Subscriber access provided by READING UNIV
Article
Effects of poly(vinyl chloride) morphological properties on the rheology/aging of plastisols and on the thermal/leaching properties of films formulated using non-conventional plasticizers Sofia Marceneiro, Rafael Alves, Irene Lobo, Isabel Dias, Elizabete Pinho, Ana M.A. Dias, Maria G. Rasteiro, and Herminio C. C. de Sousa Ind. Eng. Chem. Res., Just Accepted Manuscript • DOI: 10.1021/acs.iecr.7b03097 • Publication Date (Web): 16 Jan 2018 Downloaded from http://pubs.acs.org on January 16, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Industrial & Engineering Chemistry Research is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 42 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49
Effects of poly(vinyl chloride) morphological properties on the rheology/aging of plastisols and on the thermal/leaching properties of films formulated using nonconventional plasticizers Sofia Marceneiro1,2, Rafael Alves1, Irene Lobo2, Isabel Dias2, Elizabete de Pinho2, Ana M.A. Dias1*, M. Graça Rasteiro1*, Hermínio C. de Sousa1* 1
CIEPQPF, Chemical Engineering Department, FCTUC, University of Coimbra, Rua Sílvio Lima, Pólo II – Pinhal de Marrocos, 3030-790 Coimbra, Portugal 2 TMG Automotive, S. Cosme do Vale, Apartado 14, 4761-912 Vila Nova de Famalicão, Portugal
Abstract The efficiency of poly(vinyl chloride) PVC plasticization depends predominantly on the strength of PVC-plasticizer interactions, which ultimately depends on the intrinsic physicochemical properties of the plasticizer, but also of the polymer. The aim of this work was to study the influence of the morphological properties of different PVC grades (two emulsion (with different K values) and one micro-suspension grades) and of non-conventional greener plasticizers on the rheological/aging properties of PVCbased plastisols and on the thermal and plasticizer leaching properties of films obtained from those plastisols. Commercially available castor oil based CITROFOL® AHII and GRINDSTED® SOFT-N-SAFE were employed as plasticizers and the phosphoniumbased ionic liquid (trihexyl(tetradecyl)phosphonium bistriflamide ([P6,6,6,14][Tf2N]) as a co-plasticizer. Plastisols formulated with the conventional plasticizer di-isodecyl phthalate (DIDP) were also prepared for comparison. Obtained results showed that the highest shear stress and plastisol aging were observed for plastisols formulated using the lower molecular weight emulsion PVC grade (E70-PVC) and the conventional plasticizer DIDP. The E70-PVC systems formulated using DIDP and citrate-based plasticizer presented a pseudo-plastic behavior while all the other systems presented a Newtonian profile. Lower mixing enthalpies were also calculated for PVC/DIDP systems, indicating more favorable interactions for PVC/phthalate systems over nonconventional plasticizers. The incorporation of [P6,6,6,14][Tf2N] as a co-plasticizer significantly decreased the enthalpy of mixing of all the prepared plastisols, showing that its presence in the formulations may favor PVC/plasticizer interactions. Moreover PVC films obtained from plastisols formulated using this ionic liquid presented higher long-term thermal stability due to its negligible vapor pressure that avoids loss during usage. Keywords: emulsion poly(vinyl chloride), micro-suspension poly(vinyl chloride), nonconventional plasticizers, trihexyl(tetradecyl)phosphonium bistriflamide, plastisol rheology, PVC film properties Corresponding authors: E-mail address:
[email protected] (A.M.A. Dias); Phone: +351-239-798758; Fax: +351-239-798703 E-mail address:
[email protected] (H.C. de Sousa); Phone: +351-239-798749; Fax: +351-239-798703 E-mail address:
[email protected] (M.G. Rasteiro); Phone: +351-239-798725; Fax: +351-239-798703
1 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 2 of 42
50
1. INTRODUCTION
51
The automotive industry employs large quantities of synthetic polymers to manufacture
52
flexible products based on elastomers or artificial leather.1 The global awareness for
53
material’s sustainability, as well as the high-cost and limited resources of natural leather
54
has stimulated the development of novel synthetic composite materials for automotive
55
interiors. These materials are currently used to produce car door trims, steering wheel
56
covers, gear boot, seat upholstery, instrument panel and sun visors, by using transfer,
57
calendering, extrusion and/or rotary screen coating manufacturing processes.2
58
Poly(vinyl chloride) (PVC) is one of the most frequently used synthetic resins to
59
produce artificial leather for automotive interiors due to its low cost and tunable
60
capacity through appropriate formulation.1-5 Soft and resilient PVC based artificial
61
leather materials are obtained by plasticization of the resin using considerable amounts
62
of plasticizers (> 60 % wt/wt) which provide a liquid continuous phase to disperse the
63
PVC particles, originating plastisols.5-9 In this process PVC particles are first swollen by
64
the plasticizer and the final flexible product is obtained by gelation during heating of the
65
swelled particles.2,8,10 PVC resins commonly used to formulate plastisols are obtained
66
by emulsion (E-PVC) and micro-suspension (MS-PVC) polymerization. Although MS-
67
PVC resins present lower price/performance ratio than E-PVC grades, they can be used
68
as secondary resins and are often applied in low-fogging automotive applications.2,3
69
There is a large number of commercially available PVC resins used for industrial
70
formulations, with different molecular weight, particle size/distribution, porosity,
71
morphology and crystallinity.2,5,11 They can be classified by their K-value or viscosity
72
number, which is an indicator of their molecular weight and degree of polymerization.
73
K-values are determinant to control PVC processing since it affects the plastisol
74
stability during storage and gelation.8 For automotive interior materials, the K-values of
2 ACS Paragon Plus Environment
Page 3 of 42 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
75
PVC resins range between 64 < K-value < 80 (corresponding to medium to high
76
molecular weights).5-11 The size, structure and distribution of the PVC particles in
77
plastisols, as well as their tendency to deagglomerate and progressively swell (by the
78
incorporation of the plasticizer), are important variables that influence the rheological
79
properties of the plastisols12-15 and consequently define formulation compositions, and
80
processing conditions, that will lead to the envisaged properties of the final product.15-19
81
The efficient large scale processing of PVC plastisols depends not only on the
82
properties of the polymer particles but also on the type and concentration of the
83
plasticizers used, which also have a direct influence on the rheological properties of the
84
plastisols, and on the thermomechanical properties of the processed polymer.20 One of
85
the main requisites of an efficient plasticizer is that it should be compatible with the
86
polymer, which occurs when both the plasticizer and the polymer have similar
87
intermolecular forces. The strength of the plasticizer-polymer and plasticizer-plasticizer
88
interactions depends on the plasticizer properties including its polarity, molecular
89
weight, molecular volume and conformation.2-8 Those interactions will affect the
90
properties of the plastisol formulation (size, structure, distribution profile and
91
agglomeration of the swelled PVC particles) and consequently the properties of the final
92
material, as discussed above, and as previously reported in the literature.6-9,21
93
Ultimately, they have impact over the long-term thermomechanical stability of the final
94
products and on the emission/migration of the plasticizers (and of other additives) from
95
those materials.28
96
So far, most commonly used plasticizers include both low and high molecular weight
97
phthalates (ester side-chain lengths with less or more than 6 carbons (or Mw > 334.45
98
g.mol-1), respectively) which are highly compatible with PVC.8,9 Phthalate ester
99
plasticizers derived from isomeric C10 alcohols are the most frequently used in
3 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 42
100
automotive interiors mainly due to their relatively low volatility when compared to
101
other conventionally used low molecular weight phthalates (e.g. bis(2-ethylhexyl)
102
phthalate (DEHP), dioctyl phthalate (DOP), diisononyl phthalate (DINP)). However,
103
and since they are not covalently bonded to the polymer network, and are volatile (even
104
if to a lower extent than others as just mentioned),24,25 plasticizer migration/leaching
105
from the polymer matrix is likely to occur during PVC processing and/or usage.26 In
106
recent years, and due to more restrictive legislation that limits the incorporation of these
107
compounds in plastic-based materials, the automotive industry is exploring the use of
108
new greener, non-volatile and non-toxic phthalate-free plasticizers to overcome
109
sustainability, performance, environmental and toxicity issues.10,16-18,20-23,27 In this
110
context, natural-based plasticizers (such as citrates, epoxidized derivatives of natural
111
oils, bio-derived succinate esters, etc) are being proposed as promising friendlier
112
alternatives to phthalates in PVC plasticization.10,18,19,28,29 Nevertheless, and to date, the
113
full replacement of conventional high-molecular weight phthalate-based plasticizers by
114
these bio-derived alternatives has not been accomplished due to their higher
115
cost/performance ratios.19,29,30
116
Ionic liquids (ILs) belong to a family of compounds that have been also proposed as
117
alternative plasticizers/stabilizers for PVC, mainly because of their high thermal
118
stability,
119
physicochemical properties such as hydrophilicity, viscosity, miscibility, toxicity and
120
volatility can be tailored by selecting the proper combination of cations and anions.31-35
121
This feature can potentiate PVC-plasticizer compatibility and miscibility, avoiding their
122
migration/volatilization from the plasticized polymer network.19,31-33,36 Previously
123
reported data showed that phosphonium-based ILs (PhILs) were able to successfully
low
flammability
and
negligible
volatility.19,31-35
Moreover,
their
4 ACS Paragon Plus Environment
Page 5 of 42 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
124
plasticize PVC and improve its long-term thermal stability,19,33,36 mainly when
125
bis(trifluoromethanesulfonyl)amide (or bistriflamide) is used as counter-anion.19,35,37-39
126
The aim of this work was to study the influence of the morphological properties of
127
emulsion and micro-suspension poly(vinyl chloride) (PVC) and of non-conventional
128
greener plasticizers on the rheological/aging properties of PVC-based plastisols and on
129
the thermal and plasticizer leaching properties of films obtained from those plastisols.
130
For that purpose two emulsion (with different K values) and one micro-suspension PVC
131
grades were formulated with two commercially available castor oil based plasticizers
132
(CITROFOL® AHII and GRINDSTED® SOFT-N-SAFE) and a phosphonium-based
133
ionic liquid (trihexyl(tetradecyl)phosphonium bistriflamide, [P6,6,6,14][Tf2N]) which was
134
used as a co-plasticizer. The results were compared with those obtained when using the
135
conventional plasticizer di-isodecyl phthalate (DIDP). This study is a continuation of
136
our previous work19 which now also addresses the effect of the morphology of PVC
137
properties on PVC/plasticizer and/or PVC/(plasticizer+PhIL) interactions and
138
consequently on the properties of the plastisols and of the PVC films obtained from
139
those plastisols.
140 141
2. EXPERIMENTAL SECTION
142
2.1. Materials
143
Two emulsion PVC powders, with different K values (VICIR E 1970 P (K value = 70)
144
produced by Cires, S.A., Portugal and Vinnolit® P 75 SK (K value = 75) produced by
145
Vinnolit GmbH & Co) and one micro-suspension PVC powder (Vinnolit® P 70 HT
146
produced by Vinnolit GmbH & Co, K value = 70) were kindly provided by TMG
147
Automotive. In this work, the PVC samples obtained by emulsion polymerization were
148
identified as E70-PVC and E74-PVC (according to their K values of 70 and 74,
5 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 42
149
respectively) and the sample obtained by micro-suspension polymerization was
150
identified as MS-PVC (with K value of 70). Di-isodecyl phthalate (Jayflex® DIDP) was
151
supplied by ExxonMobil Chemical Europe, Belgium. Acetyltri-2-ethylhexyl citrate
152
(CITROFOL® AHII, hereafter abbreviated as ATEC) was supplied by Jungbunzlauer
153
Inc, Switzerland. Acetylated monoglycerides of fully hydrogenated castor oil
154
(GRINDSTED® SOFT-N-SAFE, hereafter abbreviated as COMGHA) was supplied by
155
Danisco
156
trihexyl(tetradecyl)phosphonium
157
(commercially available as Cyphos IL 109) was supplied by Cytec Industries, Canada,
158
with purity > 98 %. The chemical structures and some physicochemical properties of
159
the plasticizers used in this work are presented in Table 1. Other chemicals such as n-
160
heptane and n-hexane (purities > 99 %) were supplied by José M. Vaz Pereira SA,
161
Portugal while acetone (purity > 99 %) and Linseed Oil (purity > 98 %) were supplied
162
by Sigma-Aldrich, Portugal. All chemicals were used as received without further
163
purification.
S/A,
Denmark.
The
phosphonium
ionic
bis(trifluoromethylsulfonyl)imide,
liquid
(PhIL),
[P6,6,6,14][Tf2N]
164 165
2.2. Characterization of the PVC powder
166
The three different PVC powders studied in the present work were characterized for
167
their density, pore size distribution, particle size distribution, surface charge and
168
microstructure. The real density of the particles was measured by helium pycnometry
169
(Accupyc 1330 Micromeritics, Micromeritics Instrument, USA). The pore size
170
distribution, total pore area and bulk density of the powders were measured by mercury
171
porosimetry (Autopore IV Micromeritics, Micromeritics Instrument, USA) after
172
purging the samples for 5 minutes at 50 µm Hg to remove adsorbed water and other
173
impurities. The surface area and the pore volume of PVC powders were determined by
6 ACS Paragon Plus Environment
Page 7 of 42 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
174
nitrogen adsorption (Micromeritics, model ASAP 2000, 20Q-34001-01) using the
175
Brunauer-Emmett-Teller (BET) method and Barrett-Joyner-Halenda (BJH) method,
176
respectively. The particle size distribution of each powder was measured by Laser
177
Diffraction Spectroscopy (LDS) (Mastersizer 2000, Malvern Instruments, UK) and their
178
average surface charge (zeta potential) was measured by electrophoretic light scattering
179
(Zetasizer Nano ZS, Malvern Instruments, UK) with the solid particles dispersed at 1 %
180
(wt/wt) in milli-Q water. The microstructure of the PVC powders was analyzed by
181
Scanning Electron Microscopy (SEM) (Jeol JSM-5310, Japan) on gold-coated samples
182
with an operating voltage of 10 kV.
183 184
2.3. Preparation of plastisol samples and corresponding gelled films
185
Plastisols were prepared at room temperature by mechanical stirring (Janke & Kunkel
186
GmbH & Co, IKA-Werk, RW 24 basic, Germany) of all components (150 parts of total
187
plasticizer amount per 100 parts of polymer) at 500 rpm for 15 minutes. The total
188
plasticizer amount considers the use of plasticizers (DIDP, ATEC or COMGHA) alone
189
or their mixtures with PhIL (at 15 % (wt/wt)). Previous works reported that at this
190
composition PhIL is miscible and homogenously dispersed through the PVC matrix33,40.
191
The composition of the prepared plastisols is given in Table S1 as Supporting
192
Information. After stirring, the homogeneous mixture was vacuumed for 1 h at 1 mbar
193
to eliminate entrapped air and stored in a desiccator containing silica gel at room
194
temperature (~ 20 °C) during the entire aging period (up to 14 days) to avoid moisture
195
sorption. Each sample was coded as PVC grade/plasticizer type or as PVC
196
grade/plasticizer type/PhIL, depending if the plastisol was formulated without or with
197
[P6,6,6,14][Tf2N], respectively. PVC films with a thickness of 1 mm were obtained for
198
each formulation, at t = 0 and t = 14 days, by spreading the plastisol over a pre-heated
7 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 42
199
special support paper (release paper) and gelation in a ventilated oven at 210 ºC for 1
200
minute.
201 202
2.4. Characterization of the plastisol formulations
203
2.4.1. Rheological measurements
204
Rheological measurements were performed at constant temperature (~ 23 ºC) using a
205
controlled stress rheometer (Model RS1, Haake, Germany) with a cylindrical sensor
206
system Z34 DIN connected to a thermo controller recirculation bath (Haake Phoenix II,
207
Germany), working in controlled stress mode and at shear rates ranging between 0.5 and
208
30 s-1. Flow measurements were performed for different aging times (0, 1, 2, 7 and 14
209
days) using 50 mL of each plastisol and the results are presented as an average of at
210
least three measurements for each sample.
211 212
2.4.2. Particle size distribution measurements
213
The particle size distribution (PSD) of the PVC particles in the plastisols was measured
214
by Laser Diffraction spectroscopy (LDS) using a Mastersizer 2000 (Malvern
215
Instruments, UK) for the different aging times referred previously. Particle size
216
measurements were carried out without ultrasounds using plastisol samples dispersed in
217
n-heptane (at 1 % wt/v), following previously reported procedures.15 The results are
218
presented as an average of at least three measurements for each sample.
219 220
2.5. Characterization of the PVC films (obtained from the plastisol formulations)
221
2.5.1. Gelation degree
222
The acetone immersion test (AT) was performed on gelled films following the ASTM
223
D2152 standard.41 The gelled PVC samples (2 cm × 3 cm) were completely immersed
8 ACS Paragon Plus Environment
Page 9 of 42 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
224
in acetone for 45 minutes and examined for fractures/fragmentation, which occur in
225
case of inefficient gelation.
226 227
2.5.2. Thermal stability
228
The short-term thermal stability of the PVC films obtained immediately after preparing
229
the plastisol (t = 0 days) and after aging (t = 14 days) was analyzed using a
230
Thermogravimetric Analyzer (TA Instruments, Q500, USA). Experiments were carried
231
out between 25 ºC up to 600 ºC, at 10 ºC.min-1 under dry nitrogen atmosphere (at 100
232
mL.min-1). The long-term thermal stability of the films was measured by placing
233
rectangular samples (∼ 500 mg, 1 mm × 1 cm2) in an oven at 120 ºC and following their
234
weight loss until constant weight was observed.
235 236
2.5.3. Leaching of the plasticizers from the PVC films in different solvents
237
The amount of plasticizer(s) leached from the PVC films was measured gravimetrically
238
by immersing rectangular samples (∼ 250 mg, 1 mm × 1 cm2) in 3 ml of different
239
solvents: milli-Q water, n-hexane and linseed oil. Experiments were carried out at 25 ºC
240
without stirring. Samples were periodically weighed, after removing the excess of
241
solvent from the surface with a filter paper, and until constant weight was achieved. The
242
plasticizer(s) leached amount was calculated using the following equation:
243
Plasticizer leached amount (%) =
244
where W0 is the weight of the initial dried sample and W1 is the final weight of the dried
245
sample after leaching. Measurements were performed in triplicate for each sample.
W1 − W0 ×100 W0
(1)
246 247
2.5.4. Wetting properties of the PVC films
9 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 42
248
The wetting properties of the PVC films surfaces were evaluated by static water contact
249
angle measurements performed at room temperature (20-23 ºC) using the sessile-drop
250
(10 µL of milli-Q water) method (OCA 20, Dataphysics Instruments, Germany). The
251
results are presented as an average of three measurements that were performed on
252
different points on each sample. The water sorption capacity of the PVC films was
253
determined gravimetrically at room temperature (20-23 ºC) by monitoring the weight
254
changes of previously dried samples (1 mm × 1 cm2), at fixed time periods, after
255
immersion in milli-Q water. The water sorption capacity (WSC) of the films was
256
calculated using the following equation:
257
WSC (%) =
258
where Wd and Ws are the weights of the dried and water-swelled films (at time t),
259
respectively. These values were calculated neglecting the amount of plasticizer that is
260
leached from the films.
Ws − Wd ×100 Wd
(2)
261 262
3. RESULTS AND DISCUSSION
263
3.1. Characterization of the PVC powders
264
The properties measured to characterize the E-PVC and MS-PVC grades studied in this
265
work are summarized in Figures 1, 2 and S1 and in Table 2. The real density of the PVC
266
powders, measured by helium picnometry, is within the range known for PVC industrial
267
grades (0.97-1.45 g.cm-3)2. This property depends on the particle/grain size distribution
268
of the powders, on their compactation degree, on their morphology (shape, size and
269
porosity) and also on the chlorine content of the PVC backbone2 (since chlorine ions
270
hamper inter-chain attraction). The bulk density of the PVC powders, measured by
271
mercury porosimetry, follows an opposite trend to that observed for the real density, and
272
increases in the order E70-PVC < MS-PVC < E74-PVC. 10 ACS Paragon Plus Environment
Page 11 of 42 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
273
The results obtained by mercury porosimetry (Figure 1) and BET isotherm analyses
274
(Figure S1) show that, in general terms, all the powders present a multimodal profile
275
indicating the presence of intra-particle (0.001 to 0.1 µm), inter-particle (0.1 to 10 µm)
276
and inter/intra-grain (10 to 1000 µm) pores. This multimodal profile is more
277
pronounced for E-PVC samples when compared to MS-PVC (which presents an intense
278
peak around 1µm characteristic of inter-particle pores). These results are in agreement
279
with the SEM micrographs (inner images in Figure 1) showing that E-PVC powders
280
(E70-PVC and E74-PVC) present similar morphology and are essentially composed by
281
primary particles clustered into irregular shaped loose and larger grains and/or
282
agglomerates while the MS-PVC sample is composed by regular and non-agglomerated
283
primary particles. The higher inter-particle free volume of the E-PVC samples justifies
284
the higher BET surface area, total pore area and pore volume measured for these
285
samples, mainly for E70-PVC (13.2 m2.g-1, 38.8 m2.g-1 and 0.05 cm3.g-1, respectively)
286
as shown in Table 2. The particle size distribution of the PVC powders (Figure 2 and
287
Table 2) shows that their median diameter (d50) ranges between 2.9 and 20.3 µm,
288
following the sequence MS-PVC < E74-PVC < E70-PVC, whereas the MS-PVC
289
sample presents the highest d90/d10 ratio. Here again, the higher d50 and lower d90/d10
290
ratios measured for the E-PVC samples result from the fact that aggregates are being
291
measured instead of non-aggregated primary particles characteristic of the MS-PVC
292
sample.1,7,9,42
293
Finally, the results obtained from the zeta potential measurements showed that all the
294
PVC samples are stable, with low tendency to agglomerate, considering their negative
295
surface charge which is lower than -34 mV in all cases. The highest stability was
296
observed for the E70-PVC sample (zeta potential ~ -44 mV).
297 11 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 42
298
3.2. Characterization of the plastisols
299
The flow test results obtained for the plastisols prepared with the three different PVC
300
grades (E70-PVC, MS-PVC and E74-PVC) and plasticizers (DIDP, COMGHA and
301
ATEC) are presented in Figure 3, for as prepared and aged plastisols (stored during 14
302
days). The system E70-PVC/ATEC has been previously studied in our group19, but it
303
was repeated in the present work to evaluate the consistency of the experimental
304
procedure applied to prepare and to characterize the plastisols, which was confirmed
305
considering that reproducible values and trends were obtained in both independent
306
works. In general terms, E70-PVC plastisols, formulated using DIDP and ATEC as
307
plasticizers, present a pseudo-plastic behavior while a more Newtonian profile was
308
observed in all the other formulations. Experimental data show that higher initial shear
309
stresses were obtained for E70-PVC plastisols, independently of the plasticizer, being
310
the highest value observed when using the phthalate-based plasticizer (DIDP) (∼ 45 Pa).
311
This higher initial yield stress indicates the presence of strong intermolecular PVC-
312
DIDP interactions15,43. As previously discussed in literature2-14, phthalate-based
313
plasticizers are highly compatible with PVC, which justifies its intensive use as an
314
efficient PVC plasticizer. The system E70-PVC/DIDP also presents the most
315
pronounced aging with maximum shear stresses increasing from 46 to 93 Pa, for as
316
prepared and aged plastisols, respectively. This system is also the only that presents a
317
thixotropic behavior, after aging and for the range of shear stresses applied, with
318
prominent hysteresis. This behavior was also previously observed for E70-PVC
319
additivated with diisononyl phthalate (DINP)19. However, this formulation presented
320
lower shear stresses, mainly for as prepared plastisols, indicating that an increase in the
321
plasticizer alkyl chain seems to promote PVC-plasticizer interactions. All the other
12 ACS Paragon Plus Environment
Page 13 of 42 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
322
studied systems are characterized by maximum shear stresses lower than ∼ 40 Pa, with
323
low or no aging effect.
324
An efficient plasticizer should be able to readily establish strong interactions with the
325
polymer. However, several parameters can compromise plasticizer/polymer miscibility
326
(e.g. length/ramification of plasticizer alkyl chains, presence of polar groups, plasticizer
327
molecular weight, etc). This plasticizer/polymer miscibility, which is an indirect
328
measure of the strength of the plasticizer/polymer intermolecular interactions, can be
329
inferred (with reservations19) by comparing the solubility parameters of both
330
components. According to the Gibbs free energy theory enhanced plasticizer solvency
331
towards a given polymer results in negative ∆G values as calculated from equation 1:
332
∆G =∆H-T∆S
(3)
333
where ∆H is the enthalpy of mixing (J.mol-1), ∆S is the entropy of mixing (J.mol-1.K-1)
334
and T is the absolute temperature (K). By considering that the entropy of solution of an
335
essentially amorphous polymer like PVC is positive, it can be assumed that the sign of
336
∆G in Eq. 1 depends on ∆H which can be calculated from the Hildebrand equation: ∆H= φ sφ p (δ s − δ p )
2
337
(4)
338
where φ s , φ p are the volume fraction of the solvent and polymer, respectively, and δ s ,
339
δ p are their respective solubility parameters. As can be seen in Table S1, the enthalpies
340
of mixing calculated for plastisols formulated with ATEC (2.9-3.9 J.mol-1) and
341
COMGHA (3.1-4.5 J.mol-1) are almost twice those calculated for DIDP (1.4-2.0 J.mol-
342
1
343
The miscibility of different phthalate- and natural-based plasticizers towards PVC was
344
recently estimated following the Hansen solubility parameter theory and using the
345
interaction radius concept.44 It was reported that the presence of hydroxyl groups in the
346
plasticizer structure increases the plasticizer/polymer interaction radius, leading to poor
), which in turn are similar to those previously calculated for PVC-DINP systems.19
13 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 42
347
miscibility between the components, due to the high contribution of the hydrogen
348
bonding term. Therefore, the higher enthalpies of mixing calculated for the natural-
349
based plasticizers studied in this work may result from the higher amount of hydroxyl
350
groups present in their structure and when comparing with DIDP. Furthermore, these
351
results are in agreement with the rheological data measured for ATEC and COMGHA-
352
based plastisols, which presented lower shear stress values (between ∼ 8 and 45 Pa for
353
ATEC and between ∼ 16 and 39 Pa for COMGHA) as well as less pronounced pseudo-
354
plastic behavior and aging effect. All together, these results may indicate lower
355
miscibility of the natural-based plasticizers studied in this work towards PVC. This can
356
be due to the higher molecular weight and molecular volume of ATEC and COMGHA
357
when compared to DIDP (Table 1), since both properties may affect the diffusion of
358
these plasticizers through the PVC network. The incorporation of [P6,6,6,14][Tf2N] in
359
plastisol formulations decreases the enthalpies of mixing (by 24 % when mixed with
360
natural-based plasticizers – Table S1) indicating that it may favor PVC/plasticizer
361
interactions.
362
As can be seen in Figure 4, plastisols formulated with E70-PVC also present higher
363
limit viscosities than those formulated with MS-PVC and E74-PVC (more than 3×
364
higher). The effect of aging over the E70-PVC plastisols is also clearly observed in
365
Figure 4a, more pronouncedly when DIDP is used as plasticizer. The observed increase
366
in the viscosity of these plastisols over time results from the chemical interactions that
367
are established between the plasticizer and the E70-PVC particles. Moreover and as
368
previously discussed, E70-PVC particles are organized as looser and less compact
369
aggregates with higher free volume in-between the primary particles and consequently
370
higher inter-particle porosity, which enhance the solvation and the swelling of the PVC
371
particles by the plasticizer. This correlation between the morphological properties of the
14 ACS Paragon Plus Environment
Page 15 of 42 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
372
PVC grades (expressed in terms of particle surface area) and the relative viscosity of the
373
plastisols (normalized taking into account the intrinsic viscosity of pure plasticizers) is
374
represented in Figure 5.
375
The particle size distribution (PSD) of the plastisols shown in Figure 6 (numerical data
376
summarized in Table S2), show that the systems E70-PVC/DIDP also present the
377
highest variation in the (d90-d10)/d50 ratio during aging, in agreement with rheological
378
data. According to Figure 6, it is also evident that changes in d50 values are more
379
significant when comparing as prepared and 2 days aged plastisols and that the PSD
380
profiles of the plastisols are almost constant indicating complete solvation/swelling of
381
the PVC particles by the plasticizer(s) after 2 days of storage. The higher dispersion
382
observed for (d90-d10)/d50) values results from the different mechanisms involved in the
383
PVC particle swelling process and which include de-agglomeration of larger aggregates,
384
swelling and diffusion of the plasticizer diffusion through the polymeric matrix. When
385
comparing the PSD results of the neat E-PVC powders (Table 2) with the corresponding
386
as prepared plastisols (Table S2), a general decrease in d50 values was observed. These
387
results indicate that the studied plasticizers are able to efficiently solvate, and
388
consequently disaggregate the agglomerated E-PVC primary particles. The PSD results
389
of MS-PVC based plastisols present the less pronounced aging effect, with almost
390
constant (d90-d10)/d50 and d90/d10 ratios and with d50 values that range between 3.7 and
391
13.8 µm (Figure 6, Table S2). Moreover, d50 values of neat MS-PVC and corresponding
392
as prepared plastisols are similar. These results are justified by the morphology of the
393
micro-suspension PVC sample, composed by less friable and non-agglomerated primary
394
particles as previously discussed, which are less sensitive to the plasticizer solvating
395
effects.
15 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 42
396
The effect of the partial replacement of each plasticizer by the PhIL ([P6,6,6,14][Tf2N]) is
397
shown in Figures 3-6. In general terms, and for both E-PVC and MS-PVC grades, it can
398
be concluded that the incorporation of [P6,6,6,14][Tf2N] induced the formation of
399
Newtonian and less viscous plastisols, mainly for E70-PVC/DIDP and E70-PVC/ATEC
400
systems which can be advantageous for industrial PVC plastisols processing. Moreover,
401
plastisols formulated with [P6,6,6,14][Tf2N] also present less accentuated aging, as
402
confirmed by the low variation in (d90-d10)/d50 and d50 values during the storage period
403
(Table S2 and Figure 6). Similar trends were previously reported for related E70-
404
PVC/DINP/[P6,6,6,14][Tf2N] and E70-PVC/ATEC/[P6,6,6,14][Tf2N] systems.19
405 406
3.3. Gelation and thermal stability of PVC films obtained from different plastisols
407
The efficiency of each plasticizer (or plasticizer + PhIL mixtures) to solvate and swell
408
the PVC particles was indirectly accessed by the acetone immersion method. Although
409
this is a simple method, it is still currently used in the industry as a control procedure
410
for plasticization efficiency. According to this method, the efficient gelation of PVC
411
plastisols leads to the formation of tougher films that maintain their structure and that
412
do not dissolve when in contact with acetone. As can be seen in Table 3, most of the
413
plastisols were efficiently gelled, except those formulated with MS-PVC and E74-PVC,
414
both using ATEC as plasticizer, with and without PhIL obtained from as prepared or
415
aged plastisols, which were fragile and easily fractured. As prepared plastisols
416
formulated with E70-PVC/COMGHA and MS-PVC/DIDP also originated fragile films
417
however the corresponding aged plastisols (after 14 days) originated tough gelled films.
418
Similar behavior was observed for the plastisols formulated with the (plasticizer +
419
PhIL) mixtures indicating that the incorporation of the PhIL does not affect the gelation
420
of the PVC plastisols. Among the PVC grades studied in this work, E70-PVC is the
16 ACS Paragon Plus Environment
Page 17 of 42 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
421
only one that presents good gelation for all plasticizers, and/or plasticizer/PhIL
422
mixtures, even if after 14 days of storage in some cases. The same behavior was
423
previously observed for the same E70-PVC grade formulated with different PhILs
424
and/or plasticizers19, indicating that this PVC grade is highly compatible with different
425
plasticizers.
426
The short- and long-term thermal stability analysis of the PVC/plasticizer(s) systems
427
that presented good gelation is summarized in Table 3 and Figure S2. Experimental data
428
reported in Table 3 was also graphically represented in Figure S3 to facilitate
429
comparison among the different samples. The thermal stability parameters of the neat
430
PVC grades and pure additives (plasticizers and [P6,6,6,14][Tf2N]) were also measured
431
and are presented in Table 4. The results obtained for the pure compounds show that the
432
thermal stability increases according to the following sequences for the PVC grades:
433
MS-PVC < E70-PVC < E74-PVC and for the plasticizers: ATEC