Effect of corrosion inhibitors on in-situ leak repair ... - ACS Publications

Jun 28, 2017 - in-service water distribution pipeline leak repair via clogging. ... phosphates that could inhibit leak repair over the short term in o...
1 downloads 0 Views 1MB Size
Subscriber access provided by NEW YORK UNIV

Article

Effect of corrosion inhibitors on in-situ leak repair by precipitation of calcium carbonate in potable water pipelines Fei Wang, Christina L. Devine, and Marc A. Edwards Environ. Sci. Technol., Just Accepted Manuscript • DOI: 10.1021/acs.est.7b01380 • Publication Date (Web): 29 Jun 2017 Downloaded from http://pubs.acs.org on June 29, 2017

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

Environmental Science & Technology is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 32

Environmental Science & Technology

1

Effect of corrosion inhibitors on in-situ leak repair by precipitation of calcium

2

carbonate in potable water pipelines

3 4

Fei Wang, Christina L. Devine and Marc A. Edwards *

5

The Charles E. Via, Jr. Department of Civil & Environmental Engineering

6

Virginia Tech

7

Blacksburg, VA 24061

8 9

*Corresponding author:

10

Durham Hall 407

11

Blacksburg, VA 24061

12

Phone: (540) 231-7236

13

Fax: (540) 231-7916

14

Email: [email protected]

15 16

To submit to Environmental Science & Technology

17

June 28, 2017

18

1 ACS Paragon Plus Environment

Environmental Science & Technology

Page 2 of 32

19

Abstract

20

Corrosion inhibitors can affect calcium carbonate precipitation and associated in-situ and

21

in-service water distribution pipeline leak repair via clogging. Clogging of 150 µm

22

diameter leak holes represented by glass capillary tubes, in recirculating solutions that are

23

supersaturated with calcite (Ωcalcite=13), demonstrated that Zn, orthophosphate,

24

tripolyphosphate and hexametaphosphate corrosion/scaling inhibitors hinder clogging but

25

natural organic matter (NOM) has relatively little impact. Critical concentrations of

26

phosphates that could inhibit leak repair over the short term in one water tested were:

27

tripolyphophate (0.05 mg/L as P) < hexametaphosphate (0.1 mg/L) < orthophosphate (0.3

28

mg/L). Inhibitor blends (Zn+orthophosphate and Zn+NOM+orthophosphate) had

29

stronger inhibitory effects compared to each inhibitor (Zn, orthophosphate or NOM)

30

alone, whereas Zn+NOM showed a lesser inhibitory effect than its individual component

31

(NOM) alone presumably due to formation of smaller CaCO3 particles with a much more

32

negative Zeta-potential. Overall, increased dosing of corrosion inhibitors is probably

33

reducing the likelihood of scaling and in-situ and in-service leak repair via clogging with

34

calcium carbonate solids in potable water systems.

35

2 ACS Paragon Plus Environment

Page 3 of 32

Environmental Science & Technology

36

Introduction

37

Calcium carbonate (CaCO3) precipitation has undoubtedly been a critical operational

38

concern since potable water distribution systems were first invented. Waters highly

39

supersaturated with respect to CaCO3 can cause severe scaling problems including pipe

40

blockage and energy loss in heat transfer elements of hot water systems.1 Nearly a

41

century ago, waters that were highly undersaturated with respect to CaCO3 were also

42

assumed to be corrosive to metallic and concrete pipe infrastructure,2 leading to studies

43

attempting to reduce corrosivity by increasing the likelihood of CaCO3 precipitation as

44

monitored with Langelier 3 and similar indices.

45 46

Although use of Langelier index to guide corrosion control fell out of favor,3-7

47

engineering practice and water quality are changing in a manner that will potentially

48

thrust the problems related to CaCO3 back into the spotlight. These changes include (1)

49

potential CaCO3 precipitation inhibitors are now more commonly present naturally or

50

added to distribution systems;8 (2) an increased target temperature (> 51 °C) is suggested

51

for hot water systems in buildings to reduce the growth of pathogens such as Legionella

52

pneumophila;9 (3) rising atmospheric CO2 levels might increase calcium levels in natural

53

waters;10, 11 and (4) increasing use of deicing salt including CaCl2,12, 13 can contribute to

54

higher Ca entering both ground and surface waters.14 Researchers have found that CaCO3

55

particles can clog small leaks in potable water pipes, and may extend the lifetime of

56

distributions systems through both in-situ and in-service leak repair mechanism,15-23

57

highlighting heretofore under-appreciated benefits from CaCO3 scaling in preventing

58

pipeline degradation.

3 ACS Paragon Plus Environment

Environmental Science & Technology

Page 4 of 32

59 60

In-situ and in-service repair of leaks by CaCO3 precipitation is a potentially

61

transformative approach that attempts to use flowing waterborne or waterformed CaCO3

62

solids to clog leaks while a pipeline is still in service. Although there is no record of

63

intentional use of this approach in the context of modern potable water distribution

64

systems, the concept dates back at least to Roman engineers (≈15 BC), who dosed

65

alkaline wood-ash to new terracotta pipelines to permanently seal pressure pipe leaks.24

66

In the 1960s, leaks in concrete pipelines for irrigation waters were sealed by adding

67

anhydrous ammonia to raise pH and induce CaCO3 precipitation.25,

68

CaCO3 lining was attempted to coat the inner surface of potable water pipes to combat

69

corrosion, by targeting supersaturation of CaCO3, although the concept of small leak

70

clogging was never mentioned.27,

71

feasibility of leak crack clogging with CaCO3 precipitation, as a function of

72

supersaturation level (14-30 mg/L of Ca), surface materials (glass, hydraulic cement), and

73

crack widths (10 - 25 µm),22 and other recent studies also demonstrated the capability of

74

water-formed deposits, including CaCO3, to clog leaks and restore some strength of large

75

cracks in reactive new concrete.21 Changes in water supplies that might hinder formation

76

of CaCO3, could potentially leave a water distribution system more vulnerable to damage

77

by disabling processes that once allowed pipes to naturally heal themselves -- an

78

important problem given that upgrading damaged water infrastructure is expected to cost

79

about $1 trillion dollars over the next 25 years.29

28

26

In the 1980s,

Snyder and Letterman explicitly considered the

80 81

Two mechanisms can be operative during in-situ and in-service repair of leaks by CaCO3

4 ACS Paragon Plus Environment

Page 5 of 32

Environmental Science & Technology

82

precipitation.23 Physical clogging can occur when waterborne particles, such as soil,

83

bacteria, sand, clay, Al(OH)3, Fe(OH)3 or CaCO3, seal leaks by blockage. Precipitation on

84

the inner surfaces of leak holes can also seal leaks. Physical clogging and precipitation

85

could occur in pipes of all materials, although the importance of autogenous in-situ and

86

in-service leak repair is believed most important for concrete pipe leaks that have reactive

87

lime present in the matrix.23 Precipitation of CaCO3 is less likely in aged concrete in

88

which lime has been converted to CaCO3. Snyder’s use of inert glass cracks with width of

89

10-25 µm simulated a typical worst-case condition of tiny holes in the aged concrete of

90

the Delaware aqueduct after over 60 years (as of 2007) of exposure to a low alkalinity

91

water prone to leaching of lime.22

92 93

Corrosion inhibitors are now widely added at water utilities,8 and it is logical to suspect

94

they might have inadvertently prevented in-situ and in-service repair by CaCO3

95

precipitation in the last few decades. Specifically, to control lead and copper corrosion in

96

the USA, water treatment plants have been increasingly dosing phosphates and

97

polyphosphates since the advent of the Lead and Copper Rule (LCR) in 1991 by US

98

Environmental Protection Agency (EPA), to meet the action limit for lead of 15 µg/L in

99

tap water.8 Similarly, the Water Supply (Water Quality) Regulations of the United

100

Kingdom, the Drinking Water Directive of the European Union, the Drinking Water

101

Guidelines of Canada, the Drinking Water Standards in Japan, and the Standards for

102

Drinking Water Quality in China, have recently decreased the drinking water standard for

103

lead to 10 ug/L which will increase the impetus for phosphate dosing.30-34 However,

104

phosphates can also prevent CaCO3 precipitation.35,

36

Lin and Singer systematically

5 ACS Paragon Plus Environment

Environmental Science & Technology

Page 6 of 32

105

studied the inhibitory effects of orthophosphate (PO43-), pyrophosphate (P2O74-),

106

tripolyphosphate (P3O105-), hexametaphosphate (P6O186-) and binary-polyphosphate

107

blends at P concentrations of 10-8 M and above, and suggested that phosphates could

108

adsorb onto calcite crystal growth sites (or kinks) to inhibit calcite precipitation.35,

109

They did not identify threshold values (or the smallest values needed) for phosphates to

110

inhibit CaCO3 precipitation. In addition, NOM (e.g. fulvic acid and humic acid) that are

111

naturally present in aquatic systems, can also inhibit calcite precipitation through a

112

similar mechanism as phosphates.37-39

36

113 114

Zinc cations (or Zn2+) are sometimes present in potable water systems as a byproduct of

115

brass or galvanized iron corrosion, or are sometimes dosed along with phosphates as

116

corrosion inhibitors by water utilities,8 and these practices might also influence the

117

likelihood of leak repair. Addition of Zn2+ by itself at a concentration of 0.1-10 ppm can

118

significantly inhibit calcite precipitation,40, 41 and the formation of aragonite and vaterite

119

in addition to calcite has been observed.40, 42 Ghizellaoui and Euvrard

120

the adsorption of Zn2+ onto calcite crystal growth sites and subsequent blocking (or kink

121

blocking) or the co-precipitation of Zn2+ with CaCO3 might be operative. Wada et al.

122

also found an inhibitory effect by Zn2+, as it favored formation of aragonite instead of

123

calcite. It is possible that this change in mineralogy could also affect the likelihood of

124

scaling problems.

40

suggested that

42

125 126

Changes under consideration for dosing corrosion inhibitors (e.g. phosphates and Zn)

127

may also be important for CaCO3 precipitation in potable water systems. Although water

6 ACS Paragon Plus Environment

Page 7 of 32

Environmental Science & Technology

128

utilities were increasingly dosing phosphate corrosion inhibitors from 1991 to present to

129

control lead and copper corrosion, some water utilities are now considering whether they

130

should decrease the use of phosphates due to initial costs of adding the chemical and later

131

removing it at the sewage treatment plant, and a desire to conserve phosphate

132

resources.43-46 The dosage of Zn may also have been reduced, due to recent studies

133

inability to find it contributes to corrosion control of materials including lead, copper and

134

cement.47, 48 On the other hand, other water utilities are considering the need to increase

135

the levels of phosphates and Zn to better control lead corrosion. A key point is that there

136

is presently pressure on water utilities to consider both increasing or decreasing corrosion

137

inhibitor dose, and an improved understanding of phosphates holistic impacts on water

138

system performance including scaling is much needed.

139 140

The objective of this study was to: (1) Examine leak repair using controlled CaCO3

141

precipitation and determine the effects of corrosion inhibitors on leak repair kinetics and

142

morphology. We hypothesize that small leaks can be blocked via CaCO3 precipitation,

143

and corrosion inhibitors may impair this process, because they also inhibit CaCO3

144

precipitation. (2) Investigate the effect of single inhibitors (Zn, NOM, orthophosphate,

145

tripolyphosphate and hexametaphosphate) on leak repair over a range of conditions

146

relevant to portable water systems. Each corrosion inhibitor can exhibit different degrees

147

of impact on leak repair, because some are better inhibitors of CaCO3 precipitation (e.g.,

148

tripolyphosphate and hexametaphosphate are stronger than orthophosphate). (3)

149

Investigate the effect of mixed inhibitors on leak repair via CaCO3 precipitation, as

150

combinations of inhibitors will sometimes have stronger effects compared to single

7 ACS Paragon Plus Environment

Environmental Science & Technology

Page 8 of 32

151

inhibitors. (4) Shed light on why some existing pipelines may develop leaks that grow to

152

failure, while other leaks are self-limiting, which may be critical factors to improving the

153

longevity of these critical infrastructure assets.

154 155

Materials and methods

156

Materials

157

Solutions of CaCl2 and NaHCO3 were prepared by dissolving CaCl2·2H2O and NaHCO3

158

(Fisher Scientific) into deionized water. Similarly, solutions of Zn, NOM, orthophosphate

159

(or P1), tripolyphosphate (or P3) and hexametaphosphate (or P6) were prepared using

160

ZnCl2 (Sigma Aldrich), Na3PO4•12H2O (Fisher Scientific), Na5P3O10 and Na8P6O19

161

(Sigma Aldrich).

162 ൛஼௔మశ ൟ∙{஼ைయమష }

163

All test solutions had the same degree of supersaturation (Ω௖௔௟௖௜௧௘ =

164

calcite precipitation, which can be described in terms of the calcite solubility product

165

(Ksp,calcite=10-8.48) and the activities of dissolved Ca2+ and CO32-.

166

Ωcalcite=13 were prepared by adding CaCl2 and NaHCO3 in a 1:1 molar concentration

167

ratio (Table S1). Although Ωcalcite=13 is on the higher end of what is encountered in

168

potable water systems, it was selected to be a “worst case” test of inhibitor effectiveness

169

in preventing scaling.

49, 50

௄ೞ೛,೎ೌ೗೎೔೟೐

) to drive

The solutions with

170 171

Methods

172

CaCO3 precipitation and leak repair tests were tracked in recirculation systems with

173

simulated leaks (Figure S1). Initially, glass bottles (or reservoirs) were filled with 2 liter 8 ACS Paragon Plus Environment

Page 9 of 32

Environmental Science & Technology

174

of Ωcalcite=13 solutions. Within 10 minutes of making the solutions, a peristaltic pump

175

(model 7553-70, Cole Parmer) delivered solutions at a flow rate of 1100 mL/min through

176

hard-wall rigid clear PVC tubing (1/4” ID, McMaster Carr). To simulate concrete leaks, a

177

method similar to that of Snyder

178

capillary tubing with 150 µm ID (VitroCom) were mounted onto the side of rigid clear

179

PVC tubing using Epoxy.

22

was used, in which borosilicate heavy-wall glass

180 181

Leak rates through the glass capillaries were measured at certain times (0 h – 24 h) to

182

monitor the kinetics of clogging. Reservoir solution pH was measured every time the leak

183

rates were measured. The pH at t=10 min was measured right after a peristaltic pump

184

initially delivered solutions through the recirculating system, in addition to the initial pH

185

at t=0 min. After the experiments, liquid samples were collected from reservoirs, and

186

solids remaining in the reservoirs were collected using vacuum filtration and dried at

187

room temperature. Liquid samples were analyzed by inductively coupled plasma mass

188

spectroscopy (ICP-MS) for concentrations of dissolved Ca, by laser scattering particle

189

size distribution analyzer (Horiba LA-300) for CaCO3 particle sizes, and by Zeta-Meter

190

for zeta-potential of particles (Model 3.0+, Zeta-Meter, Inc.). Solid samples were

191

characterized by XRD and SEM. Glass capillaries were removed from the recirculation

192

systems and observed with an Amscope microscope (model IN300TC) with digital

193

camera to characterize the nature of the leak repair. Reproducibility was tested by

194

studying the onset of CaCO3 precipitation in the reservoir using beaker tests in triplicates,

195

and the system error was confirmed as