Subscriber access provided by University of Winnipeg Library
Article
Porous, Aligned and Biomimetic Fibers of Regenerated Silk Fibroin Produced by Solution Blow Spinning Adrian Magaz, Aled D. Roberts, Sheida Faraji, Tatiana R. L. Nascimento, Eliton S Medeiros, Wenzhao Zhang, Ryan D. Greenhalgh, Andreas Mautner, Xu Li, and Jonny J. Blaker Biomacromolecules, Just Accepted Manuscript • DOI: 10.1021/acs.biomac.8b01233 • Publication Date (Web): 02 Nov 2018 Downloaded from http://pubs.acs.org on November 3, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 39 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
Porous, Aligned and Biomimetic Fibers of Regenerated Silk
2
Fibroin Produced by Solution Blow Spinning
3
Adrián Magaz1,2†, Aled D. Roberts1†, Sheida Faraji1, Tatiana R.L. Nascimento3, Eliton
4
S. Medeiros3, Wenzhao Zhang1, Ryan D. Greenhalgh1⊥, Andreas Mautner4, Xu Li2,5*,
5
Jonny J. Blaker1*
6
1
7
Manchester, United Kingdom
8
2
9
Technology and Research (A*STAR), Singapore
Bio-Active Materials Group, School of Materials, The University of Manchester,
Institute of Materials Research and Engineering (IMRE), Agency for Science,
10
3
11
Universidade Federal da Paraíba, João Pessoa, Brazil
12
4
13
Research, University of Vienna, Vienna, Austria
14
5
Laboratory of Materials and Biosystems, Department of Materials Engineering,
Polymer and Composite Engineering Group, Institute of Materials Chemistry and
Department of Chemistry, National University of Singapore, Singapore
15
Present address: ⊥Department of Physiology, Development and Neuroscience,
16
University of Cambridge, United Kingdom
17
18
†Equal author contribution *Corresponding authors:
Jonny J. Blaker
Li Xu
School of Materials
Institute
of
Materials
Research
and 1
ACS Paragon Plus Environment
Biomacromolecules 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The University of Manchester
Engineering (IMRE)
Manchester, M13 9PL, UK
Singapore, 138634
tel. +44(0)161 3063578
tel. +65 64168933
e-mail:
[email protected] e-mail:
[email protected] Page 2 of 39
19 20
Abstract
21
Solution blow spinning (SBS) has emerged as a rapid and scalable technique for the
22
production of polymeric and ceramic materials into micro/nano- fibers. Here, SBS was
23
employed to produce sub-micron fibers of regenerated silk fibroin (RSF) from Bombyx
24
mori (silkworm) cocoons based on formic acid or aqueous systems. Spinning in the
25
presence of vapor permitted the production of fibers from aqueous solutions, and high
26
alignment could be obtained by modifying the SBS set-up to give a concentrated
27
channeled airflow. The combination of SBS and a thermally induced phase separation
28
technique (TIPS) resulted in the production of macro/micro- porous fibers with 3D
29
interconnected pores. Furthermore, a co-axial SBS system enabled a pH gradient and
30
kosmotropic salts to be applied at the point of fiber formation, mimicking some of the
31
aspects of the natural spinning process, fostering fiber formation by self-assembly of the
32
spinning dope. This scalable and fast production of various types of silk based fibrous
33
scaffolds could be suitable for a myriad of biomedical applications.
34
Keywords: Regenerated silk fibroin, solution blow spinning, fibers, porous fibers,
35
aligned fibers, biomimetic spinning
36 37
1. INTRODUCTION
38
Solution blow spinning (SBS) offers an efficient method to produce micro/nano- fibers 2
ACS Paragon Plus Environment
Page 3 of 39 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1,2
39
at a significantly higher rate (about ×100 times faster
) compared to conventional
40
electrospinning. By using pressurized gas as the driving force,2–5 it overcomes some of
41
the drawbacks of electrospinning including the use of electric fields and dense fibrous
42
networks with low porosities;6–9 in addition, fibers can be deposited in situ on virtually
43
any surface.4 To date, a myriad of polymers,3–5 composites 1,10,11 and ceramics 12,13 have
44
been successfully processed into fibers by SBS. The use of micro/nano- fibers is of
45
particular interest in the field of regenerative medicine due to their high surface area to
46
volume ratio and morphological resemblance to the extracellular matrix of native
47
tissues. Fibers can provide adequate topographical and mechanical cues to direct cell
48
behavior, making them suitable for the fabrication of scaffolds for tissue regeneration.14–
49
16
50
In its native state, Bombyx mori silk consists of fibrous protein filaments (silk fibroin)
51
surrounded by a glue-like layer (sericin). Among the wide range of natural materials,
52
silk fibroin has many attractive chemical, physical, and biological properties which
53
make it convenient for regenerative medicine, tissue engineering and therapeutic
54
delivery applications.17,18 Some of these properties include suitable cell-material
55
interactions, tailored biodegradability and oxygen/water permeability.19–22
56
Under natural spinning conditions, as the silk dope flows from the posterior to the
57
anterior division of the silkworm gland, the dope is sheared, water content decreases
58
from 80 to 77%, pH decreases from 6.9 to 4.8 and chaotropic ions are exchanged for
59
kosmotropic ions,23–29 contributing to fiber formation. Silk fibroin typically requires
60
reprocessing from its native state to tune properties including fiber diameter and surface
61
roughness/morphology to suit the intended application15,30. In particular, regenerated
62
silk fibroin (RSF) from aqueous solutions has previously been electrospun by blending
63
with high molecular weight poly(ethylene oxide) (PEO),21,31,32 used as a temporarily 3
ACS Paragon Plus Environment
Biomacromolecules 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 39
64
water-soluble spinning aid, and fully aqueous processes based on high molecular weight
65
silk fibroin dopes have been successfully produced via electrospinning.33,34 Recently,
66
straining flow spinning (SFS) has been used to produce high performance RSF fibers by
67
controlling the flow of the dope through its interaction with a coagulant bath
68
mimicking the balanced mild aqueous chemical environment and moderate shear forces
69
found in natural spinning glands.35 While robust RSF fibers can be mass-produced by
70
SFS, these range between 8-13 μm in diameter. SBS permits faster production rates (5
71
μL.min−1 in SFS compared with >100 μL.min−1 in SBS) and can even achieve thinner
72
fibers at the nanoscale.
73
The aim of this study is not to produce high performance robust fibers nor retain the
74
hierarchical structures of natural silks, but rather show that SBS is a suitable technique
75
that could be used to mass-produce various types of RSF sub-micron fibers with
76
potential applications in regenerative medicine. Here, to the author’s knowledge we
77
have for the first time employed SBS to process RSF into randomly aligned and aligned
78
non-porous micro/nano- fibers, utilizing both organic (formic acid) and aqueous solvent
79
systems, channeling the flow of air to the collector. Porous fibers from an aqueous
80
system were obtained by using a modified SBS system based on a thermally induced
81
phase-separation (TIPS) technique.1,37 A co-axial SBS system was also employed to
82
mimic a pH gradient as a means to replicate some of the physiological parameters of the
83
natural spinning process26 and drive secondary protein structure formation.
84
2. EXPERIMENTAL SECTION
85
2.1 Regenerated silk fibroin
86
RSF solutions from Bombyx mori silkworm cocoons (Wildfibres; Birmingham, UK)
87
were prepared following a previously described protocol
88
Briefly, cocoons were dewormed and degummed in a 0.02 M boiling Na2CO3 (Sigma-
38
35,36
,
with minor modifications.
4
ACS Paragon Plus Environment
Page 5 of 39 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
89
Aldrich, UK) aqueous solution for 30 min to remove the sericin. Degummed silk fibroin
90
was thoroughly washed in deionized water (three water changes, 20 min each) and air-
91
dried for 24h. The dried degummed silk fibroin was dissolved in 7.9 M aqueous LiBr
92
(Sigma-Aldrich, UK) to form a 16% w/v solution, with gentle continuous stirring at
93
60°C for 4h. The solution was centrifuged (10,000 ×g, 20 min) to remove any residual
94
pupa and dialyzed (3.5kDa MWCO SnakeSkin, ThermoScientific, UK) against 5L of
95
deionized water at 4°C for 3 days, with regular water changes under continuous stirring.
96
The concentration of the RSF solution after water dialysis was ~5-6% w/v. The solution
97
was centrifuged again (10,000 ×g, 20 min), and either freeze-dried for 72h (VirTis
98
BenchTop Pro; New York, USA) or concentrated for further use, described below.
99
2.2 Spinning dope formulations
100
Formic acid dopes as precursors of non-porous fibers were prepared by dissolving
101
freeze-dried RSF in formic acid (95% v/v; Sigma-Aldrich, UK) at a concentration of 8-
102
20% w/v at room temperature and stirred for 2h prior to spinning.
103
Aqueous precursor dopes were prepared by means of reverse dialysis processes.
104
Aqueous formulations as precursors for non-porous fibers were prepared by
105
concentrating an RSF solution by reverse dialysis (10 kDa MWCO SnakeSkin dialysis
106
tubing, Thermo-Scientific, UK) against a 15% w/v polyethylene glycol (PEG 10,000
107
Mw; Sigma-Aldrich, UK) aqueous solution at 4°C. Note that some PEG likely diffused
108
into the RSF solution and may have acted as a spinning aid. Prior to spinning, a 3M
109
CaCl2 (Sigma-Aldrich, UK) solution was added into the RSF system to adjust the [Ca]2+
110
to 0.3 M (~pH 7.5, 9:1 v/v ratio SF/CaCl2). The role of CaCl2 is to promote RSF
111
conformation from random coil/α-helix to β-sheet.39–41 The pH was subsequently
112
adjusted to 10.5 with a 5M NaOH (Sigma-Aldrich, UK) solution, which was found to
113
make the dope stable during the spinning process and promote fiber formation. Aqueous 5
ACS Paragon Plus Environment
Biomacromolecules 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 39
114
formulations as precursors of porous fibers and biomimetic fibers were prepared by
115
concentrating an RSF solution by reverse dialysis (3.5 kDa MWCO SnakeSkin dialysis
116
tubing, Thermo-Scientific, UK) against a 20% w/v PEG (10,000 Mw; Sigma-Aldrich,
117
UK) aqueous solution at 4°C.
118
All solutions were stored in sealed glass vials at 4ºC and spun within 24h.
119
2.3 Rheological analysis of regenerated silk fibroin solutions
120
RSF formulations at increasing concentrations were loaded into an AR-G2 rheometer
121
(TA Systems; UK), operated with a parallel plate geometry (20 mm diameter and gap
122
set to 600 μm) at 25°C and with an environmental case attached to prevent solvent
123
evaporation. Each concentration (n=2 replicates of the same solution) was subjected to a
124
logarithmic steady shear rate increase from 0.01 to 1000 s-1.42
125
2.4 Fiber production by conventional, cryogenic and co-axial solution blow
126
spinning
127
All RSF dopes were spun via a custom made SBS set-up (Scheme 1), consisting of a
128
syringe pump, connective tubing, a concentric nozzle and a compressed air source
129
controlled by a pressure regulator. Solutions were injected to the inner nozzle of the
130
SBS head using a precision syringe driver pump (N-300, New Era Pump Systems Inc.;
131
USA). Compressed air was delivered to the outer nozzle via an oil-free and water-free
132
air compressor (Bambi VT150D; Italy). The internal diameter (ID) of the SBS inner
133
nozzle was 0.8 mm, the outer diameter (OD) was 1.8 mm; the outer nozzle had an ID of
134
2 mm and an OD of 3 mm. The inner nozzle was set to protrude by ≥ +2 mm from the
135
outer nozzle into a conical shaped end.
136
Random non-porous fibers from RSF formulations based on formic acid were spun
137
directly with a conventional SBS apparatus (Scheme 1 a-b): feed rate of 50-60 6
ACS Paragon Plus Environment
Page 7 of 39 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
138
μL.min−1, air pressure of 30-40 psi (0.21-0.28 MPa) and working distance to the
139
collector of 20-30 cm. Production of random non-porous fibers from RSF aqueous
140
dopes was enhanced by spinning through a vapor immediately after the SBS nozzle.
141
Vapor was generated using different solvents (water, absolute ethanol or absolute
142
methanol) in a beaker on a hotplate (100-200°C) placed under the SBS nozzle. Ethanol
143
and methanol are known to promote β-sheet formation. Spinning parameters in this case
144
were: feed rate of 100-110 μL.min−1, air pressure of 30-60 psi (0.21-0.41 MPa) and
145
working distance of 30-40 cm to fiber collection.
146
Aligned non-porous fibers out of formic acid and aqueous systems were obtained by
147
placing a funnel between the SBS head and collector (Scheme 1c). This served to
148
channel the airflow and the fiber forming jet, aligning the fibers in flight prior to
149
collection. The same spinning parameters as previously stated for non-porous fibers
150
were used.
151
Porous fibers were obtained using RSF aqueous dopes based on a cryogenic SBS (cryo-
152
SBS) set-up (Scheme 1d).1,37 As-produced RSF aqueous formulations were sprayed into
153
fibers directly into a bath of liquid nitrogen. The feed rate was 100 μL.min−1 and the air
154
pressure 30 psi (0.21 MPa); a working distance of 15 cm and an angle of ~45° to the
155
cryogenic bath were selected to limit liquid nitrogen loss. The bath container was made
156
from an expanded-polystyrene foam box. During cryo-SBS, the level of liquid
157
nitrogen in the bath was constantly topped up to ensure that the working distance
158
remained ±2 cm of the target value. Frozen fibers were then collected into 50 mL
159
Falcon® tubes, transferred to lyophilization flasks (pre-cooled in liquid nitrogen) and
160
subsequently lyophilized (VirTis BenchTop Pro; New York, US). The external glass
161
portion of the lyophilization flask was kept under liquid nitrogen using the polystyrene
162
foam box until a vacuum of ~50 mTorr was reached, after which the outside of the flask 7
ACS Paragon Plus Environment
Biomacromolecules 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 39
163
was exposed to ambient conditions. Lyophilization was continued for a total of 72h to
164
ensure complete drying. a
Vapor phase Pressure gauge
Pressurized gas
b Air nozzle
Collector
SF solution
Nozzle
Pressurized air
Solution cone
Polymer jet Fiber
Solution pump
c
d
Pressure gauge
Pressure gauge Funnel
Nozzle
Cryogenic bath
Nozzle
e
Air nozzle Outer solution nozzle Inner solution nozzle SF solution
Pressurized air
165
f
Air nozzle Inner solution nozzle Outer solution nozzle
SF solution Outer solution Self-assembly
Pressurized air
Self-assembly
166
Scheme 1 Schematic representation of conventional, cryogenic and co-axial SBS
167
set-ups. (a-b) Conventional SBS set-up (with/without vapor phase). (c) Modified SBS
168
set-up to channel the airflow and RSF fiber jet for spinning aligned non-porous fibers.
169
(d) Cryo-SBS set-up for the production of porous fibers. (e-f) Co-axial SBS set-up to
170
induce a pH-ion gradient by (e) positive and (f) negative inner nozzle solution
171
protrusion.
172
For biomimetic fibers, a co-axial SBS head, consisting of two concentric solution
173
nozzles (inner solution nozzle, outer solution nozzle) within an outer pressurized air
174
nozzle, was employed to induce changes to the chemical environment at the point of the 8
ACS Paragon Plus Environment
Page 9 of 39 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
175
solution cone (positive protrusion of inner solution nozzle, Scheme 1e) or prior to it
176
(negative protrusion of inner solution nozzle, Scheme 1f) by flowing a secondary
177
solution through the outer solution nozzle whilst flowing the RSF solution through the
178
inner solution nozzle. The outer solution nozzle was set to protrude ≥ 2 mm from the
179
outer pressurized air nozzle; the inner solution nozzle was set to protrude ± 2 mm
180
(positively or negatively) from the outer solution nozzle. A number of kosmotropic
181
phosphate solutions adjusted to various acidic pH values (pH 2-7) and a commonly used
182
coagulant in wet-spinning (ammonium sulfate)
183
aqueous RSF solutions into fibers. Two precision syringe driver pumps were used for
184
injecting the inner and outer solutions. Successful fiber spinning was achieved with the
185
following set parameters. For the positive nozzle protrusion, inner and outer solutions
186
were injected at feed rates 100 μL.min−1 and 150 μL.min−1, respectively; for the
187
negative nozzle protrusion, the inner and outer solutions were injected at feed rates of
188
190 μL.min−1 and 100 μL.min−1, respectively. Air pressure and distance to collector
189
were maintained in both cases at 40 psi (0.28 MPa) and 40 cm.
190
2.5 Insolubilization of solution blow spun regenerated silk fibroin fibers
191
Non-woven random fiber mats were immersed in 90% v/v ethanol (EtOH) or 90% v/v
192
methanol (MeOH) baths for 10 min to further induce protein secondary structure
193
transition from α helix/random coils into β-sheets. The mats were then dried in an oven
194
at 30°C for 24h.
195
2.6 Physico-mechanical characterization of the fibers
196
2.6.1 Fiber morphology
197
Fiber morphology was assessed using scanning electron microscopy (SEM) on a Hitachi
198
S300 N (USA) and on a PhenomPro Generation 5 (USA), and field emission scanning
199
electron microscopy on a Zeiss Supra 35VP FE-SEM (Germany). Briefly, fiber mats
22
was used to induce self-assembly of
9
ACS Paragon Plus Environment
Biomacromolecules 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 39
200
(1cm x 1cm) were mounted onto aluminium stubs with double-sided conductive carbon
201
tape and sputter-coated with gold/palladium (Gatan Model 682 Precision Etching
202
Coating System, USA) to an average thickness of 3 nm; images were captured at 2.5-5
203
kV. Average fiber diameter was determined using ImageJ (Fiji 1.28, USA) software, by
204
measuring a minimum of 50 fibers per sample type.
205
2.6.2 Protein structure quantification and crystallinity assessment
206
The conformational structure of non-woven RSF fiber mats was investigated by wide-
207
angle x-ray diffraction (WAXD; PANalytical X’Pert Pro, UK) with the following
208
parameters: copper line focus X-ray tube with Ni kβ absorber (0.02 mm; Kβ=1.392250
209
Å) and Kα radiation (Kα1=1.540598 Å, Kα2=1.544426 Å, Kα ratio 0.5, Kαav=1.541874
211
Å), diffraction angle of 5-45° and scanning rate of 2°.min−1. In addition, a Fourier
212
with an iD5 attenuated total reflectance (ATR) attachment (diamond crystal) was used to
213
examine the conformational changes of the secondary structure of RSF within the amide
214
I region. For each measurement, 32 scans were recorded with a resolution of 4 cm-1 and
215
wavenumbers from 500 to 6000 cm-1. The amide I region ranging from 1600 to 1700
216
cm-1 was baseline corrected and deconvoluted by applying a second derivative
217
algorithm, a signal smoothing algorithm and a curve-fitting algorithm based on Fourier
218
Self-Deconvolution (FSD) according to references
219
at 1595 cm−1 (side chains), 1610 cm−1 (side chains), 1620 cm−1 (intermolecular β-
220
sheets), 1630 cm−1 (intermolecular β-sheets), 1640 cm−1 (random coils), 1650 cm−1
221
(random coils), 1660 cm−1 (α helices), 1670 cm−1 (β-turns), 1680 cm−1 (β-turns), 1690
222
cm−1 (β-turns) and 1700 cm−1 (intramolecular β-sheets) following reference 45. Samples
223
were run in triplicate.
224
2.6.3 Mechanical testing
210
transform infrared spectrometer (FTIR Nicolet iS5; Thermo Scientific, UK) equipped
43,44
. The band positions were fixed
10
ACS Paragon Plus Environment
Page 11 of 39 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
225
Uniaxial tensile testing of as-spun RSF mats (cardboard window frame dimensions of 5
226
mm x 5 mm) of aligned non-porous fibers was performed with a mechanical tester
227
(Instron 3344; Instron Ltd., USA). The ends of the fiber mats were embedded in epoxy
228
and taped to avoid stress concentration at the clamps during mounting to the tensile test
229
machine. Prior to testing, the sides of the window frame were cut through, enabling
230
direct loading of the sample. Samples (n=12 replicates) were subjected to uniaxial loads
231
at 2 mm.min−1, a 10N load cell was used. The strain at break and ultimate tensile
232
strength (UTS) were calculated from the maximum value of the stress-strain curve
233
before breakage, Young’s modulus from the slope of the linear portion of the curve, and
234
toughness from the area under the graph for each sample tested. The area occupied by
235
the fibers was calculated by measuring the area of the mat and subtracting the void
236
space of the fibers based on mass-density differences between the mat and single
237
fibers.46 Instruments were calibrated prior to use and all tests were performed at room
238
temperature.
239
2.6.4 Surface area analysis and fiber pore size
240
Brunauer–Emmett–Teller (BET) surface area measurements of porous fibers obtained
241
by cryo-SBS were made using a surface area and porosity analyzer (TriStar II,
242
Micromeritics, Neu-Purkersdorf, Austria). Prior to gas adsorption experiments,
243
impurities were removed via a degassing step (FlowPrep 060, Micromeritics).
244
Approximately 100 mg of sample was placed inside a glass chamber, purged with
245
nitrogen at ambient temperature overnight. Nitrogen adsorption isotherms were then
246
measured at 77 K.
247
The size of a minimum of 70 pores from SEM images of porous fibers was measured
248
using by ImageJ (Fiji 1.28, USA); measurements were performed in the horizontal
249
direction through the center of the pore. 11
ACS Paragon Plus Environment
Biomacromolecules 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 39
250
2.7 Data analysis
251
Quantitative data is presented as standard deviation (SD) of the mean values. Statistical
252
analysis of the results was performed using GraphPad Prism 7 (San Diego, USA).
253
3. RESULTS AND DISCUSSION
254
3.1 Non-porous RSF fibers obtained via SBS
255
Analysis of the viscoelastic properties of RSF formulations is of interest since solution
256
viscosity determines whether a droplet spray or continuous fibers are obtained, as it
257
affects initial droplet shape and stability of the jet trajectory during SBS.47 The viscosity
258
measurements of RSF formulations of formic acid and the aqueous system at increasing
259
concentrations are shown in Figure 1 a-b. Both systems exhibited slightly different
260
rheologies over the range of concentrations tested. For the case of RSF solutions in
261
formic acid, the viscosities were almost independent of the shear rate exhibiting
262
Newtonian-like behavior. This is consistent with work reported by Zhu et al. for RSF
263
formulations in formic acid below 20% w/v.48 Aqueous RSF formulations, on the other
264
hand, exhibited non-Newtonian shear-thinning-like behavior, more evident at high
265
solution concentrations. Shear-thinning at increasing shear rate is characteristic of
266
native silk dopes49 and suggests more entanglement of the chain networks in the
267
polymer solution,50,51 which should aid spinning by SBS.
268
The solutions over the range of different concentrations were spun via conventional
269
SBS. A systematic investigation found that non-porous fibers only formed for
270
concentrations between 10-18% w/v for solutions based on the formic acid system, and
271
between 25-30% w/v for aqueous solutions in the presence of a water/ethanol/methanol
272
vapor and pH-Ca2+ adjustment as detailed in the experimental section. Solutions lower
273
than 10% and above 18% w/v (formic acid system), or below 25% and above 30% w/v
274
(aqueous system), did not have suitable rheological properties for processing into fibers 12
ACS Paragon Plus Environment
Page 13 of 39
275
by SBS: either the nozzle got blocked frequently or the solutions resulted exclusively in
276
droplets and no fibers were formed. The spinnability windows (Figure 1 c-d) for RSF
277
solutions were established as 15-144 mPa.s (formic acid system) and 500-1500 mPa.s
278
(aqueous system), identified as the target viscosities for blow spinning RSF dopes into
279
non-porous fibers based on formic acid and aqueous systems respectively. a
b
102
Viscosity (Log[Pa.s])
Viscosity (Log[Pa.s])
101 100 10-1 10-2 10-3 100
101
102
102 101 100 10-1 10-2 10-3 100
103
101
Shear rate (Log[1/s])
c
102
103
Shear rate (Log[1/s])
d
2
5x10
3x103 2
4x10
Viscosity (mPa.s)
Viscosity (mPa.s)
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
3x102 2x102 1x102
2x103
1x103
0
0
5
280
281
10
15
20
5
SF concentration (% w/v)
10
15
20
25
30
35
SF concentration (% w/v)
5% w/v
7% w/v
8% w/v
10% w/v
11% w/v
12% w/v
15% w/v
16% w/v
17% w/v
20% w/v
21% w/v
25% w/v
27% w/v
32% w/v
282
Figure 1 Rheology of RSF solutions. (a-b) Shear sweep measurements of (a) formic
283
acid and (b) aqueous RSF solutions at increasing concentrations. Red arrows represent
284
increase in concentration. (c-d) Relationship between viscosity (at 1000 s-1 shear rate)
285
and concentration for (c) formic acid and (d) aqueous solutions, highlighting the
286
spinnability window for SBS; error bars in SD (n=2). 13
ACS Paragon Plus Environment
Biomacromolecules 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 39
287
SEM images of RSF non-porous fibers spun from formic acid are shown at 12 and 15%
288
w/v (Figure 2 a-b, Figure S1). The most stable fiber mats were obtained at a flux of 50-
289
60 μL.min−1 at an air pressure of 30-40 psi (0.21-0.28 MPa) with a working distance of
290
20-30 cm to fiber collection. Increasing the concentration of the RSF formulation
291
resulted in fibers with a greater diameter consistent with previously reported data of
292
solution blow spinning of other polymers.3,52,53 The mean diameter of randomly aligned
293
fibers based on formic acid (Figure 2a, Figure S1a) was 290 (±60) nm and 910 (±300)
294
nm for RSF solution concentrations at 12 and 15% w/v, respectively. Fiber morphology
295
was relatively smooth in both cases. Aligned fiber bundles and mats were also produced
296
at 12% w/v (Figure 2b, Figure S1b) by channeling the airflow towards the collector.
297
Fibers were quickly formed as the RSF solution exited the nozzle and consolidated
298
within less than 5 cm, meaning that by channeling the flow through greater distances
299
fiber alignment could be achieved. Aligned non-porous fibers exhibited a similar mean
300
fiber diameter (p-value non-significant) compared to that of randomly aligned non-
301
porous fibers produced from RSF formulations at the same concentration. The mean
302
fiber diameter in this case was 260 (±150) nm, and fiber morphology was smooth and
303
consistent, with no droplets/beads observed.
14
ACS Paragon Plus Environment
Page 15 of 39 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
304 305
Figure 2 SEM images of RSF non-porous fibers from formic acid and aqueous
306
solutions. (a-b) Fibers spun from formic acid at 12% w/v: (a) randomly aligned fibers;
307
(b) aligned fiber bundle with inset at higher magnification. (c-d) Fibers spun from an
308
aqueous system at 27% w/v through a water vapor: (c) randomly aligned fibers; (d)
309
aligned fibers.
310
For aqueous RSF solutions, the most stable non-porous fibers were obtained at a flux of
311
100-110 μL.min−1 at an air pressure 30-60 psi (0.21-0.41 MPa) and working distance of
312
30-40 cm. SEM images of RSF fibers spun at 27 w/v % are shown in Figure 2 c-d. The
313
structure of the fiber mats consists of non-porous fibers interconnected into a 3D porous
314
non-woven network with some conglutination; with a mean diameter of 410 (±130) nm
315
for randomly aligned fibers (Figure 2c) and 465 (±170) nm for aligned fibers (Figure
316
2d) (p-value non-significant between them). Compared to RSF fibers produced from 15
ACS Paragon Plus Environment
Biomacromolecules 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 39
317
formic acid dopes (Figure 2 a-b), these fibers had poorer morphological homogeneity,
318
which can be attributed to differences in the solvent volatility. Water has a relatively
319
high boiling point and low volatility, resulting in residual moisture content prior to
320
collection.54 In contrast, formic acid is highly volatile, meaning fibers are readily
321
formed as the RSF jets through the SBS nozzle.
322
It should be noted that some low molecular weight PEG likely diffused into the aqueous
323
RSF solutions during reverse dialysis concentration, and that this acted as a spinning aid
324
during SBS promoting fiber formation. A plasticizing effect due to the presence of PEG
325
in polylactide (PLA) blends has been reported,55 considerably increasing the elongation
326
at break, while the tensile strength remained unchanged. Low molecular weight PEG is
327
difficult to spin on its own,56,57 and only its high molecular weight form, PEO, is
328
commonly used during electrospinning of aqueous biopolymer systems due to its higher
329
viscosity that aids stabilizing the polymer jet.
330
PEG is water-soluble and can be easily removed after fiber spinning. RSF solutions for
331
aqueous non-porous fiber spinning were also concentrated up to 30% w/v by forced air-
332
flow and by reverse dialysis in PEG using a 3.5 kDa membrane, yet none of the
333
prepared solutions were able to form fibers, suggesting that concentrations >30% w/v
334
may be required. However, this is disadvantageous for industrial processing due to the
335
easy transition of highly concentrated solutions into gel and clogging of the nozzle.
336
The structure of non-porous fibers was further characterized by ATR-FTIR and WAXD
337
(Figure 3 a-c). Indeed, the conformation and structure of proteins are an important
338
factor in both their physico-chemical and mechanical properties, which ultimately
339
affects their ability to interact with biological interfaces – an important consideration for
340
tissue engineering and therapeutic delivery applications. 16
ACS Paragon Plus Environment
Page 17 of 39 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
341
The ATR-FTIR spectra of the amide I (1700-1600 cm−1) and amide II (1600-1450 cm−1)
342
bands of non-porous fibers spun from formic acid and aqueous solutions are shown in
343
Figure 3a, indicating that the typical chemical composition of silk fibroin remained
344
unaffected during SBS. A clear shift of the absorption peak of the amide I region (1700-
345
1600 cm−1) after post-treatment in ethanol and methanol can be observed.
346 347
A detailed quantification of the amide I band by curve fitting and deconvolution
348
revealed changes in the chain structure (Figure 3c). While β-sheets make up the
349
crystalline regions of silk fibroin, other more flexible structures such as β-turns or
350
random coils and α-helices account for the more amorphous structures of silk.58,59
351
Significantly greater (p