was provided by
84
Sinopharm Chemical Reagent Co., Ltd. (Beijing, China). Staphylococcus aureus (S. aureus, ATCC
85
25923) and Escherichia coli (E. Coli, ATCC 25923) were acquired from Nanjing Bianzhen
86
Biological Technology Co., Ltd. Lysogeny broth (LB) powder was supplied by Thermo Fisher
87
Scientific Inc. (Beijing, China). All chemicals were of analytical grade and used without further
88
purification.
ACS Paragon Plus Environment
Page 4 of 37
Page 5 of 37
Journal of Agricultural and Food Chemistry
89
Film Fabrication
90
Film-stripping technique. Film-stripping technique: Chitosan was dissolved in 2.0 wt%
91
glacial acetic acid to prepare 2.0-5.0 wt% solution. The concentration of sodium phytate solution
92
was 0.625-4.0 wt%. Chitosan solution was first added into a beaker and then sodium phytate
93
solution was added on the surface of the chitosan solution and promptly smoothed out. The
94
volume ratio of chitosan to sodium phytate was 5:1. Then, the chitosan-sodium phytate film was
95
spontaneously formed rapidly within 1 min at the chitosan/sodium phytate interface without
96
stirring. Only the part of chitosan contacting with the sodium phytate solution was converted into
97
film. The film was stripped using tweezers and washed with water three times to remove excess
98
chitosan and sodium phytate. After the first film was finished, sodium phytate solution left on the
99
surface of the chitosan solution was removed. Then, pouring the sodium phytate solution into the
100
surface of the chitosan solution spontaneously formed the second film. The second film was
101
stripped and washed with water as mentioned above. This stripping process could be repeated
102
continuously. Finally, the wet film was allowed to air-dry on a glass pane.
103
Layer-by-layer casting technique. The chitosan/sodium phytate multilayer films were
104
prepared based on the LBL casting technique described previously.17 A 20 mL of 2.0-5.0 wt%
105
chitosan solution was first cast on a glass plate, forming the first layer. Subsequently, another 5
106
mL of sodium phytate solution (0.625-4.0 wt%) was cast on top of the previous chitosan layer. By
107
repeating this process, chitosan/sodium phytate multilayer films consisting of 10 layers were
108
prepared. All films were easily peeled off from the supporting petri dish after they were dried in an
109
oven (60ºC). The corresponding films with n layers were denoted as (chitosan/sodium phytate)n.
110
All the films were stored in a conditioning room (25ºC and 75% RH) for 3 days before further
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
111
characterization.
112
Characterization. The light transmittance of the films was monitored using an ultraviolet
113
(UV)-visible Shimadzu 1601 PC spectrophotometer (Tokyo, Japan) by scanning from 260 to 360
114
nm.18 The films were cut into strips (1 × 4 cm2) and placed directly into the test cell of the
115
spectrophotometer. The opacity was calculated by the following equation:
A χ
116
Opacity =
117
where A was the absorbance of film at 600 nm and x was the film thickness (mm).
118
The film thickness of film was determined as the average of 5 random positions of each
119
sample using a thickness meter (MP0, Fischer, Germany). The zeta potential (ζ potential) was
120
determined by dynamic light scattering (DLS) using a Malvern Zetasizer Nano (Malvern
121
Instruments Ltd., UK). The measurements were performed on samples diluted in MilliQ water at
122
25ºC. X-ray diffraction (XRD) measurement was conducted on an X-ray diffractometer (Bruker
123
D8 ADVANCE, Karlsruhe, Germany). The diffractograms were recorded over an angular range
124
(2θ) of 4–40º, with a step size of 0.02º and a step rate of 2 s per step. Fourier transform infrared
125
spectroscopy (FTIR) was performed on a Nicolet 6700 FTIR spectrometer (Thermo Scientific,
126
USA) at a resolution of 4 cm-1 in the range of 400-4000 cm-1 by cumulating. The water vapor
127
permeability (WVP) of the films was determined gravimetrically.19 Before testing, the films were
128
conditioned at 25ºC for 3 days in a desiccator with a relative humidity (RH) of 75%. The film
129
specimen was sealed on a circular dish (diameter of 30 mm) filled with 15 g of oven dried calcium
130
chloride (CaCl2) that can maintain 0% RH in the circular dish. The circular dish was kept in the
131
test chamber and weighed every 12 hours for 3 days. The amount of water vapor that penetrated
132
through the film was determined by the weight increase of the circular dish. The WVP was
(1)
ACS Paragon Plus Environment
Page 6 of 37
Page 7 of 37
Journal of Agricultural and Food Chemistry
133 134
calculated as follows:
WVP(g / m ⋅ h ⋅ Pa ) =
m×d A×t×P
(2)
135
where m is the weight increment of the cell (g), d is the film thickness (m), A is the area exposed
136
(m2), t is the time lag for permeation (h), and P is the water vapor partial pressure difference across
137
the film (Pa).
138
The gravimetric method was used to determine the water solubility and degree of swelling of
139
the films.20 The weight of the film strips (1×4 cm2) was determined (m1). Then, the samples were
140
dried at 105ºC for 24 h to obtain the dry mass (m2). The samples were submerged in distilled
141
water at 25ºC for 24 h and achieved a constant mass (m3). Then, the samples were dried at 105ºC
142
for 24 h, after which the dry weight of the sample was determined (m4). The water solubility,
143
degree of swelling, and moisture content were calculated as follows:
144 145 146
m2 − m4 m4 m3 − m 2 Degree of swelling (%)= m2 m1 − m 2 Moisture content (%)= m1
Water solubility (%)=
(3) (4) (5)
147
Thermal analyses (TGA) of films were measured simultaneously by TGA/DSC2 (METTLER
148
TOLEDO, Greifensee, Switzerland). Approximately 3 mg of films were heated from 30 to 600ºC
149
at a heating rate of 10ºC/min. The weight loss as a function of temperature was analyzed.
150
The mechanical properties of one-step stripping film, which was somewhat soft, were
151
executed using a texture analyzer (TAXTplus, Stable Micro Systems, Surrey, U.K.), fitted with an
152
A/SPR probe. The test speed was 3 mm/s. The strong LBL casting film was determined on an
153
electronic universal testing machine (WDW3100, Changchun, China) at room temperature. The
154
samples were cut into rectangular strips (10 mm × 100 mm). The clamp distance was 20 mm, and
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
155
the draw rate was 20 mm/min. Based on the resultant stress-strain curves, the strength at break,
156
Young’s modulus, elongation at break, and toughness were obtained. Before the testing, the strips
157
were preconditioned at 75% RH for 3 days at room temperature (25ºC).
158
Scanning electron microscopy (SEM) (S-4800, Hitachi Instruments Ltd., Tokyo, Japan) was
159
used to study the morphology and topography of the surface and cross sections of the films. The
160
films were frozen in liquid nitrogen and then fractured immediately. The surfaces and the fracture
161
cross sections were sputtered with gold and then photographed. The acceleration voltage was set
162
to 1 kV.21
163
Glass transition temperature readings of the films at sub-zero temperatures were performed
164
by differential scanning calorimetry DSC1 (METTLER TOLEDO, Switzerland) at the scan rate of
165
10ºC/min from -70 to 25ºC in an argon gas atmosphere. Films were dried in a vacuum oven at
166
40ºC for 24 h to remove water without changing the solid-state structure. The samples were
167
incubated at 25ºC for 3 days under various RHs, which were controlled by the saturated water
168
vapor of 8 types of salt, according to a previous method. The 8 salts used in this study were
169
lithium chloride (RH 11%), magnesium chloride (RH 33%), potassium carbonate (RH 43%),
170
sodium bromide (RH 58%), potassium iodide (RH 69%), sodium chloride (RH 75%), potassium
171
chloride (RH 84%), and potassium sulfate (RH 97%).
172
pH and temperature stability. The stability of chitosan-sodium phytate films at different
173
pH levels and temperatures was determined using a gravimetric method to measure the erosion of
174
the films. The dried films were weighed (W0) and soaked in different pH buffer solutions (pH 2-9)
175
at room temperature or 4, 25, 37, and 60ºC water at pH 7. The films were removed from the
176
medium after 1 h of incubation, blotted using filter paper to remove excess water, and then dried
ACS Paragon Plus Environment
Page 8 of 37
Page 9 of 37
Journal of Agricultural and Food Chemistry
177
in a hot air oven at 60ºC to obtain a constant weight (Wd).22 The erosion of the films was
178
calculated according to the following equation:
W0 − Wd ×100 W0
179
Erosion (%) =
180
The stability of film in different solvents. The erosion of the films was measured to
181
determine the interaction force of films between chitosan and sodium phytate. The dried films
182
were soaked in each dissociating reagent, including sodium chloride (NaCl, 10, 50, 100, 250, and
183
500 mM) and urea (1, 2, 3, 4, and 5 M). The films were removed from the medium after 1 h of
184
incubation, blotted using filter paper to remove excess water, and then dried in a hot air oven at
185
60ºC to obtain a constant weight. The erosion of the films was determined according to the
186
above-mentioned equation (6).
(6)
187
Antibacterial property. An aliquot of 300 µL of the bacterial suspension (105 CFU/mL)
188
with 2.7 mL of LB broth was transferred into sterile tubes. The film samples were soaked in the
189
bacterial solution and incubated at 37°C for 4 h. The final inoculum was recultivated on a solid
190
agar plate surface for 24 h. We determined the antibacterial rates by the following equation:
CFUcontrol − CFU exp erimental × 100 CFUcontrol
191
Antibacterial rate (%) =
192
where the bacteria only served as the control, while the chitosan-sodium phytate film
193
(7)
prepared by the film-stripping and LBL-casting technique comprised the experimental groups.23
194
Statistical analysis. Each measurement was carried out using at least three fresh,
195
independently prepared samples. The results were reported as the mean values and standard
196
deviations. The experimental data were analyzed by the analysis of variance (ANOVA) with the
197
SPSS V.17 statistical software package (SPSS Inc., Chicago, IL). Differences were considered at a
198
significance level of 95% (p < 0.05).
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
199
RESULTS AND DISCUSSION
200
Formation of chitosan-sodium phytate film. The pH of the chitosan solution was 3.0 (ζ
201
potential = +45 mV). The sodium phytate was dissolved separately in water and the pH of the
202
solution was 11.0 (ζ potential = -13 mV). The film fabrication process of the film-stripping and
203
LBL-casting methods is shown in Figure 1. To develop an optimal strategy for the preparation of
204
smooth, uniform, strong, and biocompatible chitosan-sodium phytate films with tunable properties,
205
the parameters that influence the properties of the films were systematically investigated.
206
Characterization of chitosan-sodium phytate films
207
The thickness, opacity, and water vapor permeability. The thickness, opacity, and water
208
vapor permeability of the films were characterized (Table 1 and Table S1). The thickness of both
209
stripping and casting films increased with the increasing concentration of sodium phytate. The
210
resultant stripping film was thin with thickness of 9±1 µm, which was thinner than protocatechuic
211
acid grafted chitosan films (44.1 µm).24
212
The opacity is a critical property when films are applied to food packaging to improve
213
product appearance.25 The opacity values of stripping films with incremental sodium phytate
214
concentrations ranging from 0.625% to 5% (w/w) led to a significant decrease from 4.556±0.220
215
to 2.308±0.102 A600/mm. The LBL films presented the minimum opacity values of 0.992±0.011
216
A600/mm at 1.25% sodium phytate. The UV-vis spectrometer was used to investigate the
217
transmittance of stripping and casting films (Figure 2A, B, Figure S1). The light transmittance of
218
the films decreased sharply at around 315 nm with the increasing concentration of sodium phytate.
219
The stripping films possessed remarkably low transparency (61%, at around 315 nm) at the
220
sodium phytate concentration of 4.0 wt%. The casting films exhibited a lower transmittance of
ACS Paragon Plus Environment
Page 10 of 37
Page 11 of 37
Journal of Agricultural and Food Chemistry
221
21% at around 324 nm at the sodium phytate concentration of 4.0 wt%. Our findings suggested
222
that LBL film provided better protection of food quality from ultraviolet light damage.
223
Figure 2 (C and D) shows a few pieces of paper with the logo of Qingdao Agricultural
224
University placed under the chitosan/sodium phytate films. The logo can be seen clearly through
225
the film. The color of the stripping films did not change significantly (Figure 2C and Figure S2
226
A-B); however, the color of the casting films turned a deeper yellow (Figure 2D and Figure S2
227
C-E) with the increased concentration of sodium phytate. The obtained stripping films were glossy
228
and extremely flexible (Figure 2E), while LBL casting films were tough and pressure-resistant
229
(Figure 2F), which was due to strong interactions between chitosan and sodium phytate by
230
layer-by-layer technology. The interactions not only greatly enhanced the toughness of the films,
231
enabling them to tolerate substantial deformation, but also facilitated optically transparent
232
materials.
233
Since the stripping film surfaces were different, one side was enriched in chitosan and the
234
other was in sodium phytate. Considering the film application as coating materials, generally,
235
chitosan is first coated, and then sodium phytate is added on the surface of chitosan. Therefore, we
236
chose the surface of sodium phytate to be exposed to the high water activity environment during
237
the WVP tests. The WVP value increased with the increasing chitosan concentration. The stripping
238
film exhibited a minimum WVP of 1.654±0.062 ×10-11 g/m·h·Pa with 1.25% sodium phytate and
239
3% chitosan. Then, the WVP of stripping films increased to 5.085±0.162×10-11 g/m·h·Pa when the
240
chitosan concentration increased to 5%, and the maximum WVP occurred with 5% chitosan and
241
5% sodium phytate. However, the casting film exhibited minimum and maximum WVP values of
242
2.150±0.099×10-11
g/m·h·Pa
(with
3%
chitosan
and
0.625%
ACS Paragon Plus Environment
sodium
phytate)
and
Journal of Agricultural and Food Chemistry
243
23.549±0.918×10-11 g/m·h·Pa (with 5% chitosan and 4% sodium phytate), respectively. This
244
tendency could be explained by the higher hydrophilicity (NH3+ and -OH groups) of the films with
245
higher concentrations of chitosan and sodium phytate. The WVP values achieved for two kinds of
246
chitosan-sodium phytate films were four to five orders of magnitude lower than chitosan-based
247
films (3.32 × 10-10 g(m s Pa)-1, ≈1.20×10-6 g(m h Pa)-1).26 Bourtoom and Chinnan 27 reported that
248
the WVP value of rice starch-chitosan film increased after the incorporation of chitosan. Bonilla et
249
al.28 also suggested that the WVP value of wheat starch-glycerol films increased with the amount
250
of chitosan embedded.
251
Water solubility and degree of swelling. Water solubility and the degree of swelling are
252
important factors in determining the application of bio-based films. As shown in Figure 3A and B,
253
the moisture content (about 20%) of both the stripping and casting films was not affected by the
254
concentration of sodium phytate. However, the water solubility of the stripping films slightly
255
decreased from 21.49% to 15.16% with the increasing of sodium phytate concentration. In water,
256
the stripping film showed a decreased swelling degree from 91.63 to 66.34%, but it still
257
maintained its original shape. The water solubility and swelling degree values for the stripping
258
films were much lower than that of polyphenol-chitosan film (19.93±0.76% and 353.92±11.21%,
259
respectively), as reported by Sun et al.29 The outstanding water resistance could be ascribed to the
260
compact structure that hindered the water penetration into the films (by decreasing the permeation
261
of water into the films via capillary force). It's worth noting that for casting films, with the
262
increase of the concentration of sodium phytate, the water solubility continually increased, while
263
the degree of swelling first increased and then increased (Figure S3). Moreover, at the same
264
concentration of sodium phytate, the degree of swelling gradually increased with the increase of
ACS Paragon Plus Environment
Page 12 of 37
Page 13 of 37
Journal of Agricultural and Food Chemistry
265
chitosan concentration. This could be due to the swelling of chitosan in the presence of acetic acid.
266
Bourtoom and Chinnan 30 reported that higher solubility indicated lower water resistance.
267
Mechanical properties. To evaluate the potential of films as structural material for industry,
268
the mechanical properties of chitosan-sodium phytate films were characterized. The results of
269
tensile strength, elongation at break, and Young's modulus for films prepared by film-stripping
270
technology are shown in Table S2. The stripping film with the highest tensile strength values was
271
32.44±1.49 MPa. The stress-strain curves of the LBL films obtained from the tensile tests are
272
shown in Figure 3C and Figure S4. The tensile strength and elongation at break values of the LBL
273
films are clearly dependent on the concentration of chitosan and sodium phytate, which yields a
274
maximum tensile strength of 49.21±1.12 MPa at 4.0 wt% chitosan and 1.25 wt% sodium phytate
275
(Table S3), which was higher than that of the stripping film. When the concentration of chitosan
276
was 4.0 wt%, the elongation at break and Young’s modulus of films were 25.10±0.71% and
277
3646.68±146.63 MPa, respectively. Thus, strong interaction and good compatibility between
278
chitosan and sodium phytate could have led to uniform stress transfer through the film, resulting in
279
high mechanical strength. The value of tensile strength for LBL films was stronger than that of
280
transcinnamaldehyde-chitosan films (15-20 MPa). 31 Ho et al. 32 noted the beneficial effect of the
281
electrostatic interactions of opposite charges in composite systems on mechanical properties.
282
Thermal properties. Thermogravimetric analysis (TGA) was performed to illustrate the
283
thermal stability of both the stripping and casting films (Figure 3D-G). It can be seen that all films
284
undergo thermal degradation in three stages. The first stage of weight loss of all the films occurred
285
at up to 80ºC and was attributed to the desorption of physically adsorbed water that accounted for
286
20% of the weight of both samples. Later on, the stripping films suffered a drastic weight loss and
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
287
deacetylation of chitosan chains up at 244ºC. The casting film with 0.625% sodium phytate began
288
the step of maximum weight loss at 267.3ºC, while 1.25, 2, 2.5, and 3% were shown at 257.4,
289
260.3, 265.9, and 238.9 ºC, respectively. Finally, the weight loss continued due to charring of the
290
degraded backbone and there was almost complete degradation up to 600ºC. This result agreed
291
with some reports in the literature. 33 After the final thermal destruction, it was noteworthy that the
292
residual percentages of the casting films at 600ºC were more than 50%, while the residual
293
percentages of the stripping films were less than 50%. This result suggested that the thermal
294
stability of the casting film was higher than that of the stripping films.
295
Film-forming time of stripping films. When 5 ml of 3.0 wt% chitosan solutions were added
296
with 1 ml 1.25 wt% or 2.5 wt% sodium phytate solutions, the stripping films were immediately
297
formed at the chitosan/sodium phytate solution interface within 60 s. The chitosan solution
298
remained in the upper space of the inverted glass vial (Figure 4A, Figure S5A). Commonly,
299
tripolyphosphate (TPP) was used to prepare chitosan film. However, the chitosan-TPP film
300
exhibited a longer film-formation time of ≈1.5 h (Figure S5B). Compared with chitosan-TPP film,
301
the film-formation time of chitosan-sodium phytate film was shortened by 89%. Thus, the
302
formation time of chitosan-sodium phytate film prepared by film-stripping technology was short
303
as well as an ambient temperature. The possible formation mechanisms of film formed in a
304
chitosan/sodium phytate interface-specific manner may be due to the amidogen and hydroxy of
305
chitosan and the rich presence of the phosphate group and hydroxy of sodium phytate. They could
306
form non-covalent bonds, such as ionic bonds and hydrogen bonds, which assembled a
307
three-dimensional network at the interface of chitosan and sodium phytate.
308
The thickness of stripping film gradually increased from 9±1 µm (1 min) to 122±6 µm (30
ACS Paragon Plus Environment
Page 14 of 37
Page 15 of 37
Journal of Agricultural and Food Chemistry
309
min) (Figure 4B), and the appearance and transparency of the film became worse over time. The
310
film opacity also increased significantly with the increasing of time (Figure S6 A). The water
311
solubility and moisture content of stripping films showed no change as the preparation time
312
increased, and the lowest swelling degree of the films was found at the preparation time of 5 min
313
(Figure S6 B). In the UV-vis spectrum, the film transmittance gradually decreased with the
314
increasing of formation time, which indicated that the thicker the film, the stronger the ultraviolet
315
absorption (Figure 4C).
316
The thermal degradation of stripping films formed at different time are shown in Figure 4D
317
and E. All the stripping films had a weight loss of about 10%, which occurred because of the
318
release of water molecules from the films. Then, the weight loss in the temperature range of
319
200-240ºC corresponded to the degradation and deacetylation of chitosan. The thermal
320
degradation temperature of the films prepared at different time was similar. The FTIR spectra of
321
the stripping films prepared in various time frames are shown in Figure S7. The intensity of
322
hydroxyl groups peak at 3000-3500 cm-1 was dramatically stronger as formation time increased,
323
indicating that the interaction between chitosan and sodium phytate became stronger.
324
Stripping numbers of films. The chitosan-sodium phytate films prepared by one-step
325
film-stripping technology have a fascinating feature of consecutively stripping at room
326
temperature. The UV-vis light transmission of stripping films with ten stripping numbers are
327
shown in Figure 5A. The transparency of film slightly decreased at around 325 nm from 81% to
328
80% with the increase of stripping numbers. The thickness of the stripping film gradually
329
increased from 50±1 µm to 69±3 µm. The opacity of the films also increased with the increase of
330
stripping numbers (Table S4). Figure 5B shows that stripping numbers did not influence the
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
331
moisture content (about 20%) of the films. Moreover, the water solubility and swelling degree of
332
the stripping films only slightly changed after the tenth time.
333
The surface morphology images showed that there were no differences in the external
334
appearance, except for the ninth and tenth time, all of which were very smooth and uniform,
335
indicating that the films could be consecutively stripping (Figure 5C). SEM analysis of the
336
fractured cross-section structure of stripping films revealed there was an increasing thickness as
337
the stripping numbers increased (Figure 5D).
338
Forming the temperature of stripping film. Large differences in thickness at different
339
temperatures were observed (Figure S8 A). The thickness of chitosan-sodium phytate film
340
fabricated at 10, 25, or 80ºC was thin, or less than 50 µm. The stripping films prepared at 4ºC had
341
the lowest opacity (Figure S8 B).
342
The stripping films possessed highly remarkable light transmittance at 25ºC. Above or below
343
this temperature, the light transmittance would decrease sharply at around 315 nm (Figure S8 C).
344
The film-forming temperature did not have an impact on the moisture content (about 20%) of the
345
films (Figure S8 D). However, the water solubility of the stripping films increased significantly as
346
the temperature increased, with the minimum at 4ºC, and the swelling degree decreased slightly
347
thereafter at higher temperatures (50 and 80ºC).
348
Incubation temperature had no effect on the major chemical groups of the stripping films
349
(Figure S8 E). The thermal stability of the stripping film prepared at different temperatures was
350
evaluated by TGA, as shown in Figure S8 F and G. All the films had a weight loss of about 13% in
351
the range of 45-120ºC, owning to the release of water molecules from the films. The films made at
352
25ºC and 80ºC had maximum weight loss at 237.3 and 238.1ºC, while those made at 4, 10, and
ACS Paragon Plus Environment
Page 16 of 37
Page 17 of 37
Journal of Agricultural and Food Chemistry
353
50ºC had maximum weight loss at 219.7, 220.9, and 245.7ºC, respectively.
354
Assembling layer numbers of films. The (chitosan/sodium phytate)1 film (first layer) could
355
not form perfectly, so we started from the second layer. It was determined that the increase of the
356
thickness of the films was proportional to the increase in the number of layers (Figure S9A). The
357
(chitosan/sodium phytate)2 films had a thickness of 49±1 µm, while the (chitosan/sodium
358
phytate)11 counterpart had a thickness of 113±4 µm, suggesting that the film formation process
359
was uniform and repeatable. At room temperature, we tested the mechanical properties of films
360
with different numbers of layers (Figure S9B). We found that the tensile properties gradually
361
enhanced with the increasing number of layers and (chitosan/sodium phytate)10 films, with a
362
maximum stress of 38.81 MPa, and also had a uniaxial stretchability of 12.7%, which is superior
363
to other films. Hence, we chose chitosan/sodium phytate)10 films for the subsequent study. The
364
resultant (chitosan/sodium phytate)10 films exhibited much higher tensile strength (MPa) than the
365
chitosan and sodium alginate LBL thin films (13.0 MPa) reported by Mandapalli et al. 34
366
The surface morphology and fractured cross-section structure of films were confirmed by
367
SEM, as shown in Figure S9C-V. It is clear that the LBL films had a smooth surface. The FTIR
368
spectra of LBL casting films presented strong absorption at 3000-3500 cm-1, related to the
369
stretching vibration of the hydroxyl groups (O-H), with an increasing number of layers (Figure
370
S10), which indicated that the interactions between chitosan and sodium phytate became stronger
371
with the increasing number of layers.
372
Moisture content, glass transition temperatures, and TGA. The moisture content of the
373
stripping and casting films increased as the RH increased (Figure S11A). The highest moisture
374
content was 36.84 ± 0.37 wt% for casting film under an RH of 97%. It appeared that dried films
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
375
still had a negligible amount of water. The films were dried in a vacuum oven at 40°C for 24 h;
376
however, bound water molecules still existed. Previously, Agarwal et al. 35 reported that water
377
molecules strongly bound to silks in the films of regenerated Bombyx mori silk. To study the glass
378
transition in both stripping and casting films, DSC experiments were performed (Figure S11B, C).
379
The glass transition temperature of stripping and casting films were detected between -35 and
380
-40°C. The results showed that the glass transition temperature of the films was hardly dependent
381
on the moisture content of the films. The possible reason was that the WVP values of films were
382
four to five orders of magnitude lower than other chitosan-based films, so the films we prepared
383
had low water absorption. Moreover, the DSC results of films showed no endotherm peak of ice
384
melting, indicating that water in the films were bound water rather than free water. Therefore,
385
different humidity did not affect glass transition temperature of films.
386
Both stripping and casting films incubated at different RHs were examined by TGA, and a
387
three-step weight decrease was detected (Figure S11D and G). The first weight decrease, which
388
was due to the water removal (evaporation), proceeded up to approximately 200°C and was
389
dependent on the RH. The second decrease in weight, which was attributed to thermal degradation,
390
was detected above 250°C, when the film turned into black char. The derivative plot showed the
391
temperature at which the water removal and degradation occurred at the fastest rates (Figure S11E,
392
F, H and I). The degradation temperature was independent of the water content, suggesting that the
393
water molecules were completely removed at 200°C, and the breakage of the primary chain in the
394
chitosan molecules occurred without water. Thus, the thermal degradation of the films occurred
395
independent of the moisture content. Conversely, water removal was dependent on the moisture
396
content of the films.
ACS Paragon Plus Environment
Page 18 of 37
Page 19 of 37
Journal of Agricultural and Food Chemistry
397
Stability of films. The erosion stability of the films was evaluated in buffer media with
398
different pH values, ranging from 2 to 9 at 25ºC (Figure S12). The stripping films displayed
399
excellent stability over the whole pH range. The erosion values increased from 6.7±0.3% to 30.2 ±
400
0.7%, with the pH increasing from 2 to 9. It would be expected that the films started to slightly
401
erode above pH 6 (16.7±0.3%). When the stripping films were immersed in an alkaline
402
environment (pH >7), the films still maintained their structural integrity, even up to pH 9 (Figure
403
S12 A). However, a significant increase in the erosion of casting films was observed at pH 6
404
(25.8± 0.03%) relative to the other acidic pHs (Figure S12 B). The erosion values increased
405
substantially, ranging from 26.7 ± 0.04% (pH 7) to 72.1 ± 1.1% (pH 9) (Figure S12 B). Altogether,
406
under all the conditions, the erosion values of the stripping films were lower than that of the
407
casting films, showing preferable pH stability compared to other natural polyelectrolytes films.36
408
The erosion values of both stripping and casting films increased with the increasing of
409
temperature from 4 to 60ºC (Figure S13) as a result of the destruction of a network structure of
410
films. Interestingly, both stripping and casting films retained their temperature response as
411
chitosan chains were dissociated from the network. Compared to casting films, stripping films had
412
higher thermal stability. This result was in accordance with the chitosan-based films reported by
413
Leceta et al. 37
414
Interaction mechanism. The X-ray diffraction pattern of pure chitosan, sodium phytate, and
415
chitosan-sodium phytate films are shown in Figure S14A and B. The XRD pattern of pure chitosan
416
presented two characteristic peaks at 2θ = 10.6º and 2θ = 20.1º, which are related to the
417
occurrence of hydrated hydrogen-bonded chitosan crystallized phase form II. 38 However, both the
418
stripping and casting films revealed a very poor diffraction pattern, illustrating the amorphous
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
419
phase of the films. Significantly, there was a peak in casting films with an intensity maximum
420
around 9.3º, indicating that the casting films contained extra chitosan chains. 39
421
The FTIR spectra of pure chitosan, sodium phytate, and composite films are shown in Figure
422
S14 C and D and Figure S15. Regarding chitosan, the strong absorption at 3346 cm-1 is related to
423
the stretching vibration of the hydroxyl groups (O-H), as well as intermolecular hydrogen bonding
424
within the polysaccharide. The characteristic absorption peak appearing at 2866 cm-1
425
corresponded to the C-H stretching vibration. Two characteristic bands at 1633 cm-1 and 1540 cm-1
426
are due to C-O stretching (amide I) and N-H bending (amide II), respectively. The characteristic
427
bands of sodium phytate are centered at 965, 1074, and 3147 cm-1. The bands of 965 cm-1
428
corresponded to PO43- and the 1074 cm-1 is the characteristic band of P=O, while the peak at 3147
429
cm-1 is assigned as the OH-characteristic band.40 After film formation, the stripping film presented
430
the characteristic peak of chitosan, but the peak of chitosan disappeared at 2866 cm-1. The
431
hydroxyl groups and amide II band of the casting films shifted from 3346 to 3267 cm-1 and 1540
432
to 1547 cm-1, respectively. Furthermore, the new peak at 1389 cm-1 appeared due to the
433
intermolecular interactions between chitosan and sodium phytate, which clearly confirmed the
434
electrostatic interactions between the phosphoric groups in sodium phytate and the amino groups
435
in chitosan.
436
To further analyze the interactions involved in chitosan-sodium phytate films, the
437
dissociation test of films in dissociation reagents was studied. The dissociation reagents used were
438
NaCl and urea, which can disrupt electrostatic interactions and hydrogen bonds, respectively. The
439
erosion of stripping and casting films remarkably increased with increased concentrations of NaCl
440
and urea (Figure 6), indicating that the formation of films occurred through both electrostatic
ACS Paragon Plus Environment
Page 20 of 37
Page 21 of 37
Journal of Agricultural and Food Chemistry
441
interactions and hydrogen bonds. It was found that the ionic strength had a more noticeable effect
442
on the erosion of casting films than that of stripping films, while the stripping films mainly took
443
advantage of hydrogen bonding attractions between chitosan and sodium phytate. The strong
444
electrostatic interactions between the amidogen groups of chitosan and the phosphate groups of
445
sodium phytate would significantly densify the film structure and subsequently enhance its
446
mechanical properties.
447
Figure 6C represents the interplay change between the chitosan chains and sodium phytate of
448
films, as well as their stability, across the entire pH range. In acidic media, chitosan is fully
449
charged, and the films presented lower dissipation due to the combination of the ionization of
450
phosphate and amine groups, which revealed that the films became more rigid. A similar behavior
451
was already reported for gelatin-poly (galacturonic acid). 41 At pH 8, the
462
electrostatic repulsions between the negative charges of sodium phytate increased (drastic increase
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
463
in ζ potential) and the structural integrity for casting film was not maintained. This could be due to
464
the formation of casting film mainly through electrostatic interactions, resulting in a largely partial
465
dissolution of the films under alkaline conditions. The stripping film mainly depended on
466
hydrogen bonding, leading to only a partial dissolution of the film.
467
Antibacterial activity. Figure 7 (A) and (B) show representative images of E. Coli incubated
468
with the samples for 4 h for stripping and casting film, respectively. The pure chitosan and sodium
469
phytate solution presented a high quantity of living bacteria. For stripping films prepared with 3.0
470
wt% chitosan, there was no living bacteria when the concentration of sodium phytate was
471
increased to 2.5 wt%. With regard to casting films with 4.0 wt% chitosan, the bacteria were fully
472
inhibited above 1.25 wt% concentration of sodium phytate. Meanwhile, the number of colonies on
473
the agar was statistically analyzed. As shown in Figure 7C and Table S5, when the concentration
474
of sodium phytate was above 2.0 wt%, the stripping films and casting films exhibited excellent
475
antibacterial activity against S. aureus and E. coli (nearly 100%). Our results suggested that
476
chitosan-sodium phytate films prepared by casting technologies were superior to film-stripping
477
technologies in terms of antibacterial activity. This was due to higher solubility of casting films
478
than that of stripping films (Figure 3 and S3), which could lead to the release of higher levels of
479
antimicrobial substances.
480
In summary, we first prepared chitosan-sodium phytate films using one-step consecutive
481
stripping and layer-by-layer casting methods. The resultant films showed good water vapor
482
resistance properties. Moreover, their shapes were maintained even after 1 h of soaking in acidic
483
conditions. The yellowish color of the casting films indicated the strong electrostatic interactions
484
between chitosan and sodium phytate, which was supported by the FTIR spectra. The chitosan
ACS Paragon Plus Environment
Page 22 of 37
Page 23 of 37
Journal of Agricultural and Food Chemistry
485
films containing sodium phytate could improve UV barrier properties. No classical plasticizing
486
effect of the water on the glass transition was evident in the case of films. Importantly,
487
antibacterial experiments indicated that these casting films exhibited extremely efficient
488
antibacterial activities, indicating that chitosan-sodium phytate films can serve as a promising
489
coating to inactivate microorganisms. The chitosan-sodium phytate films provide a platform for
490
the engineering and assembly of advanced materials for food, medical, and industrial uses.
491
Supporting Information Available:
492
UV-vis transmission, opacity, WVP, solubility, swelling degree, moisture content, DSC, TGA,
493
Tg, XRD, mechanical properties and antibacterial rate of the films fabricated under other
494
preparation conditions; SEM analysis of casting films.
495
Notes
496 497 498
The authors declare no competing financial interest. ACKNOWLEDGMENTS
This work was supported by the Special Funds for Taishan Scholars Project of Shandong
499
Province (No. ts201712058).
500
REFERENCE
501
(1) Garcia-Valdez, O.; Champagne, P.; Cunningham, M. F. Graft modification of natural
502
polysaccharides via reversible deactivation radical polymerization. Prog. Polym. Sci. 2018, 76,
503
151-173.
504
(2) Alam, A.; Zhang, Y.; Kuan, H. C.; Lee, S. H.; Ma, J. Polymer composite hydrogels containing
505
carbon nanomaterials—Morphology and mechanical and functional performance. Prog. Polym.
506
Sci. 2018, 77, 1-18.
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
507
(3) Wang, B.; Torres-Rendon, J. G.; Yu, J.; Zhang, Y.; Walther, A. Aligned bioinspired cellulose
508
nanocrystal-based nanocomposites with synergetic mechanical properties and improved
509
hygromechanical performance. ACS Appl. Mater. Interfaces. 2015, 7, 4595-4607.
510
(4) Khalil, H. P. S. A.; Saurabh, C. K.; Tye, Y. Y. Seaweed based sustainable films and composites
511
for food and pharmaceutical applications: A review. Renew. Sust. Energ. Rev. 2017, 77, 353-362.
512
(5) Swartjes, J. J. T. M.; Das, T.; Sharifi, S. A functional DNase I coating to prevent adhesion of
513
bacteria and the formation of biofilm. Adv. Funct. Mater. 2013, 23, 2843-2849.
514
(6) Wang, H.; Qian, J.; Ding, F. Emerging chitosan-based films for food packaging applications. J.
515
Agric. Food Chem. 2018, 66, 395-413.
516
(7) Kerch, G. Chitosan films and coatings prevent losses of fresh fruit nutritional quality: A review.
517
Trends. Food Sci. Tech. 2015, 46, 159-166.
518
(8) Ma, X.; Lv, M.; Anderson, D. P. Natural polysaccharide composites based on modified
519
cellulose spheres and plasticized chitosan matrix. Food Hydrocolloid. 2017, 66, 276-285.
520
(9) Porta, R.; Mariniello, L.; Di, P. P. Transglutaminase crosslinked pectin- and chitosan-based
521
edible films: a review. Crit. Rev. Food Sci. 2011, 51, 223-238.
522
(10) Yang, J.; Lu, H.; Li, M.; Liu, J.; Zhang, S. L.; Xiong, L.; Sun, Q. J. Development of
523
chitosan-sodium phytate nanoparticles as a potent antibacterial agent. Carbohyd. Polym. 2017,
524
178, 311-321.
525
(11) Dost, K.; Tokul, O. Determination of phytic acid in wheat and wheat products by reverse
526
phase high performance liquid chromatography. Anal. Chim. Acta. 2006, 558, 22-27.
527
(12) Liu, H.; Mahmut, N.; Sun, P. Electrochemistry and electrocatalysis of myoglobin loaded into
528
multilayer films assembled with phytic acid and chitosan. Anal. Lett. 2012, 45, 242-250.
ACS Paragon Plus Environment
Page 24 of 37
Page 25 of 37
Journal of Agricultural and Food Chemistry
529
(13) Wang, Y.; Park, J. P.; Hong, S. H. Biologically inspired materials exhibiting repeatable
530
regeneration with self-sealing capabilities without external stimuli or catalysts. Adv. Mat. 2016, 28,
531
9961-9968.
532
(14) Denavi, G.; Tapiablácido, D. R.; Añón, M. C. Effects of drying conditions on some physical
533
properties of soy protein films. J. Food Eng. 2009, 90, 341-349.
534
(15) Humood, M.; Qin, S.; Song, Y. Influence of graphene reduction and polymer cross-linking on
535
improving the interfacial properties of multilayer thin films. ACS Appl. Mater. Inter. 2017, 6,
536
1107-1118.
537
(16) Richardson, J. J.; Björnmalm, M.; Caruso, F. Technology-driven layer-by-layer assembly of
538
nanofilms. Science. 2015, 348, 2491.
539
(17) Lei, D.; Zhu, L.; Jie, C. Robust guar gum/cellulose nanofibrils multilayer films with good
540
barrier properties. ACS Appl. Mater. Inter. 2017, 9, 5477-5485.
541
(18) Liu, F.; Antoniou, J.; Li, Y.; Yi, J.; Yokoyama, W.; Ma, J.; Zhong, F. Preparation of gelatin
542
films incorporated with tea polyphenol-nanoparticles for enhancing controlled release antioxidant
543
properties. J. Agric. Food Chem. 2015, 63, 3987-3995.
544
(19) Fan, J. M.; Ma, W.; Liu, G. Q.; Yin, S. W.; Tang, C. H.; Yang, X. Q. Preparation and
545
characterization of kidney bean protein isolate (KPI)echitosan (CH) com posite films prepared by
546
ultrasonic pretreatment. Food Hydrocolloid. 2014, 36, 60-69.
547
(20) Cmo, M. J.; Laurindo, B.; Yamashita, F. Effect of nanoclay incorporation method on
548
mechanical and water vapor barrier properties of starch-based films. Ind. Crop. Prod. 2011, 33,
549
605-610.
550
(21) Ge, S.; Li, M.; Ji, N.; Liu, J.; Mu, H.; Xiong, L.; Sun, Q. Preparation of a strong gelatin–short
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
551
linear glucan nanocomposite hydrogel by an in situ self-assembly process. J. Agric. Food Chem,
552
2017, 66, 177-186.
553
(22) Remunan-Lopez, C.; Bodmeier, R. Mechanical, water uptake and permeability properties of
554
crosslinked chitosan glutamate and alginate films. J. Control Release. 1997, 44, 215–225.
555
(23) Feng, W.; Geng, Z.; Li, Z. Controlled release behaviour and antibacterial effects of
556
antibiotic-loaded titania nanotubes. Mat. Sci. Eng. C Mater. 2016, 62, 105-112.
557
(24) Liu, J.; Meng, C. G.; Liu, S. Preparation and characterization of protocatechuic acid grafted
558
chitosan films with antioxidant activity. Food Hydrocolloid. 2017, 63, 457-466.
559
(25) Rao, M. S.; Kanatt, S. R.; Chawla, S. P.; Sharma, A. Chitosan and guar gum composite films:
560
Preparation, physical, mechanical and antimicrobial properties. Carbohyd. Polym. 2010, 82,
561
1243-1247.
562
(26) Costa, M. J.; Cerqueira, M. A.; Ruiz, H. A. Use of wheat bran arabinoxylans in
563
chitosan-based films: Effect on physicochemical properties. Ind. Crop. Prod. 2015, 66, 305-311.
564
(27) Bourtoom, T.; Chinnan, M. S. Preparation and properties of rice starch-chitosan blend
565
biodegradable film. LWT-Food Sci. Technol. LWT-Food Sci. Technol. 2008, 41, 1633–1641.
566
(28) Bonilla, J.; Atares, L.; Vargas, M.; Chiralt, A. Properties of wheat starch film-forming
567
dispersions and films as affected by chitosan addition. J. Food Eng. 2013, 114, 303–312.
568
(29) Sun, L.; Sun, J.; Chen, L. Preparation and characterization of chitosan film incorporated with
569
thinned young apple polyphenols as an active packaging material. Carbohyd. Polym. 2017, 163,
570
81-91.
571
(30) Bourtoom, T.; Chinnan, M. S. Preparation and properties of rice starch-chitosan blend
572
biodegradable film. LWT-Food Sci. Technol. 2008, 41, 1633–1641.
ACS Paragon Plus Environment
Page 26 of 37
Page 27 of 37
Journal of Agricultural and Food Chemistry
573
(31) Sun, X.; Sui, S.; Ference, C. Antimicrobial and mechanical properties of β-cyclodextrin
574
inclusion with essential oils in chitosan films. J. Agr. Food Chem. 2014, 62, 8914-8918.
575
(32) Ho, T. T. T.; Zimmermann, T.; Ohr, S.; Caseri, W. R. Composites of cationic nanofibrillated
576
cellulose and layered silicates: water vapor barrier and mechanical properties. ACS Appl. Mater.
577
Inter. 2012, 4, 4832-4840.
578
(33) Qu, X.; Wirsen, A.; Albertsson, A. C. Effect of lactic/glycolic acid side chains on the thermal
579
degradation kinetics of chitosan derivatives. Polymer. 2000, 41, 4841–4847.
580
(34) Mandapalli, P. K.; Labala, S.; Jose, A. Layer-by-Layer thin films for co-delivery of TGF-β
581
siRNA and epidermal growth factor to improve excisional wound healing. Aaps Pharmscitech,
582
2017, 1-12.
583
(35) Agarwal, N.; Hoagland, D. A.; Farris, R. J. Effect of moisture absorption on the thermal
584
properties of Bombyx mori silk fibroin films. J. Appl. Polym. Sci. 1997, 63, 401-410.
585
(36) Cheng, Y.; Lu, J.; Liu, S.; Zhao, P.; Lu, G.; Chen, J. The preparation, characterization and
586
evaluation of regenerated cellulose/collagen composite hydrogel films. Carbohydr. Polym. 2014,
587
107, 57–64.
588
(37) Leceta, I.; Guerrero, P.; Ibarburu, I.; Dueñas, M. T.; de la Caba, K. Characterization and
589
antimicrobial analysis of chitosan-based films. J. Food Eng. 2013, 116, 889-899.
590
(38) Chen, H.; Hu, X.; Chen, E.; Wu, S.; Julian McClements, D.; Liu, S.; Li, B.; Li, Y. Preparation,
591
characterization, and properties of chitosan films with cinnamaldehyde nanoemulsions. Food
592
Hydrocolloid. 2016, 61, 662-671.
593
(39) Cui, X. F.; Li, Q. F.; Li, Y.; Wang, F. H.; Jin, G.; Ding, M. H. Microstructure and corrosion
594
resistance of phytic acid conversion coatings for magnesium alloy. Appl. Surf. Sci. 2008, 255,
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
595
2098–2103.
596
(40) Suflet, D. M.; Pelin, I. M.; Timpu, D.; Popescu, I. pH-sensitive multilayers based on maleic
597
acid terpolymers with weak and strong acid moieties. Colloids Surf. A. 2013, 436, 113-122.
598
(41) Bhattarai, N.; Gunn, J.; Zhang, M. Chitosan-based hydrogels for controlled, localized drug
599
delivery. Adv. Drug Delivery Rev. 2010, 62, 83-99.
600
(42) Lee, H.; Mensire, R.; Cohen, R. E.; Rubner, M. F. Strategies for hydrogen bonding based
601
Layer-by-Layer assembly of poly(vinyl alcohol) with weak polyacids. Macromolecules. 2012, 45,
602
347-355.
ACS Paragon Plus Environment
Page 28 of 37
Page 29 of 37
Journal of Agricultural and Food Chemistry
Table 1. The thickness, opacity and WVP of the filmsa. Concentration of sodium phytate (%)b
Thickness (µm)c
Opacity
4.556±0.220a 4.300±0.141ab 4.083±0.160b 3.059±0.143c 2.700±0.113d 2.308±0.102e 1.214±0.051b 0.992±0.011d 1.048±0.032cd 1.141±0.101bc 1.195±0.049b 1.492±0.053a
Stripping film technique
0.625 1.25 2.0 2.5 3.0 4.0
9±1e 10±4de 12±3de 17±3cd 20±4bc 26±3ab
Casting film technique
0.625 1.25 2.0 2.5 3.0 4.0
70±3d 85±4c 105±3b 124±6a 128±4a 130±6a
a
WVP (×10-11 g/m×h×Pa) 2.902±0.131c 1.654±0.062e 1.786±0.076e 2.109±0.101d 2.811±0.128c 3.440±0.099b 4.052±0.182e 6.326±0.262d 6.946±0.262d 8.203±0.364c 11.642±0.541b 16.124±0.801a
The values correspond to the mean ± standard deviation. Values within each column followed by different letters indicate significant differences (P < 0.05). b The concentrations of chitosan were 3.0% and 4.0 wt% for the stripping and casting films, respectively. cThe thickness values for the casting films correspond to ten layers.
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
Chitosan
Page 30 of 37
Chitosan solution
Dissolution in acetic acid Stand degassing Stripping-film technique
Layer-by-layer casting technique
Sodium phytate Chitosan casting
Repeat
Repeat
Distributed on the surface of chitosan
Evenly coated Stripping-film
Film wash in water 45ºC drying
Air drying
Repeat for two times
Two layers of film
Repeat for ten times
Ten layers of film
Film
Soft, transparent
Ultrasoft, supertransparent
Figure 1. Preparation chart for chitosan-sodium phytate film using the film-stripping and layer-by-layer casting technique.
ACS Paragon Plus Environment
Page 31 of 37
Journal of Agricultural and Food Chemistry
0.625% 1.25% 2.0% 2.5% 3.0% 4.0%
Transmittance (%)
100 95 90
0.625% 1.25% 2.0% 2.5% 3.0% 4.0%
B 100 Transmittance (%)
A 105
85 80 75
80
60
40
70 65 60 260
20
280
300
320
340
360
260
280
300
320
340
360
Wavelength (nm)
Wavelength (nm)
C
D
E
F
Figure 2. (A) and (B) Light transmittance results at various concentrations of sodium phytate; (C) and (D) The photograph of the films and the concentration of sodium phytate from left to right: 0.625, 1.25, 2.0, 2.5, 3.0, and 4.0 wt%; (E) and (F) Digital photographs showing the flexibility of the films with 1.25 wt% of sodium phytate. (A), (C), and (E) The film prepared by film-stripping technique and the concentration of chitosan at 3.0 wt%; (B), (D), and (F) The film prepared by LBL technique and the concentration of chitosan at 4.0 wt%.
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
ab
80
bc
c
20
d
d
70 60
a b
b
b
b
B 3000
b
b
a
b c
P ercentage (% )
90
a
Solubility Swelling degree Moisture content
2000
40
c
30
c
b
c
b
c ab
a
b b
b
20
a
a
0
1.25
2.0
2.5
3.0
0.625
4.0
Concentration of sodium phytate (%)
E
80 70
0
5
10
15 20 Strain (%)
25
0.0000
-1
90
Deriv. mass (wt% °C )
0.625% 1.25% 2.0% 2.5% 3.0% 4.0%
100
20
0
1.25 2.0 2.5 3.0 4.0 Concentration of sodium phytate (%)
D 110 W e ig h t (% )
60 50
-0.0002 -0.0004
0.625% 1.25% 2.0% 2.5% 3.0% 4.0%
-0.0006 -0.0008 -0.0010
40
-0.0012
30 200
300
400
500
600
Temperature (°C)
F 100
0.625% 1.25% 2.0% 2.5% 3.0% 4.0%
90 80 70 60
100
G
0.0002 0.0000
-1
100
Deriv. mass (wt% °C )
0.625
30
10
10
0
0.625% 1.25% 2.0% 2.5% 3.0% 4.0%
C 50
d
d
1000
d
10
a
a
b
Stress (MPa)
Solubility Swelling degree Moisture content
a
W eig ht (% )
Percentage (% )
A
Page 32 of 37
200 300 400 Temperature (°C)
500
600
-0.0002 0.625% 1.25% 2.0% 2.5% 3.0% 4.0%
-0.0004 -0.0006 -0.0008 -0.0010 -0.0012
50
-0.0014 100
200
300
400
500
Temperature (°C)
600
-0.0016 100
200
300
400
500
600
Temperature (°C)
Figure 3. The solubility, swelling degree, and moisture content of the stripping film containing 3.0 wt% of chitosan (A), LBL film containing 4.0 wt% of chitosan (B); (C) Stress-strain curves of casting films with different concentrations of sodium phytate incubated at RH 75%. The concentration of chitosan is 4.0 wt%. TGA curves of films prepared by stripping film containing 3.0 wt% of chitosan (D, E) and LBL film containing 4.0 wt% of chitosan (F, G) with different concentrations of sodium phytate. Data are presented as the average of triplicate measurements with standard deviation (n = 3). Values with different letters (a, b, c, and d) are significantly different (p < 0.05).
ACS Paragon Plus Environment
30
35
Page 33 of 37
Journal of Agricultural and Food Chemistry
A
5s
0s
60s
140
C 120
120
110
Transmittance (%)
Thickness (µm)
B
30s
15s
100 80 60
90s
2min
3min 1min 5min 10min 20min 30min
100 90 80 70
40
60
20
50 40
0 0
5
10
15
20
25
260
30
280
Formation time (min) 1min 5min 10min 20min 30min
100 90
E
340
360
0.0002 0.0000
D eriv. m ass (w t% ° C -1 )
W eight (% )
D
300 320 Wavelength (nm)
80 70 60
-0.0002
1min 5min 10min 20min 30min
-0.0004 -0.0006 -0.0008 -0.0010 -0.0012
50 100
200
300
400
500
600
-0.0014 100
Temperature (°C)
200
300
400
500
Temperature (°C)
Figure 4. (A) Chitosan/sodium phytate film formation time observed from the solution flowing in the inverted vials after different time. Five milliliter 3.0 wt% chitosan was mixed with 1ml 1.25 wt% sodium phytate. (B) Thicknesses of film as a function of film-forming time. (C) UV-vis transmission spectra of the films prepared by film-stripping technique at various formation time. The concentration of chitosan and sodium phytate are 3.0 wt% and 1.25 wt%, respectively. (D) Thermal degradation of stripping films with different time. Weight changes in the film. (E) Derivative plot of (D).
ACS Paragon Plus Environment
600
Journal of Agricultural and Food Chemistry
1 2 3 4 5 6 7 8 9 10
Transm ittance (% )
100 95 90
Solubility Swelling degree Moisture content
B ab
90 Percentage (%)
A 105
Page 34 of 37
ab
ab
ab
ab c
abc
ab
a
bc
80 70 20
bc a
ab
a
a a c a
a
ab
a
a bc a
a
a
ac a
a
85
10 80 260
280
300
320
340
360
0 1
2
1
2
10 µm
10 µm
6
10 µm
D
1
50 µm
7
50 µm
10 µm
8
10 µm
2
3
50 µm
50 µm
50 µm
5
6
7
8
9
10
11
4
5
10 µm
10 µm
3
10 µm
7
4
Stripping film Number
Wavelength (nm)
C
3
8
50 µm
9
10 µm
4
50 µm
9
50 µm
Figure 5. (A) UV-vis transmission spectra, (B) The solubility, swelling degree, and moisture content of the film, (C) Surface morphology. (D) Fractured cross-section structure of stripping films prepared at different stripping film numbers. Number 1 to 10 represents films formed at the first stripping to tenth stripping, respectively. Data are presented as the average of triplicate measurements with standard deviation (n = 3). Values with different letters (a, b, and c) are significantly different (p < 0.05).
ACS Paragon Plus Environment
10
10 µm
5
50 µm
10
50 µm
Page 35 of 37
Journal of Agricultural and Food Chemistry
B 100
A 100
Stripping film Casting film
Erosion (% )
Erosion (%)
Stripping film Casting film 80
60
80
60
40
40 20
20 0
10
50
100
250
1
500
2
C OH
3
4
OH
H PO H3PO4 3 4OH
PO43- PO 34 OH
OH
2
NH3+
P =O
HO
H3PO4 NH +H3PO4 3 OH OH NH3+
PO43-PO
HO HO
OH
OH NH2
H2N
NH3+ NH2
3
4 OH
5 PO43-
3PO43- PO4
OH
NH3+
6
7
OH
pH 8
9
PO43-
PO43OH
PO43- PO43PO 3PO43- 4
OH
PO43PO43NH3+
NH2
NH2 NH3
+
H Hydrogen interaction
PO43-
3-
4
OH
Sodium phytate
5
Urea concentration (M)
Salt concentration (mM)
Chitosan
N H
HO
NH2 OH
OH
Electrostatic interaction
Figure 6. The influence of NaCl (A) and urea (B) on the erosion of the chitosan-sodium phytate films. (C) Illustration that shows the effect of pH on the molecular mobility of films and on the charges and interactions behind chitosan-sodium phytate films.
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
E. Coli. only
Page 36 of 37
1.25% Sodium phytate
4.0% Chitosan
A
3.0%+0.625%
3.0%+1.25%
3.0%+2.0%
3.0%+2.5%
3.0%+3.0%
4.0%+0.625%
4.0%+1.25%
4.0%+2.0%
4.0%+2.5%
4.0%+3.0%
B
Stripping films Casting films
Antibacterial ratio (%)
C 100
a
a
b
80
a
a
a a
2.5
3.0
b
60 40 20 0
c
c
0.5
1.0
1.5
2.0
Sodium phytate (%) Figure 7. (A) and (B) Quantitative calculation of E. Coli cultivated on LB agar covered with bacteria suspension that was in contact with stripping films (3.0 wt% chitosan) and casting films (4.0 wt% chitosan) with different concentrations of sodium phytate, respectively. (C) Antibacterial ratio of chitosan-sodium phytate film against E. Coli. Data are presented as the average of triplicate measurements with standard deviation (n = 3). Values with different letters (a, b, and c) are significantly different (p < 0.05).
ACS Paragon Plus Environment
Page 37 of 37
Journal of Agricultural and Food Chemistry
For Table of Contents Only
Stripping film
Stripping film
Casting film
Casting film
ACS Paragon Plus Environment