Subscriber access provided by The University of Texas at El Paso (UTEP)
Article
Sustainable polycarbonates from a citric acid-based rigid diol and recycled BPA-PC: From Synthesis to Properties Chengcai Pang, Xueshuang Jiang, Yan Yu, Xiaohan Liu, Jingyan Lian, Jianbiao Ma, and Hui Gao ACS Sustainable Chem. Eng., Just Accepted Manuscript • DOI: 10.1021/ acssuschemeng.8b04421 • Publication Date (Web): 19 Oct 2018 Downloaded from http://pubs.acs.org on October 21, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
Sustainable polycarbonates from a citric acid-based rigid
2
diol and recycled BPA-PC: From Synthesis to Properties
3 4
Chengcai Pang*, Xueshuang Jiang, Yan Yu, Xiaohan Liu, Jingyan Lian, Jianbiao Ma,
5
and Hui Gao*
6
School of Chemistry and Chemical Engineering, School of Material Science and
7
Engineering, Tianjin Key Laboratory of Organic Solar Cells and Photochemical
8
Conversion, Tianjin University of Technology, Binshui West Road 391, Tianjin 300384,
9
China
10
*Corresponding
11
E-mail address:
[email protected];
[email protected] author: Tel.: +86 22 60214251.
12 13 14 15 16 17 18 19 20 21 22
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2 3
Abstract: Here we present a series of homopolycarbonates (homo-PCs) and
4
copolycarbonates (co-PCs) based on a novel bicyclic diol octahydro-2,5-pentalenediol
5
(OPD) from naturally occurring citric acid and bis(hydroxyethyl ether) of bisphenol A
6
(BHEEB), synthesized by melt polycondensation. The recently developed OPD has
7
shown to be highly rigid and thermal stable building block suitable for the construction of
8
performance polymers. BHEEB, which was obtained from the chemical recycling of
9
BPA-PC, was used to compens ate for the low reactivity of OPD and to modify the
10
brittleness of polycarbonate (PC) solely based on OPD, without compromising other
11
properties. The single crystal of the endo-endo isomer of OPD was deliberately obtained
12
and its absolute stereochemistry was unambiguously identified by single crystal X-ray
13
diffraction for the first time. The polymers had Mn in the 10100−20000 g mol-1 range and
14
gradually decreased with the increasing of OPD content. NMR analyses revealed the
15
random structures of the co-PCs and the molar content of OPD in all cases was lower
16
than its corresponding feeds. Interestingly, in contrast with the semicrystalline
17
poly(octahydro-2,5-pentalenediol carbonate) (abbreviated as pre-POC) prepared in a
18
different protocol in our previous article, poly(octahydro-2,5-pentalenediol carbonate)
19
(abbreviated as POC) in this study exhibited amorphous feature with lower Tg of 74.5 ºC.
20
A “ductile−to−brittle” transition occurred with the increasing of OPD content in the PBC
21
chains, which can be ascribed to their low molecular weights and the low entangled
22
strand density due to the rather stiff polymer chains. This work combines the chemical
ACS Paragon Plus Environment
Page 2 of 38
Page 3 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
recycling and bio-based polymer together, which would bring a feasible way to satisfy
2
the demands of sustainability.
3
Keywords : rigidity, chemical recycling of BPA-PC, bicyclic diol, citric acid,
4
polycarbonate
5
INTRODUCTION
6
The preparation of polymers from renewable resources is currently receiving
7
considerable attention because of the finite reserves of crude oils and economical,
8
environmental, and social concerns.1-4 However, completely bio-renewable polymers
9
frequently suffer from some limits of mechanical and thermal properties when replacing
10
general engineering plastics, which make it necessary to utilize additional monomers, e.g.,
11
terephthalate acid and bisphenol A (BPA), to obtain essential properties required in
12
general plastics’ applications. Moreover, due to the fact that the price of recycled
13
polymers is generally lower compared to that of virgin materials,5 recycling of
14
commercial plastics to produce polymers has become much more attractive, and more
15
importantly, can effectively reduce the environmental issues caused by the plastic
16
wastes.6 So, from the sustainable, industrial and environmental point of view, the
17
synthesis of bio-based polymers should conjugate with the recycling of commercial
18
plastic wastes, especially when novel polymers with more specific and tailored properties
19
can be achieved. For example, bis(hydroxyethyl ether) of bisphenol A (BHEEB),
20
obtained by reaction of BPA-PC with renewable ethylene carbonate, has been used as
21
rigid comonomer to increase the glass transition temperature and thermal stability of
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
terephthalate polyesters.7
2
BPA-PC is a commercially available amorphous material, characterized by high
3
transparency, high glass transition temperature (Tg), impact resistance and tensile strength,
4
which is massively used in electric and electronic, automotive, and optical components.8,
5
9
6
Moreover, the safety of BPA-PC has been frequently questioned due to the toxicity of
7
BPA in the last few years.11 In this regard, it would be desirable to prepare PCs from
8
renewable but less toxic resources having comparable thermal and mechanical properties
9
to that of BPA-PC.
Unfortunately, BPA-PC is considered unsustainable because BPA is non-renewable.10
10
Among the renewable sources, several bicyclic diacetalized diols, obtained by
11
acetalization of the intramolecular hydroxyl groups from C4 and C6 sugars, are regarded
12
as suitable for the production of linear rigid polycondensates due to their outstanding
13
rigidity.12 However, the use of these bicyclic diacetalized diols for the fabrication of
14
bio-based PC is challenging due to their high prices caused by the tedious preparation
15
process and their high sensitivity to heat.13 In addition, isohexides, which is composed of
16
isosorbide, isoidide and isomannide,14 are considered as suitable candidates for replacing
17
BPA due to their natural origin, attractive rigidity,15,16 safety and chirality.17 Despite the
18
apparent merits, PCs solely based on isohexides still suffer from several drawbacks: (1)
19
relatively low molecular weights polymers were obtained due to the poor reactivity of the
20
hydroxyl groups at the 2- and 5- positions.18 (2) the corresponding homo-PC is too
21
brittle.17 (3) severely colored or cross-linked polymers were frequently obtained during
ACS Paragon Plus Environment
Page 4 of 38
Page 5 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
melt polycondensation, which was caused by the heat labile skeleton composed of two
2
tetrahydrofuran rings.19,
3
copolycondensation
4
1,4-cyclohexanedimethanol.21 However, due to the intrinsic thermolability of the
5
tetrahydrofuran rings contained in isohexides, effective ways that can avoid discoloration
6
or gelation under high temperatures are still not available.
of
20
The first two drawbacks can be solved simultaneously by isohexides
with
more
flexible
primary
diols,
e.g.,
7
Very recently, a series of random co-PCs based on a compelling bicyclic diol
8
octahydro-2,5-pentalenediol (OPD), which is derived from naturally occurring citric acid,
9
have been developed in our group. Results indicated that OPD is a highly rigid and
10
thermal stable building block suitable for the construction of performance PCs.22
11
However, due to the high stiffness and immobility of chain conformation, the main
12
demerit of solely OPD-based PC is its fragility. In this work, in order to improve the
13
toughness and compensate for the low reactivity of OPD, while at the same time retaining
14
the rigidity of OPD-based PCs, BHEEB is incorporated in the polymer chains by melt
15
polymerization with OPD in different molar ratios. Previous investigations suggested that
16
the high impact strength of BPA-PC can be attributed to its capacity of absorbing high
17
impact energy which, in turn, has been correlated with secondary relaxations involving
18
cooperative motions of BPA units in the polymer chains.23 It is worthy to note that
19
although BPA is toxic, however, BHEEB is biocompatible. In fact, ethoxylated BPA has
20
long been used in food packaging applications and restorative dentistry.24 Therefore, the
21
chemical recycling of BPA-PC through the formation of ethoxylated BPA compound is
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Page 6 of 38
of great interests from an environmental and industrial point of view.
2
Herein, we describe the green synthetic routes, the structural characterization and
3
the thermal and mechanical properties of the amorphous homo-PCs and co-PCs, prepared
4
by melt polymerization of OPD, BHEEB and diphenyl carbonate (DPC). OPD was
5
chosen in view of its natural origin and excellent rigidity and thermal stability, while
6
using BHEEB, the modified BPA from chemical recycling of commercial BPA-PC,
7
impact resistant polymers with high molecular weights can be possibly obtained. Since
8
our goal lies in the fabrication of bio-based PCs with high Tg values and impact strength,
9
special attention is paid to study the effect of OPD and BHEEB composition on polymer
10
properties, e.g., Tg value and toughness, a systematic structure-thermal and mechanical
11
properties relations study on the relevant polymers has been performed.
12
Experimental Section
13
Materials
14
Dimethyl-1,3-acetone dicarboxylate (98%), glyoxal (40% aqueous solution), glacial
15
acetic acid (99.5%) and BPA-PC (melt index 10−12 g/10min) were purchased from
16
Sigma-Aldrich
17
4-dimethylaminopyridine (DMAP) (99%), lithium acetylacetonate (LiAcac) (99%) and
18
NaBH4 (98%) were purchased from Energy Chemical Co. (Shanghai, China),
19
concentrated hydrochloric acid, methanol (99%) and chloroform (99%) were purchased
20
from Tianjin Chemical Reagent Co. (Tianjin, China) and used without further
21
purification.
(Shanghai,
China).
Ethylene
carbonate
ACS Paragon Plus Environment
(99%),
DPC
(98%),
Page 7 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
General methods
2
Chemical structure and compositions of the PCs were analyzed using 1H-NMR,
3
13C-NMR
4
were carried out using CDCl3 as the solvent at ambient temperature on a Bruker
5
AVANCE III NMR spectrometer operating at 400 and 100.6 MHz respectively, and the
6
internal standard was tetramethylsilane. The molecular weights (Mn, Mw) and the
7
molecular weight distribution (PDI) were determined by gel permeation chromatography
8
(GPC, Waters 2414 system Milford, 4 MA) at 35 ºC with the flow rate set to 1.0 mL
9
min-1. THF and monodisperse polystyrene were used as the eluent and standard,
10
respectively. The concentration of the sample was 4 mg mL-1, and the injection volume
11
was around 30 μL. The thermogravimetric analyses (TGA) was carried out on a Seiko
12
Exstar 6000 TGA quartz rod microbalance and 5−8 mg of sample was needed for each
13
polymer. The sample was then heated from 40 to 600 ºC at a heating rate of 10 ºC min-1
14
with nitrogen gas purging (50 mL min-1). The thermal characteristics of the polymers
15
were investigated using a differential scanning calorimeter (DSC, Netzsch PC-200) under
16
with nitrogen gas purging (50 mL min-1). About 5 mg of sample was heated from 30 ºC
17
to 120 ºC at a heating rate of 10 ºC min-1 and a cooling rate of 30 ºC every time and then
18
the Tg were calculated from the second heating run. Films for mechanical testing
19
measurements with a thickness of 200 μm were prepared by casting from a chloroform
20
solution at a concentration of 100 g L-1. The tensile properties were tested on dumbbell
21
type specimens (12×2×0.5 mm3) measuring the strain at 25 ºC and 3 mm s-1. Dynamic
and Fourier Transform Infrared (FT-IR) spectra. The NMR measurements
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 38
1
mechanical analysis (DMA) were carried out using a TA DMA 2928 in a controlled
2
force-tension film mode with a preload force of 0.1 N, an amplitude of 10 μm, and at a
3
fixed frequency of 1 Hz at the range of -140 to 140 ºC in a heating rate of 3 ºC min-1.
4
Sythesis of monomers
5
Synthesis of octahydro-2,5-pentalenediol (OPD)
6
Octahydro-2,5-pentalenediol
7
1,3-acetonedicarboxylate and glyoxal, the exhaustive procedure can be found in the
8
reported literature.25
9
Sythesis of BHEEB
(OPD)
was
synthesized
using
dimethyl
10
BHEEB was synthesized from chemical recycling of BPA-PC as per the reported
11
procedure.24 Briefly, BPA-PC (5.1 g), ethylene carbonate (4.22 g, 48 mmol) and sodium
12
phenoxide (0.1 mol% to BPA-PC repeating unit) were added into a three-neck flask fitted
13
with condenser and a thermometer. The flask was heated to reflux at 250 ºC under magic
14
stirring under a N2 atmosphere until the effervescence ceased. The reaction mixture was
15
cooled to room temperature and the polymer was dissolved in CHCl3 and precipitated in
16
methanol. A suspension of the precipitated polymer was dissolved in a 1 mol L-1 KOH
17
for 3 h at reflux. The white suspension was neutralized with diluted HCl and the solvent
18
evaporated under vacuum. The white solid was washed three times with water and the
19
residue was dissolved in CH2Cl2, dried with anhydrous magnesium sulfate and then
20
crystallized in cyclohexane to afford a white solid (5.8 g, yield: 91%). 1H-NMR (400
21
MHz, CDCl3): δ 7.14 (d, 4H), 6.82 (d, 4H), 4.06 (m, 4H), 3.94 (dd, 4H), 2.1 (t, 2H), 1.64
ACS Paragon Plus Environment
Page 9 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
(s, 6H).
2
Synthesis of polymers
3
Poly(octahydro-2,5-pentalenediol carbonate) (POC) and Poly(bis(hydroxyethyl ether) of
4
bisphenol A carbonate) (PBC) were obtained by reacting DPC with OPD or BHEEB,
5
respectively. The POxByC co-PCs were synthesized from a mixture of BHEEB, OPD and
6
DPC with the selected composition, where x and y represent the content of OPD and
7
BHEEB relative to the total amount of diols in the polymer chains, respectively,
8
determined by integration of the 1H NMR spectra (Table 1). The representative
9
preparation of PO29B71C is described below as a generalized polymerization procedure.
10
In a three-neck round flask fitted with a vacuum distillation outlet, OPD (0.91 g, 6.4
11
mmol), BHEEB (4.3 g, 13.6 mmol) and DPC (4.28 g, 20 mmol) were charged. Three
12
cycles of N2 and vacuum were applied to remove any residual air. LiAcac (0.1 wt %
13
based on the diols ) and DMAP (0.1 wt % based on the diols) were chosen as catalysts.
14
Transesterification reactions were carried out under N2 at 130 °C for 10 h.
15
Polycondensation reactions were performed at 230 °C for 2 h under vacuum (0.5 mbar).
16
After completion of the reactions, the resulting polymers were cooled to room
17
temperature and dissolved in chloroform, precipitated in excess of methanol to remove
18
unreacted monomers and formed oligomers. Finally, the precipitation was collected by
19
filtration and dried under vacuum for 24 h.
20
PBC: 1H-NMR (400 MHz, CDCl3): δ 7.13 (d, 4H), 6.81 (d, 4H), 4.49 (q, 4H), 4.18 (t,
21
4H), 1.63 (s, 6H). FT-IR (cm-1): 3043, 2961, 2869, 1750 (C=O), 1599, 1504, 1229, 1182,
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
916, 834, 791, 572.
2
POxByCs: 1H-NMR (400 MHz, CDCl3): δ 7.10−7.20 (d, x-4H), 6.77−6.89 (d, x-4H), 5.21
3
(m, y-1H, endo-exo), 5.08 (m, y-1H, endo-exo), 4.87−5.04 (m, y-2H, endo-endo),
4
4.42−4.54 (q, x-4H), 4.12−4.24 (t, x-4H), 2.71 (s, y-2H, endo-exo), 2.47 (s, y-2H,
5
endo-endo), 2.03−2.31 (m, y-4H, endo-endo; m, y-4H, endo-exo), 1.70−1.83 (m, y-4H,
6
endo-endo; m, y-4H, endo-exo), 1.64 (s, x-6H). FT-IR (cm-1): 3047, 2974, 2870, 1750
7
(C=O), 1605, 1504, 1240, 1173, 916, 824, 781, 561.
8 9
Figure 1. Molecular structure of the endo-endo stereoisomer in the crystal.
10
POC: 1H-NMR (400 MHz, CDCl3): δ 5.19 (m, 1H; endo-exo), 5.10 (m, 1H; endo-exo),
11
4.87−4.99 (m, 2H; endo-endo), 2.71 (s, 2H; endo-exo), 2.44 (s, 2H; endo-endo),
12
2.02−2.35 (m, 4H, endo-endo; 4H, endo-exo), 1.56−1.85 (m, 4H, endo-endo; 4H,
13
endo-exo). FT-IR (cm-1): 2968, 2876, 1750 (C=O), 1474, 1435, 1277, 1101, 952, 799.
14
Results and discussion
15
Synthesis and characterization of OPD
16
The bio-based monomer octahydro-2,5-pentalenediol (OPD) was prepared from
ACS Paragon Plus Environment
Page 10 of 38
Page 11 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
commercially available dimethyl 1,3-acetonedicarboxylate (derived from citric acid) and
2
glyoxal via Weiss-Cook condensation reaction, followed by decarboxylation under acidic
3
conditions, leading to the formation of bicyclo[3.3.0]octane-3,7-dione. Subsequent
4
reduction with NaBH4 afforded the desired bicyclic diol OPD. 1H NMR spectrum shows
5
that OPD is essentially a mixture of two stereoisomers, in which the endo-endo isomer
6
predominated over the endo-exo one (endo-endo:endo-exo = 4:1).
7
The exo-exo stereoisomer, however, is not obtained since the reduction of the
8
intermediate diketone from the endo faces is unfavorable owing to its steric hindrance.
9
The synthetic approach and the NMR spectroscopic data of OPD can be found in our
10
previous article.22 To further explore its molecular structure, the single crystal of the
11
endo-endo diastereoisomer was deliberately obtained by repeatedly recrystallization from
12
methanol. Single crystal X-ray (Figure 1) revealed its characteristic V-shaped bicyclic
13
frame composed of two cis-fused cyclopentane rings similar to isohexide, thus a fairly
14
high degree of rigidity can be expected. Because the two cyclopentane rings contained in
15
the molecular skeleton are not planar, the dihedral angle between them cannot be given
16
precisely. Alternatively, it can be described in terms of torsion angles, the torsion angle
17
of C4−C5−C1−C8 is 119.2o, and the torsion angle of C2−C1−C5−C6 is 128.4o. More
18
detailed information about the endo-endo stereoisomer can be found in Table S1 in the
19
Supporting Information.
20
Synthesis and chemical structure analysis of co-PCs
21
Homo-PC POC and PBC based on OPD and BHEEB, respectively, as well as co-PCs
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 38
1
from OPD and BHEEB, were prepared following a conventional procedure including
2
transesterification and polycondensation reactions as shown in Scheme 1. In order to find
3
the optimal reaction condition, the preparation of the targeted PO29B71C was chosen as
4
the model reaction and conducted with variable conditions including reaction
5
temperatures, stoichiometric ratio of monomers, and catalyst. When OPD was used as a
6
comonomer, the reaction temperature had a significant effect on the component of the
7
resulting polymers. In fact, at temperatures exceeding 250 ºC, the content of OPD units in
8
the resulting polymers were always lower than the initial feeds. Moreover, the longer
9
reaction time, the lower content of OPD was obtained. This phenomenon is identical to
10
our previous observations22 and can be interpreted H OH + y HO
x HO H
O
O
O O O
OH + ( x+y(
1. Transesterification, 130 °C 2. Polycondensation, 230 °C O
H O
O O
H
x
O
O
O
O
y
11 12
Scheme 1. Polymerization reactions leading to PCs
13
using a competitive transesterification mechanism. Compared with BHEEB, the
14
secondary hydroxyl groups in OPD are relatively unreactive, the reaction of DPC with
15
BHEEB has priority over that between DPC and OPD, part of the unreacted OPD or the
16
“kicked” OPD produced in the transesterification process is inevitably eliminated at high
17
temperature under vacuum. Consequently, a 10% molar excess of OPD was used to
18
compensate the expected losses, prepolymerization reactions were performed
ACS Paragon Plus Environment
Page 13 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
under a slow nitrogen flow for a period of 10 h at 130 ºC, while polycondensation
2
reactions were carried out for 2 h at 230 ºC.
3
With the aim to estimate the effects of the catalysts on both molecular weight and
4
product appearance, besides the mostly used Zn(OAc)2, SnOBu2, Ti(OBut)4 and Sb2O3,
5
the combination of LiAcac and DMAP were also used and the catalytic activity was
6
assessed. Results suggested that the combination of LiAcac and DMAP are good
7
catalysts to afford polymers with satisfied molecular weights and product appearance.
8
SnOBu2, Ti(OBut)4 and Sb2O3 were all sluggish, while the use of Zn(OAc)2 afforded
9
severely colored polymers.
10
Based on the above results, homo-PCs PBC and POC, as well as co-PCs from OPD,
11
BHEEB and DPC, were successfully synthesized. Noteworthy, as an eco-friendly
12
alternative to phosgene for carbonylation process, DPC can be produced
13 14
Figure 2. GPC traces of synthesized PCs
15
from the phenol generated as a by-product of the polycondensation process via
16
phosgene-free methods.26 All of the obtained PCs were slightly yellow, optically clear
17
products and soluble in CHCl3 and THF at room temperature. The molecular weights of
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 38
1
all the obtained polymers were estimated using GPC (Figure 2, the baselines and the
2
solvent peaks are tailored) and the data are listed in Table 1. Obviously, all
3
polycarbonates showed moderate to good molecular weights and unimodal molecular
4
weight distributions. The Mn values consistently decreased with increasing OPD content,
5
which can be mainly ascribed to its low reactivity. Besides, the bulky ring structure of
6
OPD and high boiling point of byproduct phenol (181.9 ºC) was another causing factor,
7
because the emission of phenol became more and more difficult as the degree of
8
polymerization and melt viscosity increased during the polycondensation process at 230
9
ºC under vacuum, while raising the reaction temperatures to facilitate emission in turn led
10
to the deviation of OPD content.
11
The chemical structures of the PCs were characterized using 1H-NMR spectra, as
12
shown in Figure 3. Obviously, all resonances can be correctly assigned to the various
13
protons present in the polymer chains with matching multiplicities, and the peak intensity
14
changes gradually with the variation of the corresponding monomer fraction.
15
Table 1. Molar Composition, Molecular Weight, and Microstructure of co-PCs Molar composition
Microstructure
co-PCsa
feed molecular dyads (mol %)c Lnd Yield PC Mn Mw D BB BO OO nBC nOC Re XO XB XO XB (%) POC 87 100 0 100 0 13100 29300 2.3 PO38B62C 79 42.3 57.7 38.3 61.7 10100 17100 1.7 35.6 51.6 12.8 2.4 1.5 1.08 PO29B71C 75 32.0 68.0 28.6 71.4 12500 21500 1.7 52.4 38.2 9.4 3.7 1.5 0.94 PO16B84C 80 21.6 78.4 16.3 83.7 12700 21700 1.7 PO10B90C 71 10.9 89.1 10.2 89.8 14700 24800 1.7 PBC 86 0 100 0 100 20000 34900 1.8 aMolar composition determined by integration of the 1H NMR spectra. bNumber and weight average molecular weights in g mol-1 and dispersities measured by GPC in tetrahydrofuran against PS standards. cExperimental values obtained by means of the equations using the 13C NMR data mentioned in the text. dNumber-average sequence lengths. eRandomness index of co-PCs statistically calculated on the basis of the 13C NMR analysis.
16
weightb
In Figure 3, signals at δ 7.13, 6.81, 4.49, 4.18 and 1.63 ppm were assigned to protons 11,
ACS Paragon Plus Environment
Page 15 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
12, 9, 10 and 13 of the BHEEB moiety, respectively. For all co-PCs, the signals attributed
2
to H9 (marked with an asterisk, Figure 3), whose peak density increased with the
3
increasing of the OPD content, are split into two main peaks, indicating the different
4
chemical environment caused by the stereoisomers bearing two different secondary
5
hydroxy groups. With regard to the OPD moiety, more complicated peak split was
6
observed, apart from the increased complexity caused by the coexistence of the
7
endo-endo and endo-exo isomers of OPD, the stereoirregularity of the PC (i.e., endo-endo,
8
endo-exo, exo-exo, endo-B, exo-B) results in peak split and hence significant peak
9
overlapping in the 1H NMR spectrum. For the sake of distinction, protons of the
10
endo-endo and endo-exo isomers are numbered using Arabic numerals
11
and English letters, respectively. In the case of POC, the signals of methyne hydrogen
12
atoms g and c in the endo-exo isomer appeared at 5.19 and 5.01 ppm, respectively, while
13
the methyne hydrogen atoms 3 (7) of the endo-endo isomer gave distinctively different
14
chemical shifts at around 4.87−4.99 ppm. In contrast, in the 1H-NMR spectra of co-PCs,
15
signals at 5.19 and 5.01 ppm attributed to the endo-exo isomers almost
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2
Figure 3. 1H NMR spectra of the obtained PCs
3
disappeared because their molar fractions were rather low. The bridge protons, exocyclic
4
protons and endocyclic protons in the molecular skeleton of OPD, regardless of the types
5
of stereoisomers, exhibited overlapped multiplets at around 2.45, 2.26 and 1.69 ppm,
6
respectively. Integration of the peaks corresponding to H (g/c, 3/7) and H (11) allow us to
7
quantify the composition of the co-PCs in such units. Data provided were given in Table
8
1, where it can be seen that the content of OPD in all cases was lower than its
9
corresponding feeds; in other words, an excess of OPD is
10
necessary to obtain co-PCs with desired compositions. The molar ratio of the
11
endo-endoto endo-exo isomers in POC was analyzed by integration of the proton signals
12
arising from H(g)/H(c) and H(3)/H(7), as shown in Figure S1 in the Supporting
13
Information. The obtained result is 4.03:1, which is quite approach the initiative value of
14
4:1, indicating that the difference in reactivity between the two isomers is negligible,
15
which is consistent with our previous results.22
ACS Paragon Plus Environment
Page 16 of 38
Page 17 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
FTIR analysis was used to further investigate the structural difference among the
2 3
Figure 4. FT-IR spectra of PCs
4
synthesized polymers with various OPD molar fractions (Figure 4). All FT-IR spectra
5
show identical strong absorption band at 1750 cm-1, corresponding to the typical C=O
6
stretching vibration of the carbonate linkages. The different types of diols on the both
7
side of the carbonyl groups, BHEEB or OPD, seems have negligible effect on the
8
absorption frequency. Compared to POC, the co-PCs showed more complex absorption
9
pattern. The absorption peaks at 1612 as well as 1516 cm-1, and 833 cm-1, which are
10
absent in the FTIR spectra of POC, are attributed to the C=C stretching vibration and
11
=C-H bending vibration in the benzene ring of BHEEB, respectively.27
12
In addition, the bands at 1240 cm-1 were assigned to the asymmetric stretching of C-O-C
13
in BHEEB moiety, which is in good accordance with the reported literature.28
14
The microstructures of all the co-PCs were determined by 13C NMR spectra (Figure
15
5). Because the carbonyl carbons are more sensitive to sequence effects at the dyad level
16
than any other carbon atoms, these signals in the range of 154.4−155.1 ppm were
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
analyzed to clarify the microstructure of co-PCs as far as distribution of BHEEB and
2
OPD units along the polymer chain is concerned. As a consequence of the occurrence of
3
three dyad types and also of the two orientations of the endo-exo
4 5
Figure 5. Extended 13C NMR spectra of the carbonyl carbon region in various co-PCs
6
OPD unit, this signal is expected to be split into at least six multiple peaks in the
7
expanded 13C NMR spectrum. Nevertheless, for PO38B62C and PO29B71C, only five peaks
8
with enough resolution can be discerned, arising from the five types of diol-dyads BB,
9
BO (BOendo, BOexo) and OO (OendoOendo, OendoOexo), where B and O represent BHEEB
10
and OPD units, respectively. The sixth peak attributed to the OexoOexo diol-dyad, however,
11
is not observed because of its low content. By the same reason, for PO16B84C, only four
12
peaks were present in the carbonyl carbon region, corresponding to the BB, BOendo, BOexo
13
and OendoOendo diol-dyads. With regard to PO10B90C, in which the OPD content is the
14
lowest, only two peaks corresponding to the BB and BOendo were detected. To figure out
15
the dyad contents as precisely as possible, the
16
PO29B71C were chosen and integration of the relevant peaks were performed. Based on
17
these values, the number-average sequence lengths (n) and the degree of randomness (R)
13C
NMR spectra of PO38B62C and
ACS Paragon Plus Environment
Page 18 of 38
Page 19 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
were estimated using the following equations,29 where NBC/OC, NBC/BC and NOC/OC
2
represent molar fraction of dyads, calculated from the integral intensities of signals of
3
carbonyl carbon from BO (or OB), BB, and OO dyads, respectively. nBC and nOC are the
4
number-average sequence length of BHEEB carbonate (BC) unit and OPD carbonate
5
(OC) unit, respectively. Data obtained are summarized in Table 1. Results indicated that
6
the value of R is close to 1 in both cases, leading to the conclusion that the microstructure
7
of PO38B62C and PO29B71C was essentially random. This conclusion was in good
8
agreement with those statistically calculated for the random co-PCs based on OPD and a
9
series of aliphatic or alicyclic diols reported in our previous paper,22 and can be
10
reasonably extended to PO16B84C and PO10B90C in this study.
11
𝑛BC =
12
𝑛OC =
13
𝑁BC/OC + 2𝑁BC/BC 𝑁BC/OC 𝑁BC/OC + 2𝑁OC/OC
𝑅=
𝑁BC/OC
1
𝑛BC +
1
(1) (2)
𝑛OC(3)
14
Thermal properties
15
The thermal stability of the synthesized PCs was comparatively investigated using
16
thermogravimetric analysis (TGA). TGA and TGA derivative curves of all polymers,
17
measured from 50 to 600 ºC under an inert nitrogen atmosphere, are shown in Figure 6.
18
The values of T5% and Td of the PCs are presented in Table 2. As expected, PBC exhibited
19
the highest thermal stability among all the polymers due to the excellent thermal stability
20
of BHEEB: thermal decomposition started to be detectable at about 295 ºC with onset
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 38
1
temperature (measured for 5% of weight loss) as high as 350 ºC. A
2
two-step pyrolysis profile was observed for PBC, where the second one appears as a
3
shoulder of the first peak, with maximal decomposition rates at 395 and 422 ºC,
4
respectively. The first step can be attributed to the decomposition of carbonate linkage,
5
and the second step should be mainly caused by the degradation of the ether linkage
6 7
Figure 6. TGA traces of PCs at a heating rate of 10 °C min-1
8
in BHEEB. In contrast, POC showed a notable reduction in the thermal stability with a T5%
9
value 74 ºC lower than that of PBC. Furthermore, its thermal decomposition was found to
10
happen in a single step with the maximum rate at 312 ºC. Although thus far we have been
11
unsuccessful in elucidating this relatively lower thermal stability, it is reasonable to
12
assume
that
McLafferty-type
rearrangement
similar
ACS Paragon Plus Environment
to
the
thermolysis
of
Page 21 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
isosorbide-containing PC is involved, as reported by Lee.30 With regards to co-PCs, as
2
expected, the thermal stability is tightly dependent on the molar ratios of BHEEB and
3
OPD units in the polymer chains. In fact, the replacement of BHEEB by OPD caused an
4
evenly decreasing effect in both onset and maximum decomposition rate temperature.
5
Furthermore, decomposition was found to proceed along three well differentiated stages,
6
which can be attributed to the weight loss of OC, BC short sequence, and ether linkage in
7
BHEEB, respectively.
8 9
Figure 7. Second heating DSC curves of PCs measured at a heating rate of 10 ºC min-1
10
In addition, the thermal behaviors of these PCs were determined by DSC at a
11
heating rate of 10 ºC min-1. The second DSC heating curves measured from 30–120 ºC
12
are shown in Figure 7, the thermal data are summarized in Table 2. A remarkable feature
13
of all samples is their amorphous structures with single-step glass transition temperatures.
14
PBC and POC have the lowest and the highest Tg values among all the polymers, which
15
were 54.7 ºC and 74.5 ºC, respectively, POxByCs have intermediate values between PBC
16
and POC that increased steadily with the increasing of OPD molar fraction (Figure 8).
17
For PBC, its amorphous feature is understandable because of the low packing ability of
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
BHEEB, which was caused by the presence of isopropyl groups and the rotation of
2
benzene rings in it. For co-PCs POxByCs, their amorphous feature is an expected result
3
considering the poor crystallization ability of the corresponding homo-PC (PBC and
4
POC). Moreover, their random structures determined by microstructure analysis is also
5
responsible for their amorphous features, because the regularity of the polymer chains
6
plays an important role in the crystallization.31 In the case of POC, the amorphous
7
characteristic and relatively lower Tg value is in sharp contrast with the results exhibited
8
by its analogue (abbreviated as pre-POC) reported in our previous article.22 In that case,
9
pre-POC
10 11
Figure 8. The variation tendencies of PCs’ Tg
12
composed of a mixture of two stereoisomers (endo-exo:endo-endo = 1:9) prepared in a
13
different synthetic protocol, was found to be semicrystalline with Tm and Tg of 109.1 and
14
80.4 ºC, respectively. Given that the main structural difference between POC and
15
pre-POC lies in the molar fraction of endo-exo isomers, which are 20 mol% and 10 mol%,
16
respectively, we speculate that the amorphous feature observed for POC find its origin in
17
the higher proportion of the endo-exo isomers. In fact, OPD is a conformationally
ACS Paragon Plus Environment
Page 22 of 38
Page 23 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
restricted diol that hard to crystallize due to its V-shaped bicyclic frame and the
2
puckering of the cyclopentane rings in it.22 Moreover, the molecular symmetry is another
3
important factor. Homo-PC based on the endo-endo isomers is prone to crystallize.
4
However, the incorporation of the endo-exo isomers will generate stereoirregular
5
structures due to its asymmetry, thus dramatically depress the crystalline ability of the
6
polymer chains: when the endo-exo isomer content is below 10 mol%, pre-POC is
7
semicrystalline; when this value is increased to 20 mol%, amorphous characteristic is
8
observed for POC because this proportion is high enough to prevent crystallization.
9
Concerning the Tg for POC, note that it has a Mn of 13100 g mol-1, which is about twice
10
of the value for pre-POC (Mn = 6700 g mol-1), a higher Tg is expected because Tg is
11
directly influenced by the polymer chain length.32 However,
12 13
Table 2 Thermal and mechanical properties of the synthesized PCs measured by TGA, DSC and DMA TGAa PCs
T5%
POC PO38B62C PO29B71C PO16B84C PO10B90C PBC aT
5%
(ºC)a
276 277 282 283 310 350
DSC Td
(ºC)a
312 294/378 296/383 301/384 306/394 395/422
Tg
(ºC)b
74.5 65.8 65.2 63.7 59.4 54.7
DMA E′ (20 ºC) (MPa)
Tg (ºC)c
−d − − 925 1063 1241
− − − 68.1 64.5 60.1
= temperature of 5% mass loss, Td = temperature for maximal decomposition rate. bTg = glass transition
temperature obtained from DSC during second heating at 10 ºC min-1. cDetermined using a TA DMA 2928 in a controlled force-tension film mode with a preload force of 0.1 N, an amplitude of 10 μm, and at a fixed frequency of 1 Hz at the range of -140 to 140 ºC in a heating rate of 3 ºC min-1. dNot determined due to their brittleness.
14
a significantly lower Tg was observed for POC (74.5 ºC vs. 80.4 ºC). Obviously, the
15
endo-exo isomers impart less rigidity to the polymer chains than the endo-endo isomers
16
and are thus detrimental to the Tg of the polymer. To further elucidate this apparent
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 24 of 38
1
discrepancy, comparisons of a relevant series of isomeric polycondensates based on
2
isosorbide
3
2,2,4,4-tetramethyl-1,3-cyclobutanediol (CBDO, cis-/trans-) were conducted and similar
4
thermal transition tendencies were observed. Storbeck reported the preparation of
5
aromatic polyesters from 2,5-furandicarboxylic acid and isohexides and indicated that the
6
isomannide-based polyester has a higher Tg than the corresponding isosorbide-based
7
polyester with similar molecular weight. However, the reason was not analyzed.33 Nash
8
et.al
9
2,2,4,4-tetramethyl-1,3-cyclobutanediol (CBDO, cis-/trans-) and 1,3-propanediol, and
10
claimed that the cis-rich CBDO-based copolymer has higher Tg than the corresponding
11
trans-rich CBDO-based copolymer. Investigations on the structure-property ascribed the
12
higher Tg for the former to the formation of randomly coiled polymer chains, which was
13
caused by the kinks due to the molecular geometry associated with the cis-cyclobutane
14
ring.34 Similarly, the endo-endo and endo-exo isomer of OPD can be regarded as cis- and
15
trans-, respectively. The endo-endo isomer, having both carbonate linkages on the same
16
side of the bicycle frame, tends to induce kinked polymer chains, this could result in
17
more rigid, bent and sterically hindered structures, consequently stiffens the polymer
18
similar to corrugation. Given that the molar content of the endo-endo isomers in POC is
19
lower than that in pre-POC, we believe this could be the reason explaining why POC in
20
turn afforded lower Tg, despite having much higher Mn than the latter.
21
Dynamic mechanical analysis (DMA)
(endo-exo),
synthesized
a
isomannide
series
of
terephthalate
ACS Paragon Plus Environment
(endo-endo)
copolyesters
and
from
Page 25 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
To gain insight into the effect of composition changes on the viscoelastic property, PBC,
2
PO10B90C and PO16B84C were all investigated by DMA. For PO29B71C, PO38B62C and
3
POC with relatively high OPD content, DMA tests were not performed due to their
4
brittleness. The thermo-mechanical data are recorded in Table 2, the storage modulus (E′)
5
and the loss factor tan δ as a function of temperature are shown in Figure 9 (a) and (b),
6
respectively. A drastic decrease in the E′ for all the tested samples was observed after
7
heating above Tg, further confirming their amorphous structures. Generally speaking, the
8
value of E′ tend to increase with increasing the rigid monomer content provided that the
9
samples have similar Mn.17 However, PO10B90C exhibited nearly identical E′ curve to that
10
of PBC in the whole temperature range, which can be ascribed to the combined effects of
11
its lower Mn compared to the latter and the low molar content of OPD units. In the case of
12
PO16B84C, a much lower E′ was observed, despite having the highest OPD content among
13
them, this is
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2
Figure 9. Variation of (a) E′, and (b) tan δ with temperature for PBC, PO10B90C and PO16B84C.
3
understandable because its Mn is the lowest and this value is not enough to afford E′
4
comparable to PO10B90C and PBC. In Figure 9 (b), all samples showed relaxation peaks
5
above 50 ºC, which can be ascribed to the transition from glass to rubber, the temperature
6
where the tan δ reached the maximum was defined as the Tg of the polymer samples.
7
Obviously, the Tg values determined by DMA are slightly higher than that from DSC
8
(Table 2), which can be correlated with the heat transporting hysteresis for large-scale
9
samples in DMA. As expected, the Tgs shifted to higher temperatures with increasing
10
OPD content, which was in good accordance with the results from DSC. The increased Tg
11
reflected by DMA can be interpreted by the increased rigidity induced by OPD, which
12
increased the motion resistance of the chain segments. Moreover, the tan δ curves for
ACS Paragon Plus Environment
Page 26 of 38
Page 27 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
PO10B90C and PBC show low temperature transitions at around 40 ºC. The reason for this
2
inconspicuous transition is not obvious to us, the oligomers that contained in the resultant
3
polymers may be the reason and further investigation should be carried out.
4
Tensile properties
5
To evaluate the influence of the composition on the mechanical properties, tensile tests
6
were performed using the films prepared by casting as described in the Experimental
7
Section, the Young’s modulus, ultimate tensile strength and elongation at break are given
8
in Table 3, the recorded stress-strain curves are depicted in Figure 10. In general
9
polymeric materials, the mechanical property is mainly affected by molecular structure
10
and Mn. In consequence, PBC showed excellent Young’s modulus, ultimate tensile
11
strength, and elongation at break, which were 452.1 MPa, 11.2 MPa, and 19.5%,
12
respectively. The excellent mechanical property of PBC is presumably due to a
13
combination of its high molecular weight, moderate rigidity of molecular chain and
14
superior toughness caused by the BHEEB moiety. However, for POxByC, a
15
“ductile−to−brittle” transition occurred as the OPD content increased, resulting in a
16
substantial reduction in the tensile strength and extensibility. For PO10B90C and PO16B84C,
17
the ultimate strength was 6.3 and 3.5 MPa, the elongation at break was 12.6% and 7.9%,
18
respectively. This phenomenon can be ascribed to two reasons. Firstly, compared to PBC,
19
their lower Mn values in the range of 10000−15000 g mol-1 were not high enough to
20
exhibit satisfactory mechanical strength because it was strongly influenced by Mn.
21
Secondly, the brittleness caused by OPD is a common characteristic of rigid polymers,
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 28 of 38
1
even at rather large molecular weights.17 In fact, the brittleness of glassy amorphous
2
polymers can be ascribed to the low entangled strand
3 4
Figure 10. Stress-strain curves of polymers at 25 °C and 3 mm s-1
5
density due to the rather stiff polymer chains, which predisposes the glassy polymer to
6
form weak crazes that break down readily to form cracks.35 Future studies will focus on
7
enhancing extensibility for thermally stable, bio-based plastic alternatives.
8
9
Table 3 Mechanical properties of PCs PCs
Young’s modulus (MPa)
Ultimate strength (MPa)
Strain at break (%)
PO16B84C
500.9 ± 11.3
3.5 ± 0.3
7.9 ± 1.3
PO10B90C
339.5 ± 39.0
6.3 ± 0.2
12.6 ± 1.1
PBC
452.1 ± 9.5
11.2 ± 0.9
19.5 ± 3.0
CONCLUSIONS
10
In conclusion, a series of homo-PCs and co-PCs that combine the chemical recycling of
11
BPA-PC with the use of novel bicyclic diol OPD, which is derived from naturally
12
occurring citric acid, has been successfully synthesized. Single crystal X-ray identified
13
the distinctive V-shaped skeleton of the endo-endo isomer of OPD composed of two
14
cis-fused cyclopentane rings similar to isohexides. By melt polymerization of different
15
molar feed ratios of OPD and BHEEB, co-PCs with relatively high molecular weights
ACS Paragon Plus Environment
Page 29 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
were obtained in good yields. 1H NMR spectrum showed that the molar ratio of the
2
endo-endo and the endo-exo isomers in POC is close to 4:1, which is identical to the
3
initial value in OPD, confirming pretty similar reactivity. For POxByCs, the OPD content
4
are consistently lower than the initial feed ratio, which was caused by the lower reactivity
5
of OPD compared to BHEEB. Analysis of the dyad sequence distributions using the
6
expanded
7
measurements showed that all samples are amorphous with Tg values in the order of PBC
8
< POxByC < POC. For POxByCs, their Tg values increased steadily with the increasing of
9
OPD molar fraction, further confirming the excellent rigidity of OPD. In contrast with the
10
semicrystalline pre-POC, amorphous characteristic with a lower Tg of 74.5 ºC is observed
11
for POC, which is presumably caused by the variations in molecular geometry around the
12
different isomer sites. With the increasing of the OPD content in POxByC, a
13
“ductile−to−brittle” transition occurred, a result caused by the combined effects of low
14
molecular weights and the low entangled strand density due to the rather stiff polymer
15
chains. We are currently modifying the brittleness of POC using other flexible monomers
16
or polymers, by copolymerization or melt-blending, this will be addressed in our future
17
work.
18
Supporting Information
19
Synthetic routes of OPD from citric acid; 1H-NMR spectrum of POC; Crystal data and
20
structure refinement for the endo-endo OPD.
21
Conflicts of interest
22
There are no conflicts to declare.
23
Acknowledgement
13C
NMR spectra revealed the random microstructures for all co-PCs. DSC
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 30 of 38
1
We are grateful to the National Natural Science Foundation of China (No. 51503150 &
2
No. 21674080), Tianjin Municipal Natural Science Foundation (No. 17JCQNJC03400 &
3
18JCZDJC37700), Training Project of Innovation Team of Colleges and Universities in
4
Tianjin (TD13-5020), 131 talents program of Tianjin, and the leading talents program of
5
Tianjin Educational Committee.
6
Notes and references
7
(1) Nguyen, H. T. H.; Qi, P.; Rostagno, M.; Feteha, A.; Miller, S. A., The quest for high
8
glass transition temperature bioplastics. J. Mater. Chem. A 2018, 6 (20), 9298-9331, DOI
9
10.1039/C8TA00377G.
10
(2) Schneiderman, D. K.; Hillmyer, M. A., 50th Anniversary Perspective: There Is a
11
Great Future in Sustainable Polymers. Macromolecules 2017, 50 (10), 3733-3749, DOI
12
10.1021/acs.macromol.7b00293.
13
(3) Rabnawaz, M.; Wyman, I.; Auras, R.; Cheng, S., A roadmap towards green packaging:
14
the current status and future outlook for polyesters in the packaging industry. Green
15
Chem. 2017, 19 (20), 4737-4753, DOI 10.1039/C7GC02521A.
16
(4) Upton, B. M.; Kasko, A. M., Strategies for the Conversion of Lignin to High-Value
17
Polymeric Materials: Review and Perspective. Chem. Rev. 2016, 116 (4), 2275-2306,
18
DOI 10.1021/acs.chemrev.5b00345.
19
(5) Lotti, N.; Colonna, M.; Fiorini, M.; Finelli, L.; Berti, C., Poly(butylene terephthalate)
20
modified with ethoxylated bisphenol S with increased glass transition temperature and
21
improved
22
10.1016/j.polymer.2011.01.018.
thermal
stability.
Polymer
2011,
ACS Paragon Plus Environment
52
(4),
904-911,
DOI
Page 31 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
(6) Gioia, C.; Vannini, M.; Marchese, P.; Minesso, A.; Cavalieri, R.; Colonna, M.; Celli,
2
A., Sustainable polyesters for powder coating applications from recycled PET, isosorbide
3
and succinic acid. Green Chem. 2014, 16 (4), 1807-1815, DOI 10.1039/C3GC42122H.
4
(7) Berti, C.; Colonna, M.; Fiorini, M.; Lorenzetti, C.; Marchese, P., Chemical
5
Modification of Terephthalate Polyesters by Reaction with Bis(hydroxyethyl ether) of
6
Bisphenol
7
10.1002/mame.200300111.
8
(8) Gross, S. M.; Roberts, G. W.; Kiserow, D. J.; DeSimone, J. M., Synthesis of High
9
Molecular Weight Polycarbonate by Solid-State Polymerization. Macromolecules 2001,
A.
Macromol.
Mater.
Eng.
2004,
289
(1),
49-55,
DOI
10
34 (12), 3916-3920, DOI 10.1021/ma001958h.
11
(9) Dieter, F.; Gerd, F.; Leo, M., Routes to New Aromatic Polycarbonates with Special
12
Material Properties. Angew. Chem. Int. Ed., 1991, 30 (12), 1598-1610, DOI
13
10.1002/anie.199115981.
14
(10)
15
Characterization of Renewable Poly(hydroxy)urethanes from Syringaresinol. ACS
16
Sustainable Chem. Eng. 2017, 5 (10), 8648-8656, DOI 10.1021/acssuschemeng.7b01271.
17
(11) Choi, G.-H.; Hwang, D. Y.; Suh, D. H., High Thermal Stability of Bio-Based
18
Polycarbonates Containing Cyclic Ketal Moieties. Macromolecules 2015, 48 (19),
19
6839-6845, DOI 10.1021/acs.macromol.5b01112.
20
(12) Munoz-Guerra, S.; Lavilla, C.; Japu, C.; Martinez de Ilarduya, A., Renewable
21
terephthalate polyesters from carbohydrate-based bicyclic monomers. Green Chem. 2014,
22
16 (4), 1716-1739, DOI 10.1039/C3GC42394H.
Janvier,
M.;
Ducrot,
P.-H.;
Allais,
F.,
Isocyanate-Free
ACS Paragon Plus Environment
Synthesis
and
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 32 of 38
1
(13) Lavilla, C.; Martinez de Ilarduya, A.; Alla, A.; García-Martín, M. G.; Galbis, J. A.;
2
Muñoz-Guerra, S., Bio-Based Aromatic Polyesters from a Novel Bicyclic Diol Derived
3
from d-Mannitol. Macromolecules 2012, 45 (20), 8257-8266, DOI 10.1021/ma3013288.
4
(14) Fenouillot, F.; Rousseau, A.; Colomines, G.; Saint-Loup, R.; Pascault, J. P.,
5
Polymers from renewable 1,4:3,6-dianhydrohexitols (isosorbide, isomannide and
6
isoidide):
7
10.1016/j.progpolymsci.2009.10.001.
8
(15) Beller, M.; Centi, G.; Sun, L., Cover Picture: Chemistry Future: Priorities and
9
Opportunities from the Sustainability Perspective. ChemSusChem 2017, 10 (1), 6-13,
A
review.
Prog.
Polym.
Sci.
2010,
35
(5),
578-622,
DOI
10
DOI 10.1002/cssc.201601739.
11
(16) Nôtre, J. L.; Haveren, J. v.; Es, D. S. v., Synthesis of Isoidide through Epimerization
12
of Isosorbide using Ruthenium on Carbon. ChemSusChem 2013, 6 (4), 693-700, DOI
13
10.1002/cssc.201200714.
14
(17) Park, S.-A.; Choi, J.; Ju, S.; Jegal, J.; Lee, K. M.; Hwang, S. Y.; Oh, D. X.; Park, J.,
15
Copolycarbonates of bio-based rigid isosorbide and flexible 1,4-cyclohexanedimethanol:
16
Merits over bisphenol-A based polycarbonates. Polymer 2017, 116, 153-159, DOI
17
10.1016/j.polymer.2017.03.077
18
(18) Chatti, S.; Schwarz, G.; Kricheldorf, H. R., Cyclic and Noncyclic Polycarbonates of
19
Isosorbide (1,4:3,6-Dianhydro-d-glucitol). Macromolecules 2006, 39 (26), 9064-9070,
20
DOI 10.1021/ma0606051.
21
(19) Lebarbé, T.; Maisonneuve, L.; Nguyen, T. H. N.; Gadenne, B.; Alfos, C.; Cramail,
22
H., Methyl 10-undecenoate as a raw material for the synthesis of renewable
ACS Paragon Plus Environment
Page 33 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
semi-crystalline polyesters and poly(ester-amide)s. Polym. Chem. 2012, 3 (10),
2
2842-2851, DOI 10.1039/C2PY20394D.
3
(20) Yokoe, M.; Aoi, K.; Okada, M., Biodegradable polymers based on renewable
4
resources.
5
1,4:3,6-dianhydrohexitols and aliphatic diols. J. Polym. Sci., Part A: Polym. Chem. 2003,
6
41 (15), 2312-2321, DOI 10.1002/pola.10772.
7
(21) Yoon, W. J.; Hwang, S. Y.; Koo, J. M.; Lee, Y. J.; Lee, S. U.; Im, S. S., Synthesis
8
and Characteristics of a Biobased High-Tg Terpolyester of Isosorbide, Ethylene Glycol,
9
and 1,4-Cyclohexane Dimethanol: Effect of Ethylene Glycol as a Chain Linker on
VII.
Novel
random
and
alternating
copolycarbonates
from
10
Polymerization. Macromolecules 2013, 46 (18), 7219-7231, DOI 10.1021/ma4015092.
11
(22) Liu, X.; Pang, C.; Ma, J.; Gao, H., Random Copolycarbonates Based on a
12
Renewable Bicyclic Diol Derived from Citric Acid. Macromolecules 2017, 50 (20),
13
7949-7958, DOI 10.1021/acs.macromol.7b01641.
14
(23) Li, X.; Yee, A. F., Design of Mechanically Robust High-Tg Polymers: Synthesis
15
and Dynamic Mechanical Relaxation Behavior of Glassy Poly(ester carbonate)s with
16
Cyclohexylene Rings in the Backbone. Macromolecules 2003, 36 (25), 9411-9420, DOI
17
10.1021/ma034440x.
18
(24) Gioia, C.; Vannini, M.; Celli, A.; Colonna, M.; Minesso, A., Chemical recycling of
19
post-consumer compact discs towards novel polymers for powder coating applications.
20
RSC Adv. 2016, 6 (37), 31462-31469, DOI 10.1039/C6RA06147H.
21
(25) Muesmann, T. W. T.; Wickleder, M. S.; Zitzer, C.; Christoffers, J.,
22
Octahydropentalene 2,5-Disulfonic Acid – A New Linker Molecule for Coordination
23
Polymers. Synlett 2013, 24 (8), 959-962, DOI 10.1055/s-0032-1317806.
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 34 of 38
1
(26) Ishii, H.; Ueda, M.; Takeuchi, K.; Asai, M., Oxidative carbonylation of phenol to
2
diphenyl carbonate catalyzed by bis(benzonitrile)dichloropalladium in the presence of
3
polyvinylpyrrolidone.
4
10.1016/S1566-7367(01)00002-4.
5
(27) Al-Hamouz, O. C. S.; Sweileh, B. A.; Al-Salah, H. A., Synthesis and
6
characterization of polycarbonates by melt-phase interchange reactions with alkylene and
7
arylene diphenyl dicarbonates. J. Appl. Polym. Sci. 2006, 102 (4), 3597-3609, DOI
8
10.1002/app.23996.
9
(28) Al-Qalawi, H. R.; Sweileh, B. A.; Kailani, M. H., Synthesis and characterization of
10
poly(ether carbonate)s by melt-phase interchange reactions of dihydroxy compounds with
11
alkylene and arylene diphenyl dicarbonates containing ether groups. J. Appl. Polym. Sci.
12
2012, 126 (5), 1650-1663, DOI 10.1002/app.36945.
13
(29) Duan, R.-T.; He, Q.-X.; Dong, X.; Li, D.-F.; Wang, X.-L.; Wang, Y.-Z., Renewable
14
Sugar-Based Diols with Different Rigid Structure: Comparable Investigation on
15
Improving Poly(butylene succinate) Performance. ACS Sustainable Chem. Eng. 2016, 4
16
(1), 350-362, DOI 10.1021/acssuschemeng.5b01335.
17
(30) Lee, J.; Lee, S.; Yoon, D.; Yoon, W. J.; Im, S. S.; Moon, B.; Oh, H. B., Tandem
18
mass spectrometric analysis of isosorbide-1,4-cyclohexane-dicarboxylic acid polyester
19
oligomer cations using ion-trap mass spectrometry. Rapid Commun. Mass Spectrom.
20
2013, 27 (17), 1913-1918, DOI 10.1002/rcm.6645.
21
(31) Park, J. E.; Hwang, D. Y.; Choi, G. H.; Choi, K. H.; Suh, D. H., Fast Hydrolysis
22
Polyesters with a Rigid Cyclic Diol from Camphor. Biomacromolecules 2017, 18 (8),
23
2633-2639, DOI 10.1021/acs.biomac.7b00761.
Catal.
Commun.
2001,
ACS Paragon Plus Environment
2
(1),
17-22,
DOI
Page 35 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
(32) Okada, M.; Tsunoda, K.; Tachikawa, K.; Aoi, K., Biodegradable polymers based on
2
renewable resources. IV. Enzymatic degradation of polyesters composed of
3
1,4:3.6-dianhydro-D-glucitol and aliphatic dicarboxylic acid moieties. J. Appl. Polym. Sci.
4
2000,
5
10.1002/(SICI)1097-4628(20000711)77:23.0.CO;2-C.
6
(33) Storbeck, R.; Ballauff, M., Synthesis and properties of polyesters based on
7
2,5-furandicarboxylic acid and 1,4:3,6-dianhydrohexitols. Polymer 1993, 34 (23),
8
5003-5006, DOI 10.1016/0032-3861(93)90037-B.
9
(34) Nash, Y.; Nash, T. L.; Henderson, B.; Duraia, E.-S. M.; Powell, C. E.; Sanderson, B.;
10
Beall, G. W., Study of the structure–property relationships in a high impact and shape
11
memory polyester by the stereoisomer selection of the cyclobutane diol monomer. J.
12
Mater. Sci. 2013, 48 (24), 8588-8595, DOI 10.1007/s10853-013-7685-y.
13
(35) Ryu, C. Y.; Ruokolainen, J.; Fredrickson, G. H.; Kramer, E. J.; Hahn, S. F., Chain
14
Architecture Effects on Deformation and Fracture of Block Copolymers with
15
Unentangled
16
10.1021/ma011576r.
77
Matrices.
(2),
Macromolecules
338-346,
2002,
35
17 18 19 20 21 22 23
ACS Paragon Plus Environment
(6),
DOI
2157-2166,
DOI
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2 3 4 5 6 7 8 9 10 11 12 13
For Table of Contents Use Only
14 15
A series of polycarbonates that combine the chemical recycling of BPA-PC with the use
16
of citric acid-based bicyclic octahydro-2,5-pentalenediol (OPD) were successfully
17
prepared, which showed potential as alternative candidate to replace petroleum-based
18
high-Tg polymers.
ACS Paragon Plus Environment
Page 36 of 38
Page 37 of 38 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
For Table of Contents Use Only
Sustainable polycarbonates from a citric acid-based rigid diol and recycled BPA-PC: From Synthesis to Properties
Chengcai Pang*, Xueshuang Jiang, Yan Yu, Xiaohan Liu, Jingyan Lian, Jianbiao Ma, and Hui Gao*
A series of polycarbonates that combine the chemical recycling of BPA-PC with the use of citric acid-based bicyclic octahydro-2,5-pentalenediol (OPD) were successfully prepared, which showed potential as alternative candidate to replace petroleum-based high-Tg polymers.