Role of Graphene in Reducing Fatigue Damage in ... - ACS Publications

Jul 19, 2017 - BASF Electronics Materials R&D Center Asia, Suwon, Republic of Korea, ... for Basic Science, Sungkyunkwan University, Suwon, Republic...
0 downloads 0 Views 3MB Size
Subscriber access provided by CARLETON UNIVERSITY

Communication

Role of Graphene in Reducing Fatigue Damage in Cu/Gr Nanolayered Composite Byungil Hwang, Wonsik Kim, Jaemin Kim, Subin Lee, Seoyoen Lim, Sangmin Kim, Sang Ho Oh, Seunghwa Ryu, and Seung Min Jane Han Nano Lett., Just Accepted Manuscript • DOI: 10.1021/acs.nanolett.7b01431 • Publication Date (Web): 19 Jul 2017 Downloaded from http://pubs.acs.org on July 21, 2017

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

Nano Letters is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Nano Letters

Role of Graphene in Reducing Fatigue Damage in Cu/Gr Nanolayered Composite Byungil Hwang‡1, Wonsik Kim‡1, Jaemin Kim2, Subin Lee3, Seoyoen Lim1, Sangmin Kim1, Sang Ho Oh4, Seunghwa Ryu2 and Seung Min Han1* 1. Graduate School of Energy Environment Water and Sustainability, Korea Advanced Institute of Science & Technology, Daejeon, Republic of Korea, 34141 2. Department of Mechanical Engineering & KI for the NanoCentury, Korea Advanced Institute of Science & Technology, Daejeon, Republic of Korea, 34141 3. IBS Center for Integrated Nanostructure Physics (CINAP), Institute for Basic Science, Sungkyunkwan University, Suwon, Republic of Korea, 16419 4. Department of Energy Science, Sungkyunkwan University, Suwon, Republic of Korea, 16419 ‡ These authors contributed equally to this work. *Corresponding author e-mail: [email protected]

ABSTRACT. Nanoscale metal/graphene nanolayered composite is known to have ultra-high strength as the graphene effectively blocks dislocations from penetrating through the metal/graphene interface. The same graphene interface, which has a strong sp2 bonding, can simultaneously serve as an effective interface for deflecting the fatigue cracks that are generated under cyclic bending cycles. In this study, Cu/Gr composite with repeat layer 1

ACS Paragon Plus Environment

Nano Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

spacing of 100 nm was tested for bending fatigue at 1.6% and 3.1% strain up to 1,000,000 cycles that showed for the first time a 5-6 times enhancement in fatigue resistance compared to the conventional Cu thin film. Fatigue cracks that are generated within the Cu layer were stopped by the graphene interface, which are evidenced by cross-sectional SEM and TEM images. Molecular dynamics simulations for uniaxial tension of Cu/Gr showed limited accumulation of dislocations at the film/substrate interface, which makes the fatigue crack formation and propagation through thickness of the film difficult in this materials system. Key words: Cu, graphene, nanolayered, crack, bending, MD simulation

TEXT. With recent developments in flexible and stretchable electronics, advanced materials design that can prevent mechanical failure is critical in ensuring the device reliability. The simplest solution for achieving the required flexibility and stretchability is to make use of all flexible materials; organic light emitting diodes (OLEDs) that are composed of flexible cathode and anode fabricated on a polymer substrate is a good example of all flexible materials design.1-4 In many cases, however, such all flexible, stretchable materials systems may come at the cost of the device performance; poor thermal and chemical stability of the organic materials used in organic field-effect transistors (FETs) is known to cause significant degradation, which is a major limitation that needs to be overcome in comparison to its rigid, inorganic material based counterpart.5-7 One solution for optimizing the device performance and reliability would be to utilize highest performance yet rigid materials for the key device components and to connect them using flexible, stretchable interconnects.8-10 For example, a complementary metal-oxide-semiconductor (CMOS) inverter interconnected with serpentine structured metal electrodes was shown to be highly reliable that can withstand an extreme stretchability of ~140% without any observable degradation of the electrical performance.11, 2

ACS Paragon Plus Environment

Page 2 of 18

Page 3 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Nano Letters

12

Here, the ability of the metal interconnects to withstand repeated, extreme mechanical

strains without fatigue failures is, therefore, the key to achieving high reliability. Metal interconnects used for the flexible electronics applications require robust mechanical properties, and the Institute for Interconnecting and Packaging Electronic Circuits (IPC) standards require the flexible circuit in a mobile phone to undergo more than 1,000,000 sliding and folding motions to test for operational reliability.13 Such repeated motions can cause a fatigue damage via crack formation and propagation in the metal electrode, thereby degrading the electrical properties.14, 15 Even with a small applied strain below the yield point of the metal thin film electrode, dislocations can accumulate on the film/substrate interfaces after a large number of strain cycles; the piled-up dislocations can then cause voids and extrusions, which in turn can cause cracks to be initiated at these regions with high stress concentrations.16-18 For the case of metal thin film or patterned line interconnects, any initiated cracks will quickly propagate through thickness of the metal film to cause failure or degradation of the conductivity of the electrode.15 Therefore, suppressing the crack initiation and propagation is critical for the development of a reliable metal conductor for the flexible electronics applications. Instead of using the traditional metal only interconnects, one can think of using metal/graphene nanolayered composite that can suppress the crack propagation for enhanced resistance to fatigue induced damage. Graphene is known to significantly enhance the strength of the metal when fabricated in the form of a metal/graphene nanolayered composite due to its 2D geometry and outstanding mechanical properties with strength and Young’s modulus of 130 GPa and 1TPa, respectively.19-21 By inserting the graphene layers between the metal thin films, the strength of the metal/graphene composites can be remarkably enhanced19; Cu/Gr and Ni/Gr nanolayered composites with the layer spacing of 70 nm and 3

ACS Paragon Plus Environment

Nano Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 18

100 nm, respectively, showed ultra-high strength of 1.5 GPa and 4.0 GPa under compression, which are 31% and 52% of the respective metal’s theoretical strength given by µ/10.19 Inclusion of high density of interfaces in the form of nano-crystalline22-24 or nano-twinned Cu25, or metal only nanolayered composite such as Cu/Ni26 or Cu/ Nb27 can also contribute to an increase in the initial strength by limiting dislocation motion, but the degree of strengthening is not as pronounced as the Cu/Gr nanolayered system, as explained in the Supporting information 03. Graphene with its strong sp2 bonding is expected to be superior in blocking and deflecting dislocations as well as the fatigue-induced cracks generated within the metal layer. In addition, graphene is a good conductor with electron mobility of ~15,000 cm2V-1S-1 and sheet resistance of ~350 Ohm/sq,19-21,

28, 29

which makes it an excellent

candidate for reinforcing the metal interconnects in the form of metal/graphene nanolayered composite. Therefore, the effect of graphene inclusion in the form of Cu/Gr nanolayers on the fatigue resistance was explored for the first time for potentially replacing the traditional metal interconnects. Large-scale Cu/Gr nanolayered composites were fabricated on polyimide substrate for bending fatigue tests via repeated Cu thin film depositions and wet-transfers of graphene, as shown in the schematic in Figure 1. Previously known chemical vapor deposition (CVD) method was used to grow the wafer-scale graphene (100 x 200 mm2), which was then transferred using a PMMA support layer onto a sputter deposited Cu thin film on polyimide substrate. The PMMA support layer was then removed using acetone, and the process of Cu deposition and graphene transfer was repeated with a layer spacing of 100 nm to a total thickness of 400 nm. For comparison, Cu only thin film with the same total thickness of 400 nm was also fabricated by depositing 100 nm Cu layer four times. The detailed procedure of the sample fabrication process can be found in the Supporting information 01. Cross-section 4

ACS Paragon Plus Environment

Page 5 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Nano Letters

SEM and TEM images taken at the interfaces of Cu/Gr composite clearly confirm that the graphene layers were inserted in between the Cu layers and that the Cu grains are discontinuous across the graphene interface (Figure 2). Although there is a (111) texture in the Cu layers (Supporting information 01), the in-plane orientations are not matched with the grains of underlying Cu layer. Cu/Gr interface is known to have van der Waals interaction, as revealed in several DFT calculations for different metal-graphene interfaces.30, 31. Cu only film showed a columnar grain structure that is interrupted at each 100 nm of deposition, as expected. Nano-twins were often observed for both Cu/Gr and Cu only samples, as shown in Figure 2e, f. In order to investigate the effects of the graphene inclusion on the robustness of the Cu/Gr nanolayered composite electrode during bending fatigue, repeated tensile bending strain was imposed while monitoring the electrical resistance of the specimen in-situ. Fatigue-induced crack generation and propagation is expected to cause increase in the resistance and hence, by monitoring the fractional resistance change, defined as (R-R0)/R0, where R0 and R are the initial and in-situ resistance during cycling, respectively, fatigue induced damage on the specimen can be measured. Lower fractional resistance indicates enhanced resistance to fatigue failure or enhanced fatigue resistance. Initial sheet resistances of Cu and Cu/Gr electrode were measured to be 1.53 ohm/sq and 1.74 ohm/sq, respectively, and thus it can be inferred that the inserted graphene layer acts as a sufficient conductor that does not increase the overall resistance significantly. At 1.6% bending strain condition, the fractional resistance of Cu thin film electrode was increased by 150% at 100,000 cycles and 325% at 1,000,000 cycles as shown in Figure 3a. For the case of Cu/Gr composite, the fractional resistance increase was initially greater than that of Cu electrode presumably due to the presence of defects and impurities introduced 5

ACS Paragon Plus Environment

Nano Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

during the wet transfer process, but showed a remarkable enhancement beyond 12,000 cycles; fractional resistance increase of Cu/Gr was 5 times smaller than that of Cu electrode at 1,000,000 cycles, as shown in Figure 3b. In addition, the fractional resistance increase in the Cu/Gr composite reached a plateau, whereas the resistance of Cu electrode kept increasing rapidly even at 1,000,000 cycles. At a larger bending strain of 3.1%, resistances of both the Cu electrode and Cu/Gr composite increased more rapidly, but a similar trend was observed; Cu/Gr composite showed 6 times smaller increase in fractional resistance compared to that of Cu electrode at 1,000,000 cycles, as shown in the Figure 3c. The increase in the fractional resistance of the metal thin films under bending fatigue is known to be caused by the interruption of current flow associated with formation of voids and cracks due to build-up of dislocations at the film/substrate interface.15 In the work by Kim et al., introduction of nanoholes has the effect of annihilating dislocations at the free surfaces of the nanoholes to reduce the overall dislocation density piled-up at the film/substrate interface.32 Instead of patterning the Cu thin film into nanohole arrays, which can be problematic in fabricating thin line electrodes as the width of the line approaches the nanohole dimensions, simple insertion of a graphene layer in between the un-patterned Cu layers has proven to be efficient in reducing the fatigue induced damage. The fractional resistance increase in Cu/Gr with 100 nm repeat layer spacing was reduced by a factor of 5-6 in comparison to that of the Cu thin film with same total thickness. The cause of the dramatic enhancement in the fatigue resistance of Cu/Gr composite electrode is proposed to be not only the high intrinsic strength of the composite, but also the ability of the graphene interface to deflect crack propagations and to block dislocations from piling-up all at the film/substrate interface as discussed in detail below.

6

ACS Paragon Plus Environment

Page 6 of 18

Page 7 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Nano Letters

To analyze the crack evolution in Cu thin film electrodes and Cu/Gr composites, plan view and cross-sectional SEM images of both samples before and after 1,000,000 bending cycles at 1.6% were analyzed as shown in Figure 4. Cu and Cu/Gr electrodes both indicate that cracks were formed on the top surface after bending fatigue cycling. Interestingly, the density of cracks formed in the Cu/Gr electrode was smaller than that in the Cu thin film electrode, and the Cu/Gr electrode showed shorter cracks and deflections in crack path. Cross sectional SEM images indicate that the cracks traveled through the entire thickness in the Cu thin film electrode. However, the cracks were discontinuous in the Cu/Gr composite electrode as a result of the ability of the graphene to limit crack propagation on to the next layer, as shown in Figure 4c, d. Discontinuous cracks in the Cu/Gr composite would then leave a continuous electrical pathway to cause enhanced retention of the conductivity during the bending fatigue cycles. The annular dark field scanning transmission electron microscope (ADF-STEM) and TEM images of the Cu/Gr electrode further confirmed that the crack was deflected at the Cu/Gr interface and could not penetrate through it (Figure 4e). The columnar Cu grains in each layer often have nano-twinned microstructure within the grain (Figure 2e, f and Figure S2), and such additional nano-twinned interface is expected to have an effect in the crack initiation and propagation preferentially occurring along the grain boundaries. Fatigue induced cracks are expected to start from the top most layer since it is subjected to the largest tensile bending strain. These cracks can easily propagate through the entire thickness of Cu only electrode but are deflected in the Cu/Gr interface due to the high strength and modulus of the graphene. Strong sp2 bonding with strength and modulus of 130 GPa and 1 TPa, respectively, makes graphene an extremely stiff and hard interface to cut across; thus the cracks that are generated in one of the Cu layers of the Cu/Gr nanolayered composite would therefore be blocked or deflected at the interface, which hinders further crack propagation on to the next layer. The defected cracks then do not have enough driving 7

ACS Paragon Plus Environment

Nano Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 18

force to propagate under the condition of the tensile in-plane strain imposed via bending and thus will be arrested. Second reason for hindrance of crack propagation is the smaller crack size that can be fitted into the Cu/Gr nanolayers than into the Cu thin film. Since one can think of the Cu/Gr nanolayers as Cu thin film being divided into four thinner layers with spacing of 100 nm that are separated by graphene, the crack sizes that can form within each Cu layers of the Cu/Gr composite is much smaller than those in Cu thin film electrode with equal total thickness (4 times the 100 nm thickness). According to the Griffith criterion, stress needed to propagate a crack of radius a is given by σ௙ = ቀ

ଶா(ఊೄ ାఊು ) ଵ/ଶ గ௔



, where E, γS, γP, are the

modulus, surface energy, and plastic work per unit area of the created surface, respectively. Thus, it is harder for the cracks in Cu/Gr composite to propagate than those in Cu electrode since the maximum crack size in Cu/Gr is limited to the repeat layer spacing of Cu (100 nm), which is smaller than the total thickness of the Cu only electrode without graphene (400nm). Aside from the ability of the graphene interface to hinder crack propagations, the ability in blocking dislocations from propagating across the interface that results in reduction in the density of dislocations piled-up at film/substrate interface can also contribute to enhanced fatigue resistance. In order to gain insights to the interaction of dislocations at the graphene interface, MD simulations of tensile straining of Cu and Cu/Gr composites were performed. In the MD simulation setup, a Cu thin film and a Cu/Gr sandwich structure was subject to the fixed boundary condition at the free surface in [111]Cu-direction (Figure 5 and Figure S4). A vertical crack was introduced at the free surface in [1ത1ത1ത]Cu-direction for each model, where the crack tips were propagated upon tensile strain (Figure 5 and Figure S4). In the case of the Cu thin film, the dislocation initiated from the crack tip was able to propagate through the entire thickness of Cu block, which reached to the other end of the Cu layer 8

ACS Paragon Plus Environment

Page 9 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Nano Letters

without any interference and piled-up at the film/substrate interfaces (Figure 5a, b and Supporting movie 01). On the other hand, the initiated dislocation in the Cu/Gr sandwich structure was blocked by the graphene layer (Figure 5c), and the deflection of the dislocation occurred as the strain increased further (Figure 5d, Supporting movie 02). The difficulty of dislocation propagation in the Cu/Gr sandwich structure caused higher ultimate tensile strength compared to that of the Cu block, as shown in Figure 5e. Therefore, the same graphene interface that blocks dislocations to increase the strength of the composite was shown to have a pronounced effect on blocking the crack propagation in the Cu/Gr nanolayers to result in the experimentally observed 5-6 times increase in the robustness against fatigue induced damage in comparison to Cu thin film. The details of the MD simulation can be found in Supporting information 03. In summary, the robustness of Cu/Gr composite with 100 nm repeat layer spacing against fatigue induced damage was explored for the first time and showed a remarkable 5-6 times enhancement in Cu/Gr compared to the conventional Cu only electrode when subjected to bending fatigue of 1,000,000 cycles at 1.6% and 3.1% strain. The enhancement in fatigue resistance was shown to be due to the ability of the graphene to block and deflect crack propagations; strong sp2 bonding of graphene as well as the limited crack size in Cu with smaller layer spacing both contribute to the reduced crack propagations in the Cu/Gr nanolayers. In addition, the ability of each Cu/Gr interface to block dislocations, as revealed by the MD simulations, can suppress the fatigue crack formation mechanism found in Cu only thin film via heavy dislocation build-up at the Cu film/substrate interface. It is noteworthy that this remarkable enhancement in resistance to fatigue damage of Cu/Gr, which in turn sustains the conductivity of the electrode for longer fatigue cycles, makes this Cu/Gr composite system well-suited for future flexible and stretchable interconnect applications. 9

ACS Paragon Plus Environment

Nano Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ASSOCIATED CONTENT

Supporting Information. The Supporting Information is available free of charge on the ACS Publication Website at http://pubs.acs.org. Details of the fabrication process of Cu/Gr nanolayered composites and XRD analyses of Cu and Cu/Gr composites are provided. Comparison of Cu/Gr to other interface engineered materials and additional TEM analysis of Cu/Gr nanolayers after bending cycles is also included. Lastly, details of the MD simulation and the tensile deformation movies of the Cu and Cu/Gr composites are provided.

AUTHOR INFORMATION Corresponding Author *E-mail: [email protected] Author Contributions ‡These authors contributed equally.

ACKNOWLEDGMENT This work was supported by National Research Foundation of Korea (NRF) funded by the Korea government (MSIP) under the grant No. NRF-2016R1A2B3011473 and NRF2015M3A7B7045354. We would also like to acknowledge the support from the Korea Institute of Energy Technology Evaluation and Planning (KETEP) and the Ministry of Trade, Industry & Energy (MOTIE) of the Republic of Korea under grant No. 20162000000910.

10

ACS Paragon Plus Environment

Page 10 of 18

Page 11 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Nano Letters

REFERENCES (1) Sekitani, T.; Nakajima, H.; Maeda, H.; Fukushima, T.; Aida, T.; Hata, K.; Someya, T. Nat Mater 2009, 8, 494-499. (2) Gu, G.; Burrows, P. E.; Venkatesh, S.; Forrest, S. R.; Thompson, M. E. Optics Letters 1997, 22, 172-174. (3) Sugimoto, A.; Ochi, H.; Fujimura, S.; Yoshida, A.; Miyadera, T.; Tsuchida, M. IEEE Journal of Selected Topics in Quantum Electronics 2004, 10, 107-114. (4) Han, T.-H.; Lee, Y.; Choi, M.-R.; Woo, S.-H.; Bae, S.-H.; Hong, B. H.; Ahn, J.-H.; Lee, T.-W. Nat Photon 2012, 6, 105-110. (5) Dimitrakopoulos, C. D.; Malenfant, P. R. L. Advanced Materials 2002, 14, 99-117. (6) Sun, Y.; Rogers, J. A. Advanced Materials 2007, 19, 1897-1916. (7) Torres Sevilla, G. A.; Ghoneim, M. T.; Fahad, H.; Rojas, J. P.; Hussain, A. M.; Hussain, M. M. ACS Nano 2014, 8, 9850-9856. (8) Cheng, Y.-J.; Yang, S.-H.; Hsu, C.-S. Chemical Reviews 2009, 109, 5868-5923. (9) Rogers, J. A.; Huang, Y. Proceedings of the National Academy of Sciences 2009, 106, 10875-10876. (10) Lacour, S. P.; Jones, J.; Wagner, S.; Teng, L.; Zhigang, S. Proceedings of the IEEE 2005, 93, 1459-1467. (11) Kim, D.-H.; Song, J.; Choi, W. M.; Kim, H.-S.; Kim, R.-H.; Liu, Z.; Huang, Y. Y.; Hwang, K.-C.; Zhang, Y.-w.; Rogers, J. A. Proceedings of the National Academy of Sciences 2008, 105, 18675-18680. (12) Kim, D.-H.; Ahn, J.-H.; Choi, W. M.; Kim, H.-S.; Kim, T.-H.; Song, J.; Huang, Y. Y.; Liu, Z.; Lu, C.; Rogers, J. A. Science 2008, 320, 507-511. (13) 1996, 2.4.3.1C. (14) Hwang, B.; Shin, H.-A. S.; Kim, T.; Joo, Y.-C.; Han, S. M. Small 2014, 10, 3397-3404. (15) Kim, B.-J.; Shin, H.-A. S.; Jung, S.-Y.; Cho, Y.; Kraft, O.; Choi, I.-S.; Joo, Y.-C. Acta Materialia 2013, 61, 3473-3481. (16) Zhang, G. P.; Volkert, C. A.; Schwaiger, R.; Wellner, P.; Arzt, E.; Kraft, O. Acta Materialia 2006, 54, 3127-3139. (17) Suresh, S. Fatigue of Materials 2nd Ed. , Cambridge University Press , Cambridge, UK 1999. (18) Wang, D.; Volkert, C. A.; Kraft, O. Materials Science and Engineering: A 2008, 493, 267-273. (19) Kim, Y.; Lee, J.; Yeom, M. S.; Shin, J. W.; Kim, H.; Cui, Y.; Kysar, J. W.; Hone, J.; Jung, Y.; Jeon, S.; Han, S. M. Nature Communications 2013, 4, 2114. (20) Lee, C.; Wei, X.; Kysar, J. W.; Hone, J. Science 2008, 321, 385-388. (21) Zhu, Y.; Murali, S.; Cai, W.; Li, X.; Suk, J. W.; Potts, J. R.; Ruoff, R. S. Advanced Materials 2010, 22, 3906-3924. (22) Sanders, P. G.; Eastman, J. A.; Weertman, J. R. Acta Materialia 1997, 45, 4019-4025. (23) Cheng, S.; Ma, E.; Wang, Y. M.; Kecskes, L. J.; Youssef, K. M.; Koch, C. C.; Trociewitz, U. P.; Han, K. Acta Materialia 2005, 53, 1521-1533. (24) Y. Champion, S. G. r.-M., J.-L. Bonnentien and P. Langlois. Scripta mater 2001, 44, 1609-1613. (25) Jang, D.; Cai, C.; Greer, J. R. Nano Letters 2011, 11, 1743-1746. (26) Misra, A.; Hirth, J. P.; Kung, H. Philosophical Magazine A 2002, 82, 2935-2951. (27) Beyerlein, I. J.; Mara, N. A.; Carpenter, J. S.; Nizolek, T.; Mook, W. M.; Wynn, T. A.; McCabe, R. J.; Mayeur, J. R.; Kang, K.; Zheng, S.; Wang, J.; Pollock, T. M. Journal of Materials Research 2013, 28, 1799-1812. 11

ACS Paragon Plus Environment

Nano Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

(28) Geim, A. K. Science 2009, 324, 1530-1534. (29) Huang, M.; Pascal, T. A.; Kim, H.; Goddard, W. A.; Greer, J. R. Nano Letters 2011, 11, 1241-1246. (30) Hamada, I.; Otani, M. Physical Review B 2010, 82, 153412. (31) Zhiping, X.; Markus, J. B. Journal of Physics: Condensed Matter 2010, 22, 485301. (32) Kim, B. J.; Cho, Y.; Jung, M. S.; Shin, H. A.; Moon, M. W.; Han, H. N.; Nam, K. T.; Joo, Y. C.; Choi, I. S. Small 2012, 8, 3300-6. (33) Liu, P.; Jin, Z.; Katsukis, G.; Drahushuk, L. W.; Shimizu, S.; Shih, C.-J.; Wetzel, E. D.; Taggart-Scarff, J. K.; Qing, B.; Van Vliet, K. J.; Li, R.; Wardle, B. L.; Strano, M. S. Science 2016, 353, 364-367. (34) Mishin, Y.; Mehl, M. J.; Papaconstantopoulos, D. A.; Voter, A. F.; Kress, J. D. Physical Review B 2001, 63, 224106. (35) Stuart, S. J.; Tutein, A. B.; Harrison, J. A. The Journal of Chemical Physics 2000, 112, 6472-6486.

12

ACS Paragon Plus Environment

Page 12 of 18

Page 13 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Nano Letters

Table of Contents Graphic

13

ACS Paragon Plus Environment

Nano Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 1. Illustration of wet transfer method for the fabrication of Cu/Gr composites. Waferscale graphene layer was first grown on Cu foil by CVD, and PMMA was used as a support layer to transfer graphene on 100 nm thick Cu-deposited PI substrate. This process was repeated to fabricate multilayered Cu/Gr composites.

14

ACS Paragon Plus Environment

Page 14 of 18

Page 15 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Nano Letters

twins twins

Figure 2. Cross section SEM images of (a) Cu electrode and (b) Cu/Gr composites both with total thickness of 400 nm. Cross section TEM images of Cu and Cu/Gr at low magnification (c-d) and a high magnification showing the Cu/Gr interface (e-f).

15

ACS Paragon Plus Environment

Nano Letters

3.5 3.0

0.5

Cu thin film Cu/Gr nanolayered composite

(a) 0.4

2.0 1.5 1.0

Cu thin film Cu/Gr nanolayered composite

(R-R0)/R0

2.5

(R-R0)/R0

0.0 0.0

0.3 0.2 0.1

0.5 5

5

5

5

6

2.0x10 4.0x10 6.0x10 8.0x10 1.0x10

(b)

0.0 0.0

3

5.0x10

Number of Bending Cycles

4

1.0x10

4

1.5x10

4

2.0x10

Number of Bending Cycles

12 10

(c)

8

(R-R0)/R0

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 16 of 18

6 4

Cu thin film Cu/Gr nanolayered composite

2 0 0.0

2.0x10

5

5

4.0x10

5

6.0x10

8.0x10

5

6

1.0x10

Number of Bending Cycles

Figure 3. (a) Bending fatigue test results of Cu electrode and Cu/Gr composite at 1.6% strain. Fractional resistance evolution over cycles for Cu and Cu/Gr indicate enhanced fatigue resistance by 5 fold. (b) Enlarged scale of fractional resistance at early stages of cycling. (c) Bending fatigue test results of Cu electrode and Cu/Gr composite at 3.1% strain showing 6 fold enhancement in fatigue resistance. R0 is the initial resistance before imposing bending strain.

16

ACS Paragon Plus Environment

Page 17 of 18

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Nano Letters

Figure 4. SEM images of Cu electrode and Cu/Gr composite after imposing 1,000,000 cycles of bending. (a-b) Plan-view image of Cu and Cu/Gr after bending fatigue. Insets of (a) and (b) are high magnification SEM images taken at the cracks of each specimen. Cross-sectional images showing (c) cracks that penetrate through thickness of Cu thin film and (d) discontinuous cracks in Cu/Gr composites. White arrows in (c, d) indicate current flow lines through the cracked Cu and Cu/Gr electrodes. (e) Annular dark field scanning transmission electron microscope (ADF STEM) image of Cu/Gr electrode; inset is TEM image taken at the crack indicated by yellow arrow.

17

ACS Paragon Plus Environment

Nano Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 5. Atomic shear strain maps for (a) Cu block under the strain of 4.2% and (b) 6.0%, and for (c) Cu/Gr sandwich structure under the strain of 4.2% and (d) 6.0%. (e) The calculated stress-strain curves of Cu block and Cu/Gr sandwich structure.

18

ACS Paragon Plus Environment

Page 18 of 18