Subscriber access provided by MIDWESTERN UNIVERSITY
Energy, Environmental, and Catalysis Applications
Constructing Long-Range Transfer Pathways with Ordered Acid-Base Pairs for Highly Enhanced Proton Conduction Yarong Liu, Wenjia Wu, Ping Li, Jianlong Lin, Zhihao Yang, and Jingtao Wang ACS Appl. Mater. Interfaces, Just Accepted Manuscript • DOI: 10.1021/acsami.8b21081 • Publication Date (Web): 19 Feb 2019 Downloaded from http://pubs.acs.org on February 21, 2019
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
Constructing Long-Range Transfer Pathways with Ordered Acid-Base
2
Pairs for Highly Enhanced Proton Conduction
3
Yarong Liua,1, Wenjia Wua,b,1, Ping Lia, Jianlong Lina, Zhihao Yanga, Jingtao Wang a,*
4 5 6 7
a
8
S Supporting Information ●
9
ABSTRACT: Acid-base pairs hold great superiority in creating proton defects and
10
facilitating proton transfer with less or no water. However, the existing acid-base
11
complexes failing in assembling into ordered acid-base pairs and thus cannot always take
12
full advantage of acid-base synergetic effect. Herein, polymer quantum dots (PQDs) with
13
inherent ordered acid-base pairs are utilized and anchored on dopamine coated graphene
14
oxide (DGO), and thus forming into long-range conducting pathways. The resultant
15
building blocks (nPGO) are integrated in sulfonated poly(ether ether ketone) matrix to
16
fabricate composite membrane. The constructed long-range transfer highways with ordered
17
acid-base pairs impart composite membrane significantly enhanced proton conduction
18
ability. Under hydrated state, the composite membrane attains 91% increase over the
19
control membrane in conductivity and the single cell fuel based on the membrane achieves
20
71% promotion in maximum power density. Under anhydrous condition, more striking
21
augment in conduction is observed for composite membrane, reaching 7.14 mS cm−1,
22
almost 10 times of the control membrane value (0.78 mS cm−1). Remarkably, such
23
anhydrous proton conduction performance is even comparable to that of composite
24
membrane impregnated with ionic liquids, which is hard to realize with conventional fillers.
25
Collectively, these results endow composite membranes great potential for application in
26
hydrogen-based fuel cell, sensor, and catalysis.
27 28
KEYWORDS: polymer quantum dot, inherent ordered acid-base pairs, graphene oxide, long-range transfer highways, composite membrane, proton conduction
School of Chemical Engineering and Energy, Zhengzhou University, Zhengzhou 450001, P. R. China Department of Civil and Environmental Engineering, Center for the Environmental Implications of NanoTechnology (CEINT), Duke University, Durham, North Carolina 27708, USA 1 These authors made an equivalent contribution to this work. b
1
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
1. INTRODUCTION
2
High proton conduction materials, especially ones that can work efficiently under elevated
3
temperatures and low humidity conditions, are urgently desired in the hydrogen fuel cell
4
and sensor areas.1 As the benchmark, Nafion membrane shows excellent proton conduction
5
under fully hydrated condition,2,3 while under the low-humidity and high-temperature
6
conditions, it should be not eligible because of the severe deterioration of proton
7
conduction, rooting in the loss of water.4,5 Up to now, massive endeavors have been paid
8
out for developing membranes which could be capable of working under above-mentioned
9
conditions.6-15 A general approach is to impregnate the membrane with low-volatile proton
10
solvents (e.g., N-heterocycle, phosphonic acid, and ionic liquid).6-12 This can alleviate the
11
major problems associated with proton conduction, due to the presence of low-volatile
12
proton hopping sites. However, these composite membranes always suffer from serious
13
mechanical strength decline and proton solvent leaching, resulted from the plasticizing
14
effect and water-soluble property of proton solvents.9,13-15
15
A strategy of acid-base composites offers potential to address these problems by forming
16
acid-base pairs, which generate proton defects and then enable a fast Grotthuss-type proton
17
transfer.16-28 So far, the developed acid-base pairs are commonly divided into two
18
categories. One is incorporating functionalized (acidic or basic) nanofillers into (basic or
19
acidic) polymer matrix.16-18 Ueda et al. obtained a 88 % increase in anhydrous conductivity
20
at 140 °C for the phosphoric acid-doped SPEEK membrane (from 4.0 to 7.5 mS cm−1) with
21
the introduction of 3 wt.% polybenzimidazole (PBI)-grafted graphene oxide (GO).19 The
22
other is blending basic polymers (e.g., PBI, chitosan (CS)) with acidic polymers (e.g., 2
ACS Paragon Plus Environment
Page 2 of 31
Page 3 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
sulfonated polysulfone (PSf), sulfonated poly(ether ether ketone) (SPEEK)).20-24 Fu and
2
co-workers blended SPEEK with benzimidazole-grafted polysulfone to prepare composite
3
membrane, which gave an enhanced proton conductivity of 0.2 mS cm-1 under anhydrous
4
condition in contrast to plain SPEEK membrane (0.06 mS cm-1) at 120 oC.25 However, the
5
conductivity enhancements of these membranes are limited, as the random distribution of
6
acid-base sites diminish corresponding synergistic effect of acid-base pairs in creating
7
proton defects. Furthermore, the formed acid-base pairs generally unable to construct
8
long-range highways. For the former case, it necessitates boring pretreatment to avoid the
9
precipitation of polyelectrolyte complex.26-28 While for the latter case, the inhibited chain
10
motility generated by steric hindrance of fillers always makes the acid and base sites far
11
away from each other. Accordingly, materials with inherent ordered acid-base pairs as well
12
as with potential to be engineered into long-range pathways hold great promise to conquer
13
these problems.
14
Recently, the research on polymer quantum dots (PQDs) has been paid much
15
attention.29-31 They possess some intrinsic advantages for application as efficient proton
16
carriers, including abundant conducting groups and molecular size of 2-10 nm, both of
17
which are readily to be engineered. Importantly, the inherent ordered acid-base pairs with
18
short inter-distance make it an ideal candidate for anhydrous proton conduction (Figure S1).
19
In a previous work,32 we have incorporated PQDs into Nafion and observed increased
20
proton conduction ability. However, the PQDs in Nafion were also discretely distributed.
21
Thus we speculate that more significant conduction enhancement might be achieved if
22
PQDs can be sequentially assembled. 3
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Herein, novel building blocks with inherent ordered acid-base pairs are designed and
2
prepared to create long-range proton transfer highways: anchoring PQDs on dopamine
3
coated GO (nPGO). Dopamine was introduced to increase the anchoring sites and strength,
4
thus facilitating sequential distribution of PQDs. The nPGOs were incorporated in SPEEK
5
matrix to prepare composite membrane. SPEEK was chosen due to the good film-forming
6
property, excellent thermal and chemical stabilities, acceptable proton conduction ability,
7
and low cost. By comparing the nPGOs-filled membrane to references composed of DGO
8
or PQDs, we demonstrate that the ordered acid-base pairs are assembled onto long-range
9
transfer highways along
nPGO-SPEEK
interface, giving highly enhanced proton
10
conduction. And the conduction property is well controlled by PQD loading and acid-base
11
pair amount on nPGO. The proton conductivity of composite membrane gives an obvious
12
91% increase over the control membrane and the hydrogen fuel cell output power based on
13
this membrane gains a 71% enhancement under hydrated condition. These results have
14
surpassed most SPEEK-based composite membranes. Most significantly, these ordered
15
pairs show an anhydrous conductivity of 7.14 mS cm-1 at 120 oC. This powerful proton
16
conduction ability is almost one-order of magnitude higher than that of plain SPEEK
17
membrane, even comparable to that of ionic liquid-impregnated membranes. Such
18
performances are difficult to attain by traditional fillers. Furthermore, this work gives new
19
ideas to design efficient proton conducting materials under hydrated or anhydrous
20
condition.
21
2. EXPERIMENTAL SECTION
22
2.1. Materials and Chemicals. Citric acid (CA, 99.5%), graphite powders (45 μm), and 4
ACS Paragon Plus Environment
Page 4 of 31
Page 5 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
diethylenetriamine (DETA, 99%) were purchased from Sigma-Aldrich. Sulfuric acid
2
(H2SO4, 98 wt.%), hydrogen peroxide (H2O2, 30 wt.%), N, N-dimethyl formamide (DMF),
3
and anhydrous ethyl alcohol were obtained from Bailingwei Technology Co., Ltd. Victrex®
4
poly(ether ether ketone) (PEEK, grade 381G) was got from Nanjing Yuan9bang
5
Engineering Plastics Co., Ltd. Potassium permanganate (KMnO4) was acquired from
6
Kewei Chemistry Co., Ltd. Distilled water was utilized in the whole experiment.
7
2.2. Synthesis of the Nanosheets and SPEEK. Graphite powders were oxidized to
8
prepare GO based on the Hummers’ method.33 Dopamine coated GO (DGO) was also
9
synthetized according to the method in literature.34 Here, four kinds of nPGOs, where n (n
10
= 1, 2, 3, 4) represented different PQD loading, were synthesized as following: 0.96 g citric
11
acid (2.5 mol L-1) and 540 µL diethylenetriamine (2.5 mol L-1) were dissolved in DGO
12
aqueous solution (2.0 g) under ultrasonic treatment at ambient temperature for 5 min. Next,
13
the mixture was put in a microwave-oven (750 W) to heat for 5 min, and then
14
ultrasonically washed several times using 98% w/w ethanol, for removing residual
15
unreacted substance. Afterwards, the resultant products were dispersion in water, and
16
3PGO
17
kinds of nPGOs were prepared by adjusting DETA and CA concentration (0.1, 1.0, 2.5, and
18
5.0 mol L-1), as shown in Table S1. Besides, two graphene oxide quantum dots (GQDs)
19
with elevated carbonization degree (GmGO) were yielded by altering the solution to a
20
mixture of DGO aqueous solution (1.0 g L-1) and glycerol. The mass of DGO solution and
21
glycerol was 1.0 and 1.0 g, and 0.5 and 1.5 g, for G1GO and G2GO, respectively. PEEK
22
was sulfonated to obtain SPEEK with ~ 62% sulfonation degree.35
was obtained by freeze drying process for 48 h. Using the above method, other three
5
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
2.3. Preparation of the Membranes. A certain amount of nPGO was dispersed in 8.0 g
2
DMF and treated with ultrasonication for 2 h at ambient temperature. Next, 0.7 g SPEEK
3
was immersed in the mixture. In order to get a homogeneous dispersion, the mixture was
4
beat up thoroughly overnight at room temperature, and then cast onto flat glass plates in
5
terms of the method in literature under the same conditions.34 The membranes were termed
6
as SP-nPGO-X, and X (1%, 2%, 5%, and 10%) denoted the weight percentage of nPGO.
7
Because 10 wt.% nPGO loading amount occurred agglomeration, 5 wt.% was chosen to
8
better investigate the influence of filler category on membrane performances. Using the
9
above methods, the resultant composite membranes were produced by dissolving 0.035 g
10
DGO, 0.035 g PQD, and 0.035 g GmGO into 3.5 g DMF, and named, respectively, as
11
SP-DGO-5%, SP-PQD-5%, and SP-GmGO-5%. The SPEEK control membrane (SP) was
12
also fabricated with the same method. Notably, the average thicknesses of composite
13
membranes were ranged from 41 to 74 μm (Table S2).
14
2.4. Characterization of the Nanosheets and Membranes. The morphology of the
15
nanosheets were studied via atomic force microscopy (AFM) using Bruker Dimension
16
FastScanTM and transmission electron microscopy (TEM) on FEI model TECNAI G2-TEM
17
(200 kV). The membranes were tested by wide X-ray diffractometry (WAXD) (from 5 to
18
60o) and small-angle X-ray scattering (SAXS) (0.1-4o) through a Bruker D8 Advance ECO.
19
Mechanical properties of the membranes were measured by manipulating the elongation
20
rate to 2.0 mm min-1 with Testometric 350AX. The membranes were broken by freeze
21
fracture method and observed via cross-sectional scanning electron microscopy (SEM)
22
with a JSM-7500F. Differential scanning calorimetry (DSC) was employed in 204 F1 6
ACS Paragon Plus Environment
Page 6 of 31
Page 7 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
NETZSCH. The nanosheets, prior to testing, were pressed into tablets and then immersed
2
in water for a few minutes. Under nitrogen atmosphere, the hydrated state of nanosheets
3
were also measured by heated from -60 oC to 80 oC with the heating rate of 5 oC min-1.
4
Besides, the weight fraction of bound water (ωb) was estimated by deducting the amount of
5
free water from the total water uptake (ωt). Under nitrogen atmosphere, the membranes
6
were preheated from 30 to 120 oC with the heating rate of 10 oC min-1, followed by cooling
7
down to 90 oC and then reheating up to 260 oC. An Escalab250Xi system was utilized to
8
test X-ray photoelectron spectroscopy (XPS) (Thermo Fisher Scientific, Escalab 250Xi,
9
U.S). Under nitrogen atmosphere, thermogravimetric analysis (TGA), elevating the
10
temperature from 30 to 800 oC with the heating rate of 10 oC min-1, was performed by
11
TGA-50 SHIMADZU.
12
2.5. Measurements of Water Uptake and Area Swelling. The area swelling and water
13
uptake of the membranes were tested at various temperatures (30, 40, 50, and 60 oC) in
14
accordance with the method in literature.36
15
2.6. Ion Exchange Capacity (IEC), Proton Conductivity, and Fuel Cell Performance.
16
The IEC values of membranes were tested by back-titration method.23 The anhydrous
17
temperature-dependent proton conductivity of the pre-dried membranes (from 30 to 120 oC)
18
was tested by the same method and experimental instrumentation in our previously
19
published work.11,14,32,34 These completely dried membranes were also measured at 80 oC
20
under various humidifies and recorded data points for 90 min at each humidity step. The
21
membranes were immersed in water for 48 h before the test and measured at different
22
temperatures (from 30 to 90 oC) at 100% RH. 7
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
The membrane electrode assemblies (MEAs) were fabricated by SP, SP-DGO-5%,
2
SP-nPGO-5%, and SP-GmGO-5% on the basis of the method in literature.37 The
3
performances of single fuel cell based on membrane were measured in series of
4
temperatures (from 30 to 60 oC) under 100% RH in the light of the experimental
5
instrumentation under the identical system conditions.38 The stability was tested at 60 oC
6
and 100% RH, as the constant voltage loading was 0.6 V.
7
3. RESULTS AND DISCUSSION
8
3.1. Synthesis of the Nanosheets. Quantum dot (QD)-anchored nanosheets were
9
synthetized through a one-pot, microwave-assisted condensation of DETA and CA on
10
DGO surface (Scheme 1). Poly-dopamine layer was introduced to increase the anchoring
11
sites and strength by the abundant, homogeneous affinity sites, including –NH2 and –NH–
12
(Figure S2). Here, four kinds of polymer quantum dots anchored DGO (nPGO) with
13
different PQD loadings were prepared by regulating the precursor concentration. And two
14
types of graphene like quantum dots anchored DGO (GmGO), with similar physical
15
structures to 3PGO but reduced acid-base pairs, were also synthesized through elevating
16
the carbonization degree (Table S1). TEM images, Figure 1a-d, Figures S3, show that GO
17
of single layer possesses typical sheet structure with lateral dimension of above 2 µm.
18
AFM images, Figure 1e-i, Figures S4, reveal that the thickness of GO is 1.1 nm with a
19
smooth surface. After the self-polymerization, a uniform poly-dopamine layer is coated on
20
GO surface, which elevates sheet thickness to 1.5 nm. The layer structure of DGO is well
21
maintained, while it becomes a little dark due to the presence of poly-dopamine layer.39
22
This layer brings abundant hydrophilic groups (FTIR, Figure 2a and Figure S1), thus 8
ACS Paragon Plus Environment
Page 8 of 31
Page 9 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
facilitating the adsorption of citric acid and diethylenetriamine and hence the formation of
2
PQDs/GQDs. This can be clearly observed in TEM and AFM images (Figure S5) that a
3
large amount of point-like attachments (PQDs) are distributed on DGO surface. PQDs
4
exhibit no lattice structure due to the presence of rich –NH2 and –CO2H.40 And these PQDs
5
allow nPGO generate photoluminescence effect under 365 nm UV (Figure S6). All the
6
anchored PQDs show uniform 0D structure with a size of 2-3 nm, and the size keeps
7
unchanged with the precursor concentration (0.1-5.0 mol L-1). As shown in Figure 1g-i,
8
elevating precursor concentration obviously increases the number of PQDs when the
9
concentration is below 5.0 mol L-1. Similarly, GmGO with the well-retained layer structure
10
possesses uniformly-distributed GQDs (Figure S3b and c). The size of anchored GQDs is
11
around 2.5 nm (Figure S4c). It should be noted that, the PQDs and GQDs remain firmly
12
anchored on the nanosheets although they have been fully washed by ultrasonic treatment.
9
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2 3 4
Figure 1. TEM and AFM images of the nanosheets: (a and e) GO, (b and f) DGO, (c and g) 1PGO, (d and h) 3PGO (inset: height profile along the purple line); (i) the corresponding height profiles of AFM images.
5
FTIR results confirm the coating of poly-dopamine layer on DGO surface due to the
6
existence of characteristic peak at 1381 cm-1 for C-O-H (Figure 2a).41,42 By comparison,
7
nPGO
8
N-H at 1647 and 1554 cm-1, respectively.43 Meanwhile, the intensity of these two bands
9
elevates from 1PGO to 3PGO, suggesting the increased PQD loading. XRD, Figure 2b,
10
displays an average intersheet distance of GO of 0.86 nm with a diffraction peak value of
11
10.3°.44 The diffraction peak of DGO shifts to 8.9°compared to GO, which suggests an
12
increased intersheet distance of 0.99 nm. After modification with PQDs, the ordered
13
stacking of DGO is destroyed, and the characteristic peak at around 10.0° disappears.45
gives rise to two new peaks of C=O stretching vibration band and the bending of
10
ACS Paragon Plus Environment
Page 10 of 31
Page 11 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
While a new amorphous band at 23° appears in the spectrum of nPGO, related to the
2
stacked structure of PQDs.32,40 In addition, the intensity of this band strengthens with the
3
increase of PQD loading on nanosheet, i.e., from 1PGO and 3PGO. TGA curves in Figure
4
2c show that the nanosheets undergo the water evaporation (30-150 oC), the deoxygenation
5
of oxygen containing groups (200-410 oC), and the decomposition of GO backbone
6
(420-800 oC) stages.46 Compared with GO, the presence of poly-dopamine layer and PQDs
7
postpones the starting degradation temperature of DGO and nPGO, resulting from their
8
protection for oxygen containing groups of GO (Figure S7a).13,47 Moreover, the
9
poly-dopamine layer obviously elevates the char yield of DGO at 800 oC. Compared with
10
DGO, nPGO produces lower char yield because of the polymer-like component of PQDs
11
(Figure 2c and Figure S7b). And as PQDs loading increases, the char yield of nPGO
12
gradually reduces. Based on char yield data, it shows that the loading of PQDs is relatively
13
high: up to 67 wt.% for 3PGO, which is possible to form inter-connected packing (Table
14
S1). While for 4PGO, the PQD loading decreases to 56.6 wt.%. This should be attributed to
15
the high precursor concentration and hence high solution viscosity, which may inhibit the
16
enrichment of precursor near DGO surface. For another, GmGO exhibits a close thermal
17
degradation process to nPGO. Under close QD loading, GmGO displays higher thermal
18
stability with larger char yield than nPGO. This is because of the high stability of GQDs as
19
compared to PQDs.
11
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
C=O
DGO
1
100
a
10.3
-COOH
C-O-H
PGO
C=O amide
PGO 3
N-H
GO DGO 1PGO
8.9
b
3PGO
80
GO DGO 1PGO
70
3PGO
90
Weight (%)
C-O
Relative intensity / a.u.
O-H GO
Transmittance / a.u.
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 31
c
60 50
49.6% 42.9%
40
36.2%
30
1 2
4000
3500
2100 1400 Wave number (cm-1)
700
10
20
30
2θ /
40
50
100
200
300
400
500
600
700
800
Temperature (C)
Figure 2. (a) FTIR spectra, (b) XRD patterns, and (c) TGA curves of as-prepared nanosheets.
3
3.2. Characterization of the Membranes. Afterwards, the nanosheets were integrated
4
in SPEEK matrix for fabricating proton exchange membranes. Cross-sectional SEM image
5
of SP control membrane shows uniform and smooth morphology without any cracks
6
(Figure 3a). GO makes the cross-section of SP-GO-5% become obviously crude with some
7
cracks (Figure S8).13 While SP-DGO-5% exhibits fewer wrinkles, and the polymer-filler
8
interfaces are dense (Figure 3b). This phenomenon is resulted from the strong electrostatic
9
attraction between DGO (–NH2/–NH–) and SPEEK (–SO3H), which improves interfacial
10
compatibility.34 For composite membranes with nPGO (Figure 3d and e), the cross-section
11
is also smooth and uniform, like that of SP-DGO-5%. Differently, the polymer-filler
12
interfaces of SP-nPGO-5% seem looser. These phenomena should be attributed to that the
13
inherent –NH2/–NH– would form intra-molecular interactions with –CO2H on nPGO,
14
reducing the electrostatic attraction with –SO3H of SPEEK when compared with DGO
15
(only –NH2/–NH–). This can be justified by FTIR results of composite membranes (Figure
16
S9), where the peak intensity of –SO3H for SP-nPGO-5% is stronger than that for
17
SP-DGO-5%. To further verify this speculation, G1GO and G2GO with fewer functional
18
groups (Figures S10 and S11) were synthesized through the carbonization of
19
O-/N-containing groups. The drastically reduced loading of O-/N-containing groups for 12
ACS Paragon Plus Environment
Page 13 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
GmGO weakens its interaction with SPEEK matrix (Figure S12). Therefore, the interfacial
2
compatibility becomes worse (Figure S13), even similar to that of SP-GO-5%. In addition,
3
it is interesting to find that, the polymer-filler interface of SP-nPGO-5% is more tortuous
4
when compared with SP-DGO-5%, inferring the presence of PQDs along DGO surface.
5
This meanwhile brings obvious photoluminescence effect under 365 nm UV (SP-3PGO-5%,
6
Figure 3c and f).
7 8 9
Figure 3. Cross-sectional SEM images of (a) SP, (b) SP-DGO-5%, (d) SP-1PGO-5%, and (e) SP-3PGO-5%; photographs of (c) SP-DGO-5% and (f) SP-3PGO-5% under 365 nm UV.
10
WAXD results, Figure 4a, Figures S14a and b, reveal that all SPEEK-based membranes
11
display broad bands (2θ = 8-21°) because of the semicrystalline nature of the membranes.
12
The crystallinity is evaluated by the diffraction band in form of full width at half maximum
13
(FWHM) (Table 1).48 SP obtains a FWHM value of 6.24º. By comparison, incorporating
14
DGO, 1PGO, and 3PGO makes the FWHM of composite membranes increased to 7.33º,
15
7.28º, and 7.02º, respectively, indicating reduction in crystallinity.49 Crystallinity reduction
16
should be ascribed to that, the nanosheets disturb the self-assembly of SPEEK chains 13
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 31
1
through mutual interactions. Therefore, the FWHM of SP-3PGO-5% is smaller than that of
2
SP-1PGO-5%, as it has weaker interaction with SPEEK matrix. Similarly, the FWHM of
3
SP-GmGO-5% is much smaller (Figure S14b). These speculations can be directly testified
4
by DSC as depicted in Figure 4b. The relaxation process of structural reorganization of
5
membranes results in the appearance of endothermic bands (from 179 to 214 °C).50 The
6
transition temperature (Td) of SP is 179.8 °C. Composite membranes attain elevated Td
7
values, because the interferences generated by nanosheets restrain chain mobility.51 Similar
8
to SEM and WAXD results, the Td values of the membranes decrease in order of
9
SP-DGO-5% > SP-1PGO-5% > SP-3PGO-5% > SP, in accordance with strength of
10
interfacial interactions. The nanophase separation structure of the membranes is reflected
11
by SAXS patterns (Figure 4c and Figures S14c and d). SP attains a q value of 0.21 nm-1,52
12
while DGO incorporation shifts this ionomer peak to an increased value, reaching 0.30
13
nm-1, indicating narrower ionic clusters. Compared with SP-DGO-5%,
14
composite membranes display smaller peak values, and the values for SP-1PGO-5% and
15
SP-3PGO-5% are 0.28 and 0.25 nm-1, respectively. In addition, the value for SP-GmGO-5%
16
is further decreased (Figure S14d). These phenomena should also be resulted from the
17
weakened interface interactions, resulting in larger ionic clusters relative to DGO-filled
18
composite membrane.
14
ACS Paragon Plus Environment
nPGO-filled
Page 15 of 31
184.6oC SP-3PGO-5%
Heat flow (a.u.)
Relative intensity (a.u.)
a SP SP-3PGO-5% SP-1PGO-5%
b
202.9oC SP-1PGO-5%
o
213.9 C SP-DGO-5%
179.8oC SP
SP-DGO-5% 10
20
30
40
50
2θ (degree)
60
140
160
180
200
Temperature (oC)
220
240
50
c
SP SP-DGO-5% SP-1PGO-5%
40
SP
q=0.21 nm
SP-3PGO-5%
q=0.25 nm
SP-1PGO-5%
q=0.28 nm
SP-DGO-5%
q=0.30 nm
d
SP-3PGO-5%
Stress (MPa)
Relative intensity (a.u.)
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
30
20
10
0
0.2
0.4
1
0.6
0.8 q (nm-1)
1.0
1.2
1.4
0
15
50
Strain()
55
2 3
Figure 4. (a) WAXD patterns, (b) DSC curves, (c) SAXS patterns, and (d) stress-strain curves of SPEEK control and composite membranes.
4
Table 1. The FWHM, relative FWHM, tensile strength, and elongation at break of the membranes. Tensile strength
Elongation at
[MPa]
break [%]
1
36.0
53.9
7.33±0.05
1.18
46.3
49.7
SP-1PGO-5%
7.28±0.05
1.17
31.7
17.4
SP-3PGO-5%
7.02±0.05
1.13
22.1
14.5
Membrane
FWHM(°)
Relative FWHM
SP
6.24±0.05
SP-DGO-5%
5
The mechanical properties of as-prepared membranes are exhibited in Figure 4d and
6
Figures S15a and b. The stress-strain curve of SP control membrane implies acceptable
7
mechanical properties, in which the elongation at break and tensile strength are,
8
respectively, 53.9% and 36.0 MPa (Table 1). By comparison, hybridizing GO into
9
membrane significantly reduces the mechanical properties (Figure S15a), leading the
10
elongation at break and tensile strength to 3.7% and 17.6 MPa, respectively. Compared 15
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
with SP-GO-5%, the interface attractions between nPGO and SPEEK matrix endow
2
SP-nPGO-5% with elevated tensile strength, and SP-3PGO-5% attains an elongation at
3
break of 14.5% and a tensile strength of 22.1 MPa. SP-GmGO-5% displays similar
4
mechanical properties to SP-nPGO-5% (Figure S15b). The elongation at break and tensile
5
strength of SP-DGO-5% reach to 49.7% and 46.3 MPa, respectively, because of the much
6
stronger interface attractions. Notly, TGA results imply that all membranes obtain
7
acceptable thermal stability (Figure S15c and d).
8
Water molecules can facilitate the proton transfer via vehicle and Grotthuss mechanism
9
due to the medium of proton conduction and the construction of hydrogen-bond networks.
10
SP gains the area swelling and water uptake of, respectively, 17.6% and 22.3% at 30 oC
11
(Table 2). Compared with SP, SP-GO-5% attains elevated area swelling and water uptake,
12
respectively, achieving 19.9% and 22.4%. (Figures S16 and Table S2). This should be
13
resulted from the additional space for water storage at polymer-nanosheet interfacial
14
domains.53,54 Upon modification with PQDs, the nanosheets generate electrostatic
15
attractions with SPEEK, making the interfacial domains hard to swell. The area swelling
16
and water uptake of SP-3PGO-5% are reduced to 17.7% and 20.7%, respectively.
17
Simultaneously, the area swelling and area swelling of composite membrane decrease with
18
the enhancement of interfacial attractions (Figures S16a and b). For SP-GmGO-5%, despite
19
the weak interfacial attractions, the relatively hydrophobic nature of GmGO makes
20
composite membrane exhibit lower area swelling and water uptake. In addition, the area
21
swelling and water uptake of the membranes all elevate with testing temperature (Figures
22
S16c and d), and composite membranes exhibit better structural stability than the control 16
ACS Paragon Plus Environment
Page 16 of 31
Page 17 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
ACS Applied Materials & Interfaces
membrane.
2
3
Table 2. Water uptake, area swelling, and IEC of the membranes.
a
Membrane
Water uptakea (%)
Area swellinga (%)
IEC (mmol g-1)
SP
22.3
17.6
1.76 ±0.02
SP-DGO-5%
13.3
11.2
1.62 ±0.02
SP-1PGO-5%
13.6
12.8
1.74 ±0.02
SP-3PGO-5%
20.7
17.7
1.93 ±0.02
Measurement was at 30 oC.
4
3.3. IEC and Proton Conductivity of the Membranes. Table 2 reveals that the IEC
5
value of SP is 1.76 mmol g-1. After inserting DGO into membrane, the IEC value decreases
6
to 1.62 mmol g-1 because of the appearance of acid-base pairs between DGO and SPEEK.14
7
Compared with SP-DGO-5%, SP-nPGO-5% achieves higher IEC value. For instance,
8
SP-1PGO-5%, SP-2PGO-5%, SP-3PGO-5%, and SP-4PGO-5% attain the IEC values of,
9
respectively, 1.74, 1.75, 1.93, and 1.87 mmol g-1 (Table S2). Such findings may be ascribed
10
to the intra-molecular interactions on nPGO, and thus allowing more –SO3H on SPEEK to
11
expose.
12
The investigation of proton conduction properties of the membranes are exhibited in
13
Figure 5 and Figures S17. At 30 oC and 100% RH, SP obtains the conductivity of 11.6 mS
14
cm-1 (Figure 5a). While the proton conductivity of SP-DGO-5% gains an elevated value of
15
18.4 mS cm-1. Given the reduced ionic cluster size, IEC, and water uptake, one reason for
16
the conductivity enhancement should be derived from the formed acid-base pairs along
17
polymer-nanosheet interface. Such presumption can be further testified by the increased
18
proton conductivity of SP-nPGO-5%, which possesses inherent ordered acid-base pairs in
19
proton transfer highways (Figure 5b and Figure S17a). Different from the random 17
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
acid-base pairs in SP-DGO-5%, the inherent acid-base pairs on PQDs are highly ordered
2
(Scheme 1, in order of -acid-base-acid-base-). Besides, these PQDs offer additional
3
hydrogen-bond donors and increase strong water bonding sites in SPEEK matrix, both of
4
which can jointly construct abundant water-mediated hydrogen-bonded transfer networks,
5
accelerating protons transfer through Grotthuss mechanism.32 Accordingly, SP-1PGO-5%
6
obtains a significantly enhanced conductivity of 23.1 mS cm-1. Increasing the number of
7
ordered acid-base pairs endows composite membrane with further elevated proton
8
conduction, and SP-3PGO-5% with highest PQD loading achieves a conductivity of 35.0
9
mS cm-1. In addition, SP-GmGO-5% displays lower proton conductivity than that of
10
SP-nPGO-5% due to the reduced O-/N-containing groups (i.e., acid-base pairs) (Figure
11
S17b). Another reason for the conduction augment of SP-DGO-5% as compared to SP
12
should be originated from the constructed long-range transfer highways along 2D sheet
13
interfaces. To verify this speculation, PQDs were prepared and introduced into SPEEK
14
matrix to obtain composite membrane. Despite the larger number of ordered acid-base
15
pairs (compared to nPGO), SP-PQD-5% displays a lower proton conduction ability of 21.1
16
mS cm-1 due to the dis-continuous packing of PQDs in membrane (Figure S17b).
17
Meanwhile, the conductivities of membranes all increase with the temperature (Figure 5b,
18
Figures S17a and b). The maximum hydrated conductivity of SP-3PGO-5% (76.5 mS cm-1)
19
at 90 oC is 1.9 times that of SP (11.6 mS cm-1). Besides, the extent of performance augment
20
in this study is much larger than that of most existing SPEEK composite membranes filled
21
by imidized-GO, microcapsules, N-decorated carbon nanotubes, or alkaline g-C3N4,
22
etc,55-57 highlighting the superiority of ordered acid-base pairs in boosting proton 18
ACS Paragon Plus Environment
Page 18 of 31
Page 19 of 31
conduction.
30
100% RH, 30C 0% RH, 30°C
2.8 80
2.4 2.0
25
1.6 20
1.2 15
0.8
10
0.4
5 0
SP
DG
5% O-
-
SP
S
O PG P- 1
-5%
-5%
S
SP-1PGO-5%
15.9
SP-3PGO-5%
14.6
4
21.8 SP SP-DGO-5% 16.6
2
0 20
40
60
80
Temperature (oC)
60
SP-3PGO-5%
50 40 30 20 10 30
100
40
50
60
70
80
90
Temperature (oC)
c
Ea (kJ mol-1)
b
SP SP-DGO-5% SP-1PGO-5%
70
O PG P- 3
8
6
0.0
Proton conductivity (mS cm-1)
35
a
Proton conductivity (mS cm-1)
Proton conductivity (mS cm-1)
40
Proton conductivity (mS cm-1)
1
Proton conductivity (mS cm-1)
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
120
40
RH=40%
RH=20%
RH=60%
d
30
20
10
SP-1PGO-5% SP-3PGO-5%
SP SP-DGO-5%
0 0
30
60
Time (min)
90
2 3 4 5 6
Figure 5. (a) Proton conductivity of membrane at 100% RH (30 oC) and 0% RH (30 oC), (b) temperature-dependent proton conductivity of membrane at 100% RH, (c) temperature-dependent proton conductivity of membrane at 0% RH, and (d) RH-dependent proton conductivity of membrane for 90 min at 80 oC in dry state.
7
The proton conductivity is displayed in Figure 5c and Figure S17c under anhydrous
8
condition. The conductivity of SP is 0.15 and 0.78 mS cm-1 at 30 and 120 oC, respectively.
9
SP-DGO-5% exhibits enhanced anhydrous proton conduction property. The conductivity
10
reaches, respectively, 0.35 and 1.24 mS cm-1 at 30 and 120 oC. This should be due to the
11
constructed long-range transfer highways as well as the formed acid-base pairs along it,
12
which reduce transfer energy barrier. This can be testified by the decreased Ea values of
13
SP-DGO-5% (16.6 kJ mol-1) compared to SP (21.8 kJ mol-1) (Figure 5c and Figure S17d).
14
By comparison, the introduction of nPGO with inherent ordered acid-base pairs along
15
nPGO-SPEEK
interface gives SP-nPGO-5% highly enhanced proton conductivity. The 19
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
anhydrous conductivity of SP-1PGO-5% elevates to 0.75 and 2.49 mS cm-1 at 30 and 120
2
o
3
resulted from that, protons can fast transport among the adjacent donors (–CO2H) and
4
acceptors (H2N–/–HN–) on PQDs via accelerated protonation/de-protonation process with
5
reduced enthalpy change.58,59 Moreover, the anhydrous proton conduction can be further
6
enhanced by increasing the loading of acid-base pairs. In such way, the enrichment of PQD
7
on nPGO surface possibly forms relatively continuous proton transfer highways. Thus,
8
SP-3PGO-5% gains the maximum anhydrous conductivity of 7.14 mS cm-1, almost
9
one-order of magnitude of that of SP at 120 oC. And this performance is even comparable
10
C, respectively, with a reduced Ea value of 15.9 kJ mol-1. This enhancement should be
to that of polymeric membranes impregnated with ionic liquids.8,11,14
11
In addition, RH-dependent proton conductivity of as-prepared membranes was tested
12
(Figure 5d). In contrast with SP and SP-DGO-5%, composite membranes with nPGO
13
display stronger moisture absorbing ability, especially for SP-3PQD-5%. It reaches
14
equilibrium within 15 min at each RH and then keeps a constant conductivity. While for
15
SP and SP-DGO-5%, they need more than 30 min. This strong moisture absorbing ability
16
should be derived from the hydrophilic groups on PQDs. In order to verify this speculation,
17
the powders of GO, DGO, and nPGO were pressed into tablet and then used to absorb
18
water molecules, followed by measuring their state (free or bound water) on DSC (Figure
19
S18 and Table S3).60,61 The water uptakes of GO and DGO tablets are 8.5% and 8.2%,
20
respectively, in which the ratio of bound water are 84.7% and 90.2%. By Comparison,
21
nPGO
22
14.2% and 17.6%, respectively, with the bound water ratio up to 96.5% and 98.9%.
exhibits stronger water absorbing ability: the water uptakes of 1PGO and 3PGO are
20
ACS Paragon Plus Environment
Page 20 of 31
Page 21 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
Composite membranes with other three contents of 3PGO were also prepared and tested.
2
The conductivity varies with
3
performances due to the highest PQD loading (Figure S19).
3PGO
content, and SP-3PGO-5% presents the best
4 5
Scheme 1. Schematic of the preparation and proton conduction mechanism of composite membrane.
6
3.4. Single Cell Performance. The hydrogen fuel cell performances of the membranes
7
are exhibited in Figure 6 and Figures S20. The open circuit voltages of all membranes
8
suggest respectable gas barrier ability, which are above 0.9 V. SP obtains the maximum
9
power density and current density of, respectively, 106.9 mW cm-2 and 369.6 mA cm-2 at
10
50 oC and 100% RH. Compared with SP, the power density and current density of
11
SP-DGO-5% gain increased values, respectively, reaching 120.7 mW cm-2 and 422.6 mA
12
cm-2. Such performance should be resulted from the enhanced gas barrier ability and
13
proton conduction of SP-DGO-5%. As for SP-nPGO-5%, the maximum power density and
14
current density are further highly elevated, whose trends are in accordance with the proton
15
conductivity (Figure S20a and b). Particularly, SP-3PGO-5% achieves the maximum power
16
density and current density of, respectively, 183.1 mW cm-2 and 580.7 mA cm-2, which are
17
1.6 times and 1.7 times higher than that of SP. From a comparison with other 21
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 31
1
SPEEK-based composite membranes (Table S4), it is observed that nPGO are more
2
efficient to elevate the cell output power based on membrane than most of the fillers.
3
Simultaneously, the maximum power density and current density of SP-3PGO-5% increase
4
with the operating temperatures (30-60 °C) (Figure S20c). Furthermore, the stability of the
5
operation of the MEA was also detected based on SP-3PGO-5% for more than 60 h at a
6
constant voltage of 0.6 V. Notly, the single cell based on membrane does not exhibit any
7
degradation for 60 h (Figure 6b), demonstrating an excellent operation stability.
8 9 10
Figure 6. (a) Single cell performances of the membrane under 50 oC and 100% RH, and (b) the durability of SP-3PGO-5% in single cell operated at 60 oC and 0.6 V with humidified (100% RH) H2/O2.
11
4. CONCLUSIONS
12
In summary, we have proved, in polymer electrolyte membrane,
nPGO
is capable of
13
constructing efficient long-range proton transfer highways. For this novel nanosheets,
14
PQDs are uniformly and firmly anchored on DGO, providing inherent ordered acid-base
15
pairs along sheet surface. By homogeneously dispersing in composite membrane, nPGOs
16
highly
17
low-energy-barrier transfer highways. Under hydrated condition, composite membrane
18
achieves an obvious 91% promotion over SP in proton conduction and a 71% improvement
19
in maximum power density. The performance is superior to most of the existing SPEEK
strengthen
the
proton
conduction
ability
22
ACS Paragon Plus Environment
of
membrane
by
forming
Page 23 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
membranes. More significantly, in the case of anhydrous proton conductivity, these ordered
2
acid-base pairs provide much stronger enhancement. The conductivity of SP-3PGO-5%
3
(0.78 mS cm-1) is almost one-order of magnitude higher than SP (7.14 mS cm-1) at 120 oC.
4
Such performance is comparable to that of ionic liquid-impregnated membranes, and also
5
much higher than that of composite membranes hybridized by GO, DGO, and PQDs, as
6
they fail to create ordered and long-range acid-base paired pathways. The conduction
7
property of composite membrane shows obvious dependence on the loading of acid-base
8
pairs. Accordingly, the distinctive design of these conducting materials makes great
9
potential for practical application of hydrogen-based fuel cell, sensor, and catalysis.
10
■ ASSOCIATED CONTENT
11
S Supporting Information ●
12
TEM images of 4PGO and GmGO. AFM topography images of 1PGO, 4PGO, and G2GO.
13
C 1s spectra of PQD, 3PGO, and G2GO. TGA curves of DGO, PQD, nPGO, and GmGO.
14
DSC curves of state of water in nanosheets. SEM images of SP-GO-5% and SP-G2GO-5%
15
through the cross-sectional scan. FTIR spectra, WAXD patterns, and SAXS patterns of the
16
membranes. Proton conductivity, area swelling, and water uptake of the membranes with
17
different filler contents. Anhydrous and hydrous conductivities of the membranes.
18
■ AUTHOR INFORMATION
19
Corresponding Author
20
*E-mail:
[email protected]. Tel: 86-371-63887135. Fax: 86-371-63887135.
21
Notes
22
The authors declare no competing financial interest. 23
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
■ ACKNOWLEDGMENTS
2
This work is highly acknowledged by the Program for Science & Technology Innovation
3
Talents in Universities of Henan Province (18HASTIT002) and National Natural Science
4
Foundation of China (21576244). Global Scholar Program for Doctoral Students of
5
Zhengzhou University and Fok Ying Tung Education Foundation (161065) are also
6
supported.
7
■ REFERENCES
8
(1) Sadakiyo, M.; Okawa, H.; Shigematsu, A.; Ohba, M.; Yamada, T.; Kitagawa, H. Promotion of
9
Low-Humidity Proton Conduction by Controlling Hydrophilicity in Layered Metal-Organic
10
Frameworks. J. Am. Chem. Soc. 2012, 134, 5472–5475.
11
(2) Moghaddam, S.; Pengwang, E.; Jiang, Y. B.; Garcia, A. R.; Burnett, D. J.; Brinker, C. J.; Masel, R.
12
I.; Shannon, M. A. An Inorganic-Organic Proton Exchange Membrane for Fuel Cells with a Controlled
13
Nanoscale Pore Structure. Nat. Nanotechnol. 2010, 5, 230–236.
14
(3) Patel, H. A.; Mansor, N.; Gadipelli, S.; Brett, D. J. L.; Guo, Z. Superacidity in Nafion/MOF Hybrid
15
Membranes Retains Water at Low Humidity to Enhance Proton Conduction for Fuel Cells. ACS Appl.
16
Mater. Interfaces 2016, 8, 30687–30691.
17
(4) Karim, M. R.; Hatakeyama, K.; Matsui, T.; Takehira, H.; Taniguchi, T.; Koinuma, M.; Matsumoto,
18
Y.; Akutagawa, T.; Nakamura, T.; Noro, S. I.; Yamada, T.; Kitagawa H.; Hayami S. Graphene Oxide
19
Nanosheet with High Proton Conductivity. J. Am. Chem. Soc. 2013, 135, 8097–8100.
20
(5) Bukola, S.; Liang, Y.; Korzeniewski, C.; Harris, J.; Creager, S. Selective Proton/Deuteron Transport
21
through Nafion|Graphene|Nafion Sandwich Structures at High Current Density. J. Am. Chem. Soc. 2018,
22
140, 1743–1752.
23 24
(6) Verma, A.; Scott, K. Development of High-Temperature PEMFC Based on Heteropolyacids and Polybenzimidazole. J. Solid State Electrochem. 2010, 14, 213–219.
25
(7) Kim, S.; Joarder, B.; Hurd, J. A.; Zhang, J.; Dawson, K. W.; Gelfand, B. S.; Wong, N. E.; Shimizu,
26
G. K. H. Achieving Superprotonic Conduction in Metal-Organic Frameworks through Iterative Design
27
Advances. J. Am. Chem. Soc. 2018, 140, 1077–1082. 24
ACS Paragon Plus Environment
Page 24 of 31
Page 25 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
(8) Mondal, A. N.; Tripathi, B. P.; Shahi, V.K. Highly Stable Aprotic Ionic-Liquid Doped Anhydrous
2
Proton-Conducting Polymer Electrolyte Membrane for High-Temperature Applications. J. Mater. Chem.
3
2011, 21, 4117–4124.
4
(9) Bu, F.; Zhang, Y.; Hong, L.; Zhao, W.; Li, D.; Li, J.; Na, H.; Zhao, C. 1,2,4-Triazole Functionalized
5
Poly(arylene ether ketone) for High Temperature Proton Exchange Membrane with Enhanced Oxidative
6
Stability. J. Memb. Sci. 2018, 545, 167–175.
7
(10) Campagne, B.; David, G.; Améduri, B.; Jones, D. J.; Rozière, J.; Roche, I. Novel Blend
8
Membranes of Partially Fluorinated Copolymers Bearing Azole Functions with Sulfonated PEEK for
9
PEMFC Operating at Low Relative Humidity: Influence of the Nature of the N-Heterocycle.
10
Macromolecules 2013, 46, 3046–3057.
11
(11) Zhang, H.; Wu, W.; Wang, J.; Zhang, T.; Shi, B.; Liu, J.; Cao, S. Enhanced Anhydrous Proton
12
Conductivity of Polymer Electrolyte Membrane Enabled by Facile Ionic Liquid-Based Hoping
13
Pathways. J. Memb. Sci. 2015, 476, 136–147.
14 15
(12) Jang, S.; Kim, S. Y.; Jung, H. Y.; Park, M. J. Phosphonated Polymers with Fine-Tuned Ion Clustering Behavior: Toward Efficient Proton Conductors. Macromolecules 2018, 51, 1120–1128.
16
(13) Kowsari, E.; Zare, A.; Ansari, V. Phosphoric Acid-Doped Ionic Liquid-Functionalized Graphene
17
Oxide/Sulfonated Polyimide Composites as Proton Exchange Membrane. Int. J. Hydrogen Energy 2015,
18
40, 13964–13978.
19
(14) Wu, W.; Li, Y.; Chen, P.; Liu, J.; Wang, J.; Zhang, H. Constructing Ionic Liquid-Filled Proton
20
Transfer Channels within Nanocomposite Membrane by Using Functionalized Graphene Oxide. ACS
21
Appl. Mater. Interfaces 2016, 8, 588–599.
22
(15) Singh, B.; Duong, N. M. H.; Henkensmeier, D.; Jang, J. H.; Kim, H. J.; Han, J.; Nam, S. W.
23
Influence of Different Side-Groups and Cross-Links on Phosphoric Acid Doped Radel-Based
24
Polysulfone Membranes for High Temperature Polymer Electrolyte Fuel Cells. Electrochim. Acta 2017,
25
224, 306–313.
26 27
(16) Rambabu, G.; Bhat, S. D. Amino Acid Functionalized Graphene Oxide Based Nanocomposite Membrane Electrolytes for Direct Methanol Fuel Cells. J. Memb. Sci. 2018, 551, 1–11.
28
(17) Beydaghi, H.; Javanbakht, M.; Kowsari, E. Synthesis and Characterization of Poly(vinyl
29
alcohol)/Sulfonated Graphene Oxide Nanocomposite Membranes for Use in Proton Exchange 25
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Membrane Fuel Cells (PEMFCs). Ind. Eng. Chem. Res. 2014, 53, 16621–16632.
2
(18) Anahidzade, N.; Abdolmaleki, A.; Dinari, M.; Firouz, K. Metal-Organic Framework Anchored
3
Sulfonated Poly(ether sulfone) as a High Temperature Proton Exchange Membrane for Fuel Cells. J.
4
Memb. Sci. 2018, 565, 281–292.
5
(19) Shirdast, A.; Sharif, A.; Abdollahi, M. Effect of the Incorporation of Sulfonated
6
Chitosan/Sulfonated Graphene Oxide on the Proton Conductivity of Chitosan Membranes. J. Power
7
Sources 2016, 306, 541–551.
8
(20) Jheng, L. C.; Huang, C. Y.; Hsu, S. L. C. Sulfonated MWNT and Imidazole Functionalized
9
MWNT/Polybenzimidazole Composite Membranes for High-Temperature Proton Exchange Membrane
10
Fuel Cells. Int. J. Hydrogen Energy 2013, 38, 1524–1534.
11
(21) Qiu, X.; Ueda, M.; Hu, H.; Sui, Y.; Zhang, X.; Wang, L. Poly(2,5-benzimidazole)-Grafted
12
Graphene Oxide as an Effective Proton Conductor for Construction of Nanocomposite Proton Exchange
13
Membrane. ACS Appl. Mater. Interfaces 2017, 9, 33049–33058.
14 15
(22) Mack, F.; Aniol, K.; Ellwein, C.; Kerres, J.; Zeis, R. Novel Phosphoric Acid-Doped PBI-Blends as Membranes for High-Temperature PEM Fuel Cells. J. Mater. Chem. A 2015, 3, 10864–10874.
16
(23) Muthumeenal, A.; Neelakandan, S.; Kanagaraj, P.; Nagendran, A. Synthesis and Properties of
17
Novel Proton Exchange Membranes Based on Sulfonated Polyethersulfone and N-Phthaloyl Chitosan
18
Blends for DMFC Applications. Renew. Energy 2016, 86, 922–929.
19
(24) Ahmadian-Alam, L.; Mahdavi, H. Preparation and Characterization of PVDF-Based Blend
20
Membranes as Polymer Electrolyte Membranes in Fuel Cells: Study of Factor Affecting the Proton
21
Conductivity Behavior. Polym. Adv. Technol. 2018, 29, 2287–2299.
22
(25) Fu, Y.; Manthiram, A.; Guiver, M. D. Acid-Base Blend Membranes Based on
23
2-Amino-Benzimidazole and Sulfonated Poly(ether ether ketone) for Direct Methanol Fuel Cells.
24
Electrochem. commun. 2007, 9, 905–910.
25 26
(26) Smitha, B.; Sridhar, S.; Khan, A. A. Polyelectrolyte Complexes of Chitosan and Poly(acrylic acid) as Proton Exchange Membranes for Fuel Cells. Macromolecules 2004, 37, 2233–2239.
27
(27) Li, Z.; Jiang, Z.; Tian, H.; Wang, S.; Zhang, B.; Cao, Y. Preparing Alkaline Anion Exchange
28
Membrane with Enhanced Hydroxide Conductivity via Blending Imidazolium-Functionalized and
29
Sulfonated Poly(ether ether ketone). J. Power Sources 2015, 288, 384–392. 26
ACS Paragon Plus Environment
Page 26 of 31
Page 27 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
(28) Lin, Y.-F.; Hsiao, Y.-H.; Yen, C.-Y.; Chiang, C.-L.; Lee, C.-H.; Huang, C.-C.; Ma, C.-C. M.
2
Sulfonated Poly(propylene oxide) Oligomers/Nafion® Acid-Base Blend Membranes for DMFC. J.
3
Power Sources 2007, 172, 570–577.
4
(29) Zhu, S.; Meng, Q.; Wang, L.; Zhang, J.; Song, Y.; Jin, H.; Zhang, K.; Sun, H.; Wang, H.; Yang, B.
5
Highly Photoluminescent Carbon Dots for Multicolor Patterning, Sensors, and Bioimaging. Angew.
6
Chem. Int. Ed. 2013, 52, 3953–3957.
7
(30) Kong, B.; Zhu, A.; Ding, C.; Zhao, X.; Li, B.; Tian, Y. Carbon Dot-Based Inorganic-Organic
8
Nanosystem for Two-Photon Imaging and Biosensing of pH Variation in Living Cells and Tissues. Adv.
9
Mater. 2012, 24, 5844–5848.
10 11 12 13 14 15
(31) Gupta, V.; Chaudhary, N.; Srivastava, R.; Sharma, G. D.; Bhardwaj, R.; Chand, S. Luminscent Graphene Quantum Dots for Organic Photovoltaic Devices. J. Am. Chem. Soc. 2011, 133, 9960–9963. (32) Wu, W.; Li, Y.; Liu, J.; Wang, J.; He, Y.; Davey, K.; Qiao, S. Z. Molecular-Level Hybridization of Nafion with Quantum Dots for Highly Enhanced Proton Conduction. Adv. Mater. 2018, 30, 1707516. (33) Marcano, D. C.; Kosynkin, D. V; Berlin, J. M.; Sinitskii, A.; Sun, Z.; Slesarev, A.; Alemany, L. B.; Lu, W.; Tour, J. M. Improved Synthesis of Graphene Oxide. ACS Nano 2010, 4, 4806–4814.
16
(34) He, Y.; Wang, J.; Zhang, H.; Zhang, T.; Zhang, B.; Cao, S.; Liu, J. Polydopamine-Modified
17
Graphene Oxide Nanocomposite Membrane for Proton Exchange Membrane Fuel Cell under
18
Anhydrous Conditions. J. Mater. Chem. A 2014, 2, 9548–9558.
19
(35) Ru, C.; Li, Z.; Zhao, C.; Duan, Y.; Zhuang, Z.; Bu, F.; Na, H. Enhanced Proton Conductivity of
20
Sulfonated Hybrid Poly(arylene ether ketone) Membranes by Incorporating an Amino-Sulfo
21
Bifunctionalized Metal-Organic Framework for Direct Methanol Fuel Cells. ACS Appl. Mater.
22
Interfaces 2018, 10, 7963–7973.
23 24
(36) Li, P.; Wu, W.; Liu, J.; Shi, B.; Du, Y.; Li, Y.; Wang, J. Investigating the Nanostructures and Proton Transfer Properties of Nafion-GO Hybrid Membranes. J. Memb. Sci. 2018, 555, 327–336.
25
(37) Wu, W.; Wang, J.; Liu, J.; Chen, P.; Zhang, H. Intercalating Ionic Liquid in Graphene Oxide to
26
Create Efficient and Stable Anhydrous Proton Transfer Highways for Polymer Electrolyte Membrane.
27
Int. J. Hydrogen Energy 2017, 42, 11400–11410.
28
(38) Zhao, L.; Li, Y.; Zhang, H.; Wu, W.; Liu, J.; Wang, J. Constructing Proton-Conductive Highways
29
within an Ionomer Membrane by Embedding Sulfonated Polymer Brush Modified Graphene Oxide. J. 27
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2 3
Power Sources 2015, 286, 445–457. (39) Xu, L. Q.; Yang, W. J.; Neoh, K. G.; Kang, E. T.; Fu, G. D. Dopamine-Induced Reduction and Functionalization of Graphene Oxide Nanosheets. Macromolecules 2010, 43, 8336–8339.
4
(40) Yuan, Z.; Wu, X.; Jiang, Y.; Li, Y.; Huang, J.; Hao, L.; Zhang, J.; Wang, J. Carbon
5
Dots-Incorporated Composite Membrane towards Enhanced Organic Solvent Nanofiltration
6
Performance. J. Memb. Sci. 2018, 549, 1–11.
7
(41) Kaminska, I.; Das, M. R.; Coffinier, Y.; Niedziolka-Jonsson, J.; Sobczak, J.; Woisel, P.; Lyskawa,
8
J.; Opallo, M.; Boukherroub, R.; Szunerits, S. Reduction and Functionalization of Graphene Oxide
9
Sheets Using Biomimetic Dopamine Derivatives in One Step. ACS Appl. Mater. Interfaces 2012, 4,
10
1016–1020.
11
(42) Hwang, S. H.; Kang, D.; Ruoff, R. S.; Shin, H. S.; Park, Y. Bin. Poly(vinyl alcohol) Reinforced
12
and Toughened with Poly(dopamine)-Treated Graphene Oxide, and Its Use for Humidity Sensing. ACS
13
Nano 2014, 8, 6739–6747.
14
(43) Yang, L.; Kong, J.; Yee, W. A.; Liu, W.; Phua, S. L.; Toh, C. L.; Huang, S.; Lu, X. Highly
15
Conductive Graphene by Low-Temperature Thermal Reduction and In Situ Preparation of Conductive
16
Polymer Nanocomposites. Nanoscale 2012, 4, 4968–4971.
17
(44) Pandey, R. P.; Thakur, A. K.; Shahi, V. K. Sulfonated Polyimide/Acid-Functionalized Graphene
18
Oxide Composite Polymer Electrolyte Membranes with Improved Proton Conductivity and
19
Water-Retention Properties. ACS Appl. Mater. Interfaces 2014, 6, 16993–17002.
20 21
(45) Fang, M.; Wang, K.; Lu, H.; Yang, Y.; Nutt, S. Single-Layer Graphene Nanosheets with Controlled Grafting of Polymer Chains. J. Mater. Chem. 2010, 20, 1982–1992.
22
(46) Wang, J.; Zhao, L.; Wei, D.; Wu, W.; Zhang, J.; Cheng, X. Effects of Intercalated Molecules in
23
Graphene Oxide on the Interlayer Channels for Anhydrous Proton Conduction. Ind. Eng. Chem. Res.
24
2016, 55, 11931–11942.
25 26
(47) Tang, H.; Ehlert, G. J.; Lin, Y.; Sodano, H. A. Highly Efficient Synthesis of Graphene Nanocomposites. Nano Lett. 2012, 12, 84–90.
27
(48) Yang, J. M.; Wang, S. A. Preparation of Graphene-Based Poly(vinyl alcohol)/Chitosan
28
Nanocomposites Membrane for Alkaline Solid Electrolytes Membrane. J. Memb. Sci. 2015, 477, 49–57.
29
(49) Jiang, R.; Kunz, H. R.; Fenton, J. M. Composite Silica/Nafion® Membranes Prepared by 28
ACS Paragon Plus Environment
Page 28 of 31
Page 29 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
Tetraethylorthosilicate Sol-Gel Reaction and Solution Casting for Direct Methanol Fuel Cells. J. Memb.
2
Sci. 2006, 272, 116–124.
3
(50) Dong, X.-Y.; Wang, J.-H.; Liu, S.-S.; Han, Z.; Tang, Q.-J; Li, F.-F.; Zang, S.-Q. Synergy between
4
Isomorphous Acid and Basic MOFs for Anhydrous Proton Conduction of Low-Cost Hybrid Membranes
5
at High Temperature. ACS Appl. Mater. Interfaces 2018, 10, 38209–38216.
6
(51) Yin, Y.; Wang, H.; Cao, L.; Li, Z.; Li, Z.; Gang, M.; Wang, C.; Wu, H.; Jiang, Z.; Zhang, P.
7
Sulfonated Poly(ether ether ketone)-Based Hybrid Membranes Containing Graphene Oxide with
8
Acid-Base Pairs for Direct Methanol Fuel Cells. Electrochim. Acta 2016, 203, 178–188.
9 10
(52) Eisenberg, A. Clustering of Ions in Organic Polymers. A Theoretical Approach. Macromolecules 1970, 3, 147–154.
11
(53) Liu, Q.; Shi, J.; Sun, J.; Wang, T.; Zeng, L.; Jiang, G. Graphene and Graphene Oxide Sheets
12
Supported on Silica as Versatile and High-Performance Adsorbents for Solid-Phase Extraction. Angew.
13
Chem. Int. Ed. 2011, 50, 5913–5917.
14 15
(54) Compton, O. C.; Nguyen, S. T. Graphene Oxide, Highly Reduced Graphene Oxide, and Graphene: Versatile Building Blocks for Carbon-Based Materials. Small 2010, 6, 711–723.
16
(55) Shukla, G.; Shahi, V. K. Sulfonated Poly(ether ether ketone)/Imidized Graphene Oxide Composite
17
Cation Exchange Membrane with Improved Conductivity and Stability for Electrodialytic Water
18
Desalination. Desalination 2018, https://doi.org/10.1016/j.desal.2018.03.018.
19
(56) Gong, C.; Zheng, X.; Liu, H.; Wang, G.; Cheng, F.; Zheng, G.; Wen, S.; Law, W.-C.; Tsui, C.-P.;
20
Tang, C.-Y. A New Strategy for Designing High-Performance Sulfonated Poly(ether ether ketone)
21
Polymer Electrolyte Membranes Using Inorganic Proton Conductor-Functionalized Carbon Nanotubes.
22
J. Power Sources 2016, 325, 453–464.
23
(57) Dong, C.; Wang, Q.; Cong, C.; Meng, X.; Zhou, Q. Influence of Alkaline 2D Carbon Nitride
24
Nanosheets as Fillers for Anchoring HPW and Improving Conductivity of SPEEK Nanocomposite
25
Membranes. Int. J. Hydrogen Energy 2017, 42, 10317–10328.
26 27
(58) Li, Y.; Wang, S.; He, G.; Wu, H.; Jiang, Z. Facilitated Transport of Small Molecules and Ions for Energy-Efficient Membranes. Chem. Soc. Rev. 2015, 44, 103–118.
28
(59) Wang, J.; He, Y.; Zhao, L.; Li, Y.; Cao, S.; Zhang, B.; Zhang, H. Enhanced Proton Conductivities
29
of Nanofibrous Composite Membranes Enabled by Acid-Base Pairs under Hydrated and Anhydrous 29
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Conditions. J. Memb. Sci. 2015, 482, 1–12.
2
(60) Choi, B. G.; Hong, J.; Park, Y. C.; Jung, D. H.; Hong, W. H.; Hammond, P. T.; Park, H. Innovative
3
Polymer Nanocomposite Electrolytes: Nanoscale Manipulation of Ion Channels by Functionalized
4
Graphenes. ACS Nano 2011, 5, 5167–5174.
5 6
(61) Tamura, T.; Kawakami, H. Membranes for Fuel Cell Electrolytes. Nano Lett. 2010, 10, 1324– 1328.
30
ACS Paragon Plus Environment
Page 30 of 31
Page 31 of 31 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
ACS Applied Materials & Interfaces
Graphical Abstract
2 3
4
5
31
ACS Paragon Plus Environment