pNIPAAm Microgels

School of Mechanical Engineering, Purdue University, 585 Purdue Mall, West Lafayette, ... for Photo Memory Device and Blue-Light-Triggered Release Veh...
1 downloads 0 Views 800KB Size
Subscriber access provided by Northern Illinois University

Article

Fabrication of shape controllable Janus alginate/pNIPAAm microgels via microfluidics technique and off-chip ionic crosslinking Yuandu Hu, Shibo Wang, Alireza Abbaspourrad, and Arezoo Ardekani Langmuir, Just Accepted Manuscript • DOI: 10.1021/la504422j • Publication Date (Web): 13 Jan 2015 Downloaded from http://pubs.acs.org on January 24, 2015

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

Langmuir is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Langmuir

1

Fabrication of shape controllable Janus alginate/pNIPAAm microgels

2

via microfluidics technique and off-chip ionic crosslinking

3 4

Yuandu Hu1, Shibo Wang1, Alireza Abbaspourrad3, Arezoo M. Ardekani*1,2

5

1 Department of Aerospace and Mechanical Engineering, University of Notre Dame, Notre

6

Dame, Indiana 46556, USA

7

2 School of Mechanical Engineering, Purdue University, 585 Purdue Mall, West Lafayette,

8

Indiana 47907, USA

9

3 School of Engineering and Applied Sciences, Harvard University, Cambridge,

10

Massachusetts 02138, USA

11

*Corresponding Author

12

E-mail: [email protected]

13

ABSTRACT: A novel method to fabricate shape controllable alginate/pNIPAAm

14

complex microgels is reported. Monodisperse alginate/pNIPAAm droplets are created

15

via microfluidics and crosslinked in different concentrations of hot glycerol/barium

16

acetate water solutions. By changing the initial droplet size and glycerol concentration

17

of the collecting solution, the resultant microgel shape and surface details can be

18

systematically tuned. High-speed imaging is used to visualize and explain the

19

microgel formation process.

20 21 22 23



INTRODUCTION

24

Anisotropic and multicomponent microparticles have been widely investigated in the

25

past decades for various applications.1-4 For example, the two distinguishable surface

26

areas of Janus particles make them ideal candidates for displays,5-6 target recognition,7

27

interfacial stabilizers,8 encoding,9-10 sensors,11-13 cell encapsulation14 and the detection

28

of metal ions.15 Anisotropic particles with rough surfaces can be used for Raman

29

signal enhancement7 and hydrophobic coatings,16-17 due to their enlarged surface area 1

ACS Paragon Plus Environment

Langmuir

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 18

30

compared to that of smooth particles. Droplet-based microfluidic techniques have

31

been widely used to fabricate anisotropic microparticles.4,

32

polymer microgels with different components has been achieved using water in oil

33

(w/o) emulsion droplets combined with UV-induced polymerization or ionic

34

crosslinking to solidify droplets. The solidification process mostly occurs inside the

35

microfluidic device, known as on-chip solidification method.31 Seiffert et al. have

36

developed a double T-junction PDMS-based microfluidic device to fabricate Janus

37

pNIPAAm microgels by polymerizing Janus precursor droplets inside the microfluidic

38

device.32 The Janus pNIPAAm precursor droplets were formed from two independent

39

streams of linear pNIPAAm solutions with photo-chemical reaction groups and

40

polymerized using strong UV light32. UV-polymerized anisotropic microgels can also

41

be fabricated using stop-flow lithography microfluidic techniques.19,

42

coworkers synthesized Janus microgels by injecting NIPAAm-rich and NIPAAm-poor

43

phase into a hydrodynamic focusing microfluidic device (HFMD), followed by the

44

on-chip polymerization of Janus droplets via UV light.34 Ma et al. prepared concave

45

microgels by selectively polymerizing double emulsion droplets template.35 Besides

46

UV-induced solidification of polymers, on-chip ionic crosslinking methods can be

47

used to fabricate anisotropic microgels. Marquis et al. prepared both homo-Janus and

48

hetero-Janus biopolymer microbeads by using a flow-focusing device for

49

diffusion-controlled ionic crosslinking system.

50

Janus alginate microgels by injecting sodium alginate solutions into a double

51

T-junction microfluidic device and used on-chip cross-linking of the sodium alginate

52

droplets.37 Lu et al. fabricated Janus-like chitosan-based dimer capsules using a

53

T-junction microfluidic chip with four inlets.38 However, all the above-mentioned

54

methods are limited to requiring the use of a complicated microfluidic device with

55

multiple inlets to inject three or more precursor solutions. To overcome this limitation,

56

Choi et al. employed dewetting to induce phase separation, followed by UV

57

polymerization, obtaining complex structured microgels through single emulsion

58

precursor droplets.39 This approach provides a simple method to fabricate anisotropic

59

gel particles, but it is still limited to UV polymerized precursor droplets. To the best of

36

18-30

The fabrication of

33

Kim and

Zhao et al. fabricated magnetic

2

ACS Paragon Plus Environment

Page 3 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Langmuir

60

our knowledge, there are no reports on the fabrication of anisotropic complex

61

microgels by single emulsion droplets through an off-chip ionic crosslinking method.

62

In this study, we performed a simple and versatile approach to fabricate

63

shape-controllable poly (N-isopropylacrylamide) (pNIPAAm)/sodium alginate (SA)

64

microgels using single emulsion droplets. We use a glass capillary microfluidic device

65

to generate single water-in-oil emulsions; the monodisperse pNIPAAm/sodium

66

alginate emulsions were collected in hot collecting solutions, composed of barium

67

acetate (BA) mixed with different concentrations of glycerol aqueous solutions. We

68

exploit a non-equilibrium phase separation, crosslinking properties of SA and

69

coil-to-globule phase transition of pNIPAAm within the emulsions to fabricate

70

microgels of different optical properties, geometries and surface microstructures. We

71

control particle morphology, simply by tuning experimental parameters, such as the

72

initial droplet diameter and the extent of phase separation, concentration of linear

73

pNIPAAm and concentration of glycerol in the collecting solution. These complex

74

microgels can potentially be used in the design of stimulus-responsive drug delivery

75

vehicles, cell attachment materials, and for building porous three-dimensional tissue

76

constructs.

77



78

Materials. Poly (N-isopropyl acrylamide) (carboxylic acid terminated pNIPAAm,

MATERIALS AND METHODS

79

average Mn 5000, Sigma-Aldrich),

sodium

alginate

80

hexadecane (Anhydrous, 95%), barium acetate (purity > 99%), FeCl3 (Purity >97%),

81

FeSO4·7H2O (Purity ≥ 99%), ammonia water (28.0-30.0% NH3 basis) have been

82

obtained from Sigma-Aldrich and used without further purification. Glycerol and

83

Cetyl PEG/PPG-10/1 Dimethicone Abil EM90 have been supplied by Macron Chem.

84

and Evonik Co., respectively.

85

Microfluidic setup

86

The microfluidic device is composed of coaxially aligned tapered cylindrical glass

87

capillaries, inserted into a square capillary and fixed on a glass slide. The schematic of

88

the flow-focusing capillary-based microfluidic device is shown in Figure 1. Prior to

89

inserting the cylindrical capillaries into the square capillary, we taper them using a 3

ACS Paragon Plus Environment

(W201502-SAMPLE),

Langmuir

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 18

90

micropipette puller to create a desired orifice diameter. The square capillary serves as

91

a flow channel for the outer fluid stream and also facilitates the alignment of

92

cylindrical capillaries. The left and right cylindrical capillaries serve as injection and

93

collection tubes, respectively.

94 95

Figure 1 Schematic of a co-flow glass capillary-based microfluidic device. Off-chip

96

crosslinking was achieved by keeping the tip of the collecting tube in contact with the

97

interface of a hot collecting solution, composed of barium acetate mixed with glycerol

98

aqueous solution. Mushroom-like and Janus microgels are fabricated from droplets of

99

300 µm and 150 µm diameter, respectively. The droplets were produced within the

100

glass capillary microfluidic device at room temperature (~25

) and collected into

101

glass beakers containing 4 mL of collecting solutions. The temperature of the

102

collecting solution was maintained at 45

103

The glass beakers were covered with aluminum foil during this process to minimize

104

the evaporation of water.

105

Formation of droplets

106

Aqueous solutions of pNIPAAm/sodium alginate are emulsified in continuous

107

Hexadecane oil phase containing 5 wt% Abil EM 90 that serves as surfactant (Figure

108

S1). The collecting aqueous solutions are composed of 10 wt% barium acetate and

using a hot plate for at least 12 hours.

4

ACS Paragon Plus Environment

Page 5 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Langmuir

109

0-40 wt% glycerol. The flow rates of the dispersed and continuous phases are fixed at

110

150 µL/h and 3000 µL/h, respectively.

111

Mushroom-like microgels are fabricated from initial droplets of about 300 µm

112

diameter. The orifice diameter of the injecting tube is about 80 µm, and the orifice

113

diameter of the collecting tube is 310 µm. Experiments are performed for 1 wt%

114

pNIPAAm/1wt% SA and 2 wt% pNIPAAm/1wt% SA. Larger concentrations of

115

pNIPAAm and sodium alginate lead to higher drop viscosity and formation of

116

spherical particles. Droplets are collected in glass beakers containing aqueous solution

117

of 10 wt% barium acetate and different glycerol concentrations. The collecting

118

beakers are placed on a hot plate, whose temperature is kept at 45 °C. After about 12

119

hours, the resultant fully crosslinked microgels are brought to the room temperature

120

for further characterization.

121

Janus microgels are formed out of initial droplets of 150 µm or smaller. In this case,

122

the orifice diameter of the injecting tube is 60 µm and the orifice diameter of the

123

collecting tube is 200 µm. The aqueous phase has the same composition as in the case

124

of mushroom-like microgels.

125

To observe droplet deformation at the air-water interface, we collect droplets in a

126

Polystyrene Cuvette (VWR-5ml) containing 2 mL of collecting solution. To perform

127

the temperature control experiment, we place the cuvette inside a thermostatic water

128

bath with a constant temperature of 45 °C. The high speed camera (SA4 Fastcam,

129

Photron) was focused at the interface of air and the collecting solution to monitor the

130

droplets evolution process. To investigate the effect of droplet size, we utilize

131

microfluidic devices with different injection and collection orifice sizes and we

132

operate them under the same flow rates.

133

Scanning Electron Microscope (SEM) measurements

134

To prepare samples for SEM characterization, we wash and freeze-dried Janus

135

microgels. In a typical experiment, we transferred crosslinked 150 µm microgels into

136

a 10 mL centrifuge tube and centrifuged them at 2000 rpm for 2 min. The supernatant

137

is removed and de-ionized water is added into the centrifuge tube followed by

138

redispersion of microgels; the procedure is repeated 3 times. A drop of water 5

ACS Paragon Plus Environment

Langmuir

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 6 of 18

139

containing purified microgels is put on a cleaned glass wafer (~8 mm×8 mm) and

140

freeze-dried for 2 days. The freeze-dried samples are analyzed by a Field

141

Emission-Scanning Electron Microscope (FE-SEM, Magellan 400) at a speed voltage

142

of 3 KV.

143



RESULTS AND DISCUSSIONS

144

The monodispersed droplets created inside the microfluidic device and collected in

145

collecting solutions are shown in the optical images in Fig. S1. The droplets exiting

146

the collecting tube are slowed down at the interface of the collecting solution because

147

their density is less than the density of the collecting solution (Table S1). The droplets

148

deform and crosslink at the interface, and finally settle to the bottom of the beaker,

149

which is in agreement with previous reports.40-42

150

Mushroom-like microgels

151

The mushroom-like microgels are formed out of 300 µm droplets. The observed

152

mushroom shape has been reported for pure alginate hydrogel particles in a previous

153

report.40 The shape is generated by the slow transition of the initially spherical

154

droplets at the oil/collecting solution interface and by the accompanying crosslinking

155

of the alginate via the inwards diffusion of Ba2+.41-42

156

to the sodium alginate, droplets are composed of linear pNIPAAm polymer, which is

157

one of the most widely used temperature responsive polymers, possessing a low

158

critical solution temperature (LCST) of approximately 32°C. When the temperature of

159

droplets increases above the LCST, the linear polymer undergo a coil-to-globule

160

transition and shrinks, while below the LCST the polymer chain shows a swelling

161

state. 43 Use of alcohol can results in pNIPAAm aggregation and limits its diffusivity44.

162

Consequently, we employ glycerol within the collection bath to further control the

163

morphology of microgels. This approach also enables us to tune the transparency of

164

the resultant microgels selectively due to aggregation and formation of pNIPAAm

165

microparticles within the main matrix (Figure S2). This indicates that both the

166

temperature and glycerol cause the pNIPAAm chains to shrink, and lead to a change

167

in the refractive index of the pNIPAAm/SA droplets. When the pNIPAAm/SA

168

droplets flow out of the collecting tube and contact the hot collecting solutions, the

In the present study, in addition

6

ACS Paragon Plus Environment

Page 7 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Langmuir

169

pNIPAAm chain instantly shrinks into a globule state, accompanied by a change in

170

the refractive index from 1.32 to 1.39. 45 Thus, the collapsed pNIPAAm shows darker

171

contrast due to light scattering of the aggregates and the refractive index mismatch

172

with water (nwater = 1.33). In addition, the coiled pNIPAAm is gradually entrapped into

173

the alginate network undergoing an ionic crosslinking process. Figure 2a shows

174

microgels formed using a glycerol-free collecting solution. In this case, the resultant

175

microgels exhibit an almost transparent mushroom shape. The transparent microgels

176

indicate that little to no coiled pNIPAAm is entrapped in this case. When collected in

177

40 wt% glycerol-collecting solutions, the microgels exhibit a mushroom shape with

178

large amounts of interior black dots. These black dots in the mushroom microgels are

179

pNIPAAm globules that are aggregated due to the addition of glycerol (Figure 2e).

180

This phenomenon may be attributed to the diffusion of glycerol into the

181

pNIPAAm/SA droplets and increase in the viscosity of the droplet. The inward

182

diffusion of glycerol into the droplets limits the mobility of pNIPAAm globules and

183

force them to form larger aggregates, resulting in a homogeneous entrapment of

184

pNIPAAm particles (3~5 µm) in the resultant microgels. Different concentration of

185

glycerol gives rise to different inward diffusion velocities and consequently different

186

amount of aggregates. As a result, different features are observed for individual

187

microgels collected in different glycerol concentrations. The mushroom microgel

188

droplets collected in 10 wt% glycerol solutions display two different optical contrasts

189

for each microgel, with one half nearly transparent, while the other half being opaque

190

(Figure 2b). The different contrast is attributed to the inhomogeneous distribution of

191

pNIPAAm aggregates. With increasing glycerol concentration, the mushroom-like

192

microgels gradually show a homogeneous optical contrast (Figure 2c-e). This

193

phenomenon suggests that higher glycerol concentration in the collecting solution

194

inhibit the migration of pNIPAAm globules in the droplets, and as a result, the

195

pNIPAAm particles will be uniformly distributed in the mushroom microgels.

196

Not only is the microgels’ optical properties influenced by the collecting solutions,

197

but their geometry also changes as a function of glycerol concentration in the

198

collecting solutions. The geometric factor is defined here, as the length ratio of the 7

ACS Paragon Plus Environment

Langmuir

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

199

distance between the poles (defined as L) to the diameter of the equator (defined as B),

200

shown in the inset of Figure 2k. Clearly, the geometric factor decreases with the

201

increase of glycerol concentration in the collecting solutions. The geometric factor

202

falls within the interval 0.70~0.90 (Figure 2k), and continues to decrease with

203

increasing glycerol concentration. By increasing the velocity of a continuous phase, a

204 205

Figure 2. (a-e) Optical microscope images of microgels formed out of 300 µm

206

diameter droplets, composed of 1 wt% pNIPAAm and 1 wt% sodium alginate and

207

collected in collecting solutions with different glycerol concentrations: 0, 10 wt%, 20

208

wt%, 30 wt% to 40 wt%. (f-j) Optical microscope images of microgels formed out of

209

300 µm diameter droplets, composed of 2 wt% pNIPAAm and 1 wt% sodium alginate,

210

collected in solutions with different glycerol concentrations: 0, 10 wt%, 20 wt%, 30

211

wt% to 40 wt%. (k) The plot shows the geometric factor for different glycerol

212

concentrations. All the samples were heated for 12 hours and then cooled down. All

213

the images were taken at the room temperature. 8

ACS Paragon Plus Environment

Page 8 of 18

Page 9 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Langmuir

214

droplet falling into the interface shows greater degree of deformability, which

215

provides another level of control to microgel geometry12.

216

Similarly, when the concentration of pNIPAAm inside of the droplets was increased to

217

2 wt%, more globule pNIPAAm were entrapped inside of the resultant microgels,

218

compared to that of 1 wt% pNIPAAm. Figure 2f-j show the optical microscope

219

images of microgels obtained from 2 wt% pNIPAAm/1 wt% SA droplets. As shown in

220

Figure 2f-j, the microgels collected in the same glycerol collecting solution possesses

221

higher contrast value compared to that of Figure 2a-e. The higher contrast was

222

attributed to the higher amount of globule pNIPAAm entrapped in the microgels.

223

Janus microgels

224

By controlling the droplet size, we can also control the microgel morphology and

225

obtain Janus shape particles. In the present experiment, when the initial droplet

226

diameter is decreased to 175 µm or below, the resultant microgels show Janus

227

morphology rather than the mushroom-like morphology formed out of 300 µm initial

228

droplets. When the initial droplet diameter is below this critical value, Janus particles

229

form, whereas above this value, the resultant microgels show mushroom morphology

230

(Figure S4). We attribute this change in the microgel morphology to the combined

231

effects of two factors: a) smaller droplets experience a greater extent of phase

232

separation between pNIPAAm and SA and possess pNIPAAm-rich and SA-rich

233

regions, prior to touching (impacting) the collecting solution interface46-47, and b) the

234

viscosity, surface tension and osmotic pressure difference between drops and the

235

collecting solution. The collecting solutions with higher glycerol concentrations

236

possess higher viscosity and lower interfacial tension, these properties result in a

237

greater degree of deformability in drops upon impacting the interface. Smaller

238

droplets tend to form Janus particles because they are more difficult to deform due to

239

their larger Laplace Pressure difference. The Laplace Pressure difference can be

240

calculated by the following equation ∆ =

 

, where  is the interfacial tension

241

between the droplet and outer oil phase, and is the droplet radius. We used the

242

pendant drop method to measure the surface tension between aqueous solution of 9

ACS Paragon Plus Environment

Langmuir

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

243

sodium alginate (2 wt%) and pNIPAAm (1 wt%) and hexadecane containing 5 wt. %

244

Abil EM90. The measured  is 2.35 mN / m , and the ∆ values of the 150 µm and

245

300 µm droplets are 31.33 Pa and 15.66 Pa, respectively. Larger droplets are easily

246

deformed to a mushroom shape under the driving force of Osmotic pressure

247

difference (the minimum osmotic pressure of the collecting solutions is ~ 390 mOsm,

248

which is much higher than that of droplet’s osmotic pressure (~ 10 mOsm)) between

249

inside and outside of droplets, as shown in Figure 2. Janus microgels collected in

250

different glycerol concentrations demonstrate different geometry as shown in Figure 3.

251

Figure 3a-e and Figure 3f-j represent the microgels fabricated out of droplets of 1wt%

252

pNIPAAm/1wt% SA and 2 wt% pNIPAAm/1 wt% SA, respectively. Both images

253

show the resultant microgels with two distinguishable parts: a relatively smaller part,

254

which exhibits a darker contrast, richer in pNIPAAm, and a relatively larger

255

alginate-rich part. The formation of two different phases is caused by the gradual

256

phase separation of pNIPAAm inside the droplets when in contact with the hot

257

collecting solutions (Figure S5). Compared to the larger droplets, i.e., 300 µm

258

diameter droplets, the pNIPAAm chain in smaller droplets more easily migrate to the

259

other side of the droplets and result in Janus morphology. The glycerol and the effect

260

of heat could both induce the pNIPAAm chains to shrink into a globule state (Figure

261

S2-4). Interestingly, the resultant microgels in glycerol-free collecting solutions only

262

show the convex alginate dominant part (Figure 3a and 3f). This is due to the phase

263

separation of pNIPAAm and SA within the droplets. However, the size of

264

pNIPAAm-rich part gradually decreases with increasing the glycerol concentration of

265

the collecting solution due to the entrapment of some of the coiled pNIPAAm in the

266

alginate-rich side, as shown in Figure 3b-e and 3 g-j. To quantify the relative volume

267

change of the two parts, we define the volume ratio as V1/V2 (V1 and V2 denote the

268

volumes of pNIPAAm-rich and alginate-rich parts, respectively). Similar to the

269

geometric factor for the mushroom-shaped microgels, the volume ratio of Janus

270

particles decreases with increasing the glycerol concentration of the collecting

271

solutions (See Figure 3k). The volume ratio decreased from the initial values of 0.20

272

and 0.23 for 10 wt% glycerol collecting solutions to the final values of 0.11 and 10

ACS Paragon Plus Environment

Page 10 of 18

Page 11 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Langmuir

273

nearly 0.02 for 40 wt% glycerol collecting solutions. The decrease is attributed to the

274

inward diffusion of glycerol from the collecting solutions into the droplets, which

275

hinders the pNIPAAm separation from the main droplets and leads to the uniform

276

distribution of pNIPAAm globules inside the microgels at high concentrations of

277

glycerol collecting solutions. Furthermore, the phase separation process is inhibited

278

by higher sodium alginate concentrations in the droplets (Figure S6, S7).

279 280

Figure 3. (a-e). Optical microscope images of microgels formed out of droplets of

281

150 µm diameter composed of 1 wt% pNIPAAm and 1 wt% sodium alginate and

282

collected in collecting solutions of different glycerol concentrations: 0, 10wt%, 20

283

wt%, 30 wt% to 40wt%. (f-j) Optical microscope images of microgels formed out of

284

droplets of 150 µm diameter composed of 2 wt% pNIPAAm and 1 wt% sodium

285

alginate and collected in collecting solutions of different glycerol concentrations: 0,

286

10 wt%, 20 wt%, 30 wt% to 40 wt%. (k) The plot shows the volume ratio for Janus

287

particles for different glycerol concentration of the collecting solutions.

11

ACS Paragon Plus Environment

Langmuir

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

288 289

Figure 4. Scanning Electron Microscope (SEM) images of microgels collected in

290

different concentrations of glycerol solutions: (a) 0; (b) 10 wt%; (c) 20 wt%; (d) 30

291

wt%; (e) 40 wt%.

292

Figure 4 represents SEM images of alginate-rich part of microgels formed by using

293

collecting solutions of different glycerol concentrations. It can be clearly observed

294

that the surface morphology of the microgel changes with glycerol concentration of

295

the collecting solutions. As shown in the SEM images, the number of dents on the

296

surface increases but their size decreases as the glycerol concentration in the

297

collecting solution increases.

298

Ultrasonication of Janus microgels

299

The present study demonstrates that not only we can controllably fabricate microgels

300

of different geometries by carefully adjusting the composition of collecting solution,

301

but also we can selectively isolate different part of microgel using ultrasonication.

302

Janus microgels formed in collecting solutions containing 10wt% glycerol are purified

303

by centrifugation at 2000 rpm to remove the supernatants. This procedure is repeated

304

2~3 times. The purified microgels are transferred into a 5 mL centrifuge tube and

305

sonicated in an ultrasonicator (VWR, 97043-968) for 1 min. Figure 5 shows the

306

breakup process of the initial Janus microgel formed from 10 wt% glycerol collecting

307

solution. The Janus microgels breakup when they are placed in an ultrasonicator for 1

308

min. The pNIPAAm-rich part is separated from the alginate-rich part due to the weak

309

tangling interaction between alginate molecule chains and pNIPAAm molecule

310

chains.48 Once further sonicated, the separated pNIPAAm-rich part gradually

311

dissolves (as illustrated by red arrows in Figure 5d). The pNIPAAm is a water soluble

312

polymer and gradually swells in the aqueous solution and the collapsed pNIPAAm

313

chains recover their coil structure. The same behavior is observed when Janus 12

ACS Paragon Plus Environment

Page 12 of 18

Page 13 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Langmuir

314

particles are fabricated using higher glycerol concentrations (such as 50wt% and

315

60wt%, corresponding to Figure S5 c and d, respectively) in the collecting solutions.

316 317

Figure 5. (a) and (c) shows the Janus particles (b) and (d) shows that Janus microgels

318

are broken to two parts by using external ultrasonication. Red arrows in (d) illustrate

319

disintegrated pNIPAAm. The experiment was conducted at the room temperature.

320



CONCLUSIONS

321

In summary, we report a simple method to fabricate pNIPAAm/sodium alginate

322

microgels through single emulsion generated in microfluidics combined with an

323

external ionic crosslinking process. Monodispersed droplets composed of linear

324

pNIPAAm and sodium alginate are collected in hot collecting solutions of barium

325

acetate and glycerol at different concentrations. Starting out of initial droplets of 300

326

µm and 150 µm in diameter, mushroom-like and Janus microgels can be attained. The

327

geometric factor and optical properties of the mushroom-like microgels can be simply

328

tuned by changing the glycerol concentration of the collecting solutions. Similarly, by

329

varying the glycerol concentration of the collecting solutions, the relative volume

330

ratio and the surface roughness of the Janus microgels can be varied. The Janus

331

microgels can be broken to two parts by using ultrasound and can be potentially

332

extended to other stimulus responsive materials. The resultant microgels may be

333

applied in novel optical materials, superstructure microgels, target drug delivery

334

materials, lock-key particles and highly efficient cell attachment (or regenerative 13

ACS Paragon Plus Environment

Langmuir

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

335

medicine).

336



ASSOCIATED CONTENT

337



Supporting Information

338

Supporting Information including the microfluidic fabrication of droplets and

339

other supplementary data are available free of charge at http://pubs.acs.org.

340

AUTHOR INFORMATION

341

Corresponding Author

342

*E-mail: [email protected]

343

Notes

344

The authors declare no conflict of interest.

345

ACKNOWLEDGEMENTS

346

This work was supported by the NSF Grant No. CBET-1150348. We thank Notre

347

Dame Integrated Imaging Facility Centre for the SEM measurements.

348



349 350 351 352 353 354 355 356 357 358 359 360 361 362 363 364 365 366 367 368 369 370

1.

REFERENCES

Velev, O. D.; Lenhoff, A. M.; Kaler, E. W. A class of microstructured particles through colloidal

crystallization. Science 2000, 287,2240-2243. 2.

Sacanna, S.; Korpics, M.; Rodriguez, K.; Colon-Melendez, L.; Kim, S. H.; Pine, D. J.; Yi, G. R.

Shaping colloids for self-assembly. Nat. Commun. 2013, 4,1688. 3.

Roh, K. H.; Martin, D. C.; Lahann, J. Biphasic Janus particles with nanoscale anisotropy. Nat.

Mater. 2005, 4,759-763. 4.

Zhao, Y.; Gu, H.; Xie, Z.; Shum, H. C.; Wang, B.; Gu, Z. Bioinspired multifunctional Janus

particles for droplet manipulation. J. Am. Chem. Soc. 2013, 135,54-57. 5.

Nisisako, T.; Torii, T.; Takahashi, T.; Takizawa, Y. Synthesis of monodisperse bicolored janus

particles with electrical anisotropy using a microfluidic co-flow system. Adv. Mater. 2006,

18,1152-1156. 6.

Yin, S. N.; Wang, C. F.; Yu, Z. Y.; Wang, J.; Liu, S. S.; Chen, S. Versatile bifunctional

magnetic-fluorescent responsive Janus supraballs towards the flexible bead display. Adv. Mater. 2011,

23,2915-2919. 7.

Wu, L. Y.; Ross, B. M.; Hong, S.; Lee, L. P. Bioinspired nanocorals with decoupled cellular

targeting and sensing functionality. Small 2010, 6,503-507. 8.

Walther, A.; Hoffmann, M.; Muller, A. H. Emulsion polymerization using Janus particles as

stabilizers. Angew. Chem. Int. Ed. Engl. 2008, 47,711-714. 9.

Zhao, Y.; Shum, H. C.; Chen, H.; Adams, L. L.; Gu, Z.; Weitz, D. A. Microfluidic generation of

multifunctional quantum dot barcode particles. J. Am. Chem. Soc. 2011, 133,8790-8793. 10. Pregibon, D. C.; Toner, M.; Doyle, P. S. Multifunctional encoded particles for high-throughput 14

ACS Paragon Plus Environment

Page 14 of 18

Page 15 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Langmuir

371 372 373 374 375 376 377 378 379 380 381 382 383 384 385 386 387 388 389 390 391 392 393 394 395 396 397 398 399 400 401 402 403 404 405 406 407 408 409 410 411 412 413 414

biomolecule analysis. Science 2007, 315,1393-1396. 11. Lee, K. J.; Yoon, J.; Rahmani, S.; Hwang, S.; Bhaskar, S.; Mitragotri, S.; Lahann, J. Spontaneous shape reconfigurations in multicompartmental microcylinders. Proc. Natl. Acad. Sci. U. S. A. 2012,

109,16057-16062. 12. Hu, Y.; Wang, J.; Li, C.; Wang, Q.; Wang, H.; Zhu, J.; Yang, Y. Janus photonic crystal microspheres: centrifugation-assisted generation and reversible optical property. Langmuir 2013,

29,15529-15534. 13. Shang, L.; Shangguan, F.; Cheng, Y.; Lu, J.; Xie, Z.; Zhao, Y.; Gu, Z. Microfluidic generation of magnetoresponsive Janus photonic crystal particles. Nanoscale 2013, 5,9553-9557. 14. Maeda, K.; Onoe, H.; Takinoue, M.; Takeuchi, S. Controlled synthesis of 3D multi-compartmental particles with centrifuge-based microdroplet formation from a multi-barrelled capillary. Adv. Mater.

2012, 24,1340-1346. 15. Kang, D. H.; Jung, H. S.; Ahn, N.; Yang, S. M.; Seo, S.; Suh, K. Y.; Chang, P. S.; Jeon, N. L.; Kim, J.; Kim, K. Janus-Compartmental Alginate Microbeads Having Polydiacetylene Liposomes and Magnetic Nanoparticles for Visual Lead(II) Detection. ACS Appl. Mater. Inter. 2014, 6, 10631-10637. 16. Liu, S.; Deng, R.; Li, W.; Zhu, J. Polymer Microparticles with Controllable Surface Textures Generated through Interfacial Instabilities of Emulsion Droplets. Adv. Funct. Mater. 2012,

22,1692-1697. 17. Berger, S.; Ionov, L.; Synytska, A. Engineering of Ultra-Hydrophobic Functional Coatings Using Controlled Aggregation of Bicomponent Core/Shell Janus Particles. Adv. Funct. Mater. 2011,

21,2338-2344. 18. Dendukuri, D.; Pregibon, D. C.; Collins, J.; Hatton, T. A.; Doyle, P. S. Continuous-flow lithography for high-throughput microparticle synthesis. Nat. Mater. 2006, 5,365-369. 19. Suh, S. K.; Yuet, K.; Hwang, D. K.; Bong, K. W.; Doyle, P. S.; Hatton, T. A. Synthesis of nonspherical superparamagnetic particles: in situ coprecipitation of magnetic nanoparticles in microgels prepared by stop-flow lithography. J. Am. Chem. Soc. 2012, 134,7337-7343. 20. Kim, S. H.; Abbaspourrad, A.; Weitz, D. A. Amphiphilic crescent-moon-shaped microparticles formed by selective adsorption of colloids. J. Am. Chem. Soc. 2011, 133,5516-5524. 21. Hakimi, N.; Tsai, S. S.; Cheng, C. H.; Hwang, D. K. One-step two-dimensional microfluidics-based synthesis of three-dimensional particles. Adv. Mater. 2014, 26,1393-1398. 22. Shah, R. K.; Kim, J.-W.; Weitz, D. A. Janus Supraparticles by Induced Phase Separation of Nanoparticles in Droplets. Adv. Mater. 2009, 21,1949-1953. 23. Kim, J. H.; Jeon, T. Y.; Choi, T. M.; Shim, T. S.; Kim, S. H.; Yang, S. M. Droplet microfluidics for producing functional microparticles. Langmuir 2014, 30,1473-1488. 24. Prasad, N.; Perumal, J.; Choi, C.-H.; Lee, C.-S.; Kim, D.-P. Generation of Monodisperse Inorganic-Organic Janus Microspheres in a Microfluidic Device. Adv. Funct. Mater. 2009,

19,1656-1662. 25. Jiang, K.; Xue, C.; Arya, C.; Shao, C.; George, E. O.; Devoe, D. L.; Raghavan, S. R. A new approach to in-situ "micromanufacturing": microfluidic fabrication of magnetic and fluorescent chains using chitosan microparticles as building blocks. Small 2011, 7,2470-2476. 26. Chen, Y.; Nurumbetov, G.; Chen, R.; Ballard, N.; Bon, S. A. Multicompartmental Janus microbeads from branched polymers by single-emulsion droplet microfluidics. Langmuir 2013,

29,12657-12662. 27. Kim, J.; Vanapalli, S. A. Microfluidic production of spherical and nonspherical fat particles by 15

ACS Paragon Plus Environment

Langmuir

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

415 416 417 418 419 420 421 422 423 424 425 426 427 428 429 430 431 432 433 434 435 436 437 438 439 440 441 442 443 444 445 446 447 448 449 450 451 452 453 454 455 456 457 458

thermal quenching of crystallizable oils. Langmuir 2013, 29,12307-12316. 28. Deng, N. N.; Wang, W.; Ju, X. J.; Xie, R.; Weitz, D. A.; Chu, L. Y. Wetting-induced formation of controllable monodisperse multiple emulsions in microfluidics. Lab Chip 2013, 13,4047-4052. 29. Yu, Y.; Wen, H.; Ma, J.; Lykkemark, S.; Xu, H.; Qin, J. Flexible fabrication of biomimetic bamboo-like hybrid microfibers. Adv. Mater. 2014, 26,2494-2499. 30. Lone, S.; Kim, S. H.; Nam, S. W.; Park, S.; Joo, J.; Cheong, I. W. Microfluidic synthesis of Janus particles by UV-directed phase separation. Chem. Commun. (Camb.) 2011, 47,2634-2636. 31. Tumarkin, E.; Kumacheva, E. Microfluidic generation of microgels from synthetic and natural polymers. Chem. Soc. Rev. 2009, 38,2161-2168. 32. Seiffert, S.; Romanowsky, M. B.; Weitz, D. A. Janus microgels produced from functional precursor polymers. Langmuir 2010, 26,14842-14847. 33. Hwang, D. K.; Oakey, J.; Toner, M.; Arthur, J. A.; Anseth, K. S.; Lee, S.; Zeiger, A.; Van Vliet, K. J.; Doyle, P. S. Stop-flow lithography for the production of shape-evolving degradable microgel particles. J. Am. Chem. Soc. 2009, 131,4499-4504. 34. Seo, K. D.; Doh, J.; Kim, D. S. One-step microfluidic synthesis of Janus microhydrogels with anisotropic thermo-responsive behavior and organophilic/hydrophilic loading capability. Langmuir

2013, 29,15137-15141. 35. Ma, S.; Thiele, J.; Liu, X.; Bai, Y.; Abell, C.; Huck, W. T. Fabrication of microgel particles with complex shape via selective polymerization of aqueous two-phase systems. Small 2012, 8,2356-2360. 36. Marquis, M.; Renard, D.; Cathala, B. Microfluidic generation and selective degradation of biopolymer-based Janus microbeads. Biomacromolecules 2012, 13,1197-1203. 37. Zhao, L. B.; Pan, L.; Zhang, K.; Guo, S. S.; Liu, W.; Wang, Y.; Chen, Y.; Zhao, X. Z.; Chan, H. L. Generation of Janus alginate hydrogel particles with magnetic anisotropy for cell encapsulation. Lab

Chip 2009, 9,2981-2986. 38. Lu, A. X.; Jiang, K.; DeVoe, D. L.; Raghavan, S. R. Microfluidic assembly of Janus-like dimer capsules. Langmuir 2013, 29,13624-13629. 39. Choi, C. H.; Weitz, D. A.; Lee, C. S. One step formation of controllable complex emulsions: from functional particles to simultaneous encapsulation of hydrophilic and hydrophobic agents into desired position. Adv. Mater. 2013, 25,2536-2541. 40. Mele, E.; Fragouli, D.; Ruffilli, R.; De Gregorio, G. L.; Cingolani, R.; Athanassiou, A. Complex architectures formed by alginate drops floating on liquid surfaces. Soft Matter 2013, 9,6338-6343. 41. Lin, Y. S.; Yang, C. H.; Hsu, Y. Y.; Hsieh, C. L. Microfluidic synthesis of tail-shaped alginate microparticles using slow sedimentation. Electrophoresis 2013, 34,425-431. 42. Capretto, L.; Mazzitelli, S.; Balestra, C.; Tosi, A.; Nastruzzi, C. Effect of the gelation process on the production of alginate microbeads by microfluidic chip technology. Lab Chip 2008, 8,617-621. 43. Schild, H. G. Poly (N-Isopropylacrylamide) - Experiment, Theory and Application. Progress in

Polym. Sci. 1992, 17,163-249. 44. Shimizu, S.; Kimura, M.; Maruyama, T.; Kurita, K. Studies on interaction parameters of poly(N-isopropylacrylamide) in 1-propanol-water mixtures by small-angle X-ray scattering. J. Appl.

Crystallogr. 1997, 30,712-716. 45. Garner, B. W.; Cai, T.; Ghosh, S.; Hu, Z.; Neogi, A. Refractive Index Change Due to Volume-Phase Transition in Polyacrylamide Gel Nanospheres for Optoelectronics and Bio-photonics.

Appl. Phys. Express 2009, 2,057001. 46. Hirama, H.; Kambe, T.; Aketagawa, K.; Ota, T.; Moriguchi, H.; Torii, T. Hyper alginate gel 16

ACS Paragon Plus Environment

Page 16 of 18

Page 17 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Langmuir

459 460 461 462 463 464 465

microbead formation by molecular diffusion at the hydrogel/droplet interface. Langmuir 2013,

29,519-524. 47. Zhang, H.; Tumarkin, E.; Peerani, R.; Nie, Z.; Sullan, R. M.; Walker, G. C.; Kumacheva, E. Microfluidic production of biopolymer microcapsules with controlled morphology. J. Am. Chem. Soc.

2006, 128,12205-12210. 48. Shi, J.; Alves, N. M.; Mano, J. F. Drug release of pH/temperature-responsive calcium alginate/poly(N-isopropylacrylamide) semi-IPN beads. Macromol. Biosci. 2006, 6,358-363.

466 467 468 469 470 471 472 473 474 475 476 477 478 479 480 481 482 483 484 485 486 487 488 489 490 491 492 493 494 495 496 497 498 499 500 501 502 17

ACS Paragon Plus Environment

Langmuir

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

503

Table of Contents graphic

504

18

ACS Paragon Plus Environment

Page 18 of 18