Enabling High-Areal-Capacity Lithium–Sulfur ... - ACS Publications

May 9, 2017 - Chaoji Chen, Wei Luo, Tingting Gao, Shaomao Xu, Jiaqi Dai, Glenn Pastel,. Yanbin Wang, Boyang Liu, Jianwei Song, Yanan Chen, Chunpeng ...
0 downloads 0 Views 1MB Size
Subscriber access provided by UB + Fachbibliothek Chemie | (FU-Bibliothekssystem)

Article

Enabling High-Areal-Capacity Lithium-Sulfur Batteries: Designing Anisotropic and Low-Tortuosity Porous Architectures Yiju Li, Kun Fu, Chaoji Chen, Wei Luo, Tingting Gao, Shaomao Xu, Jiaqi Dai, Glenn Pastel, Yanbin Wang, Boyang Liu, Jianwei Song, Yanan Chen, Chunpeng Yang, and Liangbing Hu ACS Nano, Just Accepted Manuscript • Publication Date (Web): 09 May 2017 Downloaded from http://pubs.acs.org on May 9, 2017

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

ACS Nano is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

Enabling High-Areal-Capacity Lithium-Sulfur Batteries: Designing Anisotropic and Low-Tortuosity Porous Architectures Yiju Li1, a, Kun Fu1, a, Chaoji Chen1, Wei Luo1, Tingting Gao1, Shaomao Xu1, Jiaqi Dai1, Glenn Pastel1, Yanbin Wang1, Boyang Liu1, Jianwei Song1, Yanan Chen1, Chunpeng Yang1, Liangbing Hu1,* 1

Department of Materials Science and Engineering, University of Maryland College Park,

College Park, Maryland, 20742, USA

*

Email: [email protected]

a

These authors contributed equally to this work. TOC Figure:

Inspired by wood, the three-dimensionally (3D) aligned porous carbon matrix filled with interconnected reduced graphene oxide (RGO) nanosheets can accommodate high sulfur mass loadings (21.3 mg cm-2) and effectively suppress polysulfide migration. The assembled lithium-sulfur (Li-S) battery combined with a polyethylene oxide (PEO) gel composite electrolyte can deliver a high areal capacity of 15.2 mAh cm-2.

Keywords: Li-S Battery, Low Tortuosity, Carbon Matrix, Polymer Electrolyte, High Areal Capacity 1 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Abstract Lithium-sulfur (Li-S) batteries have attracted much attention due to their high theoretical energy density in comparison to conventional state-of-the-art lithium-ion batteries. However, low sulfur mass loading in the cathode results in low areal capacity and impedes the practical use of Li-S cells. Inspired by wood, a cathode architecture with natural, three-dimensionally (3D) aligned microchannels filled with reduced graphene oxide (RGO) was developed as an ideal structure for high sulfur mass loading. Compared with other carbon materials, the 3D porous carbon matrix has several advantages including low tortuosity, high electrical conductivity, and good structural stability, which make it an excellent 3D light-weight current collector. The Li-S battery assembled with the wood-based sulfur electrode can deliver a high areal capacity of 15.2 mAh cm-2 with a sulfur mass loading of 21.3 mg cm-2. This work provides a facile but effective strategy to develop 3D porous electrodes for Li-S batteries, which can also be applied to other cathode materials to achieve a high areal capacity with uncompromised rate and cycling performance.

2 ACS Paragon Plus Environment

Page 2 of 28

Page 3 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

Introduction Rechargeable Li-ion batteries (LIBs) have achieved great success in consumer electronics, electric vehicles, and stationary energy storage systems.1-5 Unfortunately, the limited improvement in well-developed LIBs can hardly sustain the increasing need for high energy density

electrochemical

cells.

To

enhance

the

energy

density

limitation

of

intercalation-compound-based LIBs, the Li-S batteries that undergo conversion reactions are becoming a potential alternative for the next-generation energy storage systems. Sulfur holds a high capacity (1672 mAh g-1) as a cathode material and in conjunction with a Li metal anode, Li-S batteries can deliver a much higher energy density (2600 Wh kg-1) to outperform most contemporary energy storage devices.6-10 However, although numerous nanostructured sulfur-based composite electrodes exhibited superior electrochemical performance,11-13 the mass loading of sulfur material needs to further increase in order to achieve a higher areal energy density and meet the practical application in large-scale.14-16 Commonly, the conventional cathode in Li-S batteries is prepared through mechanically mixing elemental sulfur, binder, and conductive carbon together and using doctor-blading method. The slurry-based electrode structure usually has poor contact between the nonconductive sulfur and the conductive materials (e.g., carbon black).10 Especially, for high-mass-loading electrodes, active materials could be delaminated from current collectors and the high tortuosity of electrodes may hinder the ion transport and extend ion diffusion pathway, leading to the limited active material utilization. Moreover, the binder may block the electrons transfer and bring in some “dead” sites which can’t occur electrochemical reactions.9 Consequently, it is imperative to engineer rational electrode 3 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

structures for accommodating high sulfur mass loading to obtain high areal energy density without sacrificing the electrochemical performance.17-22 Inspired by wood, a cathode architecture with natural, 3D aligned microchannels provides an ideal structure for high sulfur mass loading. Here, we developed a 3D aligned porous carbon matrix using carbonized wood with RGO filled inside the microchannels (C-wood) for high sulfur mass loading (S@C-wood). RGO serves as an electronically conductive network to enhance the electron transport, and the oxygen functional groups on RGO nanosheets can chemically bond with the intermediate products of sulfur to locally trap them and prevent their migration to the anode.23 The C-wood matrix has an anisotropic structure and excellent anti-deformation along the aligned microchannel direction for stable and safe sulfur accommodation. The low-tortuosity and open microchannels can also allow better electrolyte permeation through the composite electrode. In addition, a design of PEO gel composite electrolyte was used to build full cells with the S@C-wood cathode and Li metal anode. With this design, the battery showed great electrochemical performance for such 3D porous electrodes. The electrode with a sulfur mass loading of 7.8 mg cm-2 showed a high areal capacity of 6.7 mAh cm-2 at a current density of 1.56 mA cm-2 and excellent cycling stability (90% retention after 50 cycles). When the sulfur mass loading is increased to 21.3 mg cm-2, the electrode can reach an even higher areal capacity of up to 15.2 mAh cm-2.

Results and Discussion The S@C-wood composite electrode was prepared by several facile steps (Figure 1). Natural wood consisting of lignin, hemicellulose and cellulose was sectioned perpendicular to the 4 ACS Paragon Plus Environment

Page 4 of 28

Page 5 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

growth direction. After carbonization and activation, the shape of the porous wood slice was reserved. RGO was filled into the microchannels of the wood carbon matrix by vacuum filtration and reduction. The resultant 3D conductive wood carbon framework with low-tortuosity and open porous microchannels enhances electrolyte permeation. The aligned porous microchannels stuffed with continuous RGO networks can accommodate high sulfur mass loading without blocking pathways for ion transport. The facile and low-cost procedure to manufacture the carbon matrix is appealing for many other fields of energy storage and conversion, such as flow batteries and hydrogen evolution reactions, due to the porous structure with low tortuosity and anisotropy.

Figure 1. Schematic illustration of the preparation process and structure of the S@C-wood composite electrode. Anisotropic natural wood is rich in aligned microchannels along the growth direction. After carbonization and activation, the long and low-tortuosity porous microchannels were perfectly retained. The 3D aligned porous carbon matrix filled with interconnected RGO networks is an ideal host for high sulfur mass loading.

5 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The morphology of the as-prepared samples is characterized using scanning electron microscopy (SEM). The top surface SEM images revealed the highly porous features of the carbonized and activated wood (Figure S1a). The 3D anisotropic and well-aligned porous structure was perfectly retained even after carbonization and activation (porosity: ~70%) (Figure 2a-c) with a typical thickness of about 800 µm (Figure S1b). Figure 2d shows the well-defined, aligned and elongated microchannels along the growth direction, which originate from the cellulose fibers in the original wood. After high-temperature carbonization, the excellent electronic conductivity of the C-wood framework along the microchannel direction makes it an ideal 3D current collector. Figure 2e displays numerous nanopores that are homogenously distributed on the wall of the microchannels in the bare wood carbon matrix. The uniform nanopores result from carbon dioxide (CO2) etching effects under high temperatures. Transmission electron microscopy (TEM) images reveal that the wall of microchannels have abundant mesopores and micropores (Figure S2). Nitrogen (N2) adsorption–desorption tests were further conducted to investigated the porosities of the bare wood carbon and C-wood (Figure S3). The specific surface areas of the bare wood carbon and C-wood are 712 and 731 m2 g-1, respectively. The high specific surface areas indicate the highly porous properties of the bare wood carbon and C-wood. In the hierarchically porous carbon materials, micropores can immobilize and trap the dissolved polysulfides and the mesopores can enhance the sulfur encapsulation and improve the electrolyte penetration.10, 24 After vacuum filtration, the RGO nanosheets were absorbed into the microchannels (Figure 2f). The SEM image of the cross-section distinctly exhibits that the parallel channels were stuffed with continuous RGO networks (Figure 2g). The interconnected RGO nanosheets 6 ACS Paragon Plus Environment

Page 6 of 28

Page 7 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

with appropriate cavities can both facilitate electron transport and electrolyte immersion (Figure 2h). Figure S4 highlights the joint where the RGO nanosheets tightly bond with the wall of microchannels, which enables fast electron transport between the RGO networks and the bare monolithic carbon matrix.

Figure 2. Morphological characterization of the C-wood matrix. (a) Photograph of a natural wood block. (b) Photograph of a carbonized and activated natural wood slice which is cut perpendicular to the growth direction. (c) SEM image of the top surface and cross-section of the bare wood carbon matrix without RGO. (d, e) Enlarged SEM images of the microchannels, demonstrating numerous nanopores on the wall. (f, g) SEM images of the top surface and cross-section of the C-wood composite. (h) Enlarged SEM image of the interconnected RGO networks.

7 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The C-wood composite carbon matrix has a high porosity and a low tortuosity, which contribute to the infiltration of sulfur into the open microchannels. Figure 3a shows a schematic illustration to demonstrate how sulfur infiltrates into the microchannels of the C-wood matrix during the heating treatment. Sulfur powders were evenly distributed on the surface of the C-wood composite, which was completely absorbed into the carbon matrix after melting at 155oC (Figure 3b and c). The obtained areal sulfur mass loading is as high as 7.8 mg cm-2. After infilrating with sulfur, the RGO networks inside the porous microchannels retain the original interconnected morphology and tightly bond with the 3D bare wood carbon skeleton (Figure 3d). Moreover, sulfur is conformally accommodated on the surface of the RGO nanosheets without any agglomeration (Figure 3e).

The elemental mappings by energy dispersive spectroscopy (EDS) show that sulfur is well dispersed in the RGO networks (Figure 3f). TEM elemental mappings further confirm the homogeneous sulfur distribution on a single RGO nanosheet with no bulky agglomerates (Figure S5). The oxygenic functional groups on GO nanosheets can immobilize sulfur species and maintain intimate touch of the conductive substrate with sulfur.23 The elemental mapping of oxygen suggests plenty of oxygenic functional groups distributed on the RGO nanosheets (Figure 3g), which can effectively confine polysulfides from dissolving throughout the electrode. Figure S6a and b reveal the morphologies and elemental mappings of S@C-wood composite electrodes with higher sulfur loadings of 15.2 and 21.3 mg cm-2, respectively. We can see that sulfur is also uniformly accommodated in the interconnected RGO networks. Even at a high sulfur mass loading of 21.3 mg cm-2, there still exists void space in the aligned 8 ACS Paragon Plus Environment

Page 8 of 28

Page 9 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

microchannels, which benefits the electrolyte penetration and tolerates sulfur volume expansion during the electrochemical reaction. For the bare wood carbon without being filled with RGO networks, the sulfur is merely dispersed on the surface inside the aligned microchannels (S@bare wood carbon) (Figure S7).

The crystal structure of as-prepared bare wood carbon, C-wood, pure sulfur and S@C-wood was revealed by X-ray diffraction (XRD) (Figure 3h). For bare wood carbon and C-wood, two broad diffraction peaks occur at ~25o and ~44o, which are assigned to the typical (002) and (100) plane reflection of carbon materials, respectively.25, 26 Except for the diffraction peak located at ~25o, the sharp and strong diffraction peaks observed in S@C-wood composite manifest the orthorhombic structure of sulfur (JCPDS card No. 08-0247).27 Raman spectroscopy was conducted to further study the structural characteristics of the samples (Figure 3i). The peaks at ~1350 and ~1580 cm−1 correspond to the D and G band, respectively. The intensity ratio of ID/IG represents the degree of disorder of the carbon materials.28 The relatively low ID/IG ratio indicates the amorphous nature of the bare wood carbon matrix surface, which is caused by CO2 activation. The resultant hierarchically nanoporous walls along the microchannels contribute to trapping polysulfides and alleviating “shuttle effects” to some extent. After sulfur infiltration into the C-wood composite carbon matrix, the characteristic peak intensity of sulfur becomes weak, indicating good accommodation and confinement of sulfur in the 3D porous C-wood matrix.29

9 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 3. Characterizations of the S@C-wood composite electrode. (a) Schematic illustration of sulfur infiltration into the microchannels of the C-wood composite in an argon atmosphere. (b, c) Photographs showing molten sulfur adsorbed into the C-wood composite at 155oC. (d, e) SEM images of the S@C-wood composite. (f, g) Elemental mappings of sulfur and oxygen in the S@C-wood composite. (h) XRD patterns of the bare wood carbon, C-wood, pure S and S@C-wood composite. (i) Raman spectra of the pure S, bare wood carbon, C-wood and S@C-wood composite.

10 ACS Paragon Plus Environment

Page 10 of 28

Page 11 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

To evaluate the electrochemical performance of the as-prepared electrodes, a Li-S cell was assembled using S@C-wood electrode as the cathode, lithium foil as the anode, and PEO gel composite membrane both as the gel electrolyte and separator (Figure 4a). The brief preparation process of the PEO gel composite membrane is illustrated in Figure S8. The PEO gel composite was uniformly covered on a piece of Celgard 2400 to form a free-standing membrane. The PEO gel composite membrane serves as a barrier which can effectively hinder the polysulfides from releasing from the porous C-wood composite carbon matrix and alleviate the attack of polysulfides at the anode.30 By contrast, a S@bare wood carbon electrode is also used as a cathode in the assembled Li-S cell.

Typical sulfur mass loading of the S@C-wood and S@bare wood carbon electrodes is about 7.8 mg cm-2, which is much higher than most slurry-based cathodes in normal Li-S batteries. Figure 4b shows the cyclic voltammograms (CVs) of the S@C-wood composite electrode at the first, second and fifth cycle at a scan rate of 0.02 mV s-1 within a voltage window of 1.0-3.5 V. Two typical cathodic peaks at 2.3 and 1.9 V correspond to the reduction of elemental sulfur (S8) to long-chain soluble lithium polysulfides (Li2Sx) (4 < x < 8) and the formation of insoluble short-chain Li2S2/Li2S, respectively. The anodic peak at 2.4-2.5 V is assigned to the lithium polysulfides/sulfides converting into elemental sulfur.31 In the initial two cycles, the area of the CVs of the S@C-wood composite electrode slightly increases, indicating an activation process, which is attributed to the re-accommodation of active material to electrochemically active sites during the first cycle.32

11 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The galvanostatic charge–discharge (GCD) curves of S@C-wood composite electrode at various cycles are shown in Figure 4c. Two discharge plateaus and one charge plateau agree well with the redox peaks in the CVs.33 After several cycles, the potential difference between the charge and discharge plateaus decreases, thereby manifesting the improved electrochemical reversibility. Figure 4d exhibits the GCD curves of the S@C-wood composite electrode at various current densities from 0.156 to 7.8 mA cm-2. No apparent overcharge occurred during the charge state, which suggests that the shuttle effect of sulfur polysulfides was effectively prevented. The reversible discharge capacity can reach up to 1274 mAh g-1, corresponding to 9.9 mAh cm-2 at 0.156 mA cm-2. With an increase in current density, the specific capacity gradually decreases to 1138 mAh g-1 (8.8 mAh cm-2), 992 (7.7), 857 (6.7), 726 (5.7) and 509 (4.0), respectively (Figure 4e). Once the current density goes back to 0.156 mA cm-2, the specific capacity recovers to 1158 mAh g-1 (9.0 mAh cm-2). These results demonstrate the outstanding rate performance of the S@C-wood composite electrode.

12 ACS Paragon Plus Environment

Page 12 of 28

Page 13 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

Figure 4. Electrochemical performance of the S@C-wood composite electrodes. (a) Schematic illustration of the Li–S cell with the PEO gel composite electrolyte (with a representative sulfur mass loading of 7.8 mg cm-2). (b, c) CVs and GCD curves of the S@C-wood composite electrode at different cycles. (d, e) Galvanostatic charge–discharge curves and rate performance of the S@C-wood composite electrode at various current densities.

Excellent electrolyte absorption by electrode materials, especially for high sulfur mass loading electrodes, is beneficial for retaining soluble polysulfides within the electrode 13 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

matrices and ensuring stable electrochemical reactions.34-36 We conducted loading tests to demonstrate the superior anti-deformation and impressive electrolyte accommodation ability of our 3D porous C-wood matrix. RGO sponge (length × width × thickness: 2.0 × 2.2 × 1.2 cm) and C-wood samples (length × width × thickness: 2.4 × 1.8 × 1.2 cm) were both fully soaked with electrolyte. As shown in Figure 5a, the structure of the C-wood matrix is nondeformable and the electrolyte is well contained inside the porous carbon host under the pressure of 22.7 kPa. By contrast, the RGO sponge itself is greatly compressed and the electrolyte overflows from the RGO sponge. The excellent anti-deformation along with the direction of the microchannels and favorable electrolyte confinement make the S@C-wood composite electrode promising for applications in the field of planar batteries. Here, we demonstrated a large piece of free-standing S@C-wood composite electrode, which is used for assembling a planar battery (Figure 5b, c). The GCD curves of the S@C-wood composite electrode with different sulfur mass loadings at 1.56 mA cm-2 are displayed in Figure 5d. Two well-defined discharge and one charge plateaus agree with the CV curves in Figure 4b. The S@C-wood composite electrodes with sulfur mass loadings of 7.8, 15.2 and 21.3 mg cm-2 can deliver high specific areal capacity of 6.7, 12.6 and 15.2 mAh cm-2, respectively.

We further explored the cycling performance of the S@C-wood composite electrodes with various sulfur mass loadings at a current density of 1.56 mA cm-2 (Figure 5e and Figure S9). The S@C-wood composite electrode with a sulfur mass loading of 7.8 mg cm-2 exhibits superior capacity retention of 90.0% after 50 cycles. As a comparison, the S@bare wood carbon electrode without being filled with RGO networks exhibits relatively poor cycling 14 ACS Paragon Plus Environment

Page 14 of 28

Page 15 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

stability (only 54.1% after 50 cycles) (Figure S10). It indicates that the interconnected long-range RGO networks serve as important reservoirs to accommodate high sulfur mass loading, except for the porous walls on the parallel microchannels. The RGO networks filled in the elongated microchannels contribute to firmly immobilizing the electrolyte inside the C-wood composite carbon matrix, which can effectively impede the migration of polysulfides to the anode and alleviate shuttling effects.37 For the high sulfur mass loading of 21.3 mg cm-2, the specific areal capacitance can still reach up to 11.2 mAh cm-2 after 50 cycles. These results further suggest that the structure of the 3D porous C-wood composite matrix can effectively prevent electrolyte leakage and confine the soluble polysulfides, ensuring stable cycling performance. We compared the areal capacity of our S@C-wood composite electrode with other recently reported sulfur electrodes.17, 38-43 Our S@C-wood composite electrode with a high sulfur mass loading of 21.3 mg cm-2 possesses an areal capacity of 15.2 mAh cm-2, which is among the highest compared with other reported Li-S batteries (Figure 5f). Note that the sulfur mass loading can still be increased in the 3D C-wood matrix, we will further improve the areal energy density by optimizing the electrode structure in the future.

15 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 5. Absorption ability and anti-deformation demonstration and electrochemical performance of S@C-wood composite electrodes with high sulfur mass loadings. (a) Photographs showing the press test of the S@RGO sponge (length × width × thickness: 2.0 × 2.2 × 1.2 cm) and S@C-wood composite (length × width × thickness: 2.4 × 1.8 × 1.2 cm) soaked with electrolyte. (b) Photographs of a large piece of S@C-wood composite (length × width × thickness: 2.0 × 1.8 × 0.1 cm). (c) Lighting up a light-emitting diode (LED) using the assembled planar cell. The use of the logo is from University of Maryland, College Park. (d) GCD curves of the S@C-wood composite electrode with different sulfur mass loadings. (e) Cycling performance of the S@C-wood composite electrode with different sulfur mass 16 ACS Paragon Plus Environment

Page 16 of 28

Page 17 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

loadings. The achieved areal capacities of our S@C-wood composite electrodes are much higher than those of normal Li-S cathodes. (f) Comparison of our areal capacity with other reported results.

17 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Conclusion Inspired by wood, we developed a 3D aligned porous carbon matrix using carbonized wood with RGO filled inside the lumens and voids. The porous matrix with low tortuosity, high electric conductivity, and good structural stability is an ideal 3D current collector for a high sulfur mass loading. The elongated and open microchannels can allow better electrolyte permeation through the composite electrode. The C-wood matrix also demonstrates excellent anti-deformation along the direction of the microchannels and favorable electrolyte confinement capacity, which contributes to immobilizing the electrolyte and impeding the migration of polysulfides. The assembled Li-S battery combined with PEO gel composite electrolyte can deliver a high areal capacity of 15.2 mAh cm-2 with a sulfur mass loading of 21.3 mg cm-2. This work presents a simple but effective wood-inspired strategy to develop composite electrodes for Li-S batteries, which can also be applied in many other energy storage and conversion applications.

18 ACS Paragon Plus Environment

Page 18 of 28

Page 19 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

Experimental Section Preparation of wood carbon In brief, a piece of natural basswood slice was cut perpendicular to the growth direction. The wood slice was pre-carbonized under 260oC for 6 h and subsequently carbonized under 1000oC for 6 h in an argon atmosphere.44 Next, the sample was activated in a CO2 atmosphere under 800oC to get the final bare wood carbon. Before activation, the bare wood carbon is about 27.0 mg cm-2 with a thickness of 800 µm (length × width × thickness: 1.0 × 1.0 × 0.08 cm). After activation using CO2, the weight of the bare wood carbon is about 18.3 mg cm-2. The percent of weight loss is ~32.2%, which indicates the bare wood carbon is highly activated. Preparation of wood carbon/RGO composite The graphene oxide (GO) was first synthesized using improved Hummers’ method.25 160 mg prepared GO powder was dispersed into 10 mL deionized water and the mixture was then probe-sonicated for 1 h to get the GO solution. The as-prepared bare wood carbon (length × width × thickness: 1.0 × 1.0 × 0.08 cm) was placed on a filter funnel and the obtained homogeneous GO solution was added onto the surface of bare wood carbon slice. The GO solution was absorbed into the bare wood carbon matrix along with the microchannels after vacuum filtration using turbo pump. The bare wood carbon filled with GO solution was then treated by freeze drying for 48 h. After freeze drying, the wood carbon/GO composite was transferred into a furnace tube and heated at 600oC for 1 h to obtain the wood carbon/RGO composite, which is denoted as C-wood. The mass densities of the RGO and bare wood carbon are about 1.6 and 18.3 mg cm-2, respectively. 19 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Preparation of S@C-wood composite electrode The S@C-wood composite electrode was synthesized using a “melt and diffusion” method. Typically, a layer of sulfur powder (Sigma-Aldrich) was uniformly covered on the top surface of C-wood composite and then sealed in a Teflon-lined stainless steel reaction vessel at 155oC for 12 h under an argon atmosphere. After the heating treatment, the free-standing S@C-wood composite electrode was obtained. The bare wood carbon without being filled with RGO and directly composited with sulfur is denoted as S@bare wood carbon. Preparation of polyethylene oxide gel composite electrolyte Niobium (Nb) and calcium (Ca) co-doped Li7La3Zr2O12 powders, as the ceramic fillers, were first prepared using the conventional solid-state-reaction method as reported by our previous work.45 Then, 400 mg ceramic fillers, 250 mg lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 400 mg PEO (molecular weight: ~600 K) were dispersed into 10 mL acetonitrile (ACN). The mixture was violently stirred under 60oC to obtain homogeneous solution. The above solution was uniformly covered onto the surface of Celgard 2400 and dried in vacuum oven at room temperature. The obtained PEO gel composite membrane was then dipped in 1,3-dioxolane and 1,2-dimethoxyethane (DOL: DME=1:1 in volume) electrolyte with 1 M LiTFSI for full absorption. Materials characterization Morphologies of the samples were observed by a Hitachi SU-70 field emission scanning electron microscope (FESEM) equipped with an energy-dispersive X-ray (EDX) analyzer and JEOL 2100 LaB6 TEM. The material crystalline phase was investigated by an X-ray diffractometer (XRD, Rigaku TTR III) with Cu Kα radiation (λ=0.15142 nm). Nitrogen 20 ACS Paragon Plus Environment

Page 20 of 28

Page 21 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

adsorption–desorption tests were conducted using Micromeritics ASAP 2020 physisorption analyzer at 77 K. The specific surface area was calculated according to the Brunauer–Emmett–Teller (BET) method using the adsorption branch of nitrogen isotherm. The chemical bond information of as-prepared samples was revealed by a Raman spectrometer with a He-Ne laser wavelength of 633 nm (Jobin-Yvon HR800). Electrochemical measurements The free-standing S@C-wood composite was directly used as the working electrode. The C-wood matrix with a thickness of 800 µm has an areal density of 19.9 mg cm-2, which can serve as an ideal light-weight 3D current collector. The areal mass loading of sulfur (7.8, 15.2 and 21.3 mg cm-2) was simply controlled by the original addition before melting. For the high sulfur mass loading (21.3 mg cm-2), the sulfur content exceeds 50wt% of the whole electrode (51.7wt%), even though taking the 3D current collector of the bare wood carbon into account. The electrolyte volume is only 7.5 µL per 1 mg of sulfur. The lithium–sulfur batteries combining a liquid electrolyte and a gel composite electrolyte were assembled in 2032 coin cells. The liquid electrolyte was 1 M LiTFSI/DOL + DME (1:1 by volume). The PEO gel composite covered Celgard 2400 both as a separator and gel composite electrolyte. The cyclic voltammetry was performed using a computer-controlled Bio-Logic potentiostat (VMP3/Z). The galvanostatic charge/discharge measurements were conducted in a voltage range of 1-3.5 V on a LAND battery tester. The specific capacity mentioned in this work was calculated based on the mass of sulfur.

21 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Acknowledgement This work was supported as part of the Nanostructures for Electrical Energy Storage (NEES), an Energy Frontier Research Center funded by the US Department of Energy, Office of Science, Basic Energy Sciences under Award number DESC0001160. Yiju Li and Tingting Gao acknowledge the China Scholarship Council (CSC) for financial support.

22 ACS Paragon Plus Environment

Page 22 of 28

Page 23 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

Reference (1) Etacheri, V.; Marom, R.; Elazari, R.; Salitra, G.; Aurbach, D. Challenges in the Development of Advanced Li-ion Batteries: A Review. Energy Environ. Sci. 2011, 4, 3243-3262. (2) Dunn, B.; Kamath, H.; Tarascon, J.-M. Electrical Energy Storage for the Grid: A Battery of Choices. Science 2011, 334, 928-935. (3) Amine, K.; Kanno, R.; Tzeng, Y. Rechargeable Lithium Batteries and Beyond: Progress, Challenges, and Future Directions. MRS Bull. 2014, 39, 395-401. (4) Manthiram, A. Materials Challenges and Opportunities of Lithium Ion Batteries. J. Phys. Chem. Lett. 2011, 2, 176-184. (5) Goodenough, J. B.; Park, K.-S. The Li-Ion Rechargeable Battery: A Perspective. J. Am. (6)

(7)

(8) (9)

Chem. Soc. 2013, 135, 1167-1176. Zhang, J.; Shi, Y.; Ding, Y.; Zhang, W.; Yu, G. In Situ Reactive Synthesis of Polypyrrole-MnO2 Coaxial Nanotubes as Sulfur Hosts for High-Performance Lithium–Sulfur Battery. Nano Lett. 2016, 16, 7276-7281. Peng, H. J.; Zhang, G.; Chen, X.; Zhang, Z. W.; Xu, W. T.; Huang, J. Q.; Zhang, Q. Enhanced Electrochemical Kinetics on Conductive Polar Mediators for Lithium–Sulfur Batteries. Angew. Chem. 2016, 128, 13184-13189. Seh, Z. W.; Sun, Y.; Zhang, Q.; Cui, Y. Designing high-energy lithium–sulfur batteries. Chem. Soc. Rev. 2016, 45, 5605-5634. Bresser, D.; Passerini, S.; Scrosati, B. Recent Progress and Remaining Challenges in Sulfur-Based Lithium Secondary Batteries-A Review. Chem. Commun. 2013, 49, 10545-10562.

(10) Manthiram, A.; Fu, Y.; Chung, S.-H.; Zu, C.; Su, Y.-S. Rechargeable Lithium–Sulfur Batteries. Chem. Rev. 2014, 114, 11751-11787. (11) Zheng, G.; Zhang, Q.; Cha, J. J.; Yang, Y.; Li, W.; Seh, Z. W.; Cui, Y. Amphiphilic surface modification of hollow carbon nanofibers for improved cycle life of lithium sulfur batteries. Nano Lett. 2013, 13, 1265-1270. (12) Li, N.; Zheng, M.; Lu, H.; Hu, Z.; Shen, C.; Chang, X.; Ji, G.; Cao, J.; Shi, Y. High-rate lithium–sulfur batteries promoted by reduced graphene oxide coating. Chem. Commun. 2012, 48, 4106-4108. (13) Moon, S.; Jung, Y. H.; Jung, W. K.; Jung, D. S.; Choi, J. W.; Kim, D. K. Encapsulated monoclinic sulfur for stable cycling of Li–S rechargeable batteries. Adv. Mater. 2013, 25, 6547-6553. (14) Chang, C. H.; Chung, S. H.; Manthiram, A. Effective Stabilization of a High‐loading Sulfur Cathode and a Lithium-Metal Anode in Li-S Batteries Utilizing SWCNT–Modulated Separators. Small 2016, 12, 174-179. 23 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

(15) Elazari, R.; Salitra, G.; Garsuch, A.; Panchenko, A.; Aurbach, D. Sulfur-Impregnated Activated Carbon Fiber Cloth as a Binder-Free Cathode for Rechargeable Li-S batteries. Adv. Mater. 2011, 23, 5641-5644. (16) Qie, L.; Manthiram, A. Uniform Li2S Precipitation on N, O-Codoped Porous Hollow Carbon Fibers for High-Energy-Density Lithium–Sulfur Batteries with Superior Stability. Chem. Commun. 2016, 52, 10964-10967. (17) Li, Z.; Zhang, J. T.; Chen, Y. M.; Li, J.; Lou, X. W. D. Pie-like Electrode Design for High-Energy Density Lithium-Sulfur Batteries. Nat. Commun. 2015, 6, 8850. (18) Song, J.; Xu, T.; Gordin, M. L.; Zhu, P.; Lv, D.; Jiang, Y. B.; Chen, Y.; Duan, Y.; Wang, D. Nitrogen-Doped Mesoporous Carbon Promoted Chemical Adsorption of Sulfur and Fabrication of High‐Areal-Capacity Sulfur Cathode with Exceptional Cycling Stability for Lithium-Sulfur Batteries. Adv. Funct. Mater. 2014, 24, 1243-1250. (19) Lu, S.; Chen, Y.; Wu, X.; Wang, Z.; Li, Y. Three-Dimensional Sulfur/Graphene Multifunctional Hybrid Sponges for Lithium-Sulfur Batteries with Large Areal Mass Loading. Sci. Rep. 2014, 4, 4629. (20) Xu, Y.; Wen, Y.; Zhu, Y.; Gaskell, K.; Cychosz, K. A.; Eichhorn, B.; Xu, K.; Wang, C. Confined Sulfur in Microporous Carbon Renders Superior Cycling Stability in Li/S Batteries. Adv. Funct. Mater. 2015, 25, 4312-4320. (21) Li, Z.; Wu, H. B.; Lou, X. W. D. Rational Designs and Engineering of Hollow Micro-/Nanostructures as Sulfur Hosts for Advanced Lithium–Sulfur Batteries. Energy Environ. Sci. 2016, 9, 3061-3070. (22) Zhang, B.; Qin, X.; Li, G.; Gao, X. Enhancement of Long Stability of Sulfur Cathode by Encapsulating Sulfur into Micropores of Carbon Spheres. Energy Environ. Sci. 2010, 3, 1531-1537. (23) Ji, L.; Rao, M.; Zheng, H.; Zhang, L.; Li, Y.; Duan, W.; Guo, J.; Cairns, E. J.; Zhang, Y. Graphene Oxide as a Sulfur Immobilizer in High Performance Lithium/Sulfur Cells. J. Am. Chem. Soc. 2011, 133, 18522-18525. (24) Wei, S.; Zhang, H.; Huang, Y.; Wang, W.; Xia, Y.; Yu, Z. Pig Bone Derived Hierarchical Porous Carbon and Its Enhanced Cycling Performance of Lithium–Sulfur Batteries. Energy Environ. Sci. 2011, 4, 736-740. (25) Li, Y.; Chen, C.; Gao, T.; Zhang, D.; Huang, X.; Pan, Y.; Ye, K.; Cheng, K.; Cao, D.; Wang, G. Synthesis of Hierarchically Porous Sandwich‐ Like Carbon Materials for High‐ Performance Supercapacitors. Chem. - Eur. J. 2016, 22, 16863-16871. (26) Xu, J.; Shui, J.; Wang, J.; Wang, M.; Liu, H.-K.; Dou, S. X.; Jeon, I.-Y.; Seo, J.-M.; Baek, J.-B.; Dai, L. Sulfur–graphene Nanostructured Cathodes via Ball-milling for High-performance Lithium–sulfur Batteries. ACS Nano 2014, 8, 10920-10930. (27) Papandrea, B.; Xu, X.; Xu, Y.; Chen, C.-Y.; Lin, Z.; Wang, G.; Luo, Y.; Liu, M.; Huang, Y.; Mai, L. Three-Dimensional Graphene Framework with Ultra-High Sulfur Content for 24 ACS Paragon Plus Environment

Page 24 of 28

Page 25 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

a Robust Lithium–Sulfur Battery. Nano Res. 2016, 9, 240-248. (28) Li, Y.; Wang, G.; Wei, T.; Fan, Z.; Yan, P. Nitrogen and Sulfur Co-Doped Porous Carbon Nanosheets Derived from Willow Catkin for Supercapacitors. Nano Energy 2016, 19, 165-175. (29) Zhou, G.; Zhao, Y.; Manthiram, A. Dual-Confined Flexible Sulfur Cathodes Encapsulated in Nitrogen-Doped Double‐Shelled Hollow Carbon Spheres and Wrapped with Graphene for Li-S Batteries. Adv. Energy Mater. 2015, 5, 1402263. (30) Hassoun, J.; Scrosati, B. A High-Performance Polymer Tin Sulfur Lithium Ion Battery. Angew. Chem., Int. Ed. 2010, 49, 2371-2374. (31) Miao, L.-X.; Wang, W.-K.; Wang, A.-B.; Yuan, K.-G.; Yang, Y.-S. A high Sulfur Content Composite with Core–Shell Structure as Cathode Material for Li–S Batteries. J. Mater. Chem. A 2013, 1, 11659-11664. (32) Su, Y.-S.; Manthiram, A. Lithium–Sulfur Batteries with a Microporous Carbon Paper as a Bifunctional Interlayer. Nat. Commun. 2012, 3, 1166. (33) Peng, H. J.; Xu, W. T.; Zhu, L.; Wang, D. W.; Huang, J. Q.; Cheng, X. B.; Yuan, Z.; Wei, F.; Zhang, Q. 3D Carbonaceous Current Collectors: The Origin of Enhanced Cycling Stability for High-Sulfur-Loading Lithium-Sulfur Batteries. Adv. Funct. Mater. 2016, 26, 6351-6358. (34) Fang, R.; Zhao, S.; Hou, P.; Cheng, M.; Wang, S.; Cheng, H. M.; Liu, C.; Li, F. 3D Interconnected Electrode Materials with Ultrahigh Areal Sulfur Loading for Li–S Batteries. Adv. Mater. 2016, 28, 3374. (35) Song, J.; Yu, Z.; Xu, T.; Chen, S.; Sohn, H.; Regula, M.; Wang, D. Flexible Freestanding Sandwich-Structured Sulfur Cathode with Superior Performance for Lithium–Sulfur Batteries. J. Mater. Chem. A 2014, 2, 8623-8627. (36) Li, Z.; Zhang, J.; Lou, X. W. D. Hollow Carbon Nanofibers Filled with MnO2 Nanosheets as Efficient Sulfur Hosts for Lithium–Sulfur Batteries. Angew. Chem., Int. Ed. 2015, 54, 12886-12890. (37) Song, J.; Yu, Z.; Gordin, M. L.; Wang, D. Advanced Sulfur Cathode Enabled by Highly Crumpled Nitrogen-Doped Graphene Sheets for High-Energy-Density Lithium–Sulfur Batteries. Nano Lett. 2016, 16, 864-870. (38) Kim, J. S.; Hwang, T. H.; Kim, B. G.; Min, J.; Choi, J. W. Lithium-Sulfur Battery with a High Areal Energy Density. Adv. Funct. Mater. 2014, 24, 5359-5367. (39) Zhou, G.; Li, L.; Ma, C.; Wang, S.; Shi, Y.; Koratkar, N.; Ren, W.; Li, F.; Cheng, H.-M. A Graphene Foam Electrode with High Sulfur Loading for Flexible and High Energy Li-S Batteries. Nano Energy 2015, 11, 356-365. (40) Seh, Z. W.; Li, W.; Cha, J. J.; Zheng, G.; Yang, Y.; McDowell, M. T.; Hsu, P.-C.; Cui, Y. Sulphur–TiO2 Yolk–Shell Nanoarchitecture with Internal Void Space for Long-Cycle Lithium–Sulfur Batteries. Nat. Commun. 2013, 4, 1331. 25 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

(41) Yuan, Z.; Peng, H. J.; Huang, J. Q.; Liu, X. Y.; Wang, D. W.; Cheng, X. B.; Zhang, Q. Hierarchical Free‐Standing Carbon‐Nanotube Paper Electrodes with Ultrahigh Sulfur‐Loading for Lithium–Sulfur Batteries. Adv. Funct. Mater. 2014, 24, 6105-6112. (42) Hu, G.; Xu, C.; Sun, Z.; Wang, S.; Cheng, H. M.; Li, F.; Ren, W. 3D Graphene‐Foam–Reduced‐Graphene‐Oxide Hybrid Nested Hierarchical Networks for High‐Performance Li–S Batteries. Adv. Mater. 2016, 28, 1603. (43) Chung, S.-H.; Chang, C.-H.; Manthiram, A. A Carbon-Cotton Cathode with Ultrahigh-Loading Capability for Statically and Dynamically Stable Lithium–Sulfur Batteries. ACS Nano 2016, 10, 10462-10470. (44) Chen, C.; Zhang, Y.; Li, Y.; Dai, J.; Song, J.; Gong, Y.; Kierzewski, I.; Xie, J.; Hu, L. All-wood, Low Tortuosity, Aqueous, Biodegradable Supercapacitors with Ultra-High Capacitance. Energy Environ. Sci. 2017, 10, 538-545. (45) Luo, W.; Gong, Y.; Zhu, Y.; Fu, K. K.; Dai, J.; Lacey, S. D.; Wang, C.; Liu, B.; Han, X.; Mo, Y. Transition from Superlithiophobicity to Superlithiophilicity of Garnet Solid-State Electrolyte. J. Am. Chem. Soc. 2016, 138, 12258-12262.

26 ACS Paragon Plus Environment

Page 26 of 28

Page 27 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Nano

Supporting Information Contents: Figure S1. SEM images of the top surface and cross-section of the bare wood carbon.

Figure S2. TEM images of bare wood carbon. Figure S3. N2 adsorption-desorption isotherm curves of the bare wood carbon and C-wood. Figure S4. SEM image of the joint between the wall of microchannels and the RGO networks.

Figure S5. TEM image and corresponding elemental mappings of single RGO nanosheet loaded with sulfur.

Figure S6. SEM images and corresponding elemental mappings of the S@C-wood composites with sulfur mass loadings of 15.2 mg cm-2 (a) and 21.3 mg cm-2 (b), respectively.

Figure S7. SEM image and corresponding elemental mappings of the S@bare wood carbon composite

Figure S8. Photographs of the fabrication process of PEO gel composite membrane.

Figure S9. Cycling performance of the S@C-wood composite electrodes with different sulfur mass loadings.

27 ACS Paragon Plus Environment

ACS Nano

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure S10. Cycling performance of S@bare wood carbon electrode with a sulfur mass loading of 7.8 mg cm-2. .

28 ACS Paragon Plus Environment

Page 28 of 28