Subscriber access provided by Georgetown University | Lauinger and Blommer Libraries
Article
Enhanced Photocatalytic Degradation of Environmental Pollutants under Visible Irradiation by a Composite Coating Shuqin Liu, Qingkun Hu, Junlang Qiu, Fuxin Wang, Wei Lin, Fang Zhu, Chao-Hai Wei, Ningbo Zhou, and Gangfeng Ouyang Environ. Sci. Technol., Just Accepted Manuscript • DOI: 10.1021/acs.est.7b00350 • Publication Date (Web): 05 Apr 2017 Downloaded from http://pubs.acs.org on April 6, 2017
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Environmental Science & Technology is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 35
Environmental Science & Technology
1
Enhanced Photocatalytic Degradation of Environmental
2
Pollutants under Visible Irradiation by a Composite
3
Coating
4 5
Shuqin Liua, Qingkun Hua, Junlang Qiua, Fuxin Wanga, Wei Lina, Fang Zhua,
6
Chaohai Weib, Ningbo Zhou*c, Gangfeng Ouyang*a
7 8
a
9
Chemistry, Sun Yat-Sen University, No.135, Xingang Xi Road, Guangzhou,
MOE Key Laboratory of Bioinorganic and Synthetic Chemistry, School of
10
Guangdong 510275, China
11
b
12
Guangzhou 510006, P. R. China.
13
c
14
Technology, Yueyang 414006, P. R. China.
College of Environment and Energy, South China University of Technology,
College of Chemistry and Chemical Engineering, Hunan Institute of Science and
15 16
* Corresponding author. Tel. & Fax: +86-2084110845
17
E-mail:
[email protected];
[email protected] 18 19 20 21
1
ACS Paragon Plus Environment
Environmental Science & Technology
22
ABSTRACT
23
Although nanotechnology has offered effective and efficient solutions for
24
environmental remediation, the full utilization of sustainable energy and the
25
avoidance of secondary pollution are still challenges. Herein, we report a two-step
26
modification strategy for TiO2 nanoparticles by first forming a thin, surface-adherent
27
polydopamine (PDA) shell onto the nanoparticles and then assembling core/shell
28
nanoparticles as a photodegradation coating. The composite coating modified from
29
TiO2 could not only realize the highly efficient utilization of photons from the visible
30
region but could also avoid the secondary pollution of nanoparticles during
31
application. Additionally, improvements in the adsorption ability after modification
32
greatly facilitated the photocatalytic process of the modified materials. A preliminary
33
in vivo study on Daphnia magna and a wastewater treatment experiment suggest that
34
treatment with the composite coating can effectively eliminate fluorene and
35
significantly reduce its lethality. We believe the two-step modification scheme can
36
open new avenues for the facile modification of nanomaterials for designed purposes,
37
especially in the field of environmental remediation.
38 39
2
ACS Paragon Plus Environment
Page 2 of 35
Page 3 of 35
Environmental Science & Technology
40
1. INTRODUCTION
41
Environmental pollution has long been a global problem due to the rapid pace of
42
urbanization and heavy industrialization.1,2 Although much effort has been spent on
43
the removal and degradation of hazardous environmental contaminants,3-5
44
environment remediation is still a topic of global concern. Over the past decades, the
45
emergence of nanotechnology has given tremendous possibilities and scope to
46
remedy polluted water by utilizing nanomaterials designed with specific
47
properties.6-8 As a well-known and the most investigated functional material in
48
semiconductor photocatalysis, TiO2 nanoparticles have been extensively used in the
49
degradation of a variety of toxic pollutants in air and water.9-11
50
Despite possessing numerous advantages, such as strong oxidizing power, high
51
stability, nontoxicity and superior photoelectric effect, the large band gap energy (3.2
52
eV) of TiO2 facilitates the necessity of utilizing ultraviolet (UV) excitation to realize
53
specific applications.12-14 However, it should be noted that only a small amount of
54
solar radiation comes from the UV region,6 which leads to requirements for
55
enhancing the utilization of photons from the visible region by TiO2 nanoparticles. A
56
viable strategy for narrowing the band gap of TiO2 can be realized by doping foreign
57
elements into the materials.15,16 The modification of TiO2 with metal elements has
58
been reported to successfully decrease the TiO2 band gap17,18 by promoting electron
59
transfer from the valence band to the conduction band and facilitating the formation
60
of oxidative species. However, the existence of some transition metals has been
61
proven to facilitate the probability of electron-hole recombination, which would lead 3
ACS Paragon Plus Environment
Environmental Science & Technology
62
to a decline in the photocatalytic performance.6 Recently, some studies have shown
63
that the band gap narrowing of TiO2 could be better realized by adding nonmetal
64
elements (N, C, S, F, etc.) into the material.9,19,20 Such modified TiO2 materials
65
showed larger response to irradiation in the visible region and increased the
66
degradation performance of hazardous pollutants under visible light irradiation,
67
especially under natural solar light irradiation.6,20
68
Currently, polydopamine (PDA) has opened a new route to the functionalization
69
of a variety of substrates since dopamine can self-polymerize and deposit PDA on
70
almost all kinds of inorganic or organic surfaces.21 In addition, PDA is expected to
71
offer a large number of active sites for binding organic pollutants via electrostatic
72
interactions, hydrogen bonding or π−π stacking interactions, owing to the existence
73
of abundant functional groups, such as catechol groups, amine groups, and aromatic
74
moieties, which are beneficial to secondary modification as well.21-24 Moreover, as a
75
major component of naturally occurring melanin, which is widely distributed in the
76
human body, the excellent biocompatibility of PDA22 decreases the occurrence of
77
adverse effects during biological and environmental applications. Therefore, in this
78
contribution, PDA was used as a nonmetal element dopant to realize the band gap
79
narrowing of rutile TiO2 by the simple immobilization of a thin, surface-adherent
80
and biocompatible PDA shell onto the TiO2 nanoparticles.
81
However, separation is another major bottleneck that limits the application of TiO2
82
nanoparticles,26-28 since it is hard to achieve photodegradation and separation
83
simultaneously in powder form and difficult to recycle TiO2 due to its suspended 4
ACS Paragon Plus Environment
Page 4 of 35
Page 5 of 35
Environmental Science & Technology
84
dispersive properties in water.28,29 Moreover, the incomplete separation of
85
nanoparticles may subsequently give rise to the secondary pollution of water.30 In
86
this context, glutaraldehyde (GA) was used to assemble the prepared TiO2/PDA
87
core/shell nanoparticles into a homogeneous photodegradation coating by connecting
88
with the abundant functional groups in PDA shells. After two-step modification of
89
rutile TiO2 nanoparticles, the resulting TiO2/PDA/GA coating possessed satisfactory
90
visible light photodegradation capacity towards organic pollutants. As expected, the
91
contaminated water treated by the composite coating was safe, as proven by
92
preliminary in vivo studies.
93
2. EXPERIMENTAL SECTION
94
2.1. Synthesis of TiO2 Nanoparticles. First, 18 mL of ammonium hydroxide
95
(30%), 32 mL of ultrapure water and 44.5 mL of TEOS were added into 750 mL
96
ethanol with stirring for 24 h. The translucent SiO2 was collected by centrifugation
97
and sintered at 500 °C. Then, 66 mL of aqueous TiCl4 (20 mM) containing 10 g of
98
the sintered product was heated at 70 °C for 1 h. SiO2 was obtained after washing,
99
drying and resintering (500 °C). Afterwards, 2.6 g of SiO2 and 6.68 g of
100
1-methylimidazolium tetrafluoroborate were mixed into 200 mL of the 120 mM TiF4
101
aqueous solution (pH=2.1), which was transferred to a Teflon-lined autoclave and
102
heated at 130 °C for 12 h. The product collected by filtration was then added into a 2
103
M NaOH aqueous solution at 80 °C for 1 h to remove SiO2. The remaining TiO2
104
nanoparticles were finally obtained by filtration, washing and drying.
105
2.2. Synthesis of TiO2/PDA Core/Shell Nanoparticles. TiO2 nanoparticles (100 5
ACS Paragon Plus Environment
Environmental Science & Technology
106
mg) and dopamine (40 mg) were dispersed in 320 mL of ultrapure water by
107
ultrasonication for 30 min to form a suspension. Subsequently, 80 mL of tris-buffer
108
(10 mM, pH: ~8.5) was added to the suspension, and the mixture was stirred at room
109
temperature for 24 h. Afterwards, the product was obtained by centrifugation,
110
washed three times with ultrapure water and ethanol, and then dried at 80 °C.
111
2.3. Preparation of TiO2/PDA/GA Coating and Fibers. First, a cleaned quartz
112
glass tube with an external diameter of 5 mm was immersed into a solution of
113
dopamine (2 mg/mL) with 10 mM tris-buffer (pH: ~8.5) overnight at room
114
temperature. The PDA-coated tube was rinsed with distilled water to remove
115
residual dopamine. Afterwards, 1 g of the TiO2/PDA core/shell nanoparticles were
116
dispersed in 1 mL of GA (50% in water) to form a viscous mixture. The mixture was
117
then spin-coated on the treated quartz glass tube and held at 60 °C for 4 h. Similarly,
118
the TiO2/PDA/GA fibers were prepared by spin-coating cleaned gas chromatograph
119
(GC) capillary columns with the viscous mixture, following the heating steps. Before
120
each use, the TiO2/PDA/GA coating and fibers were conditioned at 90 °C overnight
121
under vacuum.
122
2.4. Physical Characterizations. The detection of pollutants was carried out on
123
an Agilent 7890 gas chromatograph-flame ionization detector (GC-FID, Palo Alto,
124
CA, USA) and a gas chromatograph-mass spectrometer (GC-MS, 6890-5975 B)
125
equipped with an HP-5 MS capillary column (30 m × 0.32 mm i.d. × 0.25 µm film
126
thickness) from Agilent (Palo Alto, CA, USA). Scanning electron microscopy (SEM)
127
images and elemental mappings were obtained from a Quanta 400 Thermal FE 6
ACS Paragon Plus Environment
Page 6 of 35
Page 7 of 35
Environmental Science & Technology
128
Environmental Scanning Electron Microscope (FEI, Netherlands). Powder X-ray
129
diffraction (PXRD) patterns were recorded on a Bruker D8 ADVANCE X-ray
130
powder diffractometer (Cu kα). Transmission electron microscopy (TEM) images
131
were obtained via a JEM-2010HR transmission electron microscope (JEOL, Japan).
132
Fourier transform infrared (FTIR) spectra were recorded on a Bruker EQUINOX 55
133
Fourier transform infrared spectrometer. BET surface areas and N2 adsorption
134
isotherms (77.3 K) were obtained by a Micromeritics ASAP 2020 V3.04 H surface
135
and porosity analyzer. X-ray photoelectron spectra (XPS) patterns were recorded on
136
an ESCALab250 X-ray photoelectron spectrometer (Thermo Fisher Scientific, USA).
137
Element analysis (EA) was carried out by an Elementar Vario EL element analyzer,
138
and UV-vis diffuse reflectance spectra were collected on a UV-vis-NIR
139
spectrophotometer (Shimadzu UV-3600). Commercial polydimethylsiloxane (PDMS,
140
100 µm) and polyacrylate (PA, 85 µm) solid-phase microextraction (SPME) fibers
141
were purchased from Supelco (Bellefonte, PA, USA).
142
2.5. Adsorption of Geosmin and Fluorene. The TiO2/PDA/GA coating was
143
submersed in 10 mL of 1000 ppb geosmin or fluorene aqueous solutions in the dark.
144
Agitation was carried out using a magnetic stir bar at room temperature. The
145
real-time concentrations of the residual pollutants in the solutions were detected by
146
headspace (HS) SPME coupled with GC-FID methods (see details in the Supporting
147
Information). Similarly, the adsorption of geosmin or fluorene by the TiO2 or
148
TiO2/PDA core/shell nanoparticles was conducted by replacing the TiO2/PDA/GA
149
coating with the nanoparticles (the same amount as the coating materials). 7
ACS Paragon Plus Environment
Environmental Science & Technology
150
2.6. Photodegradation Studies. Photocatalytic experiments were carried out in a
151
homemade photoreactor (Figure 4a). In experiments with the coatings, a coated
152
quartz glass tube was submersed in 10 mL of aqueous solution of 1000 ppb geosmin
153
or fluorene under agitation after reaching extraction equilibrium. The mixture was
154
irradiated with a 350 W xenon lamp under different wavelengths. Tinfoil was
155
attached to the internal surface of the light blocking box. Photodegradation under
156
UV was conducted by equipping the lamp with a 300-400 nm filter, while
157
photodegradation under visible light was realized by equipping the lamp with a 420
158
nm cutoff filter. In addition, irradiation from UV to visible light was provided with
159
no filter equipped. After irradiation for a given time interval, the coating was
160
removed from solution. The residual concentrations of the pollutant were detected by
161
the HS-SPME and GC-FID methods. Similar to the degradation of geosmin or
162
fluorene by TiO2 nanoparticles, the TiO2/PDA core/shell nanoparticles or brush-like
163
photodegradation device was constructed by replacing the TiO2/PDA/GA coating
164
with the nanoparticles or the assembled fiber array.
165
2.7. Lethality Studies in Daphnia Magna. Daphnia magna were cultured in the
166
artificial freshwater (AFW) under the conditions described in the guidelines from the
167
Organization for Economic Cooperation and Development for the testing of
168
chemicals (OECD, 2008). The AFW was prepared according to the method
169
described previously.31 In brief, a total of 294.0 mg CaCl2·2H2O, 123.2 mg
170
MgSO4·7H2O, 5.8 mg KCl and 64.8 mg NaHCO3 were mixed into 1 L of ultrapure
171
water. The mixture was aerated vigorously for 24 h to dissolve the chemicals and 8
ACS Paragon Plus Environment
Page 8 of 35
Page 9 of 35
Environmental Science & Technology
172
stabilize the medium. The culture temperature was set at 20±0.1 °C, and the
173
photoperiod was 16:8 light:dark. Daphnia magna were fed twice a week with a
174
suspension of Scenedesmus subspicatus. In the lethality experiments, Daphnia
175
magna were cultured under untreated AFW, AFW contaminated by fluorene (1000
176
ppb in concentration) and contaminated AFW that was treated by a TiO2/PDA/GA
177
coating under visible light irradiation for 120 min. Each group contained 100
178
Daphnia magna. The lethality (%) of Daphnia magna was monitored every 12 h.
179
2.8. Coking Wastewater Treatment. Coking wastewater was collected from a
180
coke plant in Shanghai, China. Before treatment and analysis, the wastewater was
181
filtered through a 0.45 µm filter membrane to remove insoluble substances. For each
182
treatment experiment, 100 mL of coking wastewater was used.
183
3. RESULTS AND DISCUSSION
184
3.1. Synthesis of TiO2/PDA Core/Shell Nanoparticles and Assembly of
185
TiO2/PDA/GA Coating. Dopamine has been known to self-polymerize and generate
186
thin, surface-adherent PDA membranes onto virtually all types of inorganic or
187
organic substances.22 The simple immersion of TiO2 nanoparticles into a diluent of
188
dopamine (2 mg/mL), buffered to a pH typical of marine environments (10 mM tris,
189
pH 8.5), gave rise to the spontaneous formation of a homogeneous adherent polymer
190
shell on the surface of the nanoparticles (Figure 1). Rutile TiO2 nanoparticles with
191
sizes of 80-100 nm (Figure S1) were synthesized via a seeded nucleation scheme.32
192
TEM images (Figures 2a,b) of the resulting TiO2/PDA core/shell nanoparticles
193
revealed that the thickness of the outer PDA shell was almost 12 nm. Multifunctional 9
ACS Paragon Plus Environment
Environmental Science & Technology
194
groups, including catechols, amines and imines, present in the PDA shell were
195
further modified with GA. Owing to the cross-linking effect of GA, the TiO2/PDA
196
core/shell nanoparticles were assembled onto the PDA-modified quartz glass tube,
197
leading to the formation of the TiO2/PDA/GA coating (Figure 1). At variance with
198
the separated core/shell nanoparticles in Figure 2a, the TEM image of the scraped
199
coating (Figure 2d) showed that the TiO2/PDA nanoparticles were almost aggregated
200
after GA treatment, which corresponds to the self-assembly of the TiO2/PDA/GA
201
coating. High-resolution transmission electron microscopy (HRTEM) images
202
(Figures 2b and 2e) and fast Fourier transform (FFT) generated diffraction patterns
203
(inset images in Figures 2a and 2d), confirmed that the nanoparticles consisted of a
204
crystalline TiO2 core and an amorphous polymer shell. In the HRTEM images, a
205
diagnostic lattice fringe was found in the core, while no lattice fringe appeared in the
206
shell. The desired crystalline structure of the TiO2 cores in the TiO2/PDA core/shell
207
nanoparticles and the TiO2/PDA/GA coating were also validated by PXRD patterns
208
(Figure S2).
209
The surface morphologies of the TiO2/PDA core/shell nanoparticles and the
210
TiO2/PDA/GA coating exhibited distinct differences, as shown in Figures 2c and 2f.
211
After treatment by GA, numerous macropores (Figure 2f) appeared on the surface of
212
the TiO2/PDA/GA coating (inset image in Figure 2f), and almost no separated
213
particles were observed, which was greatly different from the SEM image of the
214
TiO2/PDA core/shell nanoparticles (Figure 2c). Elemental mappings (Figure S3)
215
based on energy-dispersive X-ray spectroscopy (EDS) and EA confirmed the 10
ACS Paragon Plus Environment
Page 10 of 35
Page 11 of 35
Environmental Science & Technology
216
existence of Ti, O, C and H elements in the TiO2/PDA core/shell nanoparticles and
217
the TiO2/PDA/GA coating (Table S1). In addition, the nitrogen-to-carbon (N/C)
218
atomic ratio, determined to be 0.127, of the TiO2/PDA core/shell nanoparticles was
219
close to the theoretical N/C value (0.125) of dopamine, indicating that the polymer
220
shell of the nanoparticles was derived from the polymerization of dopamine. After
221
treatment by GA, the hydrogen-to-carbon (H/C) ratio increased, while the N/C ratio
222
greatly decreased, which demonstrated the involvement of GA during the assembly
223
of the TiO2/PDA/GA coating.
224
XPS and FTIR analyses were conducted to further verify the functional groups in
225
the TiO2/PDA core/shell nanoparticles and the TiO2/PDA/GA coating. In the FTIR
226
spectra (Figure S4), bands at 450-700 cm-1 indicated the presence of Ti-O-Ti bonds,
227
and peaks from 1450 to 1600 cm-1 resulted from benzene skeletal vibrations. In
228
addition, both spectra showed a broad band from 3000-3600 cm-1, which
229
synergistically resulted from O-H bonds, N-H bonds and C-H bonds from the
230
benzene ring framework. However, the core/shell nanoparticles exhibited a distinct
231
absorption peak at approximately 1100 cm-1 due to C-N stretching vibrations, while
232
the absorption peak of the coating at the same wavenumber was much weaker, which
233
proved that amine groups in the PDA shell participated in the cross-linking reaction
234
with GA. Additionally, in the FTIR spectra of the TiO2/PDA/GA coating, peaks at
235
2870 and 2934 cm-1 were generated by C-H stretching vibrations of the methylene
236
bonds, the peaks at 1680 and 1720 cm-1 were caused by the C=O bonds of the
237
unreacted aldehyde group, and C=N bonds formed from the aldehyde-ammonia 11
ACS Paragon Plus Environment
Environmental Science & Technology
238
condensation reaction. XPS analysis (Figure S5) and EA results (Table S1) also
239
agree with the above discussion.
240
3.2. Photocatalytic Performance. By introducing nonmetal elements, including
241
C and N, onto the surface of the TiO2 nanoparticles, the PDA shell was expected to
242
narrow the band gap energy and enhance visible light absorption for the modified
243
TiO2, as shown in Figure S6a, which displays the UV-vis diffuse reflectance spectra
244
(DRS) of the proposed materials. As expected, the rutile TiO2 nanoparticles showed
245
their typical absorption edge at approximately 400 nm. In comparison with pure
246
TiO2, the TiO2/PDA core/shell nanoparticles and the TiO2/PDA/GA coating
247
exhibited significantly enhanced absorption not only in the visible region but also in
248
the UV region. In addition, it should be noted that the absorption edges of the
249
core/shell nanoparticles and the coating showed an obvious red shift relative to that
250
of TiO2, which implies that the narrowing of the band gap energy occurred after
251
modification. The band gap energies can be determined through extrapolation of the
252
adsorption edges according to the equation Eg=1240/λ. Consequently, the band gap
253
energies of the prepared materials were estimated to be approximately 3.10 eV for
254
the TiO2 nanoparticles, 2.28 eV for the TiO2/PDA core/shell nanoparticles and 2.25
255
eV for the TiO2/PDA/GA coating, indicating that the modified materials are able to
256
utilize visible light to decompose specific environmental pollutants.
257
Figure S6b presents the XPS valence band spectra of the prepared materials,
258
showing that the edges of the valence band maximum energy for the TiO2
259
nanoparticles, the TiO2/PDA core/shell nanoparticles and the TiO2/PDA/GA coating 12
ACS Paragon Plus Environment
Page 12 of 35
Page 13 of 35
Environmental Science & Technology
260
were 2.28 eV, 2.97 eV and 2.46 eV, respectively. Once the energy gap and the
261
valence band maximum energy positions are confirmed, the energy band structures
262
of the prepared materials can also be determined, as shown in Figure S6c.
263
According to the results discussed above, the as-prepared TiO2/PDA core/shell
264
nanoparticles and the TiO2/PDA/GA coating were expected to possess favorable
265
visible light photocatalysis enhancement compared with the unmodified TiO2
266
nanoparticles. Herein, geosmin and fluorene were chosen as target pollutants to
267
investigate the photocatalytic performance of the modified materials. Geosmin, a
268
bicyclic tertiary alcohol formed in aqueous environments by cyanobacteria or
269
actinomycetes,28,33 is of great importance to the water purification and aquaculture
270
industries. Although geosmin is nontoxic, its presence in drinking water causes an
271
unpleasant taste. In contrast, as one of the polycyclic aromatic hydrocarbons (PAHs)
272
that contains three fused rings, fluorene is a ubiquitous pollutant with potently
273
mutagenic and carcinogenic toxicities, which is labeled a priority pollutant by the
274
U.S. Environment Protection Agency.34 Given the above reasons, geosmin and
275
fluorene, which were commonly found in the environment, were selected as the
276
testing pollutants.
277
HS-SPME coupled with GC-FID was used in this work to determine the real-time
278
concentration of the pollutants (Figure 3a). SPME is a solvent-free and green
279
equilibrium-based sample pretreatment technique that integrates sampling, isolation
280
and enrichment into one step.35-37 It involves the utilization of a fused silica or metal
281
fiber coated with specific materials, which is introduced into or over the sample 13
ACS Paragon Plus Environment
Environmental Science & Technology
282
matrixes. After the target analytes are extracted onto the fiber, the SPME fiber is
283
transferred to the injection port of the GC to complete the desorption and analysis
284
procedures. The as-proposed SPME-GC methods could analyze a variety of
285
compounds with low detection limits. Herein, geosmin and fluorene analyzed by
286
HS-SPME-GC-FID using a PDMS fiber was validated from 1 ppb to 1000 ppb and 5
287
ppb to 1000 ppb, respectively. The calibration curves of the two pollutants showed a
288
linear response with correlation coefficients (R2) of 0.9990 and 0.9996 (Figure S7).
289
Herein, the photocatalytic decomposition of geosmin and fluorene was carried out
290
using the TiO2 nanoparticles, the TiO2/PDA core/shell nanoparticles and the
291
TiO2/PDA/GA coating under different lighting conditions. The time-dependent
292
concentrations of geosmin and fluorene are shown in Figure 3. The schematic
293
illustration in Figure 3a demonstrates the removal and analysis processes of
294
pollutants using the TiO2/PDA/GA coating. The photodegradation of pollutants using
295
the nanoparticles was conducted by replacing the coating with the dispersed
296
nanoparticles. As Figure 3b shows, the TiO2 nanoparticles can remove only 28.1% of
297
the geosmin after visible light irradiation for 120 min, which indicates the poor
298
photocatalytic ability of the TiO2 nanoparticles under visible light irradiation.
299
However, 67% and 70.2% of the geosmin was degraded with catalysis from the TiO2
300
nanoparticles under UV irradiation and UV-visible light irradiation, respectively. In
301
contrast, the TiO2/PDA core/shell nanoparticles exhibited much better photocatalytic
302
ability towards geosmin not only under visible light irradiation but also under UV
303
irradiation (Figure 3d). In detail, 90.0%, 90.9% and 92.2% of geosmin was degraded 14
ACS Paragon Plus Environment
Page 14 of 35
Page 15 of 35
Environmental Science & Technology
304
after visible, UV and UV-visible light irradiation, for 120 min, respectively. As
305
expected, the TiO2/PDA/GA coating showed favorable photocatalytic ability to
306
decompose geosmin as well and that 87.9%, 88.7% and 91.5% of the geosmin was
307
removed after treatment under visible, UV and UV-visible light irradiation for 120
308
min using the TiO2/PDA/GA coating (Figure 3f). Similarly, in the fluorene
309
decomposition experiments, only 25.6% of the pollutant was removed by the TiO2
310
nanoparticles after visible light irradiation for 120 min, while 73.0% and 74.2% of
311
the fluorene was degraded under UV and UV-visible light irradiation (Figure 3c).
312
The TiO2/PDA core/shell nanoparticles and the TiO2/PDA/GA coating also exhibited
313
much better photocatalytic ability towards fluorene, as shown in Figures 3e and 3g.
314
As a result, 98.0%, 98.2% and 99.0% of the fluorene was removed by the TiO2/PDA
315
core/shell nanoparticles and 97.3%, 98.4% and 99.0% of the fluorene was degraded
316
by the TiO2/PDA/GA coating under different lighting conditions.
317
In summary, after modification by PDA and GA, the promotion of the
318
photocatalytic ability of the prepared rutile TiO2 under visible light irradiation was
319
successfully achieved. As a matter of fact, separation is one of the major bottlenecks
320
that limits the application of nanoparticles. Apart from the involvement of separation
321
and filtration, circulating processes are difficult to achieve, considering the dispersed
322
nanoparticles form particulate suspensions. Therefore, in this context, taking
323
advantage of the cross-linking effect of GA and PDA, a TiO2/PDA/GA coating was
324
self-assembled to overcome disadvantages of the direct utilization of nanoparticles.
325
It is noted that the coating exhibited photocatalytic ability towards the pollutants 15
ACS Paragon Plus Environment
Environmental Science & Technology
326
comparable to that of the modified TiO2/PDA core/shell nanoparticles. Although the
327
coating needed 80 min to remove the pollutants, while the core/shell nanoparticles
328
needed only 40 min, the avoidance of filtration and separation processes could
329
compensate for the extra time consumption. The photodegradation of geosmin and
330
fluorene using the TiO2/PDA/GA coating under visible light irradiation was also
331
monitored for five consecutive cycles of 80 min each (Figure S8). No significant
332
reduction in the photodegradation performance was observed over the five sequential
333
cycles, demonstrating the good stability of the proposed photodegradation coating
334
under visible light irradiation.
335
Compounds that were only detected after the photocatalytic treatment of the
336
contaminated solutions, instead of the untreated ones, were determined to be
337
degradation intermediates or products of the pollutants. Degradation intermediates of
338
geosmin and fluorene in the presence of the TiO2/PDA/GA coating under visible
339
light irradiation were detected by direct immersion (DI) SPME coupled with GC-MS
340
using a PA fiber. Four peaks were found to be related to geosmin, and two peaks
341
were found to be produced by the photodegradation of fluorene, as shown in Table
342
S2. Some of the degradation intermediates listed in the table correspond to those in
343
previous reports. 38,39 The possible reaction pathways were proposed accordingly for
344
the decomposition of fluorene and geosmin, as shown in Figure S9.
345
3.3. Adsorption Ability. The adsorption performances of the prepared materials
346
towards geosmin and fluorene were examined in the dark. As displayed in Figure
347
S10, all the materials reached extraction equilibrium towards the two pollutants after 16
ACS Paragon Plus Environment
Page 16 of 35
Page 17 of 35
Environmental Science & Technology
348
60 min. Under adsorption equilibrium, 22.2%, 62.2%, and 59.7% of the geosmin and
349
28.2%, 62.2%, and 61.7% of the fluorene were adsorbed by the TiO2 nanoparticles,
350
the TiO2/PDA core/shell nanoparticles and the TiO2/PDA/GA coating, respectively.
351
Obviously, the adsorption ability of the TiO2 nanoparticles was also improved after
352
modification. Thus, the increased efficiency in the adsorption of pollutants
353
contributed to the enhanced photocatalytic ability of the composites. In fact,
354
modification by PDA and GA immensely increased the BET surface area from 24.0
355
m2/g for the TiO2 nanoparticles to 87.3 m2/g for the TiO2/PDA core/shell
356
nanoparticles and 99.0 m2/g for the TiO2/PDA/GA coating, which resulted in the
357
improvement in the adsorption efficiency mentioned above. After the modification
358
process, the modified materials exhibited significantly enhanced adsorption of
359
photons in visible region and UV region (Figure S6a), which contributed to the
360
photocatalytic process. Moreover, the adsorption improvement further facilitated the
361
photocatalytic process of the modified materials not only under visible light
362
irradiation but also under UV irradiation.
363
Adsorption kinetics were investigated to further explore the adsorption behavior
364
of the materials towards geosmin and fluorene (Figure S11 and Table S3). According
365
to the results, the adsorption processes were more accordant with the
366
pseudo-first-order kinetics. That is to say, the adsorption of the materials towards
367
geosmin and fluorene was mainly influenced by the diffusion process of the
368
compounds from the sample to the adsorbent. During the photodegradation process,
369
as the adsorbed pollutant was decomposed, the adsorption equilibrium was broken, 17
ACS Paragon Plus Environment
Environmental Science & Technology
370
and the pollutant would quickly move from the solution to the core/shell
371
nanoparticles and the coating. The efficient adsorption process significantly
372
accelerated the enrichment of the pollutant to the catalyst surface, which
373
subsequently improved the photodegradation performance.
374
3.4. In vivo Study on Daphnia Magna and Wastewater Treatment. Daphnia
375
magna is among the most sensitive researched organism to toxic compounds, which
376
is diffusely distributed in aquatic freshwater habits and has been broadly utilized in
377
aquatic risk assessment.40 Accordingly, it is always used to evaluate the toxicity
378
response of various aquatic systems.41,42 To evaluate the impact of the
379
photodegradation of toxic fluorene using the TiO2/PDA/GA coating under visible
380
light irradiation, a Daphnia magna lethality experiment was carried out. Daphnia
381
magna were cultured under untreated AFW, AFW contaminated by fluorene and the
382
contaminated AFW that was treated by the TiO2/PDA/GA coating under visible light
383
irradiation. In contaminated AFW, all Daphnia magna died after exposure to
384
fluorene for 36 h, while 96% of the Daphnia magna survived without exposure to
385
fluorene (Figure 4a). The results in Figure 4a and Movie S1 revealed that treatment
386
of contaminated AFW by the TiO2/PDA/GA coating significantly reduced the
387
lethality of the contaminated AFW such that 92% of the Daphnia magna survived.
388
The in vivo experiment suggests that treatment of contaminated water with the
389
as-prepared TiO2/PDA/GA coating might prove advantageous to decreasing the toxic
390
effects of some chemicals.
18
ACS Paragon Plus Environment
Page 18 of 35
Page 19 of 35
Environmental Science & Technology
391
Coking wastewater generated from high-temperature carbonation, coal gas
392
purification, and chemical refining in coke plants always contains a certain amount
393
of PAHs.43 To further broaden the application of the TiO2/PDA/GA coating to
394
eliminate fluorene, a coking wastewater treatment experiment was carried out. The
395
calibration curve of fluorene in a low concentration range was obtained via the
396
HS-SPME-GC-MS method using PDMS fibers (Figure S12). The wastewater
397
treatment device was setup as shown in Figure S13. It is believed to be difficult for
398
light to enter the dark brown wastewater, which would greatly lower the amount of
399
light received by the coating. To solve the mentioned limitation, the coating was
400
adhered to the glass wall of a vial, and a water-membrane was formed between the
401
coating and the glass wall. The water-membrane was thin enough to be penetrated by
402
light so that photodegradation could successfully occur. The results in Figure 4b
403
show that the initial concentration of fluorene existed in the wastewater itself was
404
158 ng/L and that no fluorene was detected in the wastewater after 520 min
405
treatment with the TiO2/PDA/GA coating under visible light irradiation. Although
406
agitation can accelerate the flow of the water-membrane, the elimination rate of
407
fluorene in coking wastewater was still much lower than that in the pure water
408
system. Moreover, the proposed TiO2/PDA/GA coating was proven to be capable of
409
removing fluorene in wastewater, which provides potential for future application of
410
the coating in industrial wastewater treatment and environmental remediation.
411
3.5. Evaluation of the Modified Degradation Device. Effective utilization of the
412
TiO2/PDA/GA coating avoids separation processes, but it takes two times longer for 19
ACS Paragon Plus Environment
Environmental Science & Technology
413
the TiO2/PDA core/shell nanoparticles to remove pollutants (Figure 3), due to the
414
much smaller contact area between the coating and the pollutants. With the purpose
415
of improving the photocatalytic efficiency of the coating, GC capillary columns with
416
external diameters of nearly 350 µm were used to prepare photodegradation fibers.
417
The fibers were subsequently assembled as a brush-like photodegradation device.
418
Under visible light irradiation, the photodegradation performance of the
419
TiO2/PDA/GA fiber array towards geosmin and fluorene was compared with those of
420
the TiO2/PDA nanoparticles and the TiO2/PDA/GA coating (Figures 4a and 4b). The
421
modified degradation device is shown in Figure 5c. According to the results in
422
Figures 4a and 4b, the fiber array exhibited an elimination rate of the pollutants
423
between that of the core/shell nanoparticles and the coating. Moreover, the fiber
424
array needed only 40 min to remove the pollutants, which is the same time required
425
for removal by the TiO2/PDA nanoparticles. Table S4 illustrated the comparison of
426
the treating time and visible light degradation ratio for the pollutants of the reported
427
non-metal modified TiO2 materials and the TiO2/PDA/GA composite proposed in
428
this work. Generally speaking, compared with other non-metal modified TiO2
429
materials, the TiO2/PDA/GA composite exhibited rapid pollutant degradation ability,
430
especially for the TiO2/PDA/GA fiber array, and satisfactory pollutant elimination
431
ratios.
432
For the purpose of further proving the effectiveness of the modified degradation
433
device, the removal of fluorene from coking wastewater was conducted (Figure S14).
434
According to Figure 5d, no fluorene was detected in wastewater after a 280 min 20
ACS Paragon Plus Environment
Page 20 of 35
Page 21 of 35
Environmental Science & Technology
435
treatment of the TiO2/PDA/GA fiber array under visible light irradiation, which was
436
240 min faster than when using the TiO2/PDA/GA coating. The above results proved
437
that the adoption of the miniature TiO2/PDA/GA fiber array could greatly improve
438
the photocatalytic efficiency of the proposed material. Actually, more time was
439
required for fiber preparation and device assembly processes. However, this will not
440
be a problem if batch production is adopted.
441
In this work, we proposed a two-step modification scheme to improve the
442
photocatalytic performance of rutile TiO2 nanoparticles under visible light. First, the
443
immobilization of a PDA shell onto the TiO2 core narrowed the band gap energy of
444
the TiO2 nanoparticles, which consequently improved the visible light response
445
compared to unmodified TiO2. Secondary modification by GA, which resulted in the
446
formation of the TiO2/PDA/GA coating, avoided separation processes for continuous
447
application of the modified materials while maintaining the photoresponse ability to
448
visible light irradiation of the TiO2/PDA core/shell nanoparticles. In other words, the
449
self-assembled nanostructured materials can be used without environmental
450
exposure to nanomaterials. Additionally, the adsorption ability of the unmodified
451
TiO2 nanoparticles was also improved after modification. The increased adsorption
452
efficiency of pollutants contributed to the photocatalytic performance enhancement
453
of the composites. The safety and effectiveness of the coating, proven by the in vivo
454
study with Daphnia magna and the coking wastewater treatment experiment,
455
suggests that it may provide an innocuous alternative to the utilization of
456
nanotechnology in environmental remediation. Since dopamine has been proven to 21
ACS Paragon Plus Environment
Environmental Science & Technology
Page 22 of 35
457
undergo a self-polymerization reaction and form a PDA membrane on almost all
458
kinds of inorganic and organic surfaces21, the two-step modification scheme
459
proposed in this work is expected to provide a versatile strategy for the modification
460
of nanomaterials and other functional substrates. We believe the findings in this
461
work could provide new insights in various fields, such as environmental science,
462
catalytic science, materials science and life science.
463
ASSOCIATED CONTENT
464
Supporting Information Available: Details of analysis geosmin, fluorene and their
465
degradation intermediates. Figures: TEM images, XRD patterns, SEM images and
466
elemental mappings, FTIR spectra, XPS spectra, UV-visible diffuse reflectance
467
spectra and band gap states, relative response of geosmin and fluorene versus their
468
concentrations,
469
adsorption performance, adsorption kinetics and coking wastewater treatment
470
devices. Tables: element analysis, intermediate products of photodegradation,
471
adsorption kinetics parameters and performance comparisons. Movie S1: (Daphnia
472
magna lethality experiment).
473
AUTHOR INFORMATION
474
Corresponding Author.
475
*Email:
[email protected] (G. Ouyang);
[email protected] (N. Zhou)
476
Notes.
477
The authors declare no competing financial interest.
recycled
photodegradation
performance, reaction
22
ACS Paragon Plus Environment
pathways,
Page 23 of 35
Environmental Science & Technology
478
ACKNOWLEDGMENTS
479
We acknowledge financial support from the projects of NNSFC (21377172,
480
21477166, 21527813, 21677182) and the NSF of Guangdong Province
481
(S2013030013474).
482
REFERENCES
483
(1) Schwarzenbach, R. P.; Escher, B. I.; Fenner, K.; Hofstetter, T. B.; Johnson, C. A.;
484
von Gunten, U.; Wehrli, B. The challenge of micropollutants in aquatic systems.
485
Science 2006, 313 (5790), 1073-1077.
486
(2) Daughton, C. G.; Ternes, T. A. Pharmaceuticals and personal care products in the
487
environment: agents of subtle change? Environ. Health Perspect. 1999, 107 (Suppl
488
6), 907-938.
489
(3) Alsbaiee, A.; Smith, B. J.; Xiao, L.; Ling, Y.; Helbling, D. E.; Dichtel, W. R.
490
Rapid removal of organic micropollutants from water by a porous β-cyclodextrin
491
polymer. Nature 2016, 529, 190-194.
492
(4) Richardson, S. D.; Ternes, T. A. Water analysis: emerging contaminants and
493
current issues. Anal. Chem. 2014, 86 (6), 2813-2848.
494
(5) Murray, K. E.; Thomas, S. M.; Bodour, A. A. Prioritizing research for trace
495
pollutants and emerging contaminants in the freshwater environment. Environ.
496
Pollut. 2010, 158 (12), 3462-3471.
497
(6) Khin, M. M.; Nair, A. S.; Babu, V. J.; Murugan, R.; Ramakrishna, S. A review on
498
nanomaterials for environmental remediation. Energy Environ. Sci. 2012, 5 (8),
499
8075-8109. 23
ACS Paragon Plus Environment
Environmental Science & Technology
Page 24 of 35
500
(7) Shannon, M. A.; Bohn, P. W.; Elimelech, M.; Georgiadis, J. G.; Marinas B. J.;
501
Mayes, A. M. Science and technology for water purification in the coming decades.
502
Nature 2008, 452 (7185), 301-310.
503
(8) Brandl, F.; Bertrand, N.; Lima, E. M.; Langer, R. Nanoparticles with
504
photoinduced precipitation for the extraction of pollutants from water and soil. Nat.
505
Commun. 2015, 6, 7765.
506
(9) Li, X.; Liu, H.; Cheng, L.; Tong, H. Photocatalytic oxidation using a new catalyst
507
TiO2 microsphere for water and wastewater treatment. Environ. Sci. Technol. 2003,
508
37 (17), 3989-3994.
509
(10) Chalasani, R.; Vasudevan, S. Cyclodextrin-functionalized Fe3O4@TiO2:
510
reusable,
511
endocrine-disrupting chemicals in water supplies. ACS Nano 2013, 7 (5), 4093-4104.
512
(11) Park, C.; La, Y.; An, T. H.; Jeong, H. Y.; Kang, S.; Joo, S. H.; Ahn, H.; Shin, T. J.
513
Kim, K. T. Mesoporous monoliths of inverse bicontinuous cubic phases of block
514
copolymer bilayers. Nat. Commun. 2015, 6, 6392.
515
(12) Liu, H.; Ma, H.; Li, X.; Li, W.; Wu, M.; Bao, X. The enhancement of TiO 2
516
photocatalytic activity by hydrogen thermal treatment. Chemosphere 2003, 50 (1),
517
39-46.
518
(13) Linsebigler, A. L.; Lu, G.; Yates, J. T. Photocatalysis on TiO2 surfaces:
519
principles, mechanisms, and selected results. Chem. Rev. 1995, 95 (3), 735-758.
520
(14) Lee, J.; Kim, J.; Choi, W. TiO2 photocatalysis for the redox conversion of
521
aquatic pollutants. ACS Symp. Ser. 2011, 1071, 199-222.
magnetic
nanoparticles
for
photocatalytic
24
ACS Paragon Plus Environment
degradation
of
Page 25 of 35
Environmental Science & Technology
522
(15) Sato, S.; Asahi, R.; Morikawa, T.; Ohwaki, T.; Aoki, K.; Taga, Y. Photocatalysts
523
sensitive to visible light. Science 2002, 295 (5555), 626-627.
524
(16) Yamashita, H.; Harada, M.; Misaka, J.; Takeuchi, M.; Neppolian, B.; Anpo, M.
525
Photocatalytic degradation of organic compounds diluted in water using visible
526
light-responsive metal ion-implanted TiO2 catalysts: Fe ion-implanted TiO2. Catal.
527
Today 2003, 84 (3), 191-196.
528
(17) Sung-Suh, H. M.; Choi, J. R.; Hah, H. J.; Sang, M. K.; Bae, Y. C. Comparison
529
of Ag deposition effects on the photocatalytic activity of nanoparticulate TiO2 under
530
visible and UV light irradiation. J. Photochem. Photobiol. 2004, 163 (1), 37-44.
531
(18) Salthammer, T.; Fuhrmann, F. Photocatalytic surface reactions on indoor wall
532
paint. Environ. Sci. Technol. 2007, 41 (18), 6573-6578.
533
(19) Kosowska, B.; Mozia, S.; Morawski, A. W.; Grzmil, B.; Janus, M.; Kalucki, K.
534
The preparation of TiO2-nitrogen doped by calcination of TiO2·xH2O under
535
ammonia atmosphere for visible light photocatalysis. Sol. Energy Mater. Sol. Cells
536
2005, 88 (3), 269-280.
537
(20) Mao, W.; Lin, X.; Zhang, W.; Chi, Z.; Lyu, R.; Cao, A.; Wan, L. Core-shell
538
structured TIO2@polydopamine for highly active visible-light photocatalysis. Chem.
539
Commun. 2016, 52(44), 7122-7125.
540
(21) Rehman, S.; Ullah, R.; Butt, A. M.; Gohar, N. D. Strategies of making TiO2 and
541
ZnO visible light active. J. Hazard. Mater. 2009, 170 (2), 560-569.
542
(22) Lee, H.; Dellatore, S. M.; Miller, W. M.; Messersmith, P. B. Mussel-inspired
543
surface chemistry for multifunctional coatings. Science 2007, 318 (5849), 426-430. 25
ACS Paragon Plus Environment
Environmental Science & Technology
544
(23) Liu, Y.; Ai, K.; Lu, L. Polydopamine and its derivative materials: synthesis and
545
promising applications in energy, environmental, and biomedical fields. Chem. Rev.
546
2014, 114 (9), 5057-5115.
547
(24) D’Ischia, M.; Napolitano, A.; Ball, V.; Chen, C. T.; Buehler, M. J.
548
Polydopamine and eumelanin: from structure-property relationships to a unified
549
tailoring strategy. Acc. Chem. Res. 2014, 47 (12), 3541-50.
550
(25) Sureshkumar, M.; Lee, C. K. Polydopamine coated magnetic-chitin (MCT)
551
particles as a new matrix for enzyme immobilization. Carbohydr. Polym. 2011, 84
552
(2), 775-780.
553
(26) Praetorius, A.; Scheringer, M.; Hungerbühler, K. Development of environmental
554
fate models for engineered nanoparticles: a case study of TiO2 nanoparticles in the
555
Rhine River. Environ. Sci. Technol. 2012, 46 (12), 6705-6713.
556
(27) Weir, A.; Westerhoff, P.; Fabricius, L.; Hristovski, K.; Von Goetz, N. Titanium
557
dioxide nanoparticles in food and personal care products. Environ. Sci. Technol.
558
2012, 46 (4), 2242-2250.
559
(28) Liu, H.; Li, X.; Leng, Y.; Li, W. An alternative approach to ascertain the
560
rate-determining steps of TiO2 photoelectrocatalytic reaction by electrochemical
561
impedance spectroscopy. J. Phys. Chem. B 2003, 107 (34), 8988-8996.
562
(29) Hoffmann, M. R.; Martin, S. T.; Choi, W.; Bahnemann, B. W. Environmental
563
Applications of Semiconductor Photocatalysis. Chem. Rev. 1995, 95 (1), 69-96.
564
(30) Chen, G.; Qiu, J.; Liu, Y.; Jiang, R.; Cai, S.; Liu, Y.; Zhu, F.; Zeng, F.; Luan, T.;
565
Ouyang, G. Carbon nanotubes act as contaminant carriers and translocate within 26
ACS Paragon Plus Environment
Page 26 of 35
Page 27 of 35
Environmental Science & Technology
566
plants. Sci. Rep. 2015, 5, 15682.
567
(31) Petersen, E. J.; Akkanen, J.; Kukkonen, J. V.; Jr, W. W. Biological uptake and
568
depuration of carbon nanotubes by daphnia magna. Environ. Sci. Technol. 2009, 43
569
(8), 2969-2975.
570
(32) Crossland, E. J. W.; Noel, N.; Sivaram, V.; Leijtens, T.; Alexander-Webber, J. A.;
571
Snaith, H. J. Mesoporous TiO2 single crystals delivering enhanced mobility and
572
optoelectronic device performance. Nature 2013, 495, 215-219.
573
(33) Wert, E. C.; Korak, J. A.; Trenholm, R. A.; Rosario-Ortiz, F. L. Effect of oxidant
574
exposure on the release of intracellular microcystin, MIB, and geosmin from three
575
cyanobacteria species. Water Res. 2014, 52, 251-259.
576
(34) Luo, S.; Chen, B.; Lin, L.; Wang, X.; Tam, N. F. Y.; Luan, T. Pyrene degradation
577
accelerated by constructed consortium of bacterium and microalga: effects of
578
degradation products on the microalgal growth. Environ. Sci. Technol. 2014, 48 (23),
579
13917-13924.
580
(35) Ouyang, G.; Vuckovic, D.; Pawliszyn, J. Nondestructive sampling of living
581
systems using in vivo solid-phase microextraction. Chem. Rev. 2011, 111 (4),
582
2784-814.
583
(36) Liu, S.; Chen, D.; Zheng, J.; Zeng, L.; Jiang, J.; Jiang, R.; Zhu, F.; Shen, Y.; Wu,
584
D.; Ouyang, G. The sensitive and selective adsorption of aromatic compounds with
585
highly crosslinked polymer nanoparticles. Nanoscale 2015, 7 (40), 16943-16951.
586
(37) Vuckovic, D.; de Lannoy, I.; Gien, B.; Shirey, R.E.; Sidisky, L. M.; Dutta, S.;
587
Pawliszyn, J. In Vivo Solid-Phase Microextraction: Capturing the Elusive Portion of 27
ACS Paragon Plus Environment
Environmental Science & Technology
588
Metabolome. Angew. Chem., Int. Ed. 2011, 50 (23), 5344-5460.
589
(38) Kinani, S.; Souissi, Y.; Kinani, A.; Vujovic, S.; Ait-Aissa, S.; Bouchonnet, S.
590
Photodegradation of fluorene in aqueous solution: Identification and biological
591
activity testing of degradation products. J. Chromatogr. A 2016, 1442, 118-128.
592
(39) Xue, Q.; Liu, Y.; Zhou, Q.; Utsumi, M.; Zhang, Z.; Sugiura, N. Photocatalytic
593
degradation of geosmin by Pd nanoparticle modified WO3, catalyst under simulated
594
solar light. Chem. Eng. J. 2016, 283, 614-621.
595
(40) Barata, C.; Varo, I.; Navarro, J. C.; Arun, S.; Porte, C. Antioxidant enzyme
596
activities and lipid peroxidation in the freshwater cladoceran Daphnia magna
597
exposed to redox cycling compounds. Comp. Biochem. Physiol. C: Pharmacol.
598
Toxicol. 2005, 140 (2), 175-186.
599
(41) Lovern, S. B.; Strickler, J. R.; Klaper, R. Behavioral and physiological changes
600
in Daphnia magna when exposed to nanoparticle suspensions (titanium dioxide,
601
nano-C60, and C60HxC70Hx). Environ. Sci. Technol. 2007, 41 (12), 4465-4470.
602
(42) Blewett, T. A.; Delompré, P. L.; He, Y.; Folkerts, E. J.; Flynn, S. L.; Alessi, D.
603
S.; Goss, G. G. The sub-lethal and reproductive effects of acute and chronic exposure
604
to flowback and produced water from hydraulic fracturing on the water flea Daphnia
605
magna. Environ. Sci. Technol. 2017, 51 (5), 3032-3039.
606
(43) Yang, W.; Li, X.; Pan, B.; Lv, L.; Zhang, W. Effective removal of effluent
607
organic matter (EfOM) from bio-treated coking wastewater by a recyclable aminated
608
hyper-cross-linked polymer. Water Res. 2013, 47 (13), 4730-4738.
609
28
ACS Paragon Plus Environment
Page 28 of 35
Page 29 of 35
Environmental Science & Technology
610
Figure Captions
611
Figure 1. Synthetic scheme of the TiO2/PDA core/shell nanoparticles and assembly
612
of the TiO2/PDA/GA coating.
613
Figure 2. (a,b) TEM images of the TiO2/PDA nanoparticles; inset is the
614
FFT-generated diffraction pattern. (c) SEM images of the TiO2/PDA nanoparticles.
615
(d,e) TEM images of the TiO2/PDA/GA coating; inset is the FFT-generated
616
diffraction pattern. (f) SEM images of the TiO2/PDA/GA coating; inset is the
617
photograph of the coating.
618
Figure 3. Photocatalytic degradation of geosmin and fluorene. (a) Schematic
619
illustration of the removal and analysis of the pollutants. (b,d,f) Removal of geosmin
620
by the TiO2 nanoparticles, the TiO2/PDA core/shell nanoparticles and the
621
TiO2/PDA/GA coating. (c,e,g) Removal of fluorene by the TiO2 nanoparticles, the
622
TiO2/PDA core/shell nanoparticles and the TiO2/PDA/GA coating.
623
Figure 4. (a) Treatment of fluorene-contaminated AFW by the TiO2/PDA/GA
624
coating significantly reduced the lethality of Daphnia magna. (b) Fluorene in coking
625
wastewater was removed by the TiO2/PDA/GA coating under visible light
626
irradiation.
627
Figure 5. Photodegradation performance of the TiO2/PDA/GA fiber array under
628
visible light irradiation. (a,b) Removal of geosmin and fluorene by the
629
TiO2/PDA/GA fiber array. (c) Schematic illustration of pollutant removal by the
630
TiO2/PDA/GA fiber array. (d) Comparison of fluorene removal in coking wastewater
631
by the TiO2/PDA/GA coating and the fiber array.
632 29
ACS Paragon Plus Environment
Environmental Science & Technology
633
Figure 1.
634
635 636 637
30
ACS Paragon Plus Environment
Page 30 of 35
Page 31 of 35
Environmental Science & Technology
638
Figure 2.
639
640 641 642 643
31
ACS Paragon Plus Environment
Environmental Science & Technology
644
Figure 3.
645
646 647 648 649
32
ACS Paragon Plus Environment
Page 32 of 35
Page 33 of 35
Environmental Science & Technology
650
Figure 4.
651
652 653 654
33
ACS Paragon Plus Environment
Environmental Science & Technology
655
Figure 5.
656
657 658 659 660
34
ACS Paragon Plus Environment
Page 34 of 35
Page 35 of 35
Environmental Science & Technology
661
For TOC only
662
663 664 665 666
35