Wet-Laid Formation and Strength Enhancement of ... - ACS Publications

Jun 20, 2017 - (1) For these attractive HEVs, however, high performance rechargeable batteries are necessary. So far almost all commercial HEVs have b...
0 downloads 4 Views 2MB Size
Subscriber access provided by Binghamton University | Libraries

Article

Wet-Laid Formation and Strength Enhancement of Alkaline Battery Separators Using Polypropylene Fibers and Polyethylene/ Polypropylene Bicomponent Fibers as Raw Materials Bingxu Zhang, Qingxi Hou, Wei Liu, Zhihui Liang, Bing Wang, and Honglei Zhang Ind. Eng. Chem. Res., Just Accepted Manuscript • DOI: 10.1021/acs.iecr.7b01664 • Publication Date (Web): 20 Jun 2017 Downloaded from http://pubs.acs.org on June 25, 2017

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

Industrial & Engineering Chemistry Research is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

1

Wet-Laid Formation and Strength Enhancement of

2

Alkaline Battery Separators Using Polypropylene Fibers

3

and Polyethylene/Polypropylene Bicomponent Fibers as

4

Raw Materials

5

Bingxu Zhang, Qingxi Hou*, Wei Liu, Zhihui Liang, Wang Bing, Honglei Zhang

6

Tianjin Key Laboratory of Pulp and Paper, Tianjin University of Science & Technology, Tianjin

7

300457, P. R. China

8

ABSTRACT: The handsheets of alkaline battery separator were made of

9

polypropylene

(PP)

fibers

and

polyethylene/polypropylene

bicomponent

10

sheath-core structure (EP) fibers in the wet-laid process followed by a hot-pressing

11

treatment. The effects of the process parameters in making the separator

12

handsheets on the formation and the resultant tensile strength, maximum pore

13

size, porosity and alkali resistance were investigated. The results showed that a

14

favorable formation could be obtained at the EP fibers addition level of not less

15

than 20%. In addition, the tensile strength, maximum pore size, porosity and alkali

16

resistance of the separator handsheets made of 60% PP fibers and 40% EP fibers

17

could meet the needs required in QB/T 4173 (2011), under the conditions of 1.5%

18

PEO and 4.0% PVA additions (on oven-dry fibers), the hot-pressing pressure of

19

0.5 MPa, and hot-pressing temperature of 135 °C for 90 s.

20

Key words: :Polypropylene fiber; Polyethylene/polypropylene bicomponent fiber;

21

Wet-laid process; Alkaline battery separator; Hot-pressing

22

■ INTRODUCTION

*

Corresponding author. E-mail address: [email protected] (Q.X. Hou) 1

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

23

The main cause for developing various types of clean cars such as fuel-cell

24

and electric vehicles is an environmental issue. Among clean cars, a hybrid electric

25

vehicle (HEV) with a rechargeable battery is considered to be the most promising

26

and, therefore, has been receiving much attention.1 For these attractive HEVs,

27

however, high performance rechargeable batteries are necessary. So far almost all

28

commercial HEVs have been equipped with alkaline batteries because of their

29

better combination of output power, capacity, long life, reliability and cost.2-3 The

30

function of an alkaline battery separator, which plays a vital role in the application

31

of alkaline batteries, is to separate the positive and negative electrodes in the

32

batteries from direct contact so as to avoid a short circuit, load the electrolyte

33

solution, and allow the conductive ions to pass through the cell. Therefore, the

34

quality of the battery separator has a great effect on discharge behavior,

35

self-discharge rate and cycle life of an alkaline battery.4-5 It is necessary for an

36

alkaline battery separator not only to possess a fairly good chemical stability and

37

affinity with the electrolyte but also to have certain properties such as a high

38

mechanical strength, suitable pore size and porosity.6

39

One of the core technologies of an alkaline battery is the use of a synthetic

40

fiber-based separator, which possesses the properties of high porosity, high

41

strength, and solvent and corrosion resistance, and so on. Furthermore, the

42

synthetic fiber-based separator especially adapts alkaline batteries to large

43

capacity, low resistance, large output power and long period of storage, therefore,

44

synthetic fibers have become the important raw materials in production of alkaline

45

battery separators.7-9

46

Currently widely used alkaline battery separators are typically manufactured

47

from polyolefin, predominantly polyethylene (PE) or polypropylene (PP).10-12 U.S. 2

ACS Paragon Plus Environment

Page 2 of 33

Page 3 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

48

Pat. No. 3,615,865 to Wetherill discloses a battery separator comprising a

49

nonwoven mat of polypropylene fibers bonded with polyacrylic acid.12 J.P. Pat. No.

50

5,311,059 to Kubo discloses alkaline manganese batteries comprising a fibrous

51

web having mixing rayon 1.5-denier and synthetic fiber 1.0-denier.13 When being

52

used as raw material to make the separators by means of the traditional

53

papermaking method used for plant fibers, PP fibers can only be interlaced with

54

one another due to the absence of hydrogen bonding between the fibers. That is to

55

say, there is no bonding force between PP fibers in the separator, resulting in a

56

very low separator’s strength and a poor formation due to the lower density of PP

57

fibers than that of water. However, PP fibers can be mixed with the low-melt fibers

58

to make alkaline battery separators. When a separator made of PE and PP fibers

59

is heated, the totally or partially melted PE fibers could act as binding ones to

60

improve the separator’s strength.14 However, the totally melted PE fibers can lead

61

to reducing in the separator’s porosity and subsequent battery quality. Among the

62

low-melt fibers, polyethylene/polypropylene bicomponent sheath-core structure

63

(EP) fibers with a PP core and a PE sheath are thought to be most promising.15

64

Heating these fibers to the temperature above the PE melting point can make the

65

fibers surface sticky, so that the bonding points between the fibers can be formed,

66

resulting in an enhancement in the separator’s strength.14,16 The battery separator

67

made of polyamide and EP fibers has a poor resistance to oxidation and may

68

cause the self-discharge of the cells.15

69

So far, a number of forming technologies to make alkaline battery separators

70

using synthetic fibers as raw materials have involved the wet-laid process,14,17-19

71

dry-laid process,20-22 and melt-blown process.23-24 The melt-blown process among

72

them has been suggested as the best way of using the fibers with a small diameter 3

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

73

and low strength, and the dry-laid one can be applied in making the separators

74

with a relatively low quality. The wet-laid process to be applied in making alkaline

75

battery separators has many advantages, such as a relative high tightness, better

76

formation, and low production cost. However, due to the severe flocculation and

77

poor dispersibility, only using low-density PP fibers to make the battery separators

78

in the wet-laid process could lead to a very poor formation of the resultant

79

separators. In addition, using PP and EP fibers simultaneously to make alkaline

80

battery separators in the wet-laid process has been rarely reported.

81

In this work, PP and EP fibers were selected to prepare alkaline battery

82

separators by using the wet-laid process. The addition of EP fibers was mainly

83

used to well disperse PP fibers in water and consequently to improve the

84

separator’s formation as well as to increase the mechanical strength of the

85

separator handsheets by hot-pressing treatment. In addition, PEO and PVA were

86

also selected to add in the fiber suspension for further enhancing the tensile

87

strength of the separator handsheets. The aim of this work is to improve the

88

separator formation in the wet-laid process and the properties such as tensile

89

strength, maximum pore size and porosity of the separator handsheet.

90

■ MATERIALS AND METHODS

91

Materials and chemicals. PP fibers (density of 0.91 g/cm3, alkali resistance

92

of 0.88%, mean fiber length of 6.56 mm and mean fiber diameter of 2.06 µm) was

93

obtained from an electronic ceramics company in Guangdong Province, China. EP

94

fibers (PE/PP biocomponent sheath-core structure, Superior grade, density of 0.95

95

g/cm3, alkali resistance of 0.32%, mean fiber length of 2.55 mm and mean fiber

96

diameter of 14.1 µm) was obtained from the Complex New Material Technology

97

(Shanghai, China) Co., Ltd. 4

ACS Paragon Plus Environment

Page 4 of 33

Page 5 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

98

Polyethylene oxide (PEO, Mw = 5000000) was purchased from Sigma Aldrich

99

Co., and polyvinyl alcohol (PVA) with a polymerization degree of 1700 and

100

alcoholysis degree of 88% was supplied by Aladdin Reagent (Shanghai) Co., Ltd.

101

N-butanol and potassium hydroxide were purchased from Sinopharm Chemical

102

Reagent Co., Ltd. All chemicals used in the experiments were analytical-grade

103

products.

104

Fiber morphology. The mean diameter and length of PP fibers were

105

determined by using the Image-Pro Plus (IPP) software and the images of a SEM

106

(JSM-IT300LV, JEOL, Japan) according to the method described in literature.25

107

The EP fiber’s morphology was analyzed by using a Fiber Tester (Model 912,

108

Lorentzen & Wettre Co. Ltd., Sweden).

109

Determination of sedimentation volume. 400 mg fibers were added into

110

800 mL deionized water to make a 0.05% fiber suspension. After being stirred for

111

15 min, the fiber suspension was poured into a 1000 mL graduated cylinder. The

112

sedimentation volume was determined according to the upper suspended volume

113

of the fiber suspension.

114

Preparation of alkaline battery separator handsheets. A series of 0.5%

115

fiber suspensions with different proportions of the PP and EP fibers, i.e., the

116

addition levels of the EP fibers were 0%, 10%, 20%, 25%, 30% and 40%,

117

respectively, were firstly made, and then the fiber suspensions were disintegrated

118

for 20000 revolutions using a standard desintegrator (970154, Lorentzen & Wettre

119

Co. Ltd., Sweden). After pouring PEO (0.5%, 1.0%, 1.5%, 2.0%, 2.5%, and 3.0%

120

on oven-dry fibers, respectively) and/or PVA (1.0%, 2.0%, 3.0%, 4.0%, 5.0%, 6.0%,

121

and 7.0% on oven-dry fibers, respectively) into the fiber suspension, stirring for 10

122

min was required. The handsheets of alkaline battery separator with a basis weight 5

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

123

of 50 g/m2 (over-dry) were made by using a sheet former (RK-ZA-KWT, PTI,

124

Austria) according to the standard method of ISO 5269–1(1998), then further

125

dehydrated in a wet paper press machine (KRK SE0808098, MAVIS, UK) and

126

subsequently dried in a drum dryer (2110, AMC, USA). Finally, the hot-pressing

127

treatment of the separator handsheets was conducted by using a hot press

128

machine (LX101-63, Lizhengxin Mechanical Equipment Co., China). The

129

hot-pressing conditions were as follows: the pressure of 0.1 MPa, 0.2 MPa, 0.3

130

MPa, 0.4 MPa, 0.5 MPa, 0.55 MPa, and 0.6 MPa, respectively; the temperature of

131

130 °C, 135 °C, 140 °C, 145 °C, 150 °C, 155 °C, and 160 °C, respectively; and the

132

hot-pressing time of 90 s.

133

Sulfonation treatment of alkaline battery separator handsheets. The

134

alkaline battery separator handsheets were soaked with concentrated sulfuric acid

135

(mass fraction of 98%) at room temperature for 5 min, 10 min, 15 min, 20 min, and

136

25 min, respectively. Then the sulfonated handsheets were taken out and

137

thoroughly washed with deionized water until the pH of the filtrate was neutral.

138

Finally, the sulfonated separator handsheets were dried in an electric heating

139

air-blowing drier (DGG-101-1, Tianjin Tianyu Experimental Instrument Co., China).

140

DSC determination. The DSC determination of the separator handsheets

141

was conducted by using a DSC (200F3, NETZSCH, Germany) under a nitrogen

142

atmosphere from 20 °C to 200 °C at a heating rate of 10 °C/min.

143

Determination of the separators performance. Physical properties. The

144

basis weight, thickness and tensile index of the separator handsheets were

145

determined according to ISO 536 (1995), ISO 534 (1998) and ISO1924–2 (1994),

146

respectively. The pore size of the separator handsheet was detected by using a

147

Capillary Flow Porometer (Porolux 100, porometer NV, Germany) according to 6

ACS Paragon Plus Environment

Page 6 of 33

Page 7 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

148

SJ/T 10171.10 (1991). The porosity of the separator handsheet was determined by

149

using the n-butanol uptake test according to the literature method,26-27 as

150

calculated by the following equation:

Porosity(%) = ( W 2 − W 1 ) / ρbV ×100

151

(1)

152

where W2 and W1 are the weights of the wet and dry separator handsheet,

153

respectively, ρb is the density of n-butanol, and V is the geometric volume of the

154

separator handsheet.

155

Alkali resistance, alkali absorption rate and alkali absorption height. The

156

alkali resistance, alkali absorption rate and alkali absorption height of the separator

157

handsheet were detected according to SJ/T 10171.6 (1991), SJ/T 10171.7 (1991)

158

and ISO 8787 (1991), respectively.

159

SEM observation. The morphologies of the separator handsheets were

160

observed by using a SEM (JSM-IT300LV, JEOL, Japan). Before observation, the

161

test samples were oven-dried in a vacuum oven at 50 °C for 4 h, and then sputter

162

coated with gold.

163

■ RESULTS AND DISCUSSION

164

Effect of the addition level of EP fibers on the handsheet formation of

165

alkaline battery separator. The effect of the addition level of EP fibers on the

166

handsheet formation of alkaline battery separator was investigated, and the result

167

is shown in Figure 1. In Figure 1, a better formation can be found as the addition

168

level of the EP fibers was 20% or more, which is accordant with the result of about

169

65% PP fibers observed by other researchers.16,28 This is because the EP fibers

170

were shorter in length and had a higher density and larger diameter than the PP

171

fibers, which effectively inhibited flocculation of the PP fibers in water. Therefore,

172

from a better formation point of view, 20% or more addition level of the EP fibers 7

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

173

was necessary to make alkaline battery separator handsheets.

174

Selection of the temperature in the hot-pressing treatment of the

175

separator handsheets. The DSC curves of the separator handsheets were shown

176

in Figure 2. It can be found in Figure 2 that the melting temperature ranged from

177

130 °C to 170 °C. According to previous studies,14,16,29 the PE sheath of the EP

178

fibers would melt slightly beyond 130 °C, which is the main reason why the tensile

179

index of the separator handsheet would increase after hot-pressing. That is

180

because the bonding points between the fibers in the separator handsheet

181

increased with an increase in the addition level of the EP fibers, resulting in an

182

enhancement in the bonding strength of the separator handsheet. Furthermore,

183

the EP fibers had a larger diameter and a shorter length than the PP fibers,

184

resulting in an increment in the porosity and pore size of the separator handsheet,

185

which can be confirmed according to the effect of the addition level of the EP fibers

186

on the porosity and maximum pore size of the separator handsheets (Figure 3).

187

However, as the hot-pressing temperature rose, the melting amount of the fibers

188

increased, leading to a decrease in the porosity of the separator handsheet.

189

Considering the porosity requirement for alkaline battery separators, the

190

hot-pressing temperature ranging from 130 °C to 150 °C would be appropriate.

191

Effect of hot-pressing temperature on the tensile strength, maximum

192

pore size and porosity of the separator handsheets. The effect of hot-pressing

193

temperature on the tensile strength, maximum pore size and porosity of the

194

separator handsheets were explored, as shown in Figure 4. It can be found in

195

Figure 4a that with the increase in hot-pressing temperature the tensile strength of

196

the separator handsheets had an overall raising trend. When the hot-pressing

197

temperature exceeded 130 °C, the PE sheath of the EP fibers might begin melting 8

ACS Paragon Plus Environment

Page 8 of 33

Page 9 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

198

and the PP fibers were then adhered to the EP fibers, resulting in an increased

199

tensile index of the separator handsheets, which is consistent with the previous

200

study.14 Actually, there is no bonding strength between the PP fibers, thus the

201

moderate melting of the PE sheath of the EP fibers becomes the main source of

202

producing the bonding strength between the PP fibers. In other words, at that time

203

the EP fibers acted as a binder between the PP fibers. However, as the

204

hot-pressing temperature exceeded 135 °C, the PE sheath of the EP fibers could

205

have completely melted, which led to changing the bonding mode between the

206

fibers in the separator handsheets from ‘contact bonding’ to ‘layered-structure

207

bonding’. Because the stress withstood by a layered-structure bonding is much

208

smaller than that by a contact bonding,30 the tensile strength of the separator

209

handsheets declined until the hot-pressing temperature reached 140 °C. As the

210

hot-pressing temperature was over 140 °C, the ‘layered-structure bonding’ could

211

have been improved greatly, leading to an ascendant trend of the tensile strength

212

once again.

213

The

hot-pressing

decreased

the

diameter

of

the

EP

fibers

and

214

correspondingly increased the tightness of the separator handsheets, as a result,

215

the maximum pore size and porosity of the handsheets were both decreased

216

(Figures 4b and c). Moreover, it can be clearly seen from Figure 4 that the

217

maximum pore size had a rapid decrease as hot-pressing temperature exceeded

218

150 °C.

219

Effect of hot-pressing pressure on the tensile strength, maximum pore

220

size and porosity of the separator handsheets. Figure 5 shows the effect of

221

hot-pressing pressure on the tensile strength, maximum pore size and porosity of

222

the separator handsheets. It can be found in Figure 5a that the tensile index had a 9

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

223

rapid increase at a hot-pressing pressure of lower than 0.5 MPa and a

224

subsequently flat trend beyond 0.5 MPa. Contrary to the trend of tensile index, the

225

maximum pore size and porosity had a rapid decrease at a hot-pressing pressure

226

of lower than 0.5 MPa and a subsequently flat trend beyond 0.5 MPa (Figures 5b

227

and c). In addition, the tensile index, maximum pore size and porosity all rose as

228

the addition level of the EP fibers in the separator handsheets increased at the

229

same hot-pressing pressures. When the proportion of the EP fibers was 40%, the

230

tensile index, maximum pore size and porosity of the resultant separator

231

handsheets reached 33.00 N—m/g, 40.91 µm and 45.71%, respectively. When the

232

pressure rose to 0.5 MPa or more, almost no changes happened to the tensile

233

index, maximum pore size, and porosity. The events above can be explained as

234

follows: under a certain addition level of the EP fibers, high hot-pressing pressure

235

could result in a large contact area and a consequently strong bonding between

236

the fibers in the separator handsheets; as a result, the pore size and porosity

237

declined. The explanation above can be also confirmed by the SEM observation

238

shown in Figure 6. It can be found from Figures 6a to c that more coating which

239

came from the melted PE sheath of the EP fibers appeared on the surface of the

240

separators handsheets, leading to the gradually decreased porosity and pore size

241

of the handsheets. Meanwhile, the bonding between the fibers in the separator

242

handsheets could be enhanced, resulting in the improved tensile strength of the

243

separator handsheets.

244

Optimization of the hot-pressing temperature and pressure for the

245

separator handsheets. Figure 7 further shows the changes of the surface and

246

cross section of the separator handsheets at a hot-pressing pressure of 0.5 MPa

247

and temperatures of 135 °C and 150 °C as follows: on the surface of the separator 10

ACS Paragon Plus Environment

Page 10 of 33

Page 11 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

248

handsheets, both the melting amount of the EP fibers and consequently the

249

binding area at a hot-pressing temperature of 150 °C (Figure 7b) were obviously

250

larger than that at 135 °C (Figure 7a); on the cross section of the separator

251

handsheets, almost all the fibers were more tightly closed with each other at

252

150 °C (Figure 7d) than that at 135 °C (Figure 7c), both leading to the decreased

253

porosity and maximum pore size.

254

In general, the requirements of the maximum pore size and porosity for

255

alkaline battery separators are less than 50 µm (QB/T 4173 (2011)) and 40% or

256

more,26,31 respectively. Based on the discussions above, the appropriate

257

hot-pressing pressure and temperature were 0.5 MPa and 135 °C, respectively.

258

Effect of PEO addition on fiber dispersion. It can be found in Figure 8 that

259

with the increase in sedimentation time the sedimentation volume of fibers in the

260

fiber suspension has a reducing trend. The sedimentation volume decreased

261

rapidly when the sedimentation time was less than 225 s, and then went flatly

262

beyond 225 s. The above can be explained as follows: the PP fibers flocculated

263

constantly before 225 s, and flocculated completely over 225 s, which is consistent

264

with the fact that the tensile index reduced with increasing the PEO dosage.

265

Figure 9 shows the effect of adding PEO on the sedimentation volume of

266

fibers in the fiber suspension. It can be seen from this figure that the sedimentation

267

volume had an increasing trend, especially when the PEO dosage was lower than

268

1.5%. This can be attributed to that the addition of PEO might increase the

269

viscosity of the fiber suspension and therefore prevented the PP fibers from

270

flocculating, thus making PP fibers and EP fibers uniformly mixed in the

271

suspension.16

272

Effects of PEO and PVA additions on tensile strength of the separator 11

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

273

handsheets. It can be found in Figure 10a that the tensile index of the separator

274

handsheets made of 60% PP fibers and 40% EP fibers just reached 33.00 N—m/g

275

at a hot-pressing pressure of 0.5 MPa and temperature of 135 °C for 90 s,

276

suggesting that it did not meet the needs of more than 40.00 N—m/g required in

277

QB/T 4173 (2011). Consequently, PEO and PVA were selected as dispersant and

278

reinforcing agent, respectively, to add to the fiber suspension for further enhancing

279

the tensile strength of the resultant separator handsheets in this work. Figure 1h

280

shows the formation of the resultant separator handsheets, seemingly no obvious

281

change compared to that shown in Figure 1g.

282

Figure 10a shows the effect of the PEO dosage on the tensile index of the

283

separator handsheets. It can be seen that the tensile index had a sharp increase

284

until the PEO dosage reached 1.5% (on oven-dry fibers) and that the maximal

285

tensile index of 40.29 N—m/g could be got at the PEO dosage of 1.5%. This is

286

because with an increase in the PEO dosage the viscosity of the fiber suspension

287

rose and the movement of the PP fibers in the fiber suspension was blocked,

288

resulting in the improved formation and resultant tensile index, which is consistent

289

with the previous report.32 However, when the PEO dosage exceeded 1.5% in the

290

handsheet-making process, the drainage time of the fiber suspension on the

291

formation web was so prolonged that the PP fibers could flocculate again,28 which

292

led to a poor formation and consequently decreased tensile strength of the

293

resultant separator handsheets.

294

Figure 10b shows the effect of the PVA dosage on the tensile index and

295

maximum pore size of the separator handsheets at the PEO dosage of 1.5% (on

296

oven-dry fibers). It can be clearly seen in Figure 10b that the tensile index

297

increased obviously until the addition level of PVA was up to 4.0% (on oven-dry 12

ACS Paragon Plus Environment

Page 12 of 33

Page 13 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

298

fibers) and then went slowly, in which the tensile index increased from 40.29 N—m/g

299

to 45.16 N—m/g, an increment of 12.1%. That can be attributed to the good bonding

300

property of the PVA between the fibers in the separator handsheets in the

301

hot-pressing treatment. However, the maximum pore size went completely

302

opposite to the tensile index, because the existence of PVA improved the bonding

303

area between the fibers, resulting in a decrease in the pore size of the separator

304

handsheet. When the PEO and PVA dosages were 1.5% and 4.0%, respectively,

305

the maximum pore size decreased from 40.31 µm to 34.19 µm, a decrement of

306

15.2%. As the addition level of PVA was further raised, the maximum pore size did

307

not meet the needs (30-50 µm) required in QB/T 4173 (2011). Therefore, at the

308

addition level of 1.5% PEO, the appropriate dosage of PVA was 4.0% on oven-dry

309

fibers.

310

Performance of the separator handsheets under the optimal conditions.

311

Based on all discussions above, the separator handsheets were also made of 60%

312

PP fibers and 40% EP fibers under the optimum conditions as follows: 1.5% PEO;

313

4.0% PVA; hot-pressing pressure of 0.5 MPa; and hot-pressing temperature of

314

135 °C for 90 s. The performance of the separator handsheets was then tested,

315

and the results are listed in Table 1. It can be seen in Table 1 that the tensile

316

strength, maximum pore size, porosity and alkali resistance of the separator

317

handsheets were qualified compared to the standard values set in QB/T 4173

318

(2011). In order to further compare the performance of the separator handsheets

319

to that of some commercial separators available in the market and the standard

320

values in QB/T 4173 (2011), the above separator handsheets were then

321

experienced a sulphonation treatment to increase their absorbing capability. The

322

result of the corresponding comparison is listed in Table 2, in which the data for 13

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

323

two commercial separators are cited in literatures.18,33 It can be seen in Table 2

324

that the tensile index and alkali absorption rate of the separator handsheets were

325

lower than those of the American product but met the needs of QB/T 4173 (2011),

326

and the alkali resistance of the separator handsheets was the highest among the

327

three samples.

328

■ CONCLUSIONS

329

The handsheets of alkaline battery separators were successfully made of PP

330

fibers and EP fibers in the wet-laid process followed by a hot-pressing treatment.

331

Both the formation issue that exists in the wet-laid process and the poor

332

corresponding tensile strength of the resultant alkaline battery separators can be

333

solved. A better formation of the separator handsheet could be obtained when the

334

addition of the EP fibers was not less than 20%. The properties such as tensile

335

strength, maximum pore size, porosity and alkali resistance of the separator

336

handsheets made of 60% PP fibers and 40% EP fibers could meet the needs

337

required in QB/T 4173 (2011) under the conditions of 1.5% PEO and 4.0% PVA

338

additions (on oven-dry fibers), the hot-pressing pressure of 0.5 MPa, and

339

hot-pressing temperature of 135 °C for 90 s.

340

■ AUTHOR INFORMATION

341

Corresponding Author

342

343 344 345 346

*Email: [email protected] (Q. X. Hou) ■ REFERENCES

(1) Bitsche, O.; Gutmann, G. Systems for hybrid cars. J. Power Sources. 2004, 127, 8–15. (2) Verbrugge, M.; Tate, E. Adaptive state of charge algorithm for nickel metal 14

ACS Paragon Plus Environment

Page 14 of 33

Page 15 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

347

hydride batteries including hysteresis phenomena. J. Power Sources. 2004, 126,

348

236–249.

349

(3) Taniguchi, A.; Fujioka, N.; Ikoma, M.; Ohta, A. Development of

350

nickel/metal-hydride batteries for EVs and HEVs. J. Power Sources. 2001, 100,

351

117–124.

352

(4) Shinyama, K.; Harada, Y.; Maeda, R.; Nakamura, H.; Matsute, S.; Nohma, T.;

353

Yonezu, I. Effect of separators on the self-discharge reaction in nickel-metal

354

hydride batteries. Res. Chem. Intermed. 2006, 32, 447–452.

355

(5) Li, X.; Song, Y.; Wang, L.; Xia, T.; Li, S. Self-discharge mechanism of Ni-MH

356

battery by using acrylic acid grafted polypropylene separator. Int. J. Hydrogen

357

Energy. 2010, 35, 3798–3801.

358 359

(6) Jiao, X. N.; Yang, W. J. Nonwoven separator for Ni-MH battery. China Text. Leader. 2005, 12, 71–74.

360

(7) Ciszewski, A.; Kunicki, J.; Gancarz, I. Usefulness of microporous

361

hydrophobic polypropylene membranes after plasma-induced graft polymerization

362

of acrylic acid for high-power nickel-cadmium batteries. Electrochim. Acta. 2007,

363

52, 5207–5212.

364

(8) Jiao, X. N.; Cheng, B.; Kang, W. M.; Yang, W. J. Nickel–metal hydride

365

battery separators fabricated from sulfonated nonwovens. J. Appl. Polym. Sci.,

366

2008, 109, 272–275.

367

(9) Gancarz, I.; Bryjak, M.; Kunicki, J.; Ciszewski, A. Microwave plasma-initiated

368

grafting of acrylic acid on Celgard 2500 membrane to prepare alkaline battery

369

separators—Characteristics of process and product. J. Appl. Polym. Sci. 2010, 116,

370

868-875.

371

(10) Ciszewski, A.; Gancarz, I.; Kunicki, J.; Bryjak, M. Plasma-modified 15

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

372

polypropylene membranes as separators in high-power alkaline batteries. Coat.

373

Technol. 2006, 201, 3676–3684.

374

(11) Ming, X.; Tang, H. L.; Wang, Y. D.; Mu, P. Ethylcellulose-coated polyolefin

375

separators for lithium-ion batteries with improved safety performance. Carbohydr.

376

Polym. 2014, 101, 1140–1146.

377 378 379 380 381 382

(12) Williams, R. C.; Goettmann, J. A.; Funk, G, L.; Gee, L. M. Wet-laid nonwoven polyolefin battery separator substrate, 6174826 US Patent, 2001. (13) Kubo, Y. Separator paper for alkaline-battery, 5,311,059 JP 1959 Patent, 1959. (14) Kritzer, P.; Cook, J. A. Nonwovens as separators for alkaline batteries an overview. J. Electrochem. Soc. 2007, 154, A481–A494.

383

(15) Kritzer, P. Separators for nickel metal hydride and nickel cadmium

384

batteries designed to reduce self-discharge rates. J. Power Sources. 2004, 137,

385

317–321.

386 387

(16) Liu, X. Y.; Chen, J. Z.; Ren, B. L. Study on polyolefin fiber battery separator paper. China Pulp Pap. 2007, 26, 15–17.

388

(17) Chen, W. J.; Shi, L. Y.; Wang, Z. Y.; Zhu, J. F.; Yang, H. J.; Mao, X. F.; Chi,

389

M. M.; Sun, L. N.; Yuan, S. Porous cellulose diacetate-SiO2 composite coating on

390

polyethylene separator for high-performance lithium-ion battery. Carbohydr. Polym.

391

2016, 147, 517–524.

392

(18) Tian, Y. C.; Gao, H. P.; Wang, J. C.; Jin, X. Y.; Wang, H. W. Preparation of

393

hydroentangled CMC composite nonwoven fabrics as high performance separator

394

for nickel metal hydride battery. Electrochim. Acta. 2015, 177, 321–326.

395

(19) Tadokoro, Y.; Uesaka, M.; Takata, Y.; Goto, F. Wet-laid nonwoven fabric for

396

battery separator, its production method and sealed type secondary battery, 16

ACS Paragon Plus Environment

Page 16 of 33

Page 17 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

397 398 399

Industrial & Engineering Chemistry Research

5888916 US Patent, 1999. (20) Tabatabaei, S. H.; Carreau, P. J.; Ajji, A. Microporous membranes obtained from PP/HDPE multilayer films by stretching. J. Membr. Sci. 2009, 345, 148–159.

400

(21) Wu, H. L.; Li, K.; Sun. T.; Liu, B.; Kou, F.; Jia, F.; Yuan, J. K.; Bai, Y.

401

Synthesis, Crystal Structure, and DNA-Binding Studies of a Ni(II) Complex with the

402

Tris (N-methylbenzimidazol -2-ylmethyl)amine Ligand. J. Chem. Sci. 2010, 65,

403

1474–1480.

404 405 406 407

(22) Kurauchi, H.; Akazawa, T. Process for producing microporous film having breakage resistance when melted, 5258156A US Patent, 1993. (23) Wang, H.; Sha, C. H.; Jin, X. Y. Hydrophilic polypropylene melt-blown nonwoven as Ni/MN battery separator. Battery Bimon. 2013, 43. 166–169.

408

(24) Wang, H.; Jin, X. Y.; Mao, N. T.; Russell, S. J. Differences in the Tensile

409

Properties and Failure Mechanism of PP/PE Core/Sheath Bicomponent and PP

410

Spunbond Fabrics in Uniaxial Conditions. Text. Res. J. 2010, 80, 1759-1767.

411

(25) Kapłonek, W.; Nadolny, K. Assessment of the grinding wheel active surface

412

condition using SEM and image analysis techniques. J. Braz. Soc. Mech. Sci. Eng.

413

2013, 35, 207–215.

414

(26) Yanilmaz, M.; Lu, Y.; Li, Y.; Zhang, X. W. SiO2/polyacrylonitrile membranes

415

via centrifugal spinning as a separator for li-ion batteries. J. Power Sources. 2015,

416

273, 1114–1119.

417

(27) Liu, Q. Z.; Xia, M.; Chen, J. H.; Tao, Y. F.; Wang, Y. D.; Liu, K.; Li, M. F.;

418

Wang,

419

alcohol-co-ethylene) nanofibrous membrane for lithium-ion battery separator.

420

Electrochim. Acta. 2015, 176, 949–955.

421

W.

W.;

Wang,

D.

High

performance

hybrid

Al2O3/poly(vinyl

(28) Shen, F. Y.; Zhang, X. F. Study of making alkaline battery separator paper 17

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

422 423 424 425 426 427 428

by wet papermaking. J. Membr. Sci. Technol. 2013, 33, 24–119. (29) Zhao, L. J.; Liu, W.; Zhou, L. C. Effect of hot press on physical properties of battery separator paper-base. China Pulp Pap. Ind. 2016, 22, 34–38. (30) Wang, Y. X. Non-woven fabric production technologies; China textile University Press: Shanghai, 1998. (31) Hu, J. W.; Xu, K.; Shen, J. R. Research and development of separators for lithium-ion batteries. Polym. Mater.: Sci. Eng. 2003, 19, 215–219.

429

(32) Gaudreault, R.; Ven, T. G. M. V. D.; Whitehead, M. A. Mechanisms of

430

flocculation with poly (ethylene oxide) and novel cofactors. Colloids Surf., A. 2005,

431

268, 131–146.

432

(33) Zhang, W. N. Preliminary research on high performance battery separator

433

of alkaline-manganese battery. M.S. Thesis, South China Univ. Technol.,

434

Guangdong, 2010.

435 436 437 438 439 440 441 442 443

18

ACS Paragon Plus Environment

Page 18 of 33

Page 19 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

Captions of Figures Figure 1. Images of the handsheet formation of alkaline battery separator with different addition levels of the EP fibers: (a) 100% PP; (b) 10% EP + 90% PP; (c) 15% EP + 85% PP; (d) 20% EP + 80% PP; (e) 30% EP + 70% PP; (f) 35% EP + 65% PP; (g) 40% EP + 60% PP;(h) (40% EP + 60% PP)/(1.5% PEO + 4.0% PVA). Figure 2. DSC curves of the separator handsheets: T1 was the initial melting temperature of PE sheath of the EP fibers; T2 was the initial melting temperature of the PP fibers and PP core of the EP fibers. Figure 3. Effect of the addition level of the EP fibers on the porosity and maximum pore size of the separator handsheets at hot-pressing pressure of 0.5 MPa and temperature of 135 °C for 90 s. Figure 4. Effect of hot-pressing temperature on the tensile index (a), maximum pore size (b) and porosity (c) of the separator handsheets at hot-pressing pressure of 0.5 MPa for 90 s. Figure 5. Effect of hot-pressing pressure on the tensile index (a), maximum pore size (b) and porosity (c) of the separator handsheets at hot-pressing temperature of 135 °C for 90 s. Figure 6. SEM images of the separator handsheets made of 60% PP fibers and 40% EP fibers under the conditions of hot-pressing pressure of 0.1 MPa (a), 0.3 MPa (b) and, 0.5 MPa (c) and hot-pressing temperature of 135 °C for 90 s. Figure 7. SEM images of the surfaces (a, 135 °C; b, 150 °C) and cross sections (c, 135 °C; d, 150 °C) of the separator handsheets made of 60% PP fibers and 40% EP fibers under the conditions of a pressure of 0.5 MPa and 19

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

temperatures of 135 °C and 150 °C for 90 s. Figure 8. Relationship of the sedimentation volume of the fibers in the fiber suspension with time. Figure 9. Effect of adding PEO on the sedimentation volume of fibers in the fiber suspension. Figure 10. Effects of PEO (a) and PVA (b) dosages on the tensile index and/or maximum pore size of the separator handsheets at hot-pressing pressure of 0.5 MPa and temperature of 135 °C for 90 s.

Captions of Tables Table 1. Performance of the separator handsheets. Table 2. The performance comparison of commercial separators and the separator handsheets expericed a sulphonation treatment.

20

ACS Paragon Plus Environment

Page 20 of 33

Page 21 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

Figure 1.

a

b

c

d

e

f

g

h

21

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

Figure 2.

Heat Flow Endo Up

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 22 of 33

20% EP + 80% PP 30% EP + 70% PP 40% EP + 60% PP (40% EP + 60% PP)/1.5% PEO (40% EP + 60% PP)/1.5% PEO/4% PVA

T1=130 oC

20

40

60

80

100

120

140

T2=170 oC

160

Temperature, oC

22

ACS Paragon Plus Environment

180

200

Page 23 of 33

Figure 3.

60 55 40% EP + 60 %PP 1.5% PEO

50

50

45 45

40

40

35 Maximum pore size Porosity

30 25

35 30

20

30

40

50

60

ES fiber dosage, %(on oven-dry fibers)

23

ACS Paragon Plus Environment

Maximum pore size, µm

55

Porosity, %

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

Industrial & Engineering Chemistry Research

a

48

b

50

Maximum pore size, µm

Figure 4.

45

45 30% EP + 70% PP 35% EP + 65% PP 40% EP + 60% PP

42 39 36 33 30 130

135

140

145

150

155

30% EP + 70% PP 35% EP + 65% PP 40% EP + 60% PP

40 35 30

27

25

160

130

135

o

c

140

52 30% EP + 70% PP 35% EP + 65% PP 40% EP + 60% PP

48 44 40 36 32 130

145

150

155

Hot-pressing tempeture, oC

Hot-pressing temperature, C

Porosity, %

Tensile index, N·m/g

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 24 of 33

135

140

145

150

155

160

Hot-pressing tempeture, oC

24

ACS Paragon Plus Environment

160

Page 25 of 33

34

b

32 30 28 30% EP + 70% PP 35% EP + 65% PP 40% EP + 60% PP

26 24 22

80 30% EP + 70% PP 35% EP + 65% PP 40% EP + 60% PP

70 60 50 40 30

0.1

0.2

0.3

0.4

0.5

0.6

0.1

c

0.2

65 30% EP + 70% PP 35% EP + 65% PP 40% EP + 40% PP

60 55 50 45 40 35 0.1

0.3

0.4

0.5

Hot-pressing pressure, MPa

Hot-pressing pressure, MPa

Porosity, %

a

Maximum pore size, µ m

Figure 5.

Tensile index, N·m/g

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

0.2

0.3

0.4

0.5

0.6

Hot-pressing pressure, MPa

25

ACS Paragon Plus Environment

0.6

Industrial & Engineering Chemistry Research

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 6.

26

ACS Paragon Plus Environment

Page 26 of 33

Page 27 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

Figure 7.

27

ACS Paragon Plus Environment

Industrial & Engineering Chemistry Research

Figure 8.

700

Sedimentation volume, mL

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 28 of 33

650 1.5% PEO 3.0% PEO

600 550

40% EP + 60% PP

500 450 0

100

200

300

400

Sedimentation time, s

28

ACS Paragon Plus Environment

500

600

Page 29 of 33

Figure 9.

560

Sedimentation volume, mL

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

540 40% EP + 60% PP sedimentation time of 2 min

520 500 480 460 440 420 0.0

0.5

1.0

1.5

2.0

2.5

PEO dosage, % (on oven-dry fibers)

29

ACS Paragon Plus Environment

3.0

Industrial & Engineering Chemistry Research

Figure 10.

42 40% EP + 60% PP

b Tensile index, N·m/g

40 38 36 34 32

42 46 39

45 40% EP + 60% PP 1.5% PEO

44

36 33

43 42

30 Tensile index Maximum pore size

41

27

40 24 0.0

0.5

1.0

1.5

2.0

2.5

3.0

0

1

2

3

4

5

6

7

PVA dosage, % (on oven-dry fibers)

PEO dosage, % (on oven-dry fibers)

30

ACS Paragon Plus Environment

8

Maximum pore size, µ m

a Tensile index, N·m/g

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 30 of 33

Page 31 of 33

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Industrial & Engineering Chemistry Research

Table 1

2

Basis weight (g/cm ) Maximum pore size (µm) Porosity (%) Tensile index (N—m/g) Alkali resistance (%) *

Standard valuea

Test sample*

30 ~ 50 30 ~ 50 ≥ 40 ≥ 40