Fiber Alignment and Liquid Crystal Orientation of Cellulose Nanocrystals in the Electrospun Nanofibrous Mats Weiguang Song, Dagang Liu, Nana Prempeh, and Renjie Song Biomacromolecules, Just Accepted Manuscript • DOI: 10.1021/acs.biomac.7b00927 • Publication Date (Web): 19 Sep 2017 Downloaded from http://pubs.acs.org on September 20, 2017
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Biomacromolecules is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
Fiber Alignment and Liquid Crystal Orientation of
2
Cellulose Nanocrystals in the Electrospun Nanofibrous
3
Mats
4
Weiguang Song,a,b Dagang Liu,*a,b,c Nana Prempeh,b Renjie Song a
5
6
7
a
Department of Chemistry, Nanjing University of Information Science and Technology, Nanjing 210044, China
8
9
b
Collaborative Innovation Center of Atmospheric Environment and Equipment
10
Technology, Nanjing University of Information Science and Technology, Nanjing
11
210044, China
12
c
Department of Physics, University of Colorado, Boulder, CO 80309, USA
13
ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
14
ABSTRACT:
15
Sulfate cellulose nanocrystal (CNC) dispersions always present specific self-assembled
16
cholesteric mesophases which is easily affected by the inherent properties of particle size,
17
surface charge and repulsion or affinity interaction, and external field force generated from ionic
18
potential of added electrolytes, magnetic or electric field, and/or mechanical shearing or
19
stretching. Aiming at understanding the liquid crystal orientation and fiber alignment under high-
20
voltage electric field, randomly distributed, uniform-aligned, or core-sheath nanofibrous mats
21
involving charged CNCs and PVA were electrospun; and amongst them, specific straight arrayed
22
fine nanofibers with average diameter of 270 nm were manufactured by using a simple and
23
versatile gap collector. Moreover, arrayed composite nanofibers regularly aligned along the
24
vertical direction of gap plates and selectively reflected frequent and continuous birefringence
25
which was regarded as nematic phases of CNCs induced by the uniaxial stretching under high-
26
voltage electric field. As a synergic effect of rigidness of nanocrystals and stretching orientation
27
of nematic phases, the aligned nanofibrous arrays exhibited a higher tensile strength and strain
28
than the randomly-oriented or core-sheath nanofibrous mats at the same loading of CNCs. By
29
contrast, mesophase transition of CNCs from cholesteric to nematic occurred in the coaxially
30
spun core-sheath nanofibers at a loss of long-ranged chiral twist. Hence, the structure-effect
31
relationship between liquid crystal orientation of charged nanorods in polymer-based fine
32
nanofibers and the flexibility or mechanical integrity of the aligned fiber array will be favorable
33
for strategic development of functional liquid crystal fabrics.
34
Keywords: Cellulose nanocrystals, PVA, Electrospinning, Nanofibrous mats, Alignment
ACS Paragon Plus Environment
Page 2 of 25
Page 3 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
35
Biomacromolecules
INTRODUCTION
36
Up until now, electrospinning has been accepted as a simple and efficient method for
37
developing polymer nanofibers with width range from 3 nm to 5 µm,1,2 depending on the
38
spinning parameters. Under a high-voltage electric field the electrospinning process itself
39
involves polymer droplets stretching and deformation into conical cylindrical threads with a
40
rapid evaporation of the solvent.3 Electrospun nanofibers have several remarkable characteristics
41
such as porosity,4 high aspect ratio,5 flexibility in surface functionalities, and special mechanical
42
and biological properties which makes them excellent candidates for applications such as
43
nanofibrous membranes or filters,6 mats in tissue engineering constructs and wound dressings,7,8
44
military wears with chemical and biological toxin-resistance,9 electronic sensors,10 and so on.
45
Generally, the flow rate, voltage, and tip-to-collector distance are thought as very important
46
processing parameters that directly affects the morphology, size distribution, and mechanical
47
performance of nanofiber,11,12 whereas, instability of polymer jet streams has often led to poorly
48
aligned fibers with varying morphology and diameters during the electrospinning process.
49
Moreover, the disorderliness in fiber formation is problematic as much more applications
50
requiring the use of fibrous mats relies heavily on well-aligned and highly ordered
51
architectures.13 Up to now, several approaches such as modification of the collection devices by
52
the use of rectangular metal frame,14 central point electrode and peripheral ring electrode,15 a pair
53
of parallel electrodes or addition of electrode,16 circular copper wire drum collector, 17 or an
54
additive electric field,18 have been considered for the development of aligned and continuous
55
nanofibers.
56
Sulfuric acid hydrolysis of native cellulose microfibrils produces suspensions of cellulose
57
nanocrystals (CNCs), which are highly stable in aqueous suspensions because of the repulsion
ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
58
among negatively charged sulfate ester bearings on the surface of CNCs.19,20 While the
59
homogeneous suspension of sulfate CNCs is solidified after a slow evaporation induced self-
60
assembly process, cholesteric liquid crystalline films with chiral reflective iridescence are
61
formed.21,22 Namely, the solidified films generated from liquid crystalline suspensions inherits a
62
short-range position arrangement and long-range chiral nematic orientation of 3-D photonic
63
CNC colloids.23 This fascinating liquid crystal properties of CNCs have received an increasing
64
attention for the fabrication of novel functional chiroptical materials.24,25 At hand, the scalization
65
and industrialization of CNC based materials of film, coating, fiber, etc., are confined by the
66
stiffness and fragile nature of CNCs. Several researches involving neutral polymers of PEG,26
67
PEO,27 and PVA,28 with excellent compatibility and affinity with/to CNCs was performed to
68
improve the flexibility of generated composites. More interestingly, both PEG,26 and PVA,28
69
presented severe impact on the structure-color and chiral nematic mesophases of CNCs due to
70
microphase separation, thereby leading to the loss of the long-range orientation and chiroptical
71
reflectivity of bulk coatings, films or fibers exceeding a critical loading content of the compatible
72
polymers.
73
More recently, nanofibrous composite mats of PVA was electrospun by employing CNCs
74
with loading dose of 0-15 wt% as effective reinforcement agents.29-31 As a matter of fact, it was
75
thought that overall tension in the spinning dope of CNCs with a high charge density on the
76
surface would self-repulse the excess charges on the jet, thus, as the charge density increase, the
77
continuity, stability, and alignment of the fibers meet great challenges in electrospinning.
78
Notwithstanding the foregoing, no research work on the alignment of nanofibrous CNC
79
composite mats as well as the orientation of CNCs in a liquid jet under high voltage electric field
80
during electrospinning is reported and discussed in detail. In this work, single-fluid of composite
ACS Paragon Plus Environment
Page 4 of 25
Page 5 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
81
dispersions or dispersion mixture containing CNC and hydrophilic PVA was deployed as
82
spinning dope and a tailored gap between a couple electrode plates or a rotating roller was
83
applied as a collection device of electrospinning. Aiming at improving the alignment of
84
nanofibers and orientation of highly surface-charged CNCs, we attempted to set up a new
85
approach to fabricate nanofiber arrays by controlling the physicochemical properties of spinning
86
dope and processing parameters, and tended to understand the mesophase orientation and
87
alignment of fibers under electrical stretching or repulsive and attractive interaction, and
88
anticipated to build up the relationship between the tailored composing structure of random
89
distribution, uniformed alignment, or core-sheath and properties of as-spun fibrous mats.
90
MATERIALS AND METHODS
91
Materials. PVA (AH-26, Mw = 114,400) having a degree of polymerization (DP) of about
92
2600 and saponification of 98% and microcrystalline cellulose (MCC, 9004-34-6) of analytical
93
grade were purchased from Sinopharm Chemical Reagent Co., Ltd. (Shanghai, China).
94
Concentrated sulfuric acid of analytical grade was purchased from Shanghai Lingfeng Chemical
95
Reagent Co. Ltd.
96
Preparation of spinning dope. Referring to our previous work,23 MCC was hydrolyzed by
97
sulfuric acid (64 wt%) at 50 oC in a water bath under vigorous mechanical stirring for 2.5 h. The
98
resultant suspension was diluted 5-fold by deionized water and then poured into cellulose
99
dialysis tube with MWCO of 8,000-14,000 to dialyze against deionized water for more than one
100
week to remove residual sulfuric acid and many small molecules. Subsequently, impurities and
101
unmodified coarse particles in the dialyzed suspension was removed by centrifugation at 12000
102
rpm for 10 min. The as-prepared CNCs after a mild sonication have a length of 150 ± 30 nm and
103
width of 35 ± 5 nm, and a negative surface charge density of 0.60 e/nm2.23 Alternatively, PVA
ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
104
was dissolved in deionized water at 90 oC under strong mechanical stirring for 1 h to produce a
105
homogeneous solution with a concentration of 10 wt%. Subsequently, CNC suspension and PVA
106
solution were mixed in specific proportions under continuous agitation for 4 days at 30 oC. The
107
individual resultant PVA/CNC mixture as a single fluidic spinning dope was then stored in the
108
refrigerator to allow a slow evaporation and absolute self-assembly at 10 oC until a desired
109
concentration of the spinnable dope was obtained.
110
Electrospinning of PVA/CNC nanofiber mats. As illustrated in Supplementary Figure
111
S1a, the electrospinning set-up of roller-collection comprised of a high voltage power supply (0-
112
50 DC kV), a micro-syringe pump (V = 20 mL) connected to a metal needle (di = 0.40 mm) or
113
coaxial spinneret (do = 2.00 mm; di = 0.40 mm), and a collector of grounded rotating cylindrical
114
roller (D = 4 cm; L = 15.5 cm) with a tip-to-collector distance of 0-20 cm. In this roller-
115
collection device, the spinneret acting as a positive electrode was connected to the high voltage
116
power supply to generate electric field. During the electrospinning process, the dope was
117
pumped through a polytetrafluoroethylene (PTFE) tube, and then injected from the metal
118
spinneret as a fluidic jet at a specific rate. After water evaporation, the solidified jet in the form
119
of nanofibers were collected on the metallic cylindrical roller. According to mass ratio of
120
CNC/PVA at 1:9, 1:3, and 1:1, the manufactured nanofibers mats with random orientation were
121
denoted as PVA/CNC10R, PVA/CNC25R, and PVA/CNC50R, respectively. Alternatively, in a
122
coaxial electrospinning process, CNC suspension and PVA solution were independently fed into
123
a coaxial spinneret at a speed of 0.2 mL/h and 0.6 mL/h, respectively, and spun in a core-shell
124
manner. The fine core-sheath nanofibers of PVA/CNC collected on the metallic cylindrical roller
125
were denoted as PVA@CNC10 and CNC10@PVA corresponding to mass ratio (1:9) of CNCs to
126
PVA in the fabricated core-sheath nanofibers.
ACS Paragon Plus Environment
Page 6 of 25
Page 7 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
127
Specifically, we set up a tailored gap collector with a couple of parallel plates (Figure S1b)
128
involving a negative metal plate of 30-mm thickness and a ground polyoxymethylene (POM)
129
plate of 30-mm thickness. On the upper right side of the POM plate a small thin metal sheet with
130
thickness of 5 mm was covered. The tailored gap-collector was built up to collect the well-
131
aligned nanofibrous mats of PVA/CNC by adjusting the applied voltage, needle-to-collector
132
distance, working temperature, and the gap distance between two plates. In this case, additional
133
substrates could be placed within the gap to support or collect the nanofibers without any
134
significant influence on the quality of the resultant nanofibers. The as-manufactured fine
135
nanofibers with good alignment were denoted PVA/CNC10A, PVA/CNC25A, and
136
PVA/CNC50A corresponding to the weight ratio of CNC/PVA at 1:9, 1:3, and 1:1, respectively.
137
The as-manufactured nanofibrous mats were vacuum dried at 40 °C for 24 h to remove any
138
residual water, and then vacuum-stored for further analysis.
139
Characterization. Zeta potential of the spinning dope was measured using a dynamic light
140
scattering (DLS, ZS90, Malvern Instruments, U.K.) with a combined laser Doppler velocimetry
141
(LDV) and phase analysis light scattering (PALS). The viscosity of the spinning dope was tested
142
using a RS6000 rheometer (Thermo Scientific, Karlsruhe, Germany) with a parallel plate
143
geometry (25 mm diameter, 0.3 mm gap) at 25 °C. Nanofibrous mats were deposited onto a
144
rectangular glass slide for liquid crystal phase observation on a polarized optical microscope
145
(POM; LV100POL, Nikon, Japan). Morphology observations were carried out on a field
146
emission scanning electron microscope (FE-SEM, Hitachi S-4700 microscope) with an
147
accelerating voltage of 20 kV. The sample mats were fixed on conductive carbon tape and then
148
sputtered with gold for SEM observations. Size distribution of nanofibers was statistically
149
analyzed by using the ImageJ Tool. Fourier-transform infrared spectroscopy (FTIR) of
ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
150
nanofibrous mats was performed on a Bio-Rad FTS 6000 FTIR spectrometer equipped with an
151
IR microscope (UMA-500); the polarized infrared beam, with rays in parallel, goes through the
152
microtomed sample mats, while the transmittance was measured with the aid of a liquid nitrogen
153
cooled Mercury Cadmium Telluride (MCT) detector. The spectra were recorded at a resolution
154
of 8 cm-1 with a spectral range of 650-4000 cm-1. During the measurement, a home-built sample
155
holder was employed to keep the mats in position at a constant inclination angle θ while a set of
156
different polarizer positions φ was scanned. Tensile properties of the standard rectangular strips
157
(40 × 100 mm2) of nanofibrous mats were performed on a Shimadzu SLBL-500N tensile tester
158
(Shimadzu Inc., Japan) at a crosshead speed of 5 mm/min. The testing results were evaluated as
159
an average of at least 10 measurements.
160
RESULTS AND DISCUSSION
161
Homogeneous composite dispersions of PVA/CNC as spinning dopes were sprayed in a
162
single-fluid manner and collected on a rotating cylindrical roller as shown in Figure S1a.
163
Judging from the fineness, continuity, defect-free, and uniformity of nanofibers, the
164
optimized spinning parameters of nanofibers obtained by roller collector were 10-16 wt%, 12 kV,
165
35 °C, 51%, 0.3 mL/h, 13 cm, and 94.7 mm/min corresponding to dope concentration, voltage,
166
temperature, relative humidity, flow rate, needle-to-collector distance, and nozzle translational
167
velocity, respectively as demonstrated in Table S1 and Figure S2-5. The as-spun winding
168
nanofibers of PVA/CNC10R presents a randomly distributed diameter widely ranging from 300
169
to 600 nm (Figure 1a), indicating the spiral path and whipping of flexible macromolecular
170
chains of PVA.
171
Interestingly, while a tailored gap between double electrode plates was substituted for roller
172
collector (Figure S1b) under voltages of 12 kV, needle-to-collector distance of 11 cm, flow rate,
ACS Paragon Plus Environment
Page 8 of 25
Page 9 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
173
0.3 mL/h; translational velocities of 28.8 mm/min (Figure S6-7), multiple jets were released and
174
the individual jets simultaneously traveled from one end of collecting electrode plane, and then
175
crossed the gap to the other end of electrode plane whilst undergoing a stretching and
176
disintegration process as shown in Video S1. The generated uniaxially aligned nanofibrous
177
arrays were finally deposited across the gap (7 cm) with the longitudinal fibrous axes
178
perpendicular to the gap plate, and the arrayed fine nanofibers of PVA/CNC10A display mean
179
diameters of 270 ± 25 nm (Figure 1b), much more uniform and smaller than PVA/CNC10R,
180
indicating a pretty strong stretching underwent between the gap plates.
181
Nonetheless, while concentrated CNC dispersion and hydrophilic PVA solution were ejected
182
in a coaxial manner, no arrayed nanofiber mats could be collected on either gap or rollers
183
because of the distinctly different fluidic properties and discordant fiber-formation behavior of
184
individual dope. Specifically, limited by the low viscosity, poor spinnability and inadequate
185
water evaporation of CNC dispersions, PVA@CNC10 with a diameter varied from 288 to 1007
186
nm displays flat and occasionally collapsed surface (Figure 1c). In the case of CNC10@PVA
187
with a wide diameter distribution (98 - 1359 nm), some droplets of CNCs caused by insufficient
188
water evaporation had a strong tendency to pool together with PVA nanothreads after a
189
continuous deposition, thereby continuously aggregating into crosslinked porous fibrous network
190
(Figure 1d). Therefore, morphology and size of four kind of nanofibers could be controlled by
191
the tailored spinning approaches and optimized processing parameters.
192
In general, due to the structure anisotropy of the CNCs,32 its aqueous dispersions at a high
193
concentration always display self-assembled tactoids with fantastic fingerprint textures as shown
194
in Figure 2a. As one component in the coaxial spinning dope, CNC fluid was discontinuously
195
ejected and elongated, thus leading to intermittent shiny birefringent segments evenly distributed
ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 25
196
inside the long fiber of PVA@CNC10 (Figure 2b), 33 otherwise, reflective iridescent CNC beads
197
(diameter of 0.7-3 µm) were dotted along the long PVA threads (average diameter of 279 nm) to
198
form into regular pearl-chain structure in CNC10@PVA (Figure 2c). When a compensator of
199
530 nm retardation plate was inserted between the polarizer and analyzer at a fixed angle of 45°,
200
nematic rather than cholesteric mesophases of CNCs were randomly distributed in the core of
201
PVA@CNC10 or at the outer surface of CNC10@PVA (Figure S8), indicating a mesophase
202
transition from the chiral twisting lamella to nematic phases of CNCs.
203
In the single-fluidic spinning dope, no mesophase of CNCs was recognized due to the
204
homogeneous and isotropic dispersion of nanorods (Figure 2d). However, under polarized light,
205
shining overlaid birefringence could be visualized in the randomly-distributed nanofibers of
206
PVA/CNC10R (Figure 2e). Moreover, frequent and continuous birefringence with selective
207
reflection was obviously visualized and regarded as nematic CNCs in the PVA/CNC10A (Figure
208
2f). Micrographs of nanofibrous mats in the presence of a 530-nm retardation plate between
209
crossed polarizers are shown in Figure 3. By changing the rotation angle of the sample,
210
continuous transition of alternating blue and orange bands were visualized in the arrayed
211
nanofiberous mats of PVA/CNC10A (Figure 3e,f) and PVA/CNC50A (Figure 3h,i).
212
Accordingly, the fuchsia-colored image regions corresponded to uniaxially fibrous orientation (n)
213
roughly parallel to the slow axis (γ) of the retardation plate whereas the orange-red hue
214
corresponded to n⊥γ, indicating high refractive index of the axis (γ) or the uniaxial fiber axis due
215
to positive birefringence anisotropy (ne > no) of CNCs.34 Specifically, PVA/CNC50A exhibited a
216
relatively strong coloration difference between longitudinal and transverse fiber axis, suggesting
217
more uniform and strong orientation along uniaxial fiber axis as a result of the intra-particle
218
repulsion of surface-charged nanorods and stretching-induced alignment under electric field
ACS Paragon Plus Environment
Page 11 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
219
(Figure 3h,i).35 In contrast, as no accordance of the γ axis to the fibrous axis, randomly-
220
distributed PVA/CNC10R did not present overall arrangement and mesophase orientation of
221
CNCs but a tilt with respect to the longitudinal axis (Figure 3a,b).
222
Polarized FTIR spectra was deployed to verify the particle orientation in the nanofibers
223
(Figure S9). The characteristic band centered at 1160 cm-1 is associated with stretching and
224
asymmetric pyranose ring breathing vibrations of cellulose; the peak at around 1100 cm-1 is
225
assigned to C-O stretching vibrations of PVA;36 and the band at around 1060 cm-1 is attributed to
226
stretching vibration of C-OH of cellulose. Polar plots of absorbance of ν
227
(1100 cm-1), ν
228
three bands of PVA/CNC10R have very few response to the rotational angle of incidence
229
polarized light from 0° to 360° and present a circular shape, indicating a total isotropic character
230
under polarized infrared light (Figure 4a). However, as evidenced by the ellipsoid or dumbbell
231
shape, polar plots of IR bands in the aligned nanofibrous arrays exhibits a significant response to
232
the polarization angle with the maximum difference occurring between absorbance of ν C-OH or ν
233
C-O-C at
234
indicator of the degree of uniaxial orientation of CNCs in the mats, dichroic ratio (R) was
235
calculated according to the following equation.36
236
R=
237
where A// and A⊥ are IR absorbance at parallel and perpendicular mode, respectively. R of the
238
randomly-distributed nanofiber of PVA/CNC10R, as listed in Table 1, is nearly equal to 1 due to
239
the isotropic character. In the case of a perfectly uniaxial orientation along the fiber axis, R
240
should be theoretically equal to infinity.37 In the arrayed fibers, R of ν
241
was high up to 1.35-1.58 or 1.52-2.09, respectively, suggesting that the orientation of CNCs
A //
C-O-C
C-OH
(1060 cm-1), ν
C-O
(1160 cm-1) of spun nanofibers are shown in Figure 4. The peak value of
parallel mode (A//) and perpendicular mode (A⊥) to the fiber axes, (Figure 4b,c,d). As an
(1)
A⊥
ACS Paragon Plus Environment
C-OH
and ν
C-O-C of
CNCs
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
242
rather than PVA occurred along the fiber axis.38 Therefore, in the gap region, the stretching and
243
the Coulombic force possibly synergistically induced the orientation of charged nanorods and
244
initiated the nematic phase formation in the jet.39,40
Page 12 of 25
245
Typical stress-strain profiles of 4 nanofiber mats are shown in Figure 5, and the resultant
246
averaged stress, stain, and elastic modulus are listed in Table 1. Reinforcement effects of a
247
certain amount of CNCs (10 wt%) are distinguished, e.g., mean tensile strength of
248
PVA/CNC10R and PVA/CNC10A were 8.27, and 10.25 MPa, respectively, much higher than
249
that of PVA (7.50 MPa); meanwhile, the modulus of PVA/CNC10R, PVA/CNC10A,
250
CNC10@PVA, and PVA@CNC10 were all much higher than that of PVA since the rigidity of
251
CNCs played a crucial role in the enhancement of tensile strength. However, fibrous mats with
252
high loading doses of CNCs (≥ 25 wt%) exhibit a sharply decreasing stress and strain in
253
comparison to PVA/CNC10. Meanwhile, tensile strength and elongation at break of
254
CNC10@PVA are higher than that of PVA@CNC10 due to the crosslinking network effects of
255
CNCs as depicted in Figure 1d. That is to say, interface contact and evaporation rate of dope
256
components are dependent factors that influence the structure, morphology and mechanical
257
properties of coaxial nanofibrous mats. Interestingly, the aligned nanofibers of PVA/CNC at the
258
same loading doses of CNCs exhibit a higher tensile stress than that of randomly distributed
259
nanofibers along the fibrous axis because both good alignment of nanofibers and continuous
260
nematic segments of CNCs in aligned nanofibers provided a substantially strong resistance to
261
external stretching force. However, the increment in tensile strength of the aligned nanofibers of
262
PVA/CNC didn’t occur at the expense of tensile strain but exhibit a higher elongation at break
263
than that of randomly distributed nanofibers at the same loading doses of CNCs. This is ascribed
264
to the fact that under uniaxial drawing along fiber axis the nematic mesophases of CNCs were re-
ACS Paragon Plus Environment
Page 13 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
265
orientated, thus leading to an extended deformation and improved flexibility.28 The aligned
266
nanofibrous mats is somewhat analogy to liquid crystal elastomers with macroscopic elastic
267
response arising from the phase separation under large deformations.
268
CONCLUSIONS
269
In this work, CNC dispersion and aqueous PVA solution as a mixed spinning dope or
270
separated dopes were sprayed in a manner of single-fluid or coaxial electrospinning and
271
collected on a rotating cylindrical roller or across a gap. Without any doubt, fine nanofibers
272
generated from single fluidic dope was continuous, smooth, and uniform due to homogenous
273
dispersion of CNC into PVA, whereas coaxial nanofiber had a larger average diameter, broader
274
size distribution and rough surface. The single-fluidic jet deposited across gap plates were well
275
aligned along the direction vertical to plates because the gap was favorable for the electric-field-
276
induced-alignment of CNCs by the uniaxial stretching as well as the movement of CNCs
277
unrestricted by the length of nanofibers as far as possible. The anisotropic and birefringent
278
character of fiber arrays oriented along the uniaxial fiber axis were certified by polarized IR and
279
POM with a retardation plate. The alignment of nanofibers was highly dependent on the
280
processing condition, and the orientation of CNCs with positive refractive index anisotropy and
281
surface charges was related to the high voltage electric field. Being different with single-fluidic
282
jet, coaxially-electrospun core-sheath nanofibers also showed birefringence under polarized light
283
because nematic mesophases of CNCs in the concentrated dispersions was switched. The
284
uniaxial, continuous orientation of CNCs played an important role in enhancement of mechanical
285
properties of the nanofibrous composite mats, e.g., average tensile strength (10.25 MPa) and
286
elongation at break (87.91%) of PVA/CNC10A were much higher than that of other spun
287
nanofibrous mats. In this work, we have provided a strategy for encapsulating homogeneously
ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
288
nematic nanorods into nanoscaled fibrous mats which is anticipated to be explored as novel
289
photonic and biological tissues, biosensors, and environmental-friendly filters.
290
Supporting Information Available. Diagram of electrospinning set-up, properties of
291
spinning dope, optimization for randomly-distributed and aligned electrospun nanofibers, POM
292
of CNCs in the core-sheath nanofibers, polarized FTIR spectra of nanofibers. This material is
293
available free of charge via the Internet at http://pubs.acs.org.
294
AUTHOR INFORMATION:
295
Corresponding author
296
∗
297
ORCID
298
Dagang Liu: 0000-0002-1320-7030
299
Notes
300
The authors declare no competing financial interest.
301
ACKNOWLEDGEMENTS
302
The authors are grateful to National Natural Science Foundation of China (Nos. 51473077 and
303
21277073), CSC scholarship (201608320064), and Six Talents Summit Program and 333 High-
304
Level Talent Cultivation Program of Jiangsu Province for financial support.
305
REFERENCES
E-mail:
[email protected] (D. Liu)
306
(1) Antaya, H.; Richardlacroix, M.; Pellerin, C. Macromolecules 2010, 43, 4986-4990.
307
(2) Yao, L.; Haas, T. W.; Guiseppi-Elie, A.; Bowlin, G. L.; Simpson, D. G.; Wnek, G. E. Chem.
308 309
Mater. 2003, 15, 1860-1864. (3) Li, D.; Babel, A.; Jenekhe, S.; Xia, Y. Adv. Mater. 2004, 16, 2062–2066.
ACS Paragon Plus Environment
Page 14 of 25
Page 15 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
310
(4) Ma, Z.; Ramakrishna, S. J. Membrane Sci. 2008, 319, 23-28.
311
(5) Zhang, H. T.; Nie, H. L.; Yu, D. G.; Wu, C. Y.; Zhang, Y. L.; White, C. J. B.; Zhu, L.
312
Desalination 2010, 256, 141-147.
313
(6) Makaremi, M.; Silva, R. T. D.; Pasbakhsh, P. J. Phys. Chem. C 2015, 119, 7949-7958.
314
(7) Stephens, J. S.; Chase, D. B.; Rabolt, J. F. Macromolecules 2004, 37, 877-881.
315
(8) Luo, Y.; Shen, H.; Fang, Y.; Cao, Y.; Huang, J.; Zhang, M.; Dai, J.; Shi, X.; Zhang, Z. J. ACS
316 317
Appl. Mater. Interface 2015, 7, 6331. (9) Unnithan, A. R.; Barakat, N. A.; Pichiah, P. B.; Gnanasekaran, G.; Nirmala, R.; Cha, Y. S.;
318
Jung, C. H.; EI-Newehy, M.; Kim, H. Y. Carbohydr. Polym. 2012, 90, 1786-93.
319
(10) Xu, L.; Dong, B.; Wang, Y.; Bai, X.; Chen, J. S.; Liu, Q.; Song, H. W. J. Phys. Chem. C
320
2010, 114, 9089-9095.
321
(11) Zong, X. H.; Kim, K.; Fang, D. F.; Ran, S. F.; Hsiao, B. S.; Chu, B. Polymer 2002, 43,
322
4403-4412.
323
(12) C. Wang, H. S. Chien, K. W. Yan, C. L. Hung, K. L. Hung, S. J. Tsai, H. J. Jhang, Polymer
324
2009, 50, 6100-6010.
325
(13) Gu, S. Y.; Ren, J.; Vancso, G. J. Eur. Polym. J. 2005, 41, 2559-2568.
326
(14) Fan, Z.; Ho, J. C.; Jacobson, Z. A.; Yerushalmi, R.; Alley, R. L.; Razavi, H.; Javey, A. Nano
327
Lett. 2008, 8, 20-25.
328
(15) Dersch, R.; Liu, T. Q.; Schaper, A. K.; Greiner, A.; Wendorff, J. H.; J. Polym. Sci. A. Polym.
329
Chem. 2003, 41, 545–553.
330
(16) Xie, J.W.; Macewan, M. R.; Ray, W. Z.; Liu, W. Y.; Siewe, D. Y.; Xia, Y. N. ACS Nano
331
2010, 4, 5027.
ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 25
332
(17) Sundaray, B.; Subramanian, V.; Natarajan, T. S.; Xiang, R. Z.; Chang, C. C.; Fann, W. S.
333
Appl. Phys. Lett. 2004, 84, 1222-1224.
334
(18) Katta, P.; Alessandro, M.; Ramsier, R. D.; Chase, G. G. Nano Lett. 2004, 4, 2215-2218.
335
(19) Marchessault, R. H.; Morehead, F. F.; Koch, M. J. J. Colloid. Sci. 1961, 16, 327-344.
336
(20) Beck-Candanedo, S.; Roman, M.; Gray, D.G. Biomacromolecules 2005, 6, 1048-1054.
337
(21) Revol, J. F.; Godbout, L.; Dong, X. M.; Gray, D. G.; Chanzy, H.; Maret, G. Liq. Cryst. 1994,
338
16, 127-134.
339
(22) Liu, D.; Chen, X.; Yue, Y.; Chen, M.; Wu, Q. Carbohydr. Polym. 2011, 84, 316-322.
340
(23) Liu, D.; Wang, S.; Ma, Z.; Tian, D.; Gu, M.; Lin, F. RSC Adv. 2014, 4, 39322-39331.
341
(24) Shopsowitz, K. E.; Qi, H.; Hamad, W. Y.; MacLachlan, M. J. Nature 2010, 468, 422-428.
342
(25) Shopsowitz, K. E.; Hamad, W. Y.; MacLachlan, M. J. J. Am. Chem. Soc. 2012, 134,
343
867−870.
344
(26) Gu, M.; Jiang, C.; Liu, D.; Prempeh, N.; Smalyukh, I. I. ACS Appl. Mater. Interface 2016, 8,
345
32565-32573.
346
(27) Zhou, C.; Chu, R.; Wu, R.; Wu, Q. Biomacromolecules 2011, 12, 2617–2625.
347
(28) Liu, D.; Li, J.; Sun, F.; Xiao, R.; Guo, Y.; Song, J. RSC Adv. 2014, 4, 30784-30789.
348
(29) Lee, J.; Deng, Y. Macromol. Res. 2012, 20, 76-83.
349
(30) Peresin, M. S.; Habibi, Y.; Zoppe, J. O.; Pawlak, J. J.; Rojas, O. J. Biomacromolecules 2010,
350
11, 674–681.
351
(31) Huan, S. Q.; Bai, L.; Cheng, W. L.; Han, G. P. Polymer 2016, 92, 25-35.
352
(32) Csoka, L.; Hoeger, I. C.; Peralta, P.; Peszlen, I.; Rojas, O. J. J. Colloid Interface Sci. 2011,
353
363, 206–212.
354
(33) Enz, E.; Lagerwall, J. J. Mater. Chem. 2010, 20, 6866–6872.
ACS Paragon Plus Environment
Page 17 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
355
(34) Liu, Q.; Campbell, M. G.; Evans, J. S.; Smalyukh, I. I. Adv. Mater. 2014, 26, 7178-7184.
356
(35) Llanos, G. R.; Sefton, M. V. Macromolecules 1991, 24, 6065-6072.
357
(36) Pedicini, A.; Farris, R. J. Polymer 2003, 44, 6857-6862.
358
(37) Haridas, M.; Smalyukh, I. I. Small 2015, 11, 5572–5580.
359
(38) Kongkhlang, T.; Tashiro, K.; Kotaki, M. Chirachanchai, S. J. Am. Chem. Soc. 2008, 130,
360
15460–15466.
361
(39) Nakashima, K.; Tsuboi, K.; Matsumoto, H.; Ishige, R.; Tokita, M.; Watanabe, J.; Tanioka, A.
362
Macromol. Rapid Comm. 2010, 31, 1641–1645.
363
(40) Herrera, N. V.; Mathew, A. P.; Wang, L. Y.; Oksman, K. Plastics, Rubber and Composites.
364
2011, 40, 57-64.
365
ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
366
Page 18 of 25
Table 1. Dichroic ratio (R) and mechanical properties of as-spun nanofibrous mats. Nanofibrous
R
R
mats
(ν C-OH)
PVA
-
-
PVA/CNC10R
0.94
PVA/CNC10A
R
Tensile
Elongation at
Elastic
stress (Pa)
break (%)
modulus (MPa)
-
7.50±0.43
77.00±7.22
38.01±2.32
1.03
0.96
8.27±0.25
20.17±4.23
853.15±14.13
1.40
1.06
1.52
10.25±0.34
87.91±7.34
185.33±4.17
PVA/CNC25R
-
-
-
4.03±0.24
3.13±0.81
430.79±7.15
PVA/CNC25A
1.58
1.08
1.86
6.48±0.13
29.51±3.33
342.72±6.8
PVA/CNC50R
-
-
-
0.40±0.032
2.86±0.31
16.96±2.02
PVA/CNC50A
1.35
1.11
2.09
2.79±0.02
8.12±0.92
236.39±5.32
CNC10@PVA
-
-
-
8.82±0.26 109.19±10.73 115.29±1.71
PVA@CNC10
-
-
-
6.84±0.32
(ν C-O) (ν C-O-C)
37.53±6.28
367
ACS Paragon Plus Environment
837.12±13.76
Page 19 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
368
Figure Captions:
369
Figure 1. SEM micrographs and histograms of width distributions for randomly orientated
370
nanofibers of PVA/CNC10R (a), well-aligned nanofibers of PVA/CNC10A (b), and core-sheath
371
nanofibers of PVA@CNC10 (c), CNC10@PVA (d), respectively.
372
Figure 2. Polarized optical micrographs of spinning dope of CNC (a) and PVA/CNC10 (d), and
373
electrospun nanofibers of PVA@CNC10 (b), CNC10@PVA (c), PVA/CNC10R (e),
374
PVA/CNC10A (f), respectively.
375
Figure 3. POM images of nanofibrous mats of PVA/CNC10R (a), PVA/CNC10A (d),
376
PVA/CNC50A (g), and POM images of nanofibrous mats of PVA/CNC10R (b,c),
377
PVA/CNC10A (e,f), PVA/CNC50A (h,i) with a full-wavelength (530 nm) retardation plate with
378
a slow axis (γ) marked by a yellow arrow.
379
Figure 4. Polar plots of the normalized absorbance as a function of rotational angle (α) for ν C-OH
380
(1060 cm-1), ν
381
PVA/CNC25A, (d) PVA/CNC50A.
382
Figure 5. Typical stress-strain profiles of PVA/CNC10R, PVA/CNC25R, PVA/CNC50R (a);
383
PVA/CNC10A,
384
PVA@CNC10 and CNC10@PVA fiber mats (c). The tensile test was performed along the fiber
385
axis.
C-O (1100
cm-1), ν
C-O-C (1160
PVA/CNC25A,
cm-1) of (a) PVA/CNC10R, (b) PVA/CNC10A, (c)
PVA/CNC50A (b);
and
ACS Paragon Plus Environment
coaxial
nanofiber mats
of
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 25
386
387 388
Figure 1. SEM micrographs and histograms of width distributions for randomly orientated
389
nanofibers of PVA/CNC10R (a), well-aligned nanofibers of PVA/CNC10A (b), and core-sheath
390
nanofibers of PVA@CNC10 (c), CNC10@PVA (d), respectively.
ACS Paragon Plus Environment
Page 21 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
391 392
Figure 2. Polarized optical micrographs of spinning dope of CNC (a) and PVA/CNC10 (d), and
393
electrospun nanofibers of PVA@CNC10 (b), CNC10@PVA (c), PVA/CNC10R (e),
394
PVA/CNC10A (f), respectively.
ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 25
395 396
Figure 3. POM images of nanofibrous mats of PVA/CNC10R (a), PVA/CNC10A (d),
397
PVA/CNC50A (g), and POM images of nanofibrous mats of PVA/CNC10R (b,c),
398
PVA/CNC10A (e,f), PVA/CNC50A (h,i) with a full-wavelength (530 nm) retardation plate with
399
a slow axis (γ) marked by a yellow arrow.
ACS Paragon Plus Environment
Page 23 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
400 401
Figure 4. Polar plots of the normalized absorbance as a function of rotational angle (α) for ν C-OH
402
(1060 cm-1), ν
403
PVA/CNC25A, (d) PVA/CNC50A.
C-O (1100
cm-1), ν
C-O-C (1160
cm-1) of (a) PVA/CNC10R, (b) PVA/CNC10A, (c)
ACS Paragon Plus Environment
Biomacromolecules
a 12
b12
PVA/CNC10R PVA/CNC25R PVA/CNC50R
10
8
8
8
6
6
6
4
4
4
2
2
2
0.06 0.04 0.02 0.00
0.06 0.04 0.02 0.00
0.06 0.04 0.02 0.00
0
5
10
15
20
25
Strain (%)
404
c 12
PVA/CNC10A PVA/CNC25A PVA/CNC50A
10
Stress (MPa)
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 24 of 25
0
20
40
60
80
PVA@CNC10 CNC10@PVA
10
100
0
Strain (%)
20
40
60
80 100 120
Strain (%)
405
Figure 5. Typical stress-strain profiles of PVA/CNC10R, PVA/CNC25R, PVA/CNC50R (a);
406
PVA/CNC10A,
407
PVA@CNC10 and CNC10@PVA fiber mats (c). The tensile test was performed along the fiber
408
axis.
PVA/CNC25A,
PVA/CNC50A (b);
and
409
ACS Paragon Plus Environment
coaxial
nanofiber mats
of
Page 25 of 25
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
410
For Table of Contents Use Only
411
Graphical Abstract:
412 413
414
415
Fiber Alignment and Liquid Crystal Orientation of Cellulose Nanocrystals in the
416
Electrospun Nanofibrous Mats
417
Weiguang Song,a,b Dagang Liu,*a,b,c Nana Prempeh,b Renjie Song a
ACS Paragon Plus Environment