1749
Langmuir 1993,9, 1749-1763
Effects of Surface Hydration on the Deposition of Silane Monolayers on Silica J. D. Le Grange* and J. L. Markham AT&T Bell Laboratories, Princeton, New Jersey 08542-0900
C . R. Kurkjian AT&T Bell Laboratories, Murray Hill, New Jersey 07974 Received December 4, 1992
The deposition of a silane monolayer on silica depends on the chemical reactions between the silane molecules and the hydroxyl groups on the silica surface. We have studied the effects of dehydration and rehydration of flat silica substrates on the deposition of a self-assembled monolayer of octadecyltrichlorosilane by wing FTIR spectroscopy and ellipsometry. The results demonstratethat monolayer coverage increases with degree of hydration of the substrate. Patches of ordered chains form on a dehydrated surface and that coverage increases with hydration. A fully hydrated surface,however, is not neceBBaTy for complete coverage of the substrate, suggesting that not every silane group is bonded to the surface. 1. Introduction
Recently, we have initiated a program to study the polymer-silica interface on optical fiber by using monolayers of silanes deposited on the silica by the technique of self-assembly. The mechanical strength of optical fiber degrades in the presence of water due to the reactivity of the silica surface with water. Static fatigue of the fiber, in which it fails under a constant applied stress after a time delay, results from the interaction of water with the stressed bonds of the silica and depends on the concentration of water in the environment. Our long term objective is to investigate possible ways of reducing fiber fatigue, by applying monolayers of various silane compounds to optical fiber and studying the fatigue behavior of that fiber in different environments. Self-assembledmonolayersare densely packed, ordered filmswhich attach to the surface by chemical bonds.'-' By depositing such a monolayer on silica, we achieve full coverage of the silica surfaceand form a hydrophobiclayer which may impede diffusion of water to the interface? By changing the chemistry of the constituent molecules and studying the effectson fiber fatigue, we hope to contribute to the understanding of the underlying mechanisms of water-mediated corrosion of silica. We have chosen octadecyltrichlorosilane(OTS),shown in Figure 1,for the initial experimentsbecause of the large amount of previous work on the depositionand characterizationof monolayers of this c o m p ~ u n d . l * ~ * ~ * ~ OTS,a long chain silane, is structurally similar to a couplingagent,such as (glycidoxypropyl)trimethoxyailane, in that both have hydrolyzable functional groups on a silicon atom which can bond to silanol groups on the silica surface. Silane coupling agents are either mixed into a polymer or applied directly to a silica substrate, in which case a cross-linked network of S i 4 bonds forms between silane molecules. In the case of optical fiber, coupling agents are mixed into the coating to enhance adhesion to ~~
(1)Maoz, R.;Sagiv, J. J. Colloid Interface Sci. 1984,100,465. (2) Gun, J.; h v i c i , R.; Sagiv, J. J. Colloid Interface Sci, 1984,101, 201. (3) Allara, D. L.; Nuzzo, R. G. Langmuir 198S,1,45. (4) Allara, D. L.; Nuzzo, R. G. Langmuir 1985,1, 52. (5) Maw, R.; Sagiv, J. Langmuir 1987,3, 1034. (6) Waseerman, S. R.; Whitaides, G. M.; Tidewell, I. M.; Ocko, B. M.; Perehan, P.S.;Axe, J. D.J. Am. Chem. SOC.1989,111,5852. (7) Anget, D. L.; Simmons,G. W.Langmuir 1991, 7 , 2236.
I
(~H2117
I
ci- si -CI
I
CI
I (CH2)17
H-0
I
-Si-
I (CH2)17
I
0 -Si-
I
I 0
A SURFACE Figure 1. Structure of octadecyltrichlorosilane (OTS)and a schematic of the molecule on the surface after depoaition by self-assembly.
the silica;however,the interactionbetweenthose molecules and the silica surface after fiber draw is not well understood. At 2200 O C , the furnace temperature in the fiber draw process, allwater moleculesand almost all OH groups are removed from the surface. A self-assembledmonolayer can be used as a model system to study the bonding of silanes to a silica surface. Although there have been numerous studies of the structure of self-assembled monolayers, the structure of the silane-silica interface has not been thoroughly characterized. Water, which is either bound to the surface or present in the solution, hydrolyzes the chlorosilanea to form silanols. These silanols then form stable bonds to the silicaupon reactingwith the surface silanolsand release water?pg It is generally assumed that a fully hydrated surface, which has 5 OH groups per 100A2,l0is necessary for self-assembled monolayer formation.6 Results from recent experimente,however, suggest that there may not be extensive chemicalbonding between the monolayer and the surface. The surface of silicon coated (8) Silberzan, P.;Leger, L.;Ausserre, D.;Benattar, J. Langmuir 1991, 7, 1647. (9) Sagiv, J. J. Am. Chem. SOC.1980,102,92. (10) Iler, R. K. The Chemistry of Silica; John Wiley & Sons: New York, 1979; Chapter 6.
0743-7463/93/2409-1749$04.00/00 1993 American Chemical Society
Le Grange et al.
1750 Langmuir, Vol. 9,No. 7, 1993 by an OTS monolayer, for example, is smoother than that of uncoated silicon, as if the monolayer covers the surface without bonding to it.* It has been observed by FTIR spectroscopy of high surface area silicas exposed to OTS solution, that the absorption peaks for water and OH do not change upon exposure to OTS," a result that is consistent with the idea that few bonds form between the monolayer and the silica surface. In this paper, we have addressed the question of the formation of bonds to the OH groups on the surface directly by studying monolayer deposition on dehydrated and partially hydrated surfaces.
2. Dehydration, Rehydration, and Hydroxyl Groups on Silica The surface chemistry of silica is controlled by the following reaction of water with the Si02 network -Si-&Si-
-
+ H20
2Si-OH
which produces silanols on the surface. Hydroxyl groups on silica can hydrogen bond to each other and to water molecules. Water molecules concentrate on the surface at silanol groups to which they either physieorb or chemisorb. These molecules are available to attack other Si-0 linkages on the surface.12 Surface silanols are also the sites to which other adsorbates, such as alkylsilanes, bond. The silica surface on fiber, therefore, needs to be hydroxylated enough to form bonds to the polymer, in our case the alkylsilane monolayer. Much work has been done previously to characterize the hydroxyl groups on hydrated and dehydrated high surface area silica. In this work we are using low area silicasand, because there has been little work on the surface chemistry of bulk fused silica, we must assume that it is similar to that of the high area silicas. The kinetics of dehydration depends on the concentration of surface silanols and temperature.1° Physisorbed water is removed from the surface by pumping at room temperature. Silanol groups are removed by heating the silica either in vacuum or under a gas flow to remove the water which evolves from the surface. At temperatures between 170 and 400 OC, silanol groups condense and eliminate water. This dehydration process is reversible because less than half the hydroxyl groups have been removed at 400 OC, and water readily reacts with the silanols remaining on the surface. Above 400-450 "C, the process starts to be less reversible as the density of silanols decreases.13 Above 700 OC, for example,all of the silanols are unpaired,isolated OH groups occurring at a density of roughly 1OH per 100 A2.14 The silica surface becomes hydrophobic above 850 OC, and chemisorption of water is inhibited.ls At lo00 "C, the temperature selected for our experiments, the surface is left with less than 1 OH per 100 A2.10 Rehydration of the silica surfaceoccursvery slowlyafter heating the glass to temperatures above 400 0C.16J7The surface becomes increasinglyhydrophobicwith increasing temperature because water molecules concentrate locally on the surface OH groups, leaving an increasingly larger area dry as the density of OH decreaseswith temperature. Above 800 OC water molecules can concentrate on the (11) Tripp, C. P.; Hair, M. L. Langmuir 1992,8,1120. (12) Pantano,C. G. In Strength of Inorganic Glass;Kurkjian, C. R., ed.; Plenum Press: New York, 1985. (13) Armistead, C. G.; Hockey, J. A. Trans. Faraday SOC.1967, 63, 2549. (14) Thorp,J. M. J. Phys. Chem. 1969,65,869, 1741. (15) Hair, M. L.Znfrared Spectroscopy in Surface Chemistry;Marcel Dekker, Inc.: New York, 1967; Chapter 4. (16) Young, G. J. J. Colloid Sci. 1968, 13, 67. (17) Fnpiat, J. J.; Gastuche, M. C.; Brichard, R. J. Phys. Chem. 1962, 66,805.
isolated OH groups, but because these occur at a low density, almost all of the silica surface remains dry.16The more a surface is dehydrated, i.e. the more hydroxyl groups are removed, the longer rehydration takes. A silicaaerogel heated at 1100 "C for 10 h has 0.06 OH per 100 A2 and requires 60 h in boiling water to be rehydrated. Silica dehydrated to 0.66 OH per 100 A2 after 10 h at 900 OC requires several years in room temperature water to be rehydrated.1°J8 3. Experimental Methods Monolayers of OTS were deposited by the self-assembly technique on plates of fused silica (Hereaus Amersil T08) and on the oxide surface of silicon wafers,which were either hydrated, dehydrated, or rehydrated. The thickness and relative order of the hydrocarbon chains were determined by ellipsometry of the monolayers on oxidized silicon and transmission FTIR spectroscopy of the monolayers on silica. All of the silica slides and silicon wafers were cleaned in an ultrasonic bath of high-purity water to remove dust and then boiled for 20 min in a mixture of water, ammonium hydroxide, and hydrogen peroxide at a ratio of 6 l : l by volume. The slides were rinsed in an overflow rinse for a half hour and then blown off with dry nitrogen. Before use they were stored under highpurity water at room temperature for at least 24 h. We dehydrated the slides by baking them in a g h tube furnace at lo00 "C for 10h under a constant flow of dry nitrogen. The nitrogen waa the boil-off from a liquid nitrogen supply. Upon removal from the furnace the slides were either submerged immediately in the OTS solution for monolayer deposition or submerged in water for rehydration. A 2.5 X 10-9M solution of OTS in a mixture of 20%CCW80% Isopar Gle by volume was prepared 30 min before deposition.' The Isopar G was run through an alumina column, equilibrated overnight with a trace of water (2 drops per 1OOmL)and decanted into the solution flask. The substrates were immersed in the solution for 30 min and then rinsed sequentially in carbon tetrachloride, ethanol, and carbon tetrachloride. Eachrinse step consisted of drenching the sample with the solventfrom a squeeze bottle a minimum of ten times. OTS is deposited on the oxide layer of siliconwafers as a control to ensure that there are no problem with either the solution or deposition procedure. The thickness of the monolayer ie then measuredwithaGaertnerL115Bellipaometer. Wehaveaeeumed that the monolayer has the same index, 1.46, aa the oxide layer on the silicon and, therefore, measure the change in the effective thickness of the oxide after OTS deposition. This is done by comparing the thickness of the layer on two pieces of the same wafer that have undergone all of the same promsing stepe prior to OTS deposition on one of the pieces. The assumption of 1.46 for the index of the silane film is a reasonable one because organic films typically have indices of refraction in the range of 1.4 to 1.5;moreover it has been shown that a variation of 0.05 in index changes the thickness obtained by only 1 A.6 The thickness measured for each sample is an average over roughly 10 different spots on the sample. The degree of ordering between the hydrocarbon chaine of monolayers on fused silica has been measured by FTIR spectroscopy in transmission. The spectra were obtained with a Nicolet 7199spectrometer equipped with a liquid nitrogen cooled mercury cadmium telluride detector sensitive over the range of 400 to 4000 wavenumbers. All spectra were averaged over 1024 scans at a resolution of 1 or 2 cm-'. Spectra of monolayers were ratioed to background spectra measured from the substrate silica. The silica plates were cut into halves prior to the cleaning and dehydratioddeposition proceeses. The halves used for background scans were exposed to all of the same procedures as the sample halves, except for the deposition step. The peak p i t i o n and width (fwhm) of the C-H stretch at 2918 cm-l were studied for f i s deposited on substrates, which were either hydrated, dehydrated, or rehydrated, to determine the effect of surface ~
~~~
(18) Agzamkheaev, A. A.; Zhuravlev, L. T.; Kieelev, A. V.; Shengeliya, K. Y. Kollordn. Zh.1974,36, 1145. (19) Ieopar G is obtained from Euon.
Silane Deposition Table I. Ellipeometry of OTS on Oxidized Silicon OTS f i i thickness (A) degree of hydration hydrated overnight 28 f 2 14.2h 6.4 dehydrated' 29 h 2 dehydratedb 28+2 rehydrated in water a Ambient humidity in room outaide furnace estimated to be l e 30%. Ambient humidity in room outaide furnace estimated to be 50-60%.
Langmuir, Vol. 9, No. 7,1993 1761
99.65
-
Y
z
?
-
i5 98.95 C
" 1
Table 11. FTIR Spectra of OTS on Fwed Silica 98.60 peak position fwhm degrw of 98.25 hydration (cm-l) ABS (%) (cm-9 hydrated overnight 2918.0 + 0.6 1.40 + 0.36 16 h 2 97.80 dehydrated' 2918.6 + 1.1 0.64 + 0.2 16 h 3 I I I I I I I I I 3350 3272 3194 3118 3098 2960 2082 2804 2726 2848 rehydrated 13 h 2 2917.9 h 0.5 1.36 h 0.26 WAVENUMBERS Ambient humidity outaide furnace estimated to be M % . Figure 2. FTIR transmission spectra,in the region of the C-H stretching modes, of OTS monolayers on silica surfaces that are hydroxyl groups on OTS deposition. Baselines of the transfully hydrated (dotted line), rehydrated in room temperature water (solidline),and dehydrated(dashedline)beforemonolayer mission spectra were corrected for excess slope and shifted to deposition. 100% transmission. Peak positions and widths were then determined using the software routines of the instrument.
4. Results and Discussion
OTS monolayers deposited on silica are characterized either by ellipsometry of monolayers on the oxide layer of silicon wafers or by FTIR spectroscopy of monolayers on fusedsilica. Results of these measurementsfor monolayers deposited on silica that is hydrated, dehydrated, or rehydrated are summarized in Tables I and 11. OTS on Hydrated Silica. OTS monolayersdeposited on the fully hydrated oxide surface of pieces of silicon wafer are measured to be 28 f 2 A thick after subtracting the thickness of the native oxide on a reference wafer. The native oxide is 11.3 i 1.4 A. The measured thickness of 28 A is an average over samples from 10 experiments and is in reasonable agreement with previous measurements which range from 23 to 26 A6v7The difference of several angstroms between this value and previously published values may be explained by a combination of factors such as the accuracy of the ellipsometric calculation for such a thin film,the estimation of the monolayer index, and the variation in the underlying oxide thickness. Given these sources of uncertainty in calculating thickness, the measured value of 28 A is consistent with the thickness expected for a densely packed monolayer with chains oriented normal to the substrate in an &-trans configuration. OTS monolayers on fused silica plates are characterized by FTIR spectroscopic measurements in transmission. Although the signal-to-noise ratio is smaller than that obtained by internal reflectiontechniques,there is enough signal from the layers on the two sides of the slide to monitor the C-H stretching modes at 2861 and 2918 cm-l. The 2918-cm-' peak is particularly useful as both its position and width are affected by the degree of conformational ordering in the alkyl chains. It has been shown in spectral calculations that the symmetric and antisymmetric C-H stretches shift roughly 6 cm-1 in going from an ordered, all trans alkyl chain to a disordered chain with We have velified this effect by comparing gauche the spectrum from a KBr pellet of stertric acid with that of liquid Nujol. The peak position for stearic acid, located at 2916 cm-l, shifts to 2924 cm-l in Nujol, a long chain hydrocarbonliquid. In addition, the peak width for Nujol of 62 wavenumbers is considerably broader than the 27 (20) Snyder, R. G.; Stausa, H. L.; Elliger, C. A. J. Phys. Chem. 1982, 86, 5145.
wavenumber width of that peak in the spectrum of stearic acid. The spectrum, plotted by the dotted line in Figure 2, of an OTS monolayer deposited on a fully hydrated fused silica plate, exhibits a C-H stretching peak at 2918 cm-l with a peak width (fwhm) of 16 cm-'. Both the position and width of the peak are in agreement with attenuated total reflection (ATR) measurements of OTS deposited on the hydrated oxide surface of ~ilicon.'*2~ OTS on Dehydrated Silica. Deposition of OTS monolayers on dehydrated silica is extremely sensitive to the humidity to which the silica is exposed after removal from the furnace. Monolayers deposited on the oxidized surface of silicon following dehydration at lo00 O C in a nitrogen atmosphere ranged in thicknese from 14.2 i 6.4 A thick in the winter to 28 f 2 A in the spring months. We estimate that the relative humidity in the lab varies from a low of 10% in the winter to a maximum value of 60% in the summer. The transmission FTIR spectra of OTS monolayers on fused silica that is dehydrated, ale0 suggest a strong dependenceof deposition on relative humidity. The C-H stretching mode at 2918 cm-l is broadened and less intense than in the fully hydrated case; however, none of the spectra exhibita shiftas would be expected for a morlolayer of disordered chains. The intensity and peak widths are sensitiveto relative humidity. The spectrum in Figure 3, for example, is from a monolayer deposited after surface dehydration in the winter. Although the signal-to-noise is too low to determine the peak position by the software of the instrument, it does not appear to be shiftad from 2918 cm-l. Spectra of OTS deposited on dehydrated fused silica in the spring months, as shown by the dashed line in Figure 2, exhibit a more intense C-H stretching peak which is only slightly broadened. Positions, widths, and heights of the 2918-cm-I peak are tabulated in Table II; each number represents an average of ten independent samples prepared at the specified conditions. The values for monolayers on dehydrated subatrates are obtained only from experiments run after April (Le. the samples that exhibit spectra with large enough signal-to-noise to analyze). In order to eliminate rehydration of the silica surface by high relative humidity (in the spring and summer months), we have tried transferring the elides from the furnace to the OTS solution in a glovebag inflated with (21) T h a n , N.; &an,
A.; Penner, T. L. Langmuir 1989,6,101.
Le Grange et 41.
1752 Langmuir, Vol. 9, No. 7, 1993 R
I
100.62
100.07
HO -SI
1
I 0
-
L
E5
99.52
98.97
-
-0 -Si - 0-Si-
0-Si
I
I
I
I
0
OH
R
I
- 0 -SiI I
OH
OH
R
I
R
I
0- Si -OH HO-S I-
I OH
I
0
Figure 4. Proposed structure for an OTS monolayer in which roughly one in five chains forms a bond to the silica surface.
$1 98.42
97.87
97.32 3350
R
I
SURFACE
W
5
R
R
3272
3194
3116
3038 2960 2882 WAVENUMBERS
2804
2726
2648
Figure 3. FTIR transmiseion spectrum of OTS on fused silica exposed to OTS solution at low ambient humidity (estimatedto be 10-3096).
argon. The spectra of OTS monolayers on these substrates exhibit similar widths and intensities for the C-H stretch peak. The dependenceof depositionon relative humidity, therefore, must be either from the amount of residual water in the drynitrogen lines or from the concentrationof water in the OTS solution. Since the dry nitrogen is from the liquid nitrogensupply,it ismore liiely that the dehydrated silica is picking up water from the OTS solution. The extent of this rehydration depends on relative humidity because of the variation in the concentration of water in the OTS solution and in the vapor above it. X-ray photoelectron spectra ( X P S ) of monolayers deposited on dehydrated surfaces, however, do not exhibit peaks for chlorine?i22 This indicates that even at low relative humidity there is enough water present in the solution to hydrolyze the chlorosilane groups and that the variation in deposition with relative humidity is not due to incomplete hydrolysis of the OTS. XPS spectra22also show low levels of carbon for the surfaces of the background substrates indicating that variations in the spectra are not due to surface contamination. This is especiallytrue for dehydrated surfaces which have the lowest level of residual carbon. This is not surprising as any organic contaminants are vaporized in the lo00 "C furnace. The decrease in thickness observed by ellipsometry of monolayers on oxidized wafers may be explained either by submonolayer coverage, i.e. islands of molecules with ordered chains, or by a homogeneous distribution of molecules with disordered chains. It appears, however, since the C-H stretch is not shifted in wavenumber but the intensity is still less than that of a monolayer on a hydrated surface, that the molecules are driven by strong chain-chain interactions to form dense patches on the surface. The surface coverage changes with the number of hydroxyl groups on the substrate surface, and at some critical degree of hydroxylation, monolayer coverage is achieved. OTS on Rehydrated Silica. If dehydrated silica substrates are submerged in liquid water at room temperature for several minutes, the resulting density of hydroxyl groups on the surface is sufficient for deposition of OTS monolayers which are indistinguishable from monolayers deposited on fully hydrated surfaces. The thickness of monolayers grown on these rehydrated surfaces is 28 f 2 A, as measured by ellipsometry.
FTIR transmission spectra of OTS monolayers on rehydrated fused silica,as shown by the solid line in Figure 2, indicate that after a few minutes in water there are enough hydroxyl groups on the surface for the surface to be completely covered by a dense monolayer of ordered hydrocarbon chains. The absorptionintensity, width, and position of the higher energy C-H stretching mode tabulated in Table I1are indistinguishablefromthe values for monolayersdeposited on fully hydrated surfaceswithin the standard deviations between different samples of the same type. It has been observed in experiments measuring reaction rates of water with high surface area silicasthat two types of strained ring defects on the surface react with water at time constants of 17 me and 1 s at 100% RH,23 corresponding to time constants of 170me and 10 s at the lower limit of 10% relative humidity in the winter. Clearly, the faster process, which occurs at t