Transformation of 2D Planes into 3D Soft and Flexible Structures with Embedded Electrical Functionality Hyunmin Moon, Namsun Chou, Hee Won Seo, Kyeongyeon Lee, Jinhee Park, and Sohee Kim ACS Appl. Mater. Interfaces, Just Accepted Manuscript • DOI: 10.1021/acsami.9b09578 • Publication Date (Web): 21 Aug 2019 Downloaded from pubs.acs.org on August 21, 2019
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
Transformation of 2D Planes into 3D Soft and
2
Flexible
3
Functionality
4
AUTHOR NAMES
5
Hyunmin Moon,† Namsun Chou,‡ Hee Won Seo,† Kyeongyeon Lee,† Jinhee Park,§ and
6
Sohee Kim*,†
7
AUTHOR ADDRESS
8
†Department
9
Technology (DGIST), Daegu, 42988, Republic of Korea
Structures
with
Embedded
Electrical
of Robotics Engineering, Daegu Gyeongbuk Institute of Science and
10
‡Center
for BioMicroSystems, Korea Institute of Science and Technology (KIST), Seoul,
11
02792, Republic of Korea
ACS Paragon Plus Environment
1
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
§Department
2
Technology (DGIST), Daegu, 42988, Republic of Korea
3
KEYWORDS
4
flexible and soft 3D structure, selective bonding, PDMS, parylene-C, MEMS
Page 2 of 52
of Emerging Materials Science, Daegu Gyeongbuk Institute of Science and
5
ACS Paragon Plus Environment
2
Page 3 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
ABSTRACT
2
Three-dimensional (3D) structures composed of flexible and soft materials have been in
3
demand for implantable biomedical devices. However, the fabrication of 3D structures
4
using MEMS techniques has limitations in terms of the materials and the scale of the
5
structures. Here, a technique to selectively bond polydimethylsiloxane (PDMS) and
6
parylene-C by plasma treatment is reported, with which 2D structures that are fabricated
7
using micro electro mechanical systems (MEMS) techniques are turned into 3D structures
8
by the inflation of selectively non-bonded patterns. The bonding strength and the bonding
9
mechanism were analyzed by mechanical tests and chemical analyses, respectively. We
10
fabricated soft and flexible 3D structures with various patterns and dimensions, even with
11
embedded electrical functions, including light emitting diodes and electrocorticogram
12
electrodes. Based on these results, the flexible, soft, and MEMS-capable 3D structures
13
that are obtained by the developed selective bonding technique are promising for
14
applications in a wide range of biomedical applications.
ACS Paragon Plus Environment
3
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 52
1
TEXT
2
1. Introduction
3
Three-dimensional (3D) structures are desirable for many applications, such as
4
biomedical electrodes,1-6 biomedical scaffolds,7-10 microelectromechanical systems
5
(MEMS),11-14 batteries,15-19 and further novel structure fabrication.20-22 3D structures with
6
various functions and dimensions, from the nanoscale to the microscale, have satisfied
7
the requirements for research purposes. Despite such efforts towards the generation of
8
3D structures, there are still problems that remain.23,24 The types of materials that are
9
used for MEMS fabrications, such as photolithography, are limited to inorganic silicon.
10
Additionally, because MEMS techniques conventionally aim for elaboration and
11
miniaturization, the feature size of the generated 3D structures is limited to the nanoscale
12
to microscale ranges.
13
Recently, as a solution for the limited scale of 3D structures, a membrane of silicon
14
(as a body) and a polymer of SU-8 (as an epoxy) were used to generate 3D structures.24,25
15
The MEMS techniques were processed on a two-dimensional (2D) plane, and
ACS Paragon Plus Environment
4
Page 5 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
mesostructures were fabricated by induced compressive buckling. However, although
2
fabricating mesoscale structures was possible, the selection of materials is still limited to
3
inorganic materials, namely, silicon. On the other hand, Whiteside and his colleagues
4
have fabricated a 3D structure for a gaiting robot entirely consisting of soft materials such
5
as polydimethylsiloxane (PDMS) and Ecoflex.26,27 They fabricated the 3D structure using
6
a molding technique and bonding of the top and bottom layers. However, the elaborate
7
alignment between the top and bottom layers during bonding was challenging, and further
8
MEMS processes on the fabricated device were not possible.
9
In particular, in the study of implantable biomedical devices such as neural interfaces,
10
biocompatibility is one of the essential considerations for the selection of materials.
11
Moreover, because of the mechanical properties similar to biological tissues, flexible and
12
soft polymers are given priority over stiff and inorganic materials as the device material.
13
Hence, we developed a novel technique that can transform 2D planar structures into 3D
14
structures by selective bonding between PDMS and parylene-C through plasma
15
treatment on the selected areas. Both materials have the highest biocompatibility of USP
ACS Paragon Plus Environment
5
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 52
1
class VI, high flexibility, and low stiffness. Moreover, this technique enables bonding in
2
one process because plasma is selectively treated on the top surface of the entire
3
structure, unlike other techniques that require bonding of two layers with elaborate
4
alignment. For this reason, additional MEMS processes are possible after the bonding
5
between layers. After extensive mechanical and chemical analyses, we fabricated various
6
3D structures by the inflation of non-bonded areas (hereafter referred to as ‘balloons’)
7
created by the selective bonding technique. Moreover, 3D structures including electrical
8
functions, such as light emitting diodes (LEDs) or electrocorticogram (ECoG) electrodes,
9
were also fabricated by using MEMS processes after the selective bonding step. All
10
electrical connections remained intact after the inflation of balloons, resulting in
11
electrically functional, soft and flexible 3D structures in mesoscale. With flexible, soft, and
12
biocompatible properties of the used materials, we expect that the flexible 3D electronic
13
devices fabricated by the selective bonding technique can be used for various biomedical
14
applications.
ACS Paragon Plus Environment
6
Page 7 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
ACS Applied Materials & Interfaces
2. Results and discussion
2
2.1. Soft and flexible 3D structures that integrate electrical functions. Figure 1a shows
3
the principle to fabricate a 3D soft and flexible structure with embedded conductive lines.
4
Owing to the flexibility and stretchability of the used materials, the non-bonded area
5
inflates upon fluid injection, creating a 3D structure. Prior to the fluid injection, conductive
6
lines and patterns can be formed on the 2D plane, just as the conventional MEMS
7
processes. At the bonded area, the PDMS layer adheres covalently onto the parylene-C
8
layer because the hydroxyl and carboxyl groups are terminated at the surface of PDMS
9
and parylene-C, respectively. These groups form a covalent bond between PDMS and
10
parylene-C. More details of the bonding mechanism are presented in Section 2.4. Figure
11
1b shows the method of selective bonding between PDMS and parylene-C. The whole
12
structure consists of a PDMS layer, a parylene-C layer, and a second PDMS layer with
13
thicknesses of 180 μm, 1 μm, and 180 μm, respectively. The first PDMS layer and
14
parylene-C layer adhere firmly during the deposition of parylene-C onto PDMS. Generally,
15
PDMS on the parylene-C layer does not adhere well due to the hydrophobicity of
ACS Paragon Plus Environment
7
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 52
1
parylene-C. However, we developed a technique for selective bonding between PDMS
2
and parylene-C using nitrogen and oxygen plasma treatment. By masking the plasma,
3
non-bonded areas are generated where PDMS and parylene-C can easily detach from
4
each other if enough force is applied. Figure 1c shows the method of fluid injection into
5
the non-bonded areas. A soft and flexible 3D structured device is demonstrated, which
6
was generated by the injection of red-stained liquid into the non-bonded area (Movie S1).
7
More details regarding the methods of selective bonding and fluid injection are explained
8
in Figures S1 and S2, respectively.
9
2.2. Adhesion evaluation depending on plasma conditions. Plasma conditions
10
(nitrogen flow rate, oxygen flow rate, power, and treatment time) enormously affect the
11
bonding strength. We investigated the different plasma conditions as summarized in
12
Table S1. Samples were evaluated by T-peeling tests following ASTM D1876-08 (n=3 for
13
each plasma condition).28 The T-peeling test method is explained in Experimental Section.
14
The samples were prepared such that the region with a length of 15 mm was not treated
15
by plasma and the region with a length of 20 mm was treated by plasma (Figure 2a). We
ACS Paragon Plus Environment
8
Page 9 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
measured the peeling force between the second PDMS layer and the parylene-C layer,
2
as shown in Figure 2b-e. A little force was measured during the first 30 mm of stage
3
movement, in which the non-treated area of the sample was peeled off. The force then
4
started to increase with no detachment of the bonded area at the ‘location of detachment’,
5
where the plasma-treated area began. After that, no increase in force was observed
6
during detachment of the plasma-treated area and then, the force abruptly increased
7
before the layers were entirely detached, which indicates the accumulated force by the
8
stretching of the PDMS layer. In the insets of Figure 2b-e, the forces measured at the
9
moment of detachment are presented. In terms of nitrogen flow rate, there was a tendency
10
for the larger amount of nitrogen gas to generate stronger bonding (Figure 2b). On the
11
other hand, among the oxygen flow rates of 0, 5, 10, 15, 20, 25 and 50 sccm that were
12
used, 10 sccm produced the strongest bonding (Figure 2c). It was assumed that a large
13
amount of oxygen gas produces silica on the surface of the second PDMS layer, which
14
inhibits the penetration of plasma through the PDMS layer. Low oxygen flow rate reduced
15
the reactions at the parylene-C surface by plasma treatment. As the plasma power and
16
treatment time are related to plasma energy, higher plasma energy corresponded to
ACS Paragon Plus Environment
9
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 52
1
stronger bonding (Figure 2d,e). In particular, 200 W of plasma power generated a strong
2
bonding, even underneath the masked area: 6 mm of the masked area from the ‘location
3
of detachment’ was bonded with this strong plasma power. Although high plasma power
4
generates stronger bonding, it can be a problem in creating fine patterns.
5
In addition, we defined five bonding levels according to the observed detachment
6
behaviors after T-peeling tests: over-bonding, critical bonding, partial bonding, increased
7
adhesion, and no bonding. From the T-peeling tests, it was observed that the location of
8
PDMS breakage was different depending on the five bonding levels (Figure 2f-k). We
9
changed the nitrogen flow rate and plasma power, while the oxygen flow rate and
10
treatment time were fixed to be 10 sccm and 30 minutes, respectively. The plasma
11
conditions used to generate each bonding level are presented in Figure S3a. In the over-
12
bonded and critically bonded samples, the bonding between PDMS and parylene-C was
13
generated sharply at the edge of the masked area (Figure 2g,h). But, the over-bonded
14
samples showed the increased force underneath the masked area during T-peeling tests.
15
In the samples with partial bonding, the second PDMS layer was broken in the middle
ACS Paragon Plus Environment
10
Page 11 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
region of the plasma treated area (Figure 2i). Lastly, in the samples with the bonding level
2
of increased adhesion or no bonding, the whole PDMS layer was detached from the
3
parylene-C layer because of weak bonding between them (Figure 2j,k). The samples with
4
increased adhesion showed a certain amount of tension in the samples during the T-
5
peeling test, whereas the samples with no bonding level did not. For precise patterning
6
of bonded areas, critical bonding is desired. Figure S3b shows the plasma conditions
7
used to achieve critical bonding.
8
2.3. Quantitative analysis of bonding strength. To measure the quantitative strength
9
of bonding in the orthogonal direction, we conducted pull-off tests following ASTM D4541-
10
09.29 The pull-off test method is explained in Experimental Section. A dolly was pulled
11
with a pressure rate of 0.2 MPa/sec using an adhesion tester (Figure 3a). The maximum
12
bonding strength was measured following the predefined five bonding levels of over-
13
bonding, critical bonding, partial bonding, increased adhesion, and no bonding, which
14
were 4.02±0.21, 3.95±0.21, 2.92±0.24, 2.35±0.11, and 1.19±0.11 MPa, respectively (n
15
≥9 for each bonding level) (Figure 3b). As expected, over-bonded samples showed the
ACS Paragon Plus Environment
11
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 52
1
strongest bonding strength, and slightly low values were obtained in the critically bonded
2
samples. The sample with no bonding level showed the weakest bonding strength. The
3
bonded interface between the second PDMS layer and the parylene-C layer was exposed
4
after pull-off tests as shown in Figure 3c-g. Outside of the dolly, the second PDMS layer
5
was intact, covering the parylene-C layer. In the samples with increased adhesion or no
6
bonding levels, the pull-off test resulted in the transparent surface of exposed parylene-
7
C, because the force was not exerted at the interface of the PDMS and parylene-C during
8
the pull-off test. When the parylene-C layer was stretched by a relatively weak bonding
9
strength, the transparent parylene-C layer was transformed to an opaque surface in the
10
samples with partial bonding and increased adhesion levels. The strong bonding strength
11
in the samples with critical bonding and over-bonding levels generated a surface with
12
torn-out parylene-C. More damages in the parylene-C layer were observed as the
13
bonding strength increased, even the second PDMS layer remained partially in the over-
14
bonded samples. The exposed surfaces were classified into five morphologies according
15
to the five bonding levels: intact PDMS surface, transparent parylene-C surface, opaque
16
parylene-C surface, torn-out parylene-C surface, and remaining PDMS surface.
ACS Paragon Plus Environment
12
Page 13 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
2.4. Chemical analysis of the bonded interface. To investigate the mechanism of
2
bond formation between PDMS and parylene-C upon the plasma treatment, five different
3
locations of the exposed surfaces after pull-off tests were analyzed by X-ray
4
photoelectron spectroscopy (XPS). The chemical structures of PDMS and parylene-C are
5
shown in Figure S4. PDMS and parylene-C layers can be recognized by detecting silicon
6
(Si) and chlorine (Cl) peaks, respectively. In the intact PDMS surface and remaining
7
PDMS surface, carbon (C), Si, and oxygen (O) peaks, which compose the PDMS, were
8
detected. In these locations, the mechanism of bond cannot be analyzed because the
9
bonded interface activated by plasma treatment was not exposed. Cl peaks were found
10
at the transparent surface, the opaque surface, and the torn-out parylene-C surface,
11
where the second PDMS layer did not cover the parylene-C layer after the pull-off test
12
(Figure 4a). For more accurate analysis, C and Cl peaks at the parylene-C exposed
13
surfaces are magnified in Figure 4b,c. In the C (1s) spectrum (Figure 4b), the transparent
14
surface that did not make the bond with PDMS contained a peak at 285.1 eV arisen from
15
C-C bond. In the opaque surface with relatively weak bonding and the torn-out parylene-C
16
surface with strong bonding, a new peak at 290.8 eV appeared, indicating the C-O bond
ACS Paragon Plus Environment
13
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 52
1
formation.30,31 In particular, the intensity ratios of the two peaks at 290.8 eV to 285.1 eV
2
were 0, 0.86, and 1.64 at the transparent, opaque, and torn-out parylene-C surfaces,
3
respectively, implying more oxidized parylene-C resulted in stronger bonding. In the Cl
4
(2p) spectrum (Figure 4c), the peaks at 200.4 eV (Cl 2p3/2) and 202.0 eV (Cl 2p1/2)
5
appeared at the transparent surface.32 In addition, the intense peaks at 204.8 eV (Cl 2p3/2)
6
and 207.0 eV (Cl 2p1/2) were observed at the opaque and torn-out parylene-C surfaces,
7
which presumably implies that the migrated Cl atoms from parylene-C to PDMS form the
8
additional bonds with O on the oxidized PDMS side by the plasma treatment.33,34 The
9
intensity ratios of the two peaks at 207.0 eV to 200.4 eV increased according to the
10
bonding strength.
11
The cross-sectional areas of the over-bonded samples were also analyzed by
12
transmission electron microscopy energy dispersive X-ray spectroscopy (TEM-EDS). For
13
TEM-EDS analysis, the samples are required to have a thickness under 200 μm. Hence,
14
we prepared the bonded samples by the cryosectioning method detailed in Figure S5.
15
The surface and line analyses of the cross-sectional samples were conducted as shown
ACS Paragon Plus Environment
14
Page 15 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
in Figure S6. Figure 5a shows the cross-sectional analysis of an over-bonded sample.
2
We could certainly distinguish the first PDMS layer (parylene-C deposited PDMS), the
3
parylene-C layer, and the second PDMS layer (plasma-treated PDMS) through a TEM
4
image. The distribution of Si, O, C, and Cl atoms depended on the chemical structure of
5
PDMS and parylene-C. Si and O atoms were dispersed only inside PDMS while C atoms
6
existed in both PDMS and parylene-C. Interestingly, Cl atoms of parylene-C were
7
detected at the upper and lower interfaces between PDMS and parylene-C. As parylene-
8
C was infiltrated into PDMS during deposition,35,36 Cl atoms were expected to be detected
9
at the interface between parylene-C-deposited PDMS and parylene-C. On the other hand,
10
at the interface between plasma-treated PDMS and parylene-C, Cl atoms diffused into
11
PDMS by the nitrogen and oxygen plasma treatment, leading to the formation of an
12
overlapping narrow region with Si and Cl atoms. To see the interface between plasma-
13
treated PDMS and parylene-C more clearly, we conducted line scanning for the cross-
14
section of over-bonded samples (Figure 5b). A distance of 0.5 μm represents the interface
15
between plasma-treated PDMS and parylene-C. In parylene-C, only C was observed
16
while Si, Cl, O and C were detected inside the PDMS. Interestingly, in the region spanning
ACS Paragon Plus Environment
15
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 52
1
from the interface to approximately 0.5 μm into the PDMS, increased intensities of Cl and
2
O were measured. Therefore, we speculate that the migrated Cl reacts with the oxidized
3
PDMS during plasma treatment. Consequently, based on the overall evidences from XPS
4
and TEM-EDS analyses, we propose that the strong covalent bonds were formed
5
between oxidized parylene-C with carboxyl groups37,38 and PDMS with hydroxyl
6
groups39,40 (Figure 5c). Additionally, the C-Cl bonds of parylene-C were partially broken,
7
and this broken Cl newly formed the bonds with O in the oxidized PDMS.
8
2.5. Applications. Using the developed selective bonding technique, we generated
9
soft and flexible 3D mesostructures with various dimensions and fluidic channel patterns.
10
Either air or dyed water was injected into the non-bonded areas for the generation of 3D
11
structures. Figure 6a shows a 3D balloon-shaped structure with a diameter of 20 mm.
12
Figure 6b shows an array of balloons with 5 mm in diameter, where nine balloons were
13
connected through a fluidic channel. Figure 6c shows an array of nine balloons but with
14
three fluidic channels, so that three different fluids can be injected into different balloons.
15
Figure 6d-f show various 3D curved structures with the shapes of normal bending,
ACS Paragon Plus Environment
16
Page 17 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
trapezoidal bending, and spiral bending, respectively. The force of fluid injection into the
2
balloons created the curved shapes. As shown in the figures, the 3D curved structures
3
were capable of gripping objects with different shapes. The normally bent structure
4
enveloped a tube in a transverse direction and lifted it up. The trapezoidally bent structure
5
could wrap a funnel with inclined surface and pick it up. The spiral structure wrapped a
6
tube in a longitudinal direction and lifted it up.
7
For the integration of electrical functions, we fabricated the 3D structured devices
8
embedding LEDs or ECoG electrodes. Figure 7a,b show three-dimensionally bent
9
structures consisting of five balloons and an inflated balloon, respectively, with
10
enlightened LEDs. All LEDs lit up before and after considerable air injection into the
11
balloons. These lighted LEDs confirmed no disconnection of conductive metal lines after
12
the inflation of balloons. As another application, Figure 8a shows the ECoG electrode
13
array that formed a conformal contact with the cortical surface of a model brain. A stained
14
liquid was injected into the non-bonded area of the ECoG electrode array, clearly
15
demonstrating the conformal contact between the electrodes and the cortical surface, not
ACS Paragon Plus Environment
17
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 52
1
only on the gyrus but also on the sulcus. The soft and flexible 3D structured ECoG
2
electrodes, in conformal contact with the cortical surface, were evaluated in terms of
3
ECoG recording. Seven recording electrodes in the ECoG electrode array were
4
connected to a signal acquisition system through a flexible printed circuit board (FPCB)
5
cable. The emulated action potentials with three different waveforms were injected into
6
the model brain made of agarose. These emulated and recorded signals were band-pass
7
filtered with cuff-off frequency of 1000-8000 Hz. Figure 8b shows the injected and
8
recorded action potentials by the ECoG electrodes. All seven recording electrodes
9
detected the emulated action potentials. The signal to noise ratio (SNR) of the measured
10
signals was 6.62 on average. In addition, three different waveforms could be classified
11
from all seven electrodes because of this high SNR. It is because the developed 3D ECoG
12
electrode array could form conformal contact with the curved cortical surface by filling the
13
space inside the skull stably.
14
3. Conclusion
ACS Paragon Plus Environment
18
Page 19 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
Using the selective bonding technique, MEMS processed 2D planes could be turned into
2
3D soft and flexible structures with various sizes and patterns of non-bonded areas. The
3
proposed technique generates bonded and unbonded areas between PDMS and
4
parylene-C layers selectively, using plasma treatment on the top surface of the entire
5
structure. After all processes are done on a 2D plane, the selectively bonded 2D structure
6
is then transformed into a 3D structure upon fluid injection into the unbonded area.
7
Previously, to generate soft 3D structures in the mesoscale, the techniques to transfer
8
and stamp patterns on pre-strained substrates or manual bonding of two polymeric layers
9
using glue were used.24-27 Unlike those previous methods, using the proposed technique,
10
the necessary treatment to bond layers is performed only at the top surface of the entire
11
structure consisting of multiple polymeric layers, not at the interface to be bonded. This
12
in turn enables further MEMS processes to fabricate metal patterns in the 2D plane before
13
turning it into the 3D structure, thereby resulting in soft and flexible mesoscale 3D
14
structures with embedded metal patterns in the micrometer scale. However, a few
15
limitations are also identified. As an individual balloon pattern requires a fluid injection
16
inlet composed of small PDMS pieces, the presence of many individual balloons would
ACS Paragon Plus Environment
19
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 52
1
enlarge the entire structure. To achieve the critically bonded interface, the thickness of
2
the second PDMS layer is required to be 180 μm or lower. Additionally, to create stable
3
3D structures and not to burst the fluidic channel during fluid injection, the smallest width
4
of the fluidic channel is limited to 500 μm. As the fluidic channel acts as a resistance
5
against fluid flow, a narrow fluidic channel induces a higher pressure than a wide channel.
6
On the other hand, in a state of moderate pressure inside the fluidic channel, the fluid can
7
be injected into the non-bonded areas with various dimensions, that is, from wafer-scale
8
to several hundreds of micrometers.
9
Because PDMS and parylene-C are flexible, soft, and biocompatible, the devices
10
fabricated using this selective bonding technique can be used for implantable biomedical
11
devices. A 3D balloon-shaped or curved device can stably fit to various locations with
12
cavities filled with body fluids. In particular, the fabrication of electrodes or metal patterns
13
using MEMS techniques enables the 3D devices generated by selective bonding to
14
function as various sensors or actuators. Furthermore, if various drugs are injected into
15
the non-bonded areas of the selectively bonded 2D structures, instead of air or water, the
ACS Paragon Plus Environment
20
Page 21 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
device can contain drugs for a certain period of time and deliver them to the implanted
2
site. Consequently, many novel applications of 3D soft and flexible devices that are
3
fabricated using the proposed bonding technique are expected in the field of implantable
4
biomedical devices, ranging from neural interfaces to drug delivery systems.
5
4. Experimental section
6
4.1. Selective bonding between PDMS and parylene-C. PDMS (Sylgard 184, Dow
7
Corning Corp., Midland, MI, USA) and parylene-C (parylene-C dimer, Nuri-Tech Corp.,
8
Incheon, Korea) were used for the generation of soft and flexible 3D structures. The
9
structure was composed of three layers in total: the first PDMS layer, the parylene-C
10
layer, and the second PDMS layer. The PDMS was mixed at a weight ratio of 1:10 (curing
11
agent:monomer) and degassed in a desiccator. The first PDMS layer was spin coated for
12
60 seconds at 500 rpm and cured in a dry oven at 120 °C for 1 hour. A 1 μm parylene-C
13
layer was deposited using a parylene coater (NRPC-500, Nuri-Tech Corp., Incheon,
14
Korea). The parylene-C layer firmly adhered to the first PDMS layer as it was deposited
15
onto the first PDMS layer through chemical vapor deposition.35,36 Then, the second PDMS
ACS Paragon Plus Environment
21
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 52
1
layer was spin-coated at 500 rpm for 60 seconds and cured in a dry oven at 120 °C for 1
2
hour. The bonding area was patterned by masking the second PDMS layer with a PVC
3
film that was patterned using a film cutting plotter (CE5000-40-CRP, Graphtec Corp.,
4
Yokohama, Japan). For the generation of selective bonding between the second PDMS
5
layer and the parylene-C layer, the structure was treated by nitrogen and oxygen mixed
6
plasma using reactive ion etching, RIE (VITA, Femto Science, Gyeonggi-do, Korea). For
7
precise patterning of the bonded area, we needed to achieve critical bonding among five
8
classified bonding levels (see Figure 2f-k). The critical bonding level was obtained using
9
a nitrogen flow rate of 200 sccm, an oxygen flow rate of 10 sccm, power of 150 W, and
10
treatment time of 30 minutes (Figure S3). The detailed processes are explained in Figure
11
S1.
12
4.2. Generation of a 3D structure by fluid injection. After the fabrication of selectively
13
bonded samples in a 2D plane, fluid injection into the non-bonded area turns them into
14
3D structures by inflating the non-bonded area. A PDMS piece with a size of 5 mm by 5
15
mm was covalently bonded to both the first and second PDMS layers by oxygen plasma
ACS Paragon Plus Environment
22
Page 23 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
treatment with an oxygen flow rate of 40 sccm and power of 70 W. One side of the PDMS
2
piece with whole sample was excavated using a biopsy punch (Rapid-Core 1.2 mm, WPI,
3
Sarasota, FL, USA). A silicone tube was inserted into the punched hole, and a syringe
4
was connected to the end of the silicone tube. A fluid was injected into the non-bonded
5
area of the structure, which acted as the fluidic channel, using a syringe pump (Fusion
6
100, Chemyx Inc., Stafford, TX, USA). The details of the fluid injection are presented in
7
Figure S2.
8
4.3. T-peeling test for the evaluation of plasma conditions. The experiment utilized a
9
customized stretching setup consisting of an XY-axis stage (CROSS 130-HSM, Owis
10
GmbH, Staufen im Breisgau, Germany), a force meter (ZTA-50N, Imada Inc., Toyohashi,
11
Japan), and a sample holder according to ASTM D1876-08. This setup is described in
12
more detail in Figure S7a. After holding both PDMS layers of the samples, the second
13
PDMS layer was peeled, stretched and detached from the other layer by moving the stage
14
with a direction of 180° and a speed of 500 μm/sec. The induced force from the stretching
15
and detaching was measured by the force meter.
ACS Paragon Plus Environment
23
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 24 of 52
1
4.4. Pull-off test for the quantitative evaluation of bonding strength. The pull-off test
2
was conducted using an adhesion tester (PosiTest AT-A, DeFelsko, Ogdensburg, NY,
3
USA) according to ASTM D4541-09. The setup of the pull-off test is detailed in Figure
4
S7b. The first PDMS layer was spin-coated onto the silicon wafer treated by oxygen
5
plasma. When the first PDMS layer was cured, this PDMS layer and the silicon wafer
6
were bonded covalently each other. A dolly with 20 mm diameter was attached onto the
7
second PDMS layer using an epoxy and connected to the adhesion tester. The bonded
8
samples were cut along the edge of the dolly, to keep the area to be pulled constant. The
9
dolly was pulled with a pressure rate of 0.2 MPa/sec. The maximum bonding strength
10
was measured when the second PDMS layer detached from the parylene-C layer.
11
4.5. Cryosectioning of the bonded region for TEM-EDS analysis. The cross-sectional
12
area of the bonded samples was chemically analyzed by TEM-EDS. For sampling of the
13
cross-sectional area, the bonded samples were embedded in an epoxy mixture of Epon-
14
812, DDSA (2-dodecenylsuccinic anhydride), NMA (nadic methyl anhydride) and DPM-
15
30 (2,4,6-tris(dimethylaminomethyl)phenol) with a volume ratio of 45, 36.25, 18.75, and
ACS Paragon Plus Environment
24
Page 25 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
1.25%, respectively. The embedded samples were cured in an oven at 60 °C for 48 hours.
2
The cross-sectional surface of the bonded area was exposed by cutting the embedded
3
sample using an ultramicrotome (EM UC7, Leica Microsystems, Wetzlar, Germany) at -
4
180 °C. The sliced sample, with a thickness of 100 μm, was examined by TEM-EDS
5
analysis. Further details of cryosectioning are shown in Figure S6.
6
4.6. Fabrication of conductive lines and patterns. To integrate electrical functions,
7
selectively bonded samples in a 2D plane were prepared. The parylene-C layer with a
8
thickness of 500 nm was deposited onto the top surface of the whole structure. This layer
9
was used to prevent cracks in the conductive metal layer deposited afterwards.41 Then,
10
the conductive metal layer consisting of Ti/Au was sputtered in thicknesses of 25/300 nm
11
and patterned by wet etching with the help of a positive photoresist (AZ9260, Merck KGaA,
12
Darmstadt, Germany). The insulation layer of parylene-C was deposited in a thickness of
13
4.3 μm and patterned by RIE to create the openings. LEDs (SML-P1, ROHM Co., Kyoto,
14
Japan) were integrated using eutectic gallium-indium (EGaIn, Sigma-Aldrich., St.Louis,
15
MO, USA). The detailed method to integrate electrical functions is found in Figure S8.
ACS Paragon Plus Environment
25
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 26 of 52
1
ACS Paragon Plus Environment
26
Page 27 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
ACS Applied Materials & Interfaces
FIGURE.
2
3
Figure 1. Fabrication of a soft and flexible 3D structure. (a) Photograph and schematic
4
image of a 3D structure with embedded conductive lines and pads. Fluid injection into the
5
non-bonded area generates the 3D structure. The bonded area is formed between PDMS
6
and parylene-C by the covalent bond between hydroxyl and carboxyl groups. (b)
ACS Paragon Plus Environment
27
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 28 of 52
1
Methodology of selective bonding. Using a nitrogen and oxygen plasma treatment, the
2
second PDMS layer and the parylene-C layer are selectively bonded. (c) Generation of a
3
3D structure by the inflation of the non-bonded area upon fluid injection. The scale bars
4
are 5 mm.
ACS Paragon Plus Environment
28
Page 29 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
2
Figure 2. Mechanical analysis of bonding strength according to the plasma conditions by
3
T-peeling test. (a) Schematic of the T-peeling test setup with the used sample dimensions.
4
The force was measured during the peeling between layers, according to varying plasma
5
conditions: (b) nitrogen flow rate, (c) oxygen flow rate, (d) power, and (e) treatment time
6
(n=3 for each plasma condition). To investigate the effect of the nitrogen and oxygen flow
7
rates, the power of 50 W and the treatment time of 30 min were fixed. To investigate the
ACS Paragon Plus Environment
29
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 30 of 52
1
effect of power and time, the oxygen and nitrogen flow rates of 50 sccm were fixed. (f)
2
The bonding levels were classified into the different locations of PDMS breakage after T-
3
peeling tests. The images following five bonding levels show (g) over-bonding, (h) critical
4
bonding, (i) partial bonding, (j) increased adhesion, and (k) no bonding. The scale bar is
5
10 mm.
ACS Paragon Plus Environment
30
Page 31 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
2
Figure 3. Method and results of pull-off test. (a) Schematic of the pull-off test setup. After
3
the dolly was pulled off, measuring a maximum strength, the interface between the
4
second PDMS layer and the parylene-C layer was exposed. (b) Measured bonding
5
strengths for each predefined bonding level (n ≥ 9 for each bonding level). (c-g)
6
Photographic images of the exposed surfaces after pull-off tests. There are five different
7
morphologies, which are indicated by arrows, according to bonding levels: (c) over-
ACS Paragon Plus Environment
31
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 32 of 52
1
bonding, (d) critical bonding, (e) partial bonding, (f) increased adhesion, and (g) no
2
bonding.
ACS Paragon Plus Environment
32
Page 33 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
2
Figure 4. XPS results of the exposed surfaces of the bonded interface after pull-off test.
3
Si, O, and C from the PDMS and Cl from parylene-C were detected at the locations of (a)
4
transparent parylene-C surface, opaque parylene-C surface, and torn-out parylene-C
5
surface. Magnified C and Cl peaks detected at three exposed parylene-C surfaces after
ACS Paragon Plus Environment
33
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 34 of 52
1
pull-off tests: (b) C 1s spectra including C-C and C-O bonds and (c) Cl 2p spectra
2
containing C-Cl and O-Cl bonds. Stronger bonding exhibits larger shifts of peak intensity
3
from C-C bond to C-O bond and from C-Cl bond to O-Cl bond.
ACS Paragon Plus Environment
34
Page 35 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
2
Figure 5. Chemical analysis of the bonded interface between PDMS and parylene-C by
3
TEM-EDS. (a) TEM-EDS results of the cross-sectional area of over-bonded samples,
4
showing the atomic distribution in the cross-section containing the interface (scale bar: 1
5
μm). The line analysis was performed for the 2 μm distance from the center of parylene-
6
C. (b) Intensity levels of different atoms along with the line crossing the interface between
7
plasma-treated PDMS and parylene-C. (c) The proposed mechanism of selective bonding
8
between PDMS and parylene-C.
ACS Paragon Plus Environment
35
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 36 of 52
1
2
Figure 6. Generation of various 3D structures with air and dyed water injection. (a)
3
Circular balloon with a 20 mm diameter. Arrays containing nine balloons with (b) one
4
fluidic channel and (c) three fluidic channels. (d) Bent structure enveloping a tube and
5
lifting it up. (e) Trapezoidally bent structure wrapping a funnel and picking it up. (f) Spiral
6
structure wrapping a tube and holding it up. The scale bars are 10 mm.
7
ACS Paragon Plus Environment
36
Page 37 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
2
Figure 7. 3D structured soft and flexible devices embedding electronic components.
3
Demonstration of intact conductive lines by lighting LEDs after the fluid injection in cases
4
of (a) a bent structure consisting of five balloons and (b) a single balloon structure. The
5
scale bars are 5 mm.
ACS Paragon Plus Environment
37
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 38 of 52
1 2 3
Figure 8. 3D structured soft and flexible ECoG electrode array. (a) ECoG sensing device
4
fitted on the curved cortical surface, by filling the space between the skull and the brain.
5
For the evaluation of recording performance, emulated action potentials (A.P.) were
6
injected into an agarose brain model (scale bars: 10 mm). (b) Emulated and recorded
7
action potentials by an electrode of the ECoG device. Emulated and recorded action
8
potentials by all seven electrodes in a magnified time scale. Three different waveforms of
9
action potentials were clearly distinguishable by all seven recording electrodes.
ACS Paragon Plus Environment
38
Page 39 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
ASSOCIATED CONTENT
2
Supporting Information
3
The Supporting Information is available free of charge on the ACS Publications website
4
at DOI:
5
Figure S1: Processes of selective bonding between PDMS and parylene-C; Figure S2:
6
Fluid injection to transform 2D structures into 3D structures; Figure S3: Plasma conditions
7
resulting in five different bonding levels and optimization for critical bonding; Figure S4:
8
Chemical structures of PDMS and parylene-C; Figure S5: Cryosectioning of samples
9
containing the bonded interface; Figure S6: Sample preparation and method for TEM-
10
EDS; Figure S7: Experimental setups for the measurement of bonding strength; Figure
11
S8: Fabrication of conductive lines and pads; Table S1: Plasma conditions for the T-
12
peeling test.
13
AUTHOR INFORMATION
14
Corresponding Author
ACS Paragon Plus Environment
39
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 40 of 52
1
*Email:
[email protected] (S.K.)
2
Author Contributions
3
H.M. and N.C. contributed equally to this work. H.M., N.C., and S.K. conceived the idea
4
and designed the experiments. H.M., N.C., and K.L. fabricated the 3D soft and flexible
5
structures. H.M., and N.C. performed T-peeling tests. H.M. and H.W.S. performed pull-
6
off tests. H.M. and N.C. performed XPS and TEM-EDS. J.P. analyzed XPS and TEM-
7
EDS results. H.M. carried out the fabrication and experiment regarding 3D soft and
8
flexible device with embedded electrical functionality. H.M., N.C., and S.K. wrote the
9
manuscript. All authors have given approval to the final version of the manuscript.
10
Notes
11
The authors declare no competing financial interest.
12
ACKNOWLEDGMENT
13
This work was supported by grants from the Basic Science Research Program (NRF-
14
2017R1A2B2004598) of the National Research Foundation of Korea (NRF) and the
ACS Paragon Plus Environment
40
Page 41 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
DGIST R&D Program (19-RT-01) funded by the Korean government (Ministry of Science
2
and ICT, MSIT). The authors would like to thank H.J., J.P., and H.L. (Center for Core
3
Research Facilities in DGIST) for discussions regarding the parylene-C coater, EDS, and
4
Bio-TEM, respectively.
5
REFERENCES
6
(1) Xiang, Z.; Liu, J.; Lee, C. A Flexible Three-Dimensional Electrode Mesh: An
7
Enabling Technology for Wireless Brain–Computer Interface Prostheses. Microsystems
8
& Nanoengineering 2016, 2, 16012.
9 10
(2) Takeuchi, S.; Suzuki, T.; Mabuchi, K.; Fujita, H. 3D Flexible Multichannel Neural Probe Array. Journal of Micromechanics and Microengineering 2004, 14 (1), 104-107.
11
(3) Xu, L.; Gutbrod, S. R.; Bonifas, A. P.; Su, Y.; Sulkin, M. S.; Lu, N.; Chung, H. J.;
12
Jang, K. I.; Liu, Z.; Ying, M.; Lu, C.; Webb, R. C.; Kim, J. S.; Laughner, J. I.; Cheng, H.;
13
Liu, Y.; Ameen, A.; Jeong, J. W.; Kim, G. T.; Huang, Y.; Efimov, I. R.; Rogers, J. A. 3D
14
Multifunctional Integumentary Membranes for Spatiotemporal Cardiac Measurements
15
and Stimulation across the Entire Epicardium. Nat. Commun. 2014, 5, 3329.
ACS Paragon Plus Environment
41
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 42 of 52
1
(4) Kim, D. H.; Lu, N.; Ghaffari, R.; Kim, Y. S.; Lee, S. P.; Xu, L.; Wu, J.; Kim, R. H.;
2
Song, J.; Liu, Z.; Viventi, J.; de Graff, B.; Elolampi, B.; Mansour, M.; Slepian, M. J.; Hwang,
3
S.; Moss, J. D.; Won, S. M.; Huang, Y.; Litt, B.; Rogers, J. A. Materials for Multifunctional
4
Balloon Catheters with Capabilities in Cardiac Electrophysiological Mapping and Ablation
5
Therapy. Nat. Mater. 2011, 10 (4), 316-323.
6
(5) Kang, X. Y.; Liu, J. Q.; Tian, H. C.; Yang, B.; Nuli, Y. N.; Yang, C. S. Self-Closed
7
Parylene
8
Microelectromechanical Systems 2015, 24 (2), 319-332.
9 10
Cuff
Electrode
for
Peripheral
Nerve
Recording.
Journal
of
(6) Liang, H.; Lo, P.; Lai, W.; Fang, W. In 3D Multi-Function Bio-Sphere Drosophila
Behavior platform, IEEE SENSORS, Nov. 1-4, 2015.
11
(7) Chen, W.; Chen, S.; Morsi, Y.; El-Hamshary, H.; El-Newhy, M.; Fan, C.; Mo, X.
12
Superabsorbent 3D Scaffold Based on Electrospun Nanofibers for Cartilage Tissue
13
Engineering. ACS Appl. Mater. Interfaces 2016, 8 (37), 24415-24425.
ACS Paragon Plus Environment
42
Page 43 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
(8) Jin, L.; Xu, Q.; Kuddannaya, S.; Li, C.; Zhang, Y.; Wang, Z. Fabrication and
2
Characterization of Three-Dimensional (3D) Core-Shell Structure Nanofibers Designed
3
for 3D Dynamic Cell Culture. ACS Appl. Mater. Interfaces 2017, 9 (21), 17718-17726.
4
(9) Yu, M.; Huang, Y.; Ballweg, J.; Shin, H.; Huang, M.; Savage, D. E.; Lagally, M. G.;
5
Dent, E. W.; Blick, R. H.; Williams, J. C. Semiconductor Nanomembrane Tubes: Three-
6
Dimensional Confinement for Controlled Neurite Outgrowth. ACS Nano 2011, 5 (4), 2447-
7
2457.
8
(10) Tian, B.; Liu, J.; Dvir, T.; Jin, L.; Tsui, J. H.; Qing, Q.; Suo, Z.; Langer, R.; Kohane,
9
D. S.; Lieber, C. M. Macroporous Nanowire Nanoelectronic Scaffolds for Synthetic
10
Tissues. Nat. Mater. 2012, 11 (11), 986-994.
11
(11) Holken, I.; Neubuser, G.; Postica, V.; Bumke, L.; Lupan, O.; Baum, M.; Mishra, Y.
12
K.; Kienle, L.; Adelung, R. Sacrificial Template Synthesis and Properties of 3D Hollow-
13
Silicon Nano- and Microstructures. ACS Appl. Mater. Interfaces 2016, 8 (31), 20491-
14
20498.
ACS Paragon Plus Environment
43
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2
3
Page 44 of 52
(12) Rogers, J.; Huang, Y. G.; Schmidt, O. G.; Gracias, D. H. Origami MEMS and NEMS. Mrs Bulletin 2016, 41 (2), 123-129.
(13) Syms, R. R. A.; Yeatman, E. M.; Bright, V. M.; Whitesides, G. M. Surface Tension-
4
Powered
Self-Assembly
of
Microstructures
-
the
5
Microelectromechanical Systems 2003, 12 (4), 387-417.
State-of-the-Art.
Journal of
6
(14) Piyawattanametha, W.; Patterson, P. R.; Hah, D.; Toshiyoshi, H.; Wu, M. C.
7
Surface- and Bulk-Micromachined Two-Dimensional Scanner Driven by Angular Vertical
8
Comb Actuators. Journal of Microelectromechanical Systems 2005, 14 (6), 1329-1338.
9
(15) Yang, Y.; Liu, W.; Wu, N.; Wang, X.; Zhang, T.; Chen, L.; Zeng, R.; Wang, Y.; Lu,
10
J.; Fu, L.; Xiao, L.; Zhuang, L. Tuning the Morphology of Li2O2 by Noble and 3D Metals:
11
A Planar Model Electrode Study for Li-O2 Battery. ACS Appl. Mater. Interfaces 2017, 9
12
(23), 19800-19806.
ACS Paragon Plus Environment
44
Page 45 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
(16) Li, X.; Guan, C.; Hu, Y.; Wang, J. Nanoflakes of Ni-Co LDH and Bi2O3 Assembled
2
in 3D Carbon Fiber Network for High-Performance Aqueous Rechargeable Ni/Bi Battery.
3
ACS Appl. Mater. Interfaces 2017, 9 (31), 26008-26015.
4
(17) Ning, H.; Pikul, J. H.; Zhang, R.; Li, X.; Xu, S.; Wang, J.; Rogers, J. A.; King, W.
5
P.; Braun, P. V. Holographic Patterning of High-Performance on-Chip 3D Lithium-Ion
6
Microbatteries. Proc. Natl. Acad. Sci. USA 2015, 112 (21), 6573-6578.
7 8
(18) Sun, K.; Wei, T. S.; Ahn, B. Y.; Seo, J. Y.; Dillon, S. J.; Lewis, J. A. 3D Printing of Interdigitated Li-Ion Microbattery Architectures. Adv. Mater. 2013, 25 (33), 4539-4543.
9
(19) Deng, J. W.; Ji, H. X.; Yan, C. L.; Zhang, J. X.; Si, W. P.; Baunack, S.; Oswald, S.;
10
Mei, Y. F.; Schmidt, O. G. Naturally Rolled-Up C/Si/C Trilayer Nanomembranes as Stable
11
Anodes for Lithium-Ion Batteries with Remarkable Cycling Performance. Angewandte
12
Chemie-International Edition 2013, 52 (8), 2326-2330.
ACS Paragon Plus Environment
45
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 46 of 52
1
(20) Bartlett, N. W.; Tolley, M. T.; Overvelde, J. T.; Weaver, J. C.; Mosadegh, B.;
2
Bertoldi, K.; Whitesides, G. M.; Wood, R. J. A 3D-Printed, Functionally Graded Soft Robot
3
Powered by Combustion. Science 2015, 349 (6244), 161-165.
4 5
6 7
(21) Jang, D.; Meza, L. R.; Greer, F.; Greer, J. R. Fabrication and Deformation of ThreeDimensional Hollow Ceramic Nanostructures. Nat. Mater. 2013, 12 (10), 893-898.
(22) Shenoy, V. B.; Gracias, D. H. Self-Folding Thin-Film Materials: From Nanopolyhedra to Graphene Origami. MRS Bulletin 2012, 37 (4), 847-854.
8
(23) Li, H.; Guo, X.; Nuzzo, R. G.; Jimmy Hsia, K. Capillary Induced Self-Assembly of
9
Thin Foils into 3D Structures. Journal of the Mechanics and Physics of Solids 2010, 58
10
(12), 2033-2042.
11
(24) Yan, Z.; Zhang, F.; Liu, F.; Han, M.; Ou, D.; Liu, Y.; Lin, Q.; Guo, X.; Fu, H.; Xie,
12
Z.; Gao, M.; Huang, Y.; Kim, J.; Qiu, Y.; Nan, K.; Kim, J.; Gutruf, P.; Luo, H.; Zhao, A.;
13
Hwang, K. C.; Huang, Y.; Zhang, Y.; Rogers, J. A. Mechanical Assembly of Complex, 3D
ACS Paragon Plus Environment
46
Page 47 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
Mesostructures from Releasable Multilayers of Advanced Materials. Sci. Adv. 2016, 2 (9),
2
e1601014.
3
(25) Yan, Z.; Han, M.; Yang, Y.; Nan, K.; Luan, H.; Luo, Y.; Zhang, Y.; Huang, Y.;
4
Rogers, J. A. Deterministic Assembly of 3D Mesostructures in Advanced Materials via
5
Compressive Buckling: A Short Review of Recent Progress. Extreme Mechanics Letters
6
2017, 11, 96-104.
7
(26) Shepherd, R. F.; Ilievski, F.; Choi, W.; Morin, S. A.; Stokes, A. A.; Mazzeo, A. D.;
8
Chen, X.; Wang, M.; Whitesides, G. M. Multigait Soft Robot. Proceedings of the National
9
Academy of Sciences of the United States of America 2011, 108 (51), 20400-20403.
10 11
12 13
(27) Kim, S.; Laschi, C.; Trimmer, B. Soft Robotics: A Bioinspired Evolution in Robotics.
Trends Biotechnol 2013, 31 (5), 287-294.
(28) Standard Test Methods for Peel Resistance of Adhesives (T-Peel Test): D187608; ASTM International: West Conshohocken, PA, 2015.
ACS Paragon Plus Environment
47
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2
Page 48 of 52
(29) Standard Test Method for Pull-Off Strength of Coatings Using Portable Adhesion
Testers: D4541-09; ASTM International: West Conshohocken, PA, 2009.
3
(30) Golda, M.; Brzychczy-Wloch, M.; Faryna, M.; Engvall, K.; Kotarba, A. Oxygen
4
Plasma Functionalization of Parylene C Coating for Implants Surface: Nanotopography
5
and Active Sites for Drug Anchoring. Materials Science & Engineering C-Materials for
6
Biological Applications 2013, 33 (7), 4221-4227.
7
(31) Golda-Cepa, M.; Brzychczy-Wloch, M.; Engvall, K.; Aminlashgari, N.; Hakkarainen,
8
M.; Kotarba, A. Microbiological Investigations of Oxygen Plasma Treated Parylene C
9
Surfaces for Metal Implant Coating. Materials Science & Engineering C-Materials for
10
Biological Applications 2015, 52, 273-281.
11
(32) Ishizaki, T.; Wada, Y.; Chiba, S.; Kumagai, S.; Lee, H.; Serizawa, A.; Li, O. L.;
12
Panomsuwan, G. Effects of Halogen Doping on Nanocarbon Catalysts Synthesized by a
13
Solution Plasma Process for the Oxygen Reduction Reaction. Physical Chemistry
14
Chemical Physics 2016, 18 (31), 21843-21851.
ACS Paragon Plus Environment
48
Page 49 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
(33) Moulder, J. F., Chastain, J. Handbook of X-ray Photoelectron Spectroscopy: A
2
Reference Book of Standard Spectra for Identification and Interpretation of XPS Data.
3
Physical Electronics Division, Perkin-Elmer Corporation: 1992; pp 33-70.
4
(34) Sugiyama, S.; Satomi, K.; Shigemoto, N.; Hayashi, H.; Moffat, J. B. Formation of
5
Chlorine Species over Magnesium-Oxide in the Oxidative Coupling of Methane in the
6
Presence of Carbon-Tetrachloride. Catalysis Letters 1994, 25 (3-4), 201-208.
7
(35) Lei, Y.; Liu, Y.; Wang, W.; Wu, W.; Li, Z. Studies on Parylene C-Caulked PDMS
8
(pcPDMS) for Low Permeability Required Microfluidics Applications. Lab Chip 2011, 11
9
(7), 1385-1388.
10
(36) Liu, Y. P.; Zhang, L. Q.; Mo, C.; Cao, Y. P.; Wu, W. G.; Wang, W. Caulking
11
Polydimethylsiloxane Molecular Networks by Thermal Chemical Vapor Deposition of
12
Parylene-C. Lab on a Chip 2016, 16 (21), 4220-4229.
ACS Paragon Plus Environment
49
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 50 of 52
1
(37) Hosseini, S.; Ibrahim, F.; Djordjevic, I.; Koole, L. H. Recent Advances in Surface
2
Functionalization Techniques on Polymethacrylate Materials for Optical Biosensor
3
Applications. Analyst 2014, 139 (12), 2933-2943.
4
(38) Pimanpang, S.; Wang, P. I.; Juneja, J. S.; Wang, G. C.; Lu, T. M. Interfacial
5
Interaction of In Situ Cu Growth on Tetrasulfide Self-Assembled Monolayer on Plasma
6
Treated Parylene Surface. Journal of Vacuum Science & Technology A 2006, 24 (5),
7
1884-1891.
8
(39) Vlachopoulou, M. E.; Tserepi, A.; Pavli, P.; Argitis, P.; Sanopoulou, M.; Misiakos,
9
K. A Low Temperature Surface Modification Assisted Method for Bonding Plastic
10
Substrates. J. Micromech. Microeng. 2009, 19 (1), 015007.
11
(40) Aran, K.; Sasso, L. A.; Kamdar, N.; Zahn, J. D. Irreversible, Direct Bonding of
12
Nanoporous Polymer Membranes to PDMS or Glass Microdevices. Lab Chip 2010, 10
13
(5), 548-552.
ACS Paragon Plus Environment
50
Page 51 of 52 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2
ACS Applied Materials & Interfaces
(41) Chou, N.; Jeong, J.; Kim, S. Crack-Free and Reliable Lithographical Patterning Methods on PDMS Substrate. J. Micromech. Microeng. 2013, 23 (12), 125035.
3
ACS Paragon Plus Environment
51
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Page 52 of 52
BRIEFS
2
3
Table of Contents graphic.
ACS Paragon Plus Environment
52