Evolution of Nitrogen-Related Defects in Graphitic Carbon Nitride Nanosheets Probed by Positron Annihilation and Photoluminescence Spectroscopy Biswajit Choudhury, Kamal Kumar Paul, Dirtha Sanyal, Anil Hazarika, and Pravat Kumar Giri J. Phys. Chem. C, Just Accepted Manuscript • DOI: 10.1021/acs.jpcc.8b01388 • Publication Date (Web): 06 Apr 2018 Downloaded from http://pubs.acs.org on April 8, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
Evolution of Nitrogen-Related Defects in Graphitic Carbon Nitride Nanosheets Probed by Positron Annihilation and Photoluminescence Spectroscopy Biswajit Choudhury1*, Kamal Kumar Paul2, Dirtha Sanyal3,4, Anil Hazarika5, P. K. Giri2 1
Physical Sciences Division, Institute of Advanced Study in Science and Technology, Paschim Boragaon, Guwahati 781035, India 2
Department of Physics, Indian Institute of Technology Guwahati, Guwahati 781039, India 3 4
Variable Energy Cyclotron Center, 1/AF Bidhanngar, Kolkata 700064, India
Homi Bhabha National Institute, Training School Complex, Anushakti Nagar, Mumbai 400094, India
5
Department of Electronics and Communication Engineering, Tezpur University, Tezpur 784028, India
*Corresponding Author:
[email protected] ,
[email protected] , Phone: +918486912412
1
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 2 of 44
ABSTRACT: Defects play a pivotal role in the device performance of a photocatalytic, light emitting or photovoltaic system. Herein, graphitic carbon nitride (g-C3N4) nanosheets are prepared at different calcination temperatures, and the evolution of defects in the system is studied by positron annihilation spectroscopy (PAS) and photoluminescence (PL) spectroscopy. Steady-state PL spectra show that free and defect bound excitonic emissions peaked at 2.78 eV, 2.58 eV and 2.38 eV are dominant with above bandgap excitation. Time-resolved PL studies reveal a significant enhancement of excitonic lifetime from 17.4 ns for free exciton to 27.4 ns in case of defect bound exciton. We provide a direct correlation between the defects observed by PAS with that of the excitonic lifetime found from the PL studies. Below bandgap excitation activates defect emission and it is characterized by a short carrier lifetime (~0.14 ns). Excitation power-dependent PL study with 405 nm laser shows progressive red-shift and narrowing of the emission line. We have interpreted the different PL features with defect band-filling of exciton, interplanar, intraplanar, interchain exciton migration, etc. These results are significant for tuning the optoelectronic properties of g-C3N4 nanosheets and exploiting its applications in various emerging areas.
2
ACS Paragon Plus Environment
Page 3 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
1. INTRODUCTION 1
Carbon nitride with graphene-like layered structures has drawn full attention for water splitting
2
reaction and in the decontamination of aqueous organic pollutants under visible light.1-4 The
3
system has a bandgap of 2.7 eV and builds up of s-heptazine units with tertiary nitrogen bridging
4
the nearest heptazine structures.1,3 Graphitic carbon nitride (g-C3N4) can be synthesized by
5
simple thermal condensation method from low-cost precursors, viz., thiourea,5 melamine,6
6
cyanamide,7 urea,3,8, etc. Temperature has a direct influence on the degree of condensation and
7
packing between layers, which otherwise influences the π conjugation in the sp2 bonded
8
framework.9 The high calcination temperature is known to reduce the interlayer distance in C3N4.
9
Compactness of the layers has an impact on the spectral red-shift in absorption and
10
photoluminescence. Wu et al. with density functional calculation studied the effect of interlayer
11
electron coupling on the optical properties of C3N4.10 In another study, Chen et al. reported that
12
the steric interactions of the lone pair electrons on adjacent nitrogen atom could tune the visible
13
light absorption in C3N4.11 C3N4 emits strong blue light under UV excitation.12 Its strong
14
excitonic emission in the visible region, thermal resistance, and tunable bandgap makes C3N4 a
15
popular choice for light-emitting diodes, luminescence-based bio, and chemosensor.13-16 Excitons
16
generated in the heptazine unit of C3N4 are reported to undergo facile migration along π stacking
17
direction in C3N4.17 Long distance exciton transport is necessary for photovoltaic and light
18
emitting diode applications.18-19 C3N4 quantum dots incorporated into polymer cells show
19
superior solar cell performance wherein the π conjugated system of C3N4 acts as charge transport
20
medium in the hybrid solar cell.19 Cui et al. observed sufficiently long excitonic lifetime in
21
phenyl modified graphitic carbon nitride and its possible requirements for advanced optical
22
super-resolution techniques.20 3
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 44
23
Defects are inevitable in C3N4 as its structure evolves through the formation of several
24
intermediates, such as cyanuric acid, melon, etc.21 The various uncondensed defects in C3N4 are
25
–NH2/NH, cyano/cyanide (C≡N, -NCN-) and oxygenated functional groups (-OH, -COOH).21,22
26
Besides, intrinsic defect such as N and carbon vacancies are also generated in C3N4 in the
27
thermal condensation process.23-25 Dong et al. observed efficient N2 fixation ability of N
28
deficient carbon nitride.23 Similarly, Tay suggested positive attributes of a defect in enhancing
29
photocatalytic H2 production in C3N4.24 With surface photovoltage spectroscopy (SPV), Wu and
30
his team measured the presence of NH/-NH2 related shallow and deep trap states in the bandgap
31
of C3N4.26 It was speculated that these defects are detrimental to the efficient production of H2.
32
In the present study, we aim to understand the specific nature and evolution of defects in
33
C3N4 as a function of its calcination temperature by using positron annihilation spectroscopy
34
(PAS) and photoluminescence (PL) spectroscopy techniques. We investigate the influence of
35
structural defects on the excitonic emission in C3N4. A detailed understanding of the nature of
36
defects in C3N4 and its impact on the excitonic luminescence and decay processes is necessary
37
before the implementation of this material in optoelectronics, photovoltaics, and solar cell
38
applications. Here, we employ steady-state and time-resolved spectroscopy techniques to identify
39
the free excitonic, bound excitonic and defect-related emissions and their decay dynamics. C3N4
40
are grown at different calcination temperatures. To the best of our knowledge and understanding,
41
for the first time, we have employed PAS to identify the nature of defects in C3N4 nanosheets
42
and provided a direct correlation between results of PAS and PL. PAS is a unique nuclear solid-
43
state technique to study the electron density and electron momentum distribution and in
44
particular, vacancy-type defects in the material.27-28 Free and defect bound excitonic emission
45
and trap state related luminescence and the associated carrier lifetime in C3N4 are studied with 4
ACS Paragon Plus Environment
Page 5 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
46
photoexcitation energies above and below the optical bandgap of the samples. Our results show
47
that defect bound excitons have sufficiently longer lifetime than that of the free excitons.
48 49
2. EXPERIMENTAL
50
2.1.
Preparation of graphitic carbon nitride (g-C3N4) at various temperatures
51
Graphitic carbon nitride was synthesized by thermal condensation method. Typically, urea was
52
taken in a beaker and heated in a reaction hood till it was scorched. The dried powder was
53
crushed in a mortar to get fine white powder. The powder was taken in a crucible covered with a
54
lid and heated in a tube furnace at 420 oC for 2 h. The final product was whitish yellow which
55
was again finely ground and kept in a sample vial. Similarly, calcination of dried urea was
56
performed at 470 oC, 520 oC, 570 oC, respectively.
57
2.2.
Materials Characterisation
58
X-ray diffraction (XRD) was performed in a Bruker D8 Advance X-ray diffractometer (0.154 nm
59
Cu Kα radiation, 40 kV, 40 mA) for the diffraction range 2θ~10-35o. Low and high-resolution
60
transmission electron microscope (TEM) images were collected in FEI Technai G2 20 S-Twin.
61
The operating voltage was 200 kV, and the spectral resolution was 2.4 Å. Fourier transform
62
infrared (FTIR) spectroscopy data were recorded in a Perkin Elmer, Spectrum BX
63
spectrophotometer. TGA was performed in a Perkin Elmer TGA 4000 series. The measurement
64
was performed under N2 flow at a heating rate of 10 oC/min. Diffuse reflectance spectra (DRS)
65
of the samples were collected in a Shimadzu UV–visible spectrometer (Model 2450) with BaSO4
66
as the standard reference. Steady-state photoluminescence spectra of the samples were monitored
67
in Fluoromax-4, Horiba Scientific spectrometer with an excitation and emission slit width of 2
68
nm. Laser power dependent PL studies were performed using a 405 nm (3.06 eV) diode laser 5
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 44
69
(Cube, coherent) equipped with cooled charge-coupled (CCD) detector (Princeton instruments,
70
PIXIS 100B). Time-resolved photoluminescence (TRPL) spectra were recorded using a
71
picosecond time-resolved luminescence spectrometer (Edinburgh Instruments, model: FSP920).
72
The chemical compositions of the samples were evaluated with X-ray photoelectron
73
spectroscopy (XPS) PHI X-tool automated photoelectron spectrometer (ULVAC-PHI, Japan).
74
The source was Al Kα X-ray beam source (1486.6 eV), and the recorded beam current was 20
75
mA. In XPS measurement, adventitious carbon (AdC) C 1s signal at 284.8 eV is considered as
76
binding energy (B.E.) reference.29,30 Au 4f signal might be considered as a B.E. reference peak
77
for carbon materials to reduce the error (0.1±0.2) while considering C 1s as reference.29,30
78
However, correct referencing of Au 4f signal for B.E. correction is not properly resolved and
79
thus, C 1s referencing is considered as widely adopted method for B.E. correction.29 Therefore,
80
in consensus with the report,30 we have considered C 1s at 284.8 eV for binding energy (B.E.)
81
corrections of different elements in C3N4. Defects were identified with positron annihilation
82
spectroscopy (PAS). In the present study, coincidence Doppler broadening (CDB) experiments
83
with two identical HPGe detectors of 12 % efficiency (Type, PGC 1216sp of DSG, Germany)
84
having energy resolution of 1.15 at 514 keV of 85Sr was used in coincidence. A 10 µCi22 NaCl
85
source encapsulated in a 1.5 micron-thin nickel foil was used as a positron source. The details of
86
the experimental set-up were mentioned elsewhere.31 The total counts under the CDB 511 keV
87
spectra of about 107 had been recorded in a dual ADC-based multiparameter data acquisition
88
system (MPA-3 of FAST ComTec., Germany). The CDB spectra had been analyzed by
89
constructing the area normalized ratio-curve method.
90 91 6
ACS Paragon Plus Environment
Page 7 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
92
The Journal of Physical Chemistry
3. Results and discussion
93
Figure 1 shows the XRD pattern of g-C3N4 processed at different temperatures. For all the
94
samples we have observed two diffraction peaks corresponding to (002) (2θ = 27o) and (100)
95
crystallographic planes (2θ = 12.6o).3 The shifting of (002) peak to higher diffraction angle with
96
calcination temperature is shown in the inset of Figure 1. Calculated d-spacing results for the
97
(002) and (100) planes at various calcination temperatures are inserted in Table S1. A reduction
98
in the d-spacing with calcination temperature for (002) plane indicates tight packing of layers
99
along the π-stacking direction of aromatic g-CN units. A reduced stacking distance will increase
100
the repulsion of the lone pair on aromatic as well as on bridging N atoms, favouring buckling of
101
nanosheets at higher calcination temperatures.32,33 As for the (100) peak, the d-spacing slightly
102
increases with calcination temperature. An increase in d-spacing indicates a larger intraplanar
103
distance of s-heptazine unit resulting from steric repulsion of lone pair electrons present on
104
neighbouring nitrogen atoms in s-heptazine unit.32,34
105 106 107
Figure 1 XRD pattern of C3N4 synthesized at different calcination temperatures. Inset shows the expanded view of (002) peak revealing clear peak shift. 7
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 44
108
Figure 2 displays TEM images of C3N4 grown at the different calcination temperature. As seen in
109
the low-resolution TEM images of CN420, CN470, CN520, and CN570 in Figure 2a, 2c, 2e and
110
2g, the as-grown C3N4 nanosheets at different temperatures acquire corrugated morphology with
111
porous structures. The corrugation in the nanosheets is believed to result from the repulsion of
112
lone pair electrons on bridging nitrogen in the s-heptazine unit of the adjacent layers.35 The pore-
113
like features can be well visualized in the high-resolution images of the samples (Figure 2b, 2d,
114
2f, and 2h). High-resolution images show that the nanosheets contain tightly packed layers with
115
approximately ~10-18 layers in the condensed thick structures of the nanosheets. FTIR spectra
116
(see in Figure S1, supporting information) of the samples reveal different types of C-N bonding
117
or presence of uncondensed CN, -CNH in the system. The broad absorption band between 3700-
118
3000 cm-1 comes from –NH vibration, -OH vibration, etc.36,37 The fingerprint region (1705-800
119
cm-1) of g-C3N4 contains several absorption bands. These bands are associated with symmetric,
120
asymmetric, bending vibration of aromatic and bridging C-N (or C=N) bonds in the s-heptazine
121
units of C3N4.38,39 Thermogravimetric analysis (TGA) of C3N4 prepared at different calcination
122
temperatures are shown in Figure S2 (supporting information). For CN420, there is 7 % weight
123
loss till temperature reaches 200 oC, and from 200-450 oC the weight loss is 2 %. In case of
124
CN470, CN520 and CN570 the total weight loss is 6 %, 3.5 %, and 0.5 %, respectively, till
125
temperature reaches 470 oC. The initial weight loss up to 200 oC is due to the removal of
126
adsorbed water and the final weight loss is due to the decomposition of intermediates, such as
127
cyanuric acid, ammeline, and ammelide, formed during the condensation of C3N4.40 The total
128
weight loss for the samples is very low, which indicates that C3N4 is the stable species with
129
fewer impurities. The rapid weight loss above 470 oC is due to the removal of the nitrogenated
8
ACS Paragon Plus Environment
Page 9 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
130
impurities and gases.41 Above 650 oC there is more than 95 % weight loss which is due to the
131
decomposition of C3N4.40
132 133 134
Figure 2 Low- and high- resolution TEM images of: (a-b) CN420, (c-d) CN470, (e-f) CN520 and (g-h) CN570.
135
The chemical composition of as-prepared C3N4 nanosheets is studied with X-ray
136
photoelectron spectroscopy (XPS). The C 1s XPS spectrum for CN520 is shown in Figure 3a,
137
and those of other samples are shown in Figure S3. In CN520, C 1s peak at 288.1 eV can be
138
assigned to sp2 hybridized N-C=N in aromatic s-heptazine ring, and the shoulder peak at 284.7
139
eV is arising from the adventitious carbon.5,42,43 The weak C 1s peak at 286.2 eV is probably
140
occurring due to the presence of nitrogen-related defects in the graphitic carbon nitride system
141
and attributed to N-CH=N bonding structure in the system.43 The high-resolution N 1s spectrum
142
for CN520 is deconvoluted into three components with peaks centered at 398.4 eV, 400.1 eV,
143
and 404.1 eV, respectively (Figure 3b). N 1s spectra for rest of the samples are included in
144
Figure S3. The dominant peak at 398.4 eV can be ascribed to two coordinated N atom (N2C in C-
145
N=C in aromatic ring), and the shoulder peak at 400.1 eV is attributed to three coordinated N 9
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 44
146
atom (N3C, tertiary nitrogen N-(C3) groups).5,23 The additional minor peak at 404.1 eV can be
147
assigned to cyano group or π-excitation.37 We measured the peak-area ratio of N2C to N3C for
148
C3N4 calcined at different temperatures. It is seen that N2C/N3C ratio changes as 2.14 (CN420),
149
2.36 (CN470), 0.83 (CN520) and 0.92 (CN570). A lower value of N2C/N3C indicates the presence
150
of nitrogen-vacancy at the N2C site, and from the measured values it is evident that CN520
151
experiences higher nitrogen loses at the two coordinated sites (N2C).25, 42,43 This implies a higher
152
density of nitrogen-vacancy defects in CN520.
153
154
Figure 3 Core level (a) C 1s and (b) N 1s peak XPS spectrum of CN520
155
To support our prediction from XPS that CN520 contains higher nitrogen-related vacancy
156
centers, we have employed positron annihilation spectroscopy (PAS) technique. PAS is a
157
powerful tool to identify vacancy-type defects in a material.
10
ACS Paragon Plus Environment
Page 11 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
158 159 160 161
Figure 4 (a) Ratio of area normalized CDB spectra of calcined C3N4 with respect to area normalized CDB spectra of 420 oC calcined C3N4. (b) Doppler broadening shape parameter, Sparameter, for differently calcined C3N4 samples.
162
We have considered coincidence Doppler broadening (CDB) method to determine the
163
nature of defects in C3N4.44 Figure 4a represents the ratio of area normalized CDB spectra of
164
calcined (470, 520 and 570 oC) C3N4 samples concerning the area normalized CDB spectra of
165
C3N4 calcined at 420 oC. It is clear from the Figure 4a that due to calcination at a higher
166
temperature, i.e., 520 oC and 570 oC, the ratio curve shows a broad dip in the momentum value
167
p L ~ 10×10-3 m 0c . The dip around p L = 10×10-3 m 0c represents more open volume defects in the
168
sample since the core electron wave functions are localized and do not span inside the available
169
volumes.31 One can identify the core electrons with which positrons are less annihilating by
170
estimating the kinetic energy of the electrons corresponding to the p L ~ 10×10-3 m 0c . Positrons
171
are almost thermalized before annihilation and using Virial theorem approximation (in the atom
172
the expectation value of the kinetic energy of an electron, is equal to the binding energy of the
173
electron), one can calculate the E kin using p L = (2m 0 E kin ) 2 .45 The calculated kinetic energy
174
corresponds to p L ~ 10×10-3 m 0c ~ 26 eV. In C3N4 nanosheets the core electron near to this value
175
is the only 2s electron of the nitrogen atom (~37 eV). This shows that due to calcination at 520
1
11
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 44
176
0
177
nitrogen-vacancy is less in case of 420 0C and 470 0C calcined samples.
178
The Doppler broadening shape parameter, S-parameter has been calculated for all the calcined
179
C3N4 samples. The S-parameter of the Doppler broadening of the positron annihilation gamma-
180
ray line profile N(E) vs. E is defined as the ratio of the counts in the central area
181
(511 keV − E ≤ 0.85 keV)
182
parameter represents the fraction of positrons annihilating with the “low” momentum electrons to
183
the “higher” momentum electrons. An increase of S-parameter indicates the increase of defects
184
in the system.31,45 Figure 4b depicts an enlargement of S-parameter due to calcination at 520 0C
185
and 570 0C sample. It is also clear from Figure 4b that the maximum defects can be generated in
186
the sample calcined at 520 0C, which is in agreement with the ratio curve analysis.
C, a large density of nitrogen vacancies has been created in the C3N4 sample, but the density of
(
and the counts in the total area 511 keV − E ≤ 4.25 keV ) . Thus S-
187
Figure 5a shows the Kubelka-Munk absorption plots of g-C3N4 prepared at different
188
calcination temperatures. The corresponding reflectance plot of the samples is shown in Figure
189
S4a. The samples show two absorption bands centered at 277 nm and 378 nm. These bands are
190
attributable to π-π* transition of the aromatic sp2 C=N unit and n-π* transition involving
191
nonbonding electrons on N atom in aromatic sp2 (C=N) and bridging sp3 (C-N).46,47 The bandgap
192
of the samples is determined from the plot of [F(R)hv]1/2 vs. hν (Figure 5b,Table S1). The
193
bandgap in C3N4 is a measure of indirect optical transition from Г to M in the Brillouin zone.48 It
194
is seen from table S1 that the bandgap of the samples decreases with an increase in calcination
195
temperature up to 520 °C. Up to this temperature the bandgap variation follows the trend 2.83 eV
196
(CN420), 2.75 eV (CN470) and 2.73 eV (CN520). The bandgap again increases to 2.85 eV in
197
CN570. The decrease in the bandgap can be attributed to the presence of intermediate defect 12
ACS Paragon Plus Environment
Page 13 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
198
states, such as uncondensed NH/NH2, or structural defects such as nitrogen vacancies.24,26 The
199
enlargement in the bandgap in completely grown CN570 is attributable to quantum confinement
200
effect. The intermediate defect states constitute the Urbach energy (Eu) tail below the optical
201
bandgap of the samples.
202 203 204
Figure 5 (a) Kubelka-Munk absorption plots, and (b) Tauc plots for the band gap calculation for C3N4 samples calcined at different temperatures.
205
We have determined Urbach energy for each sample from the slope of the linear fitting
206
between lnF(R) vs. hν.49 The measured values of Eu for different samples are included in Table
207
S1. There is an inverse relationship between Eg and Eu (Figure S4b). The samples with higher
208
bandgap have lower Eu and vice-versa. A higher Urbach energy value indicates the presence of
209
intermediate defect states in the samples. These defect states are mostly nitrogen-related as
210
manifested by the results of PAS. The overall trend of variation of S-parameter and the variation
211
in the bandgap with calcination temperature is more or less correlated, although not quite
212
matched. This is expected since positron probes only defects. However, for determining the
213
bandgap, defect is one of the many parameters. There are other parameters which might
13
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 44
214
influence the bandgap modification in C3N4. These include interlayer electron-electron coupling,
215
conjugation of π electron system, interlayer periodicity, etc.10,50, 51
216 217
Figure 6a shows the steady-state PL spectra of as-grown C3N4 nanosheets under an optical excitation energy 3.35 eV, well above the samples bandgap.
218 219 220 221
Figure 6 (a) PL spectra of C3N4 nanosheets grown at different temperatures under an excitation energy of 3.35 eV. The inset shows a magnified view of the PL spectrum of CN420. (b) PL spectra of CN520 obtained under different excitation energies.
222
The spectrum has a maximum emission in the blue region and a low energy tail extending down
223
to 1.8 eV. The blue emission is due to exciton generated in the s-heptazine ring.52 The excitonic
224
emission is red-shifted by ~0.08 eV as the calcination temperature increases from 420-470 °C
225
(Figure S5, supporting information). No change in the position of emission energy is monitored
226
at 520 °C and 570 °C. The observed spectral red-shift might be corroborated by the structural
227
changes in the as-grown C3N4. The changes include degree of condensation of the layers during
228
growth of C3N4, extrinsic and intrinsic defect formation, such as –NH/-NH2 surface
229
decomposition, an aromatic ring and bridging N defect formation, etc.43,46,53 Growth temperature
230
also affects the line-width of an excitonic emission. There is an increment in full-width at half 14
ACS Paragon Plus Environment
Page 15 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
231
maximum (FWHM) by ~0.1 eV on increasing the calcination temperature from 420-470 0C, as
232
seen in Figure S5. Above 470 0C and up to 570 0C, there is a marginal increase in the PL line-
233
width. The structural changes might also be responsible for the broader distribution of emission
234
centers, resulting in the broadening of emission peak.14,54 DFT based theoretical study has also
235
reported that PL properties of C3N4 exhibit extensive modifications in the presence of defects.
236
This has resulted in a synergetic effect of interlayer periodicity and formation of structural
237
defects.50 Since interlayer distance diminishes with increasing calcination temperature (as
238
revealed from the XRD analysis), possible exciton-exciton coupling and scattering might also
239
contribute to the broadening of the PL peak.55 We have also measured the impact of excitation
240
energy variation on the excitonic emission of C3N4. Figure 6b shows the PL spectra of CN520
241
under excitation energies of 3.35 eV, 3.54 eV, 3.75 eV, 4.00 eV and 4.27 eV. There is a
242
monotonic decrease in PL intensity with increasing excitation energy, which may be due to a
243
decrease in intensity of excitation light (a Xenon lamp) at higher energy (from near visible to
244
UV).56 Note that the position of the blue PL band is almost unchanged irrespective of the
245
incident excitation energy. Non-dependence of emission energy on excitation energy suggests
246
that excitonic emission occurs from the same excited π* state irrespective of probing energy.57
247
The emission spectrum of C3N4 (Figure 6) has a low energy tail emission
248
alongside the strong excitonic emission. To extract different emissive components from the
249
broad PL spectrum, we have deconvoluted the PL spectrum of CN520 with three Gaussian
250
peaks. The peaks are centered at 2.78 eV, 2.58 eV, and 2.38 eV, respectively (Figure 7a). In
251
conformity with the bandgap values determined for the absorption spectra and in agreement with
252
literature report, we infer that the intense emission peak at 2.78 eV is the excitonic peak.52 Other
253
emission peaks at 2.58 eV and 2.38 eV are lower than the measured bandgap of the samples. 15
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 44
254
Therefore, these emissions cannot be related to the free excitonic emission. We speculate that
255
these excitonic emissions are associated with structural defects in C3N4 nanosheets.
256 257 258 259 260 261
Figure 7 (a) Decovoluted (Gaussian) PL spectrum of CN520 under excitation of 3.35 eV. (b) TRPL (logarithmic plot) spectra of CN520 excited at 3.30 eV and monitored at 2.78 eV, 2.58 eV and 2.38 eV emission energies. (c) Plot showing a relation of S-parameter (left Y-axis) and average bound excitonic lifetime (τav at 2.38 eV) (right Y-axis) as a function of calcination temperature, which demonstrates a direct correlation between the S-parameter and τav.
262
263
For a detailed understanding of the associated PL decay, we have recorded the TRPL spectra for
264
different samples at the deconvoluted emission energies. TRPL spectra for CN520 at emission
265
energies 2.78 eV, 2.58 eV and 2.38 eV are obtained under excitation energy of 3.3 eV, and the
266
results are shown in Figure 7b. The decay profile is recorded for 0-200 ns time scale and the
267
amplitudes and lifetime components are listed in Table 1. It is found that the excitonic emission
268
at 2.78 eV has an average lifetime of 17.4 ns, whereas for the 2.58 eV and 2.38 eV emission
269
peaks the lifetimes are extended to 25.2 ns and 27.4 ns, respectively. Therefore, this extended 16
ACS Paragon Plus Environment
Page 17 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
270
carrier lifetime may be due to the involvement of bound excitons in the transition. The TRPL
271
spectra for the other samples are shown in Figure S6. From the PAS analysis, we have found that
272
S-parameter measures the nitrogen-vacancy defects in the system. Higher the S-parameter,
273
higher is the concentration of defects in the system. Figure 7c shows a comparison of the average
274
lifetime (τav) obtained for different samples for the bound excitonic emission. It is seen that
275
CN520 which has the highest defect content (the highest S-parameter) also possesses the longest
276
average PL lifetime for bound excitonic emission. Thus, a direct correlation between the vacancy
277
type defects and the excitonic lifetime established through this data allows us to unambiguously
278
identify the corresponding emissions as bound excitonic emissions in C3N4.
279 280
Table 1. TRPL Data of CN520 Excited at 3.3 eV and Monitored at 2.78 eV, 2.58 eV and 2.38 eV
Emission Energy. Sample
Emission (eV)
Lifetime (ns)
τ 1 (a1 )
CN520
τ 2 (a 2 )
τ av (ns) τ 3 (a 3 )
2.78 eV
1.1 (0.22)
5.0 (0.53)
23.6 (0.25)
17.4 ns
2.58 eV
1.9 (0.29)
7.0 (0.46)
33.6 (0.25)
25.2 ns
2.38 eV
1.8 (0.25)
6.9 (0.48)
36.0 (0.22)
27.4 ns
281
282
From the three components ( τ1 , τ 2 , τ3 ) of the excitonic lifetime in Table 1 for CN520, it
283
is clear that τ1 component does not change much for the three emission peaks. It is τ 2 and mostly
284
the τ3 component, which shows a large difference from that of free excitonic emission. It is seen
285
that the excitonic emission has an average lifetime of 17.4 ns, whereas for the 2.58 eV and 2.38
286
eV emission peaks the lifetimes are extended to 25.2 ns and 27.4 ns, respectively.
287
Now we elaborate on the origin of different lifetime components ( τ1 , τ 2 , τ3 ) for free 17
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 44
288
excitonic emission at 2.78 eV. Figure 8 gives a schematic view of different pathways of exciton
289
migration.
290 291 292 293 294
Figure 8 Schematic shows exciton migration in (a) π-stacking direction (interplanar), and (b) intraplanar migration (1) and intrachain (2) migration. Free excitons (F-exciton), when attached to nitrogen related defects (N-defects) create bound excitons (DB-exciton). Exciton migration is prohibited if C-H or N-H moiety terminates the heptazine link.
295
After photoexcitation, excitons that are confined to the aromatic ring undergo fast recombination
296
and gives rise to the fast decay component ( τ1 ). Excitons generated in the s-heptazine might also
297
migrate in the extended s-heptazine rings of C3N4 following different pathways. Excitons might
298
undergo facile interplanar migration along a π-stacking direction (Figure 8a) and transport from
299
one layer to another giving rise to the long exciton lifetimes ( τ 2 and τ 3 ).17 The other possible 18
ACS Paragon Plus Environment
Page 19 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
300
pathways of exciton migration that could result in the long excitonic lifetime could be as
301
depicted in Figure 8b. In interplanar migration, exciton moves between two connected s-
302
heptazine units with different symmetry planes. In intrachain migration exciton moves along the
303
s-heptazine chains through bridging N atom giving long excitonic lifetime, however, considering
304
its migration is not interrupted by the presence of N-H bonds or C-H bonds. Thus, we have
305
considered interplanar, intraplanar and intrachain migration as the possible pathways for
306
migration that could result in the long components of the free excitonic lifetime ( τ 2 and τ 3 ).
307
However, reports show that exciton migration follows an exponential decrease with stacking
308
distance.52 Table S1 shows that interplanar (or pi-stacking) distance of adjacent layers in C3N4
309
are separated by ~3.2 A . However, for intraplanar migration or migration along the heptazine
310
chains the exciton sitting on the nearest s-heptazine are separated by ~6.9 A (Table S1).
311
Therefore, exciton coupling and migration are supposed to be weak in this direction. Therefore,
312
we can predict that intraplanar and intrachain exciton migration can be responsible for the
313
τ 2 component. However, it is the interplanar or π-stacking direction which is sought to be the
314
most suitable pathway for long transport of exciton in C3N4 giving the longest τ3 component. If
315
we compare the different components ( τ1 , τ 2 , τ3 ) of lifetime for free excitonic (2.78 eV) and
316
bound excitonic emission (2.58 eV and 2.38 eV), we can easily interpret that it is the
317
τ3 component which is quite long in case of bound exciton emission compared to free emission.
318
Excitons bound to defect are relaxed for a longer period in the defect states before it finds a
319
recombination center. In this way, the defect bound excitons show high fluorescence stability
320
over the longer timescale.
0
0
19
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 44
321
To understand the response of the defect bound excitons to laser power excitation, we
322
have taken PL spectra of CN520 under diode-pumped solid-state laser. Figure 9a shows the
323
normalized PL spectra of CN520 under excitation of 3.06 eV (405 nm).
324 325 326 327 328
Figure 9 Normalized PL spectra of CN520 for different excitation power (intensity). The samples are excited with a solid-state laser of energy 3.06 eV. (b) Changes in emission energy (left Y-axis), full width at half maximum (FWHM) (right Y-axis) with laser power. The inset shows the PL emission intensity as a function of excitation laser power.
329
The emission spectra are recorded under laser power of 5 mW, 10 mW, 15 mW, 20 mW
330
and 25 mW. The un-normalized PL spectrum is shown in Figure S7. The emission intensity,
331
position and line-width display clear dependence on incident laser power, as shown in Figure 9b.
332
First, we will emphasize the changes in emission intensity with probing laser power. As shown
333
in the inset of Figure 9b, the emission intensity increases slightly on increasing the laser power
334
from 5 mW to 10 mW. There is a significant enhancement in PL intensity at a laser power of 15
335
mW. However, saturation of PL intensity occurs at higher excitation power (>15 mW). From the
336
previous study, it is understood that the emission intensity (IPL) of a sample exhibits a linear
337
variation with incident laser power following the relation, I PL ∞Lα , where L is excitation power
338
and α is power factor.58 In case of free excitonic emission, the emission intensity scales linearly
339
with laser power, whereas for bound excitonic emission the intensity varies linearly at low 20
ACS Paragon Plus Environment
Page 21 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
340
excitation power and deviates from linearity and saturates at high laser power.59 Therefore, we
341
might speculate that the non-linear intensity variation and saturation is resulted by these defect
342
bound excitons of C3N4. The position of emission energy is unchanged for the laser power of 5
343
mW and 10 mW (Figure 9b). There is a red-shift by ~0.5 eV when the laser power is set at 15
344
mW. On increasing the laser power from 15 mW to 20 mW, there is a shift of ~0.1 eV, and in
345
between 15 mW to 25 mW the shifting is ~0.2 eV. A similar trend is observed for FWHM
346
variation with laser power. Several factors have been associated with the red-shift of PL band
347
including laser heating effect, defect level population with photoexcited carriers, bandgap
348
renormalization, energy transfer, etc.58,60 Laser heating effect is prominent in nanoparticles
349
where heat conduction among nanoparticles is poor, and the heating effect is localized on a
350
single nanoparticle.61 However, in C3N4, having a conjugated 2D network, the heat energy might
351
go easy transfer throughout the system and therefore, localized heating effect as such may not be
352
prominent. Moreover, laser-induced local heating is known to cause spectral red-shift and
353
quenching in emission intensity by enhancing electron-phonon interaction and increasing non-
354
radiative recombination centers.62,63 No such spectral features have been observed in the PL
355
spectra. Therefore, laser heating is not the principal reason for the changes observed in emission
356
profile. The observed changes in PL feature can be associated with defect level population with
357
carriers.64 Since the system is excited with 3.06 eV laser, which is above the bandgap of the
358
samples, bound excitons are generated in the system. The number density of such excitons shows
359
dependence on incident laser power. At incident laser power of 5 mW and 10 mW, less number
360
of excitons could occupy the defect states near the conduction band edge. As laser power is
361
increased to 15 mW, large numbers of excitons could fill up the defect spaces distributed near
362
the band edge. Exciton distribution is expected to be non-uniform, and the number of radiative 21
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 44
363
recombination centers participating in luminescence appeared to be very high giving the spectral
364
broadness or increase in FWHM (Figure 9b). However, when the laser power is increased to 15
365
mW and 20 mW, the upper-level population saturates, and the excitons start to fill-up underlying
366
defect levels. Many of the excitons undergo exciton-exciton scattering and decay non-
367
radiatively. Only those excitons which can occupy the defect levels contribute to luminescence.
368
In the lower lying defect levels the exciton distribution appears to be uniform, and since the
369
number of radiative emission centers in these states seems to be less, the emission spectra attain
370
a narrow and symmetric feature.
371
C3N4 displays defect related sub-bandgap emission when the samples are photoexcited
372
with energies below the optical bandgap. In C3N4 the types of defects are nitrogen related, and
373
these could be cyano (C≡N), NH2, nitrogen vacancy, etc. PAS has characterized presence of
374
these nitrogen related defects. Figure 10a shows the normalized PL spectra of the samples
375
excited at 2.69 eV, 2.61 eV, 2.53 eV, 2.45 eV and 2.38 eV. Unlike above bandgap (BG)
376
photoexcitation where there is a band-to-band optical transition, photoexcitation below BG
377
triggers band to defect (D) transition, viz. π→D or LP→D. A broad asymmetric PL band
378
covering 2.1-2.55 eV spectral range is seen under excitation of 2.69 eV. As the photoexcitation
379
energy is decreased, the PL band becomes narrower and is gradually shifted towards lower
380
energy side. There is a red-shift of PL band by 0.3 eV when the excitation energy is changed
381
from 2.69 eV to 2.38 eV. The red-shift indicates that the trapped charge carriers jump from
382
different defect states to recombine with the holes. Moreover, the asymmetric and broad PL band
383
attains
384
Broadening/narrowing of PL band and its asymmetric/symmetric characteristics depend on the
385
filling up of empty defect levels with photoexcited charge carriers. At higher excitation energy
narrow
and
symmetric
features
as
the
excitation
energy
is
decreased.
22
ACS Paragon Plus Environment
Page 23 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
386
the defect levels near the conduction band-edge are filled up with charge carriers (shown in
387
schematic in Figure 10b).
388 389 390 391 392 393
Figure 10 (a) Photoluminescence spectra of CN520 at different excitation energy. The excitations are below the optical bandgap of the grown nanosheets. (b) Schematic showing below bandgap excitation and emissions due to carrier trapped in different defect states. Different band states in the valence band and conduction band, nitrogen lone pair (LP) state and nitrogen-related defect states are shown. (c) TRPL spectrum (logarithmic plot) of CN520 excited at 2.45 eV.
394
395
When the initial defect levels are filled up, the remaining charge carriers hop to its underlying
396
defect levels. Inhomogeneous distribution of charge carriers in these states might have resulted in
397
a broad PL band at an excitation of 2.69 eV. The narrowing and symmetric feature of PL band at
398
lower excitation energy indicates homogenous carrier distribution in the underlying defect levels.
399
TRPL data is recorded for CN520 with excitation at 2.45 eV and monitored at the emission
400
energy of 2.24 eV (Figure 10c). The three components of carrier lifetime are very short in case of
401
defect emissions (Table S2). Unlike the case of free and bound excitonic emission having an
402
average lifetime of 17.4 ns and 27.4 ns, the average lifetime of defect emissions is very short of
403
the order of 0.14 ns. From the analyzed results of PL under above and below band gap excitation,
404
we might infer that nitrogen related defects could extend the lifetime of free exciton when we
405
choose the excitation energy above the bandgap. Below bandgap excitation releases free carriers, 23
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 24 of 44
406
which are excited directly to the trapped centers underlying the bandgap of C3N4. The defect-
407
related PL band has low stability and decays with a very short lifetime.
4. Conclusions
408
409
In
summary,
we
employed
positron
annihilation,
steady-state
and
time-resolved
410
photoluminescence spectroscopy to probe the evolution of nitrogen-related defects in C3N4 with
411
calcination temperature. After photoexcitation, the excitonic emission in the intraplanar,
412
interplanar or intrachain direction gives rise to the shorter and longer decay components.
413
Excitons bound to nitrogen-related defect states decay with a lifetime of 27.4 ns, which is longer
414
than the free excitonic emission decay of 17.4 ns. Defect emission shows dependence on
415
excitation energy, and the lifetime of defect emission is only 0.14 ns. We have also demonstrated
416
laser power dependent excitonic emission in C3N4 with above bandgap excitation. The spectral
417
red-shift is mostly resulted by the band filling effect in which exciton readily fills up the
418
nitrogen-related defect states. This study provides a direct correlation between the defects
419
monitored by the PAS and PL and establishes the significant role of nitrogen-vacancy defects in
420
controlling the bound excitonic lifetime in C4N4 nanosheets. These results are significant for
421
tuning the optical properties of C3N4 nanosheets for ensuing applications in optoelectronics,
422
energy, and environment.
423
424
ASSOCIATED CONTENT
425
Figures of XPS, FTIR, TGA, Time-resolved PL, laser power dependent PL are included in the
426
Supporting Information. 24
ACS Paragon Plus Environment
Page 25 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
427
ACKNOWLEDGMENTS
428
The authors would like to thank central instruments facility (CIF) IIT Guwahati for providing
429
various characterisation facilities. BC would like to thank Department of Science and
430
Technology (DST), Govt. of India for providing DST Inspire faculty award (IFA15/MS-62) to
431
pursue this work. We thank Prof. M. Fujii, Kobe University, for the XPS measurement.
432 433
References
434 435
(1) Wang, X.; Maeda, K.; Thomas, A.; Takanabe, K.; Xin, W.; Carlsson, J.M.; Domen, K.;
436
Antonietti, M. A Metal Free Polymeric Photocatalyst for Hydrogen Production From Water
437
Under Visible Light. Nature Mater. 2009, 8, 76-80.
438
(2) Wang,X.; Maeda,K.; Chen,X.; Takanabe,K.; Domen,K.; Hou,Y.; Fu,X.; Antonietti, M.
439
Polymer Semiconductors for Artificial Photosynthesis: Hydrogen Evolution by Mesoporous
440
Graphitic Carbon Nitride with Visible Light, J. Am. Chem. Soc. 2009, 131, 1680-1681.
441
(3) Choudhury, B.; Giri, P.K. Isotype Heterostucture of Bulk and Nanosheets of Graphitic
442
Carbon Nitride for Efficient Visible Light Photodegradation of Methylene Blue. RSC Adv. 2016,
443
6, 24976-24984.
444
(4) Zheng, Q.; Durkin, D.P.; Elenewski, J.E.; Sun, Y.; Banek, N.A.; Hua, L.; Chen, H.; Wagner,
445
M.J.; Zhang, W.; Shuai, D. Visible-Light-Responsive Graphitic Carbon Nitride: Rational Design
446
and Photocatalytic Applications for Water Treatment. Environ. Sci. Technol. 2016, 50, 12938–
447
12948.
25
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 26 of 44
448
(5) Xu J.; Wang,Y.; Zhu, Y. Nanoporous Graphitic Carbon Nitride with Enhanced Photocatalytic
449
Performance. Langmuir 2013, 29, 10566−10572.
450
(6) Yan, S.C.; Li, Z.S.; Zou, Z.G. Photodegradation Performance of g-C3N4 Fabricated by
451
Directly Heating Melamine. Langmuir 2009, 25, 10397–10401.
452
(7) Fan, X.; Xing, Z.; Shu, Z.; Zhang, L.; Wang, L.; Shi, J. Improved Photocatalytic Activity of g-
453
C3N4 derived from Cynamide-Urea Solution. RSC Adv. 2015, 5, 8323-8328.
454
(8) Rajender, G.; Choudhury, B.; Giri, P.K. In-situ Decoration of Plasmonic Au Nanoparticles on
455
Graphene Quantum Dots-Graphitic Carbon Nitride Hybrid and Evaluation of its Visible Light
456
Photocatalytic Performance. Nanotechnology 2017, 28, 395703.
457
(9) Ho, W.; Zhang, Z.; Xu, M.; Zhang, X.; Wang, X.; Huang, Y. Enhanced Visible-Light Driven
458
Photocatalytic Removal of NO: Effect on Layer Distortion on g-C3N4 by H2 heating. Appl.
459
Catal., B 2015, 179, 106-112.
460
(10) Wu, F.; Liu, Y.; Yu, G.; Shen, D.; Wang, Y.; Kan, E. Visible-Light-Absorption in Graphitic
461
C3N4 Bilayer: Enhanced by Interlayer Coupling. J. Phys. Chem. Lett. 2012, 3, 3330−3334.
462
(11) Chen, Y.; Wang, B.; Lin, S.; Zhang, Y.; Wang, X. Activation of n→π* Transitions in Two
463
Dimensional Conjugated Polymers for Visible Light Photocatalysis, J. Phys. Chem. C 2014, 118,
464
29981–29989.
465
(12) Zhang, Y.; Pan, Q.; Chai, G.; Liang, M.;Dong, G.; Zhang, Q.; Qiu, J. Synthesis and
466
Luminescence Mechanism of Multicolour-Emitting g-C3N4 Nanopowders by Low Temperature
467
Thermal Condensation of Melamine. Sci. Rep. 2013, 3, 1943.
468
(13) Xu, J.; Shalom, M.; Piersimoni, F.; Antonietti, M.; Neher, D.; Brenner, T. Color-Tunable
469
Photoluminescence and NIR Electroluminescence in Carbon Nitride Thin Films and Light-
470
Emitting Diodes. Adv. Opt. Mater. 2015, 3, 913-917. 26
ACS Paragon Plus Environment
Page 27 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
471
(14) Gan, Z.; Shan, Y.; Chen, J.; Gui, Q.; Zhang, Q.; Nie, S. The Origins of the Broadband
472
Photoluminescence from Carbon Nitrides and Applications to White Light Emitting. Nano Res.
473
2016, 9, 1801-1812.
474
(15) Lee, E. Z.; Lee, S. U.; Heo, N.-S.; Stucky, G. D.; Jun, Y.-S.; Hong, W. H. A Fluorescent
475
Sensor for Selective Detection of Cyanide Using Mesoporous Graphitic Carbon (IV) Nitride.
476
Chem. Commun. 2012, 48, 3942 − 3944.
477
(16) Xiang, M.H.; Liu, J.W.; Li, N.; Tang, H.; Yu, R.Q.; Jiang, J.H. A Fluorescent Graphitic
478
Carbon Nitride Nanosheet Biosensor For Highly Sensitive, Label-Free Detection of Alkaline
479
Phosphatise. Nanoscale. 2016, 8, 4727-4732.
480
(17) Merschjann, C; Tschierlei, S; Tyborski, T; Kailasam, K; Orthmann, S; Hollmann, D;
481
Niedrig, T S; Thomas, A; Lochbrunner S. Complementing Graphenes: 1D Interplanar charge
482
Transport in Polymeric Graphitic Carbon Nitrides. Adv. Mater. 2015, 27, 7993.
483
(18) Burlakov, V.M.; Kawata, K.; Assender, H.E.; Briggs, G.A.D.; Ruseckas, A.; Samuel,
484
I.D.W.Discrete Hopping Model of Exciton Transport in Disordered Media. Phys. Rev. B 2005,
485
72, 075206.
27
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 28 of 44
486
(19) Chen, X.; Liu, Q.; Wu, Q.; Du, P.; Zhu, J.; Dai, S.; Yang, S. Incorporating Graphitic Carbon
487
Nitride (g-C3N4) Quantum Dots into Bulk-Heterojunction Polymer Solar Cells Leads to
488
Efficiency Enhancement. Adv. Funct. Mater. 2016, 26, 1719-1728.
489
(20) Cui, Q.; Xu, J.; Wang, X.; Li, L.; Antonietti, M.; Shalom, M. Phenyl-Modified Carbon
490
Nitride Quantum Dots with Distinct Photoluminescence Behavior. Angew. Chem., Int. Ed. 2016,
491
55, 3672-3676.
492
(21) Lau, V.W.-h; Yu, V.W.-z; Ehrat, F.; Botari, T.; Moudrakovski, I.; Simon, T.; Duppel, V.;
493
Medina, E.; Stolarczyk, J.; Feldmann, J., et al. Urea-Modified Carbon Nitrides: Enhancing
494
Photocatalytic Hydrogen Evolution by Rational Defect Engineering. Adv. Energy Mater. 2017, 7,
495
1602251.
496
(22) Wu, W.; Zhang, J.; Fan, W.; Li, Z.; Wang, L.; Li, X.; Wang, Y.; Wang, R.; Zheng, J.; Wu,
497
M., et al. Remedying Defects in Carbon Nitride To Improve Both Photooxidation and H2
498
Generation Efficiencies. ACS Catalysis 2016, 6, 3365-3371.
499
(23) Dong, G.; Ho, W.; Wang, C. Selective Photocatalytic N2 Fixation Dependent on g-C3N4
500
Induced by Nitrogen Vacancies. J. Mater. Chem. A 2015, 3, 23435-23441.
501
(24) Tay, Q.; Kanhere, P.; Ng, C.F.; Chen, S.; Chakraborty, S.; Cheng, A.; Huan, H.; Sum, T.C.;
502
Ahuja, R.; Chen, Z. Defect Engineered g-C3N4 for Efficient Visible Light Photocatalytic
503
Hydrogen Production. Chem. Mater.2015, 27, 4930-4933.
504
(25) Li, S.; Dong, G.; Hailili, R.; Yang, L.; Li, Y.; Wang, F.; Zeng, Y.; Wang, C. Effective
505
Photocatalytic H2O2 Production Under Visible Light Irradiation at g-C3N4 Modulated by Carbon
506
Vacancies. Appl. Catal., B 2016, 190, 26-35.
28
ACS Paragon Plus Environment
Page 29 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
507
(26) Wu, P.; Wang, J.; Zhao, J.; Guo, L.; Osterloh, F.E. Structural Defects in g-C3N4 Limit
508
Visible Light Driven Hydrogen Evolution and Photovoltage. J. Mater. Chem. A 2014, 2, 20338-
509
20344.
510
(27) Hautojärvi, P.; Corbel, C. Positron Spectroscopy of Solids; IOS Press: Amsterdam, 1995.
511
(28) Dutta, S.; Chattopadhyay, S.; Sarkar, A.; Chakrabarti, M.; Sanyal, D.; Jana, D. Role of
512
Defects in Tailoring Structural, Electrical and Optical Properties of ZnO. Prog. Mater.Sci. 2009,
513
54, 89-136.
514
(29) Greczynski, G.; Hultman, L. C1s Peak of Adventitious Carbon Aligns to the Vacuum
515
Level: Dire Consequences for Material’s Bonding Assignment by Photoelectron Spectroscopy,
516
ChemPhysChem 2017, 18, 1507-1512.
517
(30) https://xpssimplified.com/elements/carbon.php
518
(
519
Polycrystalline ZnO During Annealing Below 300 0C as Studied by In-situ Positron Annihilation
520
Spectroscopy. J. Mater. Sci. 2017, 52, 7615-7623.
521
(32) Tyborski,T.; Merschjann, C.; Orthmann,S.;Yang,F.; Steiner,; M-Ch Lux, Niedrig, Th
522
Schedel, Crystal Structure of Polymeric Carbon Nitride and the Determination of its Process-
523
Temperature-Induced Modifications. J. Phys.: Condens. Matter 2013, 25, 395402.
524
(33) Guo, Q.; Zhang, Y.; Zhang, H.S.; Liu, Y.; Zhao, Y.J.; Qiu, J.; Dong, G. 3D Foam Strutted
525
Graphene Carbon Nitride With Highly Stable Optoelectronic Properties, Adv. Funct. Mater.
526
2017, 27, 1703711.
31) Luitel, H.; Sanyal,D.; Gogurla, N.; Sarkar, A. Defect Generation and Recovery in
29
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
527
(34) Dai, H.; Gao, X.; Liu, E.; Yang, Y.; Hou, W.; Kang, L.; Fan, J.; Hu, X. Synthesis and
528
Characterisation of Graphitic Carbon Nitride Sub-Microscpheres Using Microwave Method
529
Under Mild Condition. Diamond Relat. Mater. 2013, 38, 109-117.
530
(35) Gracia, J.; Kroll, P. Corrugated Layered Heptazine-Based Carbon Nitride: The Lowest
531
Energy Modifications Of C3N4 Ground State. J. Mater. Chem. 2013, 19, 3013–3019.
532
(36) Lan, H.; Li, L.; An, X.; Liu, F.; Chen, C.; Liu, H.; Qu, J. Microstructure of Carbon Nitride
533
Affecting Synergetic Photocatalytic Activity: Hydrogen Bonds vs. Structural Defects, Appl.
534
Catal., B 2017, 204, 49-57.
535
(37) Qiu, P.; Chen, H.; Xu, C.; Zhou, N.; Jiang, F.; Wang, X.; Fu, Y. Fabrication of an Exfoliated
536
Graphitic Carbon Nitride as a Highly Active Visible Light Photocatalyst. J. Mater. Chem. A 2015,3,
537
24237-24244.
538
(38) Yu, Y.; Zhou, Q.; Wang, J. The Ultra-Rapid Synthesis of 2D Graphitic Carbon Nitride
539
Nanosheets via Direct Microwave Heating for Field Emission. Chem. Commun. 2016, 52, 3396-
540
3399.
Page 30 of 44
541
(39) Panasiuk, Y.V.; Raevskaya, A.E.; Stroyuk, O.L.; Lytvyn, P.M.; Kuchmiy, S.Y. Preparation 542
and Optical Properties of Highly Luminescent Colloidal Single-Layer Carbon Nitride. RSC Adv. 543
2015, 5, 46843-46849. 544
(40) Xu, J.; Li,Y.; Peng,S.; Lu, G.; Li, S. Eosin Y-sensitized Graphitic Carbon Nitride Fabricated
545
By Heating Urea For Visible Light Photocatalytic Hydrogen Evolution: The Effiect Of The
546
Pyrolysis Temperature of Urea. Phys. Chem. Chem. Phys. 2013, 15, 7657-7665.
30
ACS Paragon Plus Environment
Page 31 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
547
(41) Schmidt, C.L.; Jansen, M. New Directions in Carbonitride Research: Synthesis Of Resin-
548
Like Dense-Packed C3N4 Using a Hydrogen-Free Precursor. J. Mater. Chem. 2010, 20, 4183–
549
4192.
550
(42) Niu, P.; Liu, G.; Cheng, H.M. Nitrogen Vacancy Promoted Photocatalytic Activity of
551
Graphitic Carbon Nitride, J. Phys. Chem. C 2012, 116, 11013-11018.
552
(43) Niu, P.; Yin, L.C.; Yang, Y.Q.; Liu, G.; Cheng, H.M. Increasing the Visible Light
553
Absorption of Graphitic Carbon Nitride (melon) Photocatalysts by Homogenous Self-
554
Modifications with Nitrogen Vacancies. Adv. Mater. 2014, 26, 8046-8052.
555
(44) Guin, S.N.; Banerjee,S.; Sanyal,D.; Pati, S.K.; Biswas, K. Origin of the Order-Disorder
556
Transition and the Associated Anomalous Change of Thermopower in AgBiS2 Nanocrystals: A
557
Combined Experimental and Theoretical Study. Inorg. Chem. 2016, 55, 6323-6331.
558
(45) Myler, U.; Simpson, P.J. Survey of Elemental Specificity in Positron Annihilation Peak
559
Shapes. Phys. Rev. B 1997, 56, 14303.
560
(46) Bian, J.; Huang, C.; Zhang, R.Q. Graphitic Carbon Nitride Film: An Emerging Star for
561
Catalytic and Optoelectronic Applications. ChemSusChem. 2016, 9, 2723-2735.
562
(47) Butchosa, C.; Guiglion, P.; Zwijnenburg, M.A.Carbon Nitride Photocatalysts for Water
563
Splitting: A Computational Persepective. J. Phys. Chem. C 2014, 118, 24833–24842.
564
(48) Xu, Y.; Gao, S.P. Band Gap of C3N4 in the GW Approximation. Int. J. Hydrogen Energy
565
2012, 37, 11072-11080.
566
(49) Choudhury, B.; Choudhury, A. Oxygen Defect Dependent Variation of Band gap, Urbach
567
Energy and Luminescence Property of Anatase, Anatase-Rutile Mixed Phase and of Rutile
568
Phases of TiO2 Nanoparticles, Phys. E 2014, 56, 364-371. 31
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 32 of 44
569
(50) Guo, Q.; Zhang, Y.; Qiu, J.; Dong, G. Engineering the Electronic Structure and Optical
570
Properties of g-C3N4 By Non Metal Ion Doping, J. Mater. Chem. C 2016, 4, 6839-6847.
571
(51) Dong, G.; Zhang, Y.; Pan, Q.; Qiu, J. A Fantastic Graphitic Carbon Nitride Material:
572
Electronic Structure, Photocatalytic and Photoelectronic Properties, J. Photochem. Photobiol., C
573
2014, 20, 33-50.
574
(52) Merschjann, C.; Tyborski, T.; Orthmann, S.; Yang, F.; Schwarzburg, K.; Lublow, M.; Lux-
575
Steiner, M.C.; Niedrig, S.T. Photophysics of Polymeric Carbon Nitride: An Optical
576
Quasimonomer. Phys. Rev. B 2013, 87, 205204.
577
(53) Yuan, Y.; Zhang, L.; Xing, J.; Utama, M.; Lu, X.; Du, K.; Li, Y.; Hu, X.; Wang, S.; Genc.
578
A., et al. High Yield Synthesis And Optical Properties of g-C3N4. Nanoscale 2015, 7, 12343-
579
12350.
580
(54) Zhang, H.; Yu, A. Photophysics and Photocatalysis of Carbon Nitrides Synthesized at
581
Different Temperatures. J. Phys. Chem. C 2014, 118, 11628-11635.
582
(55) Kose, M.E. Evaluation of Excitonic Coupling And Charge Transport Integrals in P3HT
583
Nanocrystals, J. Phys. Chem. C 2011, 115, 13076–13082.
584
(56) https://www.hamamatsu.com/resources/pdf/etd/Xe-HgXe_TLS1016E.pdf
585
(57) Bian, J.; Li. J.;Kalytchuk, S.; Wang, Y.; Li, Q.; Lau, T.C.; Niehaus, T.A.; Rogach, A.L.;
586
Zhang, R.Q. Efficient Emission Facilitated by Multiple Energy Level Transitions in Uniform
587
Graphitic Carbon Nitride Films, ChemPhysChem 2015,16, 954-959.
588
32
ACS Paragon Plus Environment
Page 33 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
589
(58) Yan, H.; Yang, Y.; Fu, Z.; Yang, B.; Zuo, J.; Fu, S. Excitation-Power Dependence of the
590
Near-Band-Edge Photoluminescence of ZnO Inverse Opals and Nanocrystal films, J. Lumin.
591
2008, 128, 245-249.
592
(59) Tongay, S.; Suh, J.; Ataca, C.; Fan, W.; Luce, A.; Kang, J.S.; Liu, J.; Ko, C.;
593
Raghunathanan, R.; Zhou, J., et al. Defects Activated Photoluminescence in Two Dimensional
594
Semiconductors: Interplay Between Bound, Charged and Free Excitons, Sci. Rep. 2013, 3, 2657.
595
(60) Wang, H.; Ji, Z.; Qu, S.; Wang, G.; Jiang, Y.; Liu, B.; Xu, X.; Mino, H. Influence of
596
Excitation Power and Temperature on Photoluminescence in InGaN/GaN Multiple Quantum
597
Wells, Opt. Express 2012, 20, 3932-3940.
598
(61) Verma, P.;Irmer, G.; Monecke, J. Laser Power Dependence of the Photoluminescence From
599
CdSxSe1-x Nanoparticles in Glass, J. Phys. : Condens. Matter 2000, 12, 1097-1110.
600
(62) Guo, J.; Xu, J.; Zhuang, X.; Wang, Y.; Zhou, H.; Shan, Z.; Ren, P.; Guo, P.; Zhang, Q.;
601
Wan, Q., et al. Laser Photoluminescence Red Shift of ZnTe Nanostructure: The Effect of Twin
602
Structure, Chem. Phys. Lett. 2013, 576, 26-30.
603
(63) Ikhmayies, S.J.; Bitar, R.N.A.; Dependence of Photoluminescence of CdS:In Thin Films on
604
Excitation Power of the Laser, J. Lumin. 2014, 149, 240-244.
605
(64) Dang, G.T.; Kanbe, H.; Kawaharamura, T.; Taniwaki, M. Pulsed Laser Excitation Power
606
Dependence of Photoluminescence Peak Energies in Bulk ZnO. J. Appl. Phys. 2011, 110,
607
083508.
608 609 610 611 33
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
612
Page 34 of 44
TOC GRAPHIC
613
614
34
ACS Paragon Plus Environment
Page 35 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
Figure 1 XRD pattern of C3N4 synthesized at different calcination temperatures. Inset shows the expanded view of (002) peak revealing clear peak shift. 72x65mm (600 x 600 DPI)
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 2 Low- and high- resolution TEM images of: (a-b) CN420, (c-d) CN470, (e-f) CN520 and (g-h) CN570. 71x34mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 36 of 44
Page 37 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
Figure 3 Core level (a) C 1s and (b) N 1s peak XPS spectrum of CN520 54x20mm (300 x 300 DPI)
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 4 (a) Ratio of area normalized CDB spectra of calcined C3N4 with respect to area normalized CDB spectra of 420 oC calcined C3N4. (b) Doppler broadening shape parameter, S-parameter, for differently calcined C3N4 samples. 53x20mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 38 of 44
Page 39 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
Figure 5 (a) Kubelka-Munk absorption plots, and (b) Tauc plots for the band gap calculation for C3N4 samples calcined at different temperatures. 40x18mm (300 x 300 DPI)
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 6 (a) PL spectra of C3N4 nanosheets grown at different temperatures under an excitation energy of 3.35 eV. The inset shows a magnified view of the PL spectrum of CN420. (b) PL spectra of CN520 obtained under different excitation energies. 62x24mm (600 x 600 DPI)
ACS Paragon Plus Environment
Page 40 of 44
Page 41 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
Figure 7 (a) Decovoluted (Gaussian) PL spectrum of CN520 under excitation of 3.35 eV. (b) TRPL (logarithmic plot) spectra of CN520 excited at 3.30 eV and monitored at 2.78 eV, 2.58 eV and 2.38 eV emission energies. (c) Plot showing a relation of S-parameter (left Y-axis) and average bound excitonic lifetime (tav at 2.38 eV) (right Y-axis) as a function of calcination temperature, which demonstrates a direct correlation between the S-parameter and tav. 80x42mm (600 x 600 DPI)
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 8 Schematic shows exciton migration in (a) π-stacking direction (interplanar), and (b) intraplanar migration (1) and intrachain (2) migration. Free excitons (F-exciton), when attached to nitrogen related defects (N-defects) create bound excitons (DB-exciton). Exciton migration is prohibited if C-H or N-H moiety terminates the heptazine link. 129x126mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 42 of 44
Page 43 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The Journal of Physical Chemistry
Figure 9 Normalized PL spectra of CN520 for different excitation power (intensity). The samples are excited with a solid-state laser of energy 3.06 eV. (b) Changes in emission energy (left Y-axis), full width at half maximum (FWHM) (right Y-axis) with laser power. The inset shows the PL emission intensity as a function of excitation laser power. 52x19mm (600 x 600 DPI)
ACS Paragon Plus Environment
The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 10 (a) Photoluminescence spectra of CN520 at different excitation energy. The excitations are below the optical bandgap of the grown nanosheets. (b) Schematic showing below bandgap excitation and emissions due to carrier trapped in different defect states. Different band states in the valence band and conduction band, nitrogen lone pair (LP) state and nitrogen-related defect states are shown. (c) TRPL spectrum (logarithmic plot) of CN520 excited at 2.45 eV. 60x20mm (300 x 300 DPI)