Subscriber access provided by UNIV OF CALIFORNIA SAN DIEGO LIBRARIES
Article
Preparation and performance of silica/epoxy groupfunctionalized bio-based elastomer nanocomposite He Qiao, Wenji Xu, Mingyuan Chao, Jun Liu, Weiwei Lei, Xinxin Zhou, Runguo Wang, and Liqun Zhang Ind. Eng. Chem. Res., Just Accepted Manuscript • DOI: 10.1021/acs.iecr.6b03517 • Publication Date (Web): 06 Jan 2017 Downloaded from http://pubs.acs.org on January 10, 2017
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Industrial & Engineering Chemistry Research is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
3
Preparation and performance of silica/epoxy group-functionalized bio-based elastomer nanocomposite
4
He Qiao,a,b Wenji Xu,a,b Mingyuan Chao,b Jun Liu,a,b Weiwei Lei,a,b Xinxin Zhou,a,b
5
Runguo Wang, b * Liqun Zhang a, b*
6
a
7
Technology, Beijing 100029, China
8
b
9
Materials, Beijing 100029, China
1 2
State Key Laboratory of Organic-Inorganic Composites, Beijing University of Chemical
Key Laboratory of Beijing City for Preparation and Processing of Novel Polymer
10 11 12 13 14 15 16 17 18 19
1
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 2 of 34
20
KEYWORDS: bio-based elastomer; silica; interfacial interaction
21
ABSTRACT:
22
itaconate-ter-isoprene-ter-glycidyl methacrylate) (PDBIIG) was synthesized via redox
23
emulsion
24
group-included monomer. The silica/PDBIIG nanocomposite was prepared without
25
adding silane coupling agents. Ring-opening reaction, which occurred between the
26
hydroxyl groups on the silica surfaces and the epoxy groups of the PDBIIG chains during
27
mixing and vulcanization, was confirmed via bound rubber tests and Fourier transform
28
infrared spectroscopy. This reaction was facilitated through heat treatment at 150 °C
29
effectively. The introduction of covalent bonds significantly improved the interfacial
30
interaction and dispersion of silica, which was indicated by transmission electron
31
microscopy and rubber process analyzer (RPA) results. With the same silica loading and
32
compounding procedure, the inclusion of 3.7 wt.% GMA increased the modulus at 100%
33
strain by 150.0% and the modulus at 300% strain by 152.3%. For the dynamic
34
mechanical properties, the nanocomposite with GMA exhibited higher wet skid resistance
35
and lower rolling resistance than the nanocomposite without GMA.
36
1. Introduction
Epoxy
group-functionalized
polymerization
using
glycidyl
bio-based
methacrylate
elastomer
(GMA)
poly
as
the
(dibutyl
epoxy
37
Elastomers have excellent elasticity and play a significant role in national defense,
38
industries, and daily living. With the dwindling fossil resources, soaring energy demand, 2
ACS Paragon Plus Environment
Page 3 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
39
and growing environmental concerns, bio-based elastomers derived from renewable
40
resources have attracted increasing attention1-3. Natural rubber is a typical bio-based
41
elastomer, which is directly acquired from the natural rubber tree Hevea brasiliensis.
42
However, natural rubber faces several serious problems, such as the harsh growth
43
conditions of rubber trees, fungal disease threat to rubber trees, and increasing allergic
44
reactions to the proteins in natural rubber 4; thus, the development of bio-based
45
synthesized elastomers, particularly those for engineering applications, is highly
46
important and urgent 5. Several types of bio-based synthesized elastomers, including polyester elastomers 6-10,
47
11-17
itaconic acid-based elastomers
49
rubber 22, have been developed in recent years. The present study is related to an itaconic
50
acid-based elastomer poly (dibutyl itaconate-co-isoprene) (PDBII) and its relevant
51
nanocomposites. Itaconic acid is a bio-based building block chemical with multiple
52
functional groups; this acid is produced industrially through the fermentation of sugars23,
53
24
54
are promising bio-based monomers for bio-based elastomers 11-15. Comonomer isoprene is
55
used to increase the flexibility of macromolecular chains and to provide crosslink points
56
for elastomers. Bio-isoprene from renewable resources is expected to become available in
57
the market in the near future because of numerous efforts devotedly working on it 22, 25.
58
, polyurethane elastomers
18-21
48
, and the bio-isoprene
. Itaconate esters made through the esterification of itaconic acid and bio-based alcohols
The addition of a filler is necessary to improve elastomer properties 3
ACS Paragon Plus Environment
26, 27
. Silica is a
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
59
non-petroleum-based filler and is widely used in the rubber industry because it can
60
provide excellent mechanical properties, low rolling resistance, and high wet skid
61
resistance
62
polar silica is prone to agglomerating because of its abundant surface hydroxyl groups,
63
thereby leading to the poor dispersion of silica and the weak interfacial interaction
64
between silica and elastomers 30, 31. The most common method to solve these problems is
65
to use silane coupling agents, such as bis-(γ-triethoxysilylpropyl)-tetrasulfide (Si69) and
66
3-(mercaptopropyl trimethoxysilane (KH590), which can modify the silica surface and
67
link silica with elastomer macromolecules
68
(VOCs), such as methanol and ethanol, are released during high-temperature silanization
69
at approximately 150 °C 32, 35, 36; these compounds are harmful to the environment and to
70
operators. The functionalization of the elastomer matrix can also improve the dispersion
71
of silica and the interfacial interaction between silica and elastomer. The hydroxyl groups
72
on the silica surface are numerous; hence, if we endow the bio-based PDBII with
73
functional groups that can react directly with the hydroxyl groups, then interfacial
74
interaction improves by forming covalent bonds at the interfaces. The dispersion of silica
75
can also be improved. The ring-opening reaction between the epoxides and hydroxyl
76
groups of silica occurs with the help of a mechanical force and increased temperature 37-41.
77
Thus, we intend to functionalize PDBII with epoxy groups. The addition of epoxy
78
group-included comonomer in the polymerization can realize this idea easily. Glycidyl
28, 29
. The present study used silica to reinforce bio-based PDBII. However,
31-34
. However, volatile organic compounds
4
ACS Paragon Plus Environment
Page 4 of 34
Page 5 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
79
methacrylate (GMA) is a bifunctional chemical with a double bond and an epoxy group.
80
It was chosen as the appropriate third comonomer for PDBII in this study. The terpolymer
81
poly (dibutyl itaconate-ter-isoprene-ter-glycidyl methacrylate) (PDBIIG) was designed as
82
the matrix of the silica-filled nanocomposite. The designed schematic is shown in Figure
83
1.
84
In the present work, epoxy group-functionalized bio-based elastomer PDBIIG was
85
synthesized via mild free-radical redox emulsion polymerization, and silica/PDBIIG
86
nanocomposite was prepared via simple mechanical blending. Silica was covalently
87
linked with PDBIIG because of the ring-opening reaction between silica and PDBIIG.
88
The direct matrix–filler linkage avoids the addition of any silane coupling agent and
89
inhibits the release of VOCs during processing. The ring-opening reaction between silica
90
and PDBIIG during mixing and vulcanization was discussed and affirmed. The effects of
91
the covalent bonding interfaces on the interfacial interaction between silica and elastomer,
92
the dispersion of silica, the dynamic mechanical properties, and the static mechanical
93
properties of the nanocomposite were investigated. Our research on elastomer
94
functionalization through polymerization to improve interfacial interaction between the
95
filler and the matrix provides a new idea for preparing nanocomposite with desired
96
properties.
97
5
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
98 99 100
Figure 1. Designed schematic of the nanocomposite with covalent linkage between silica and the elastomer.
101
2. Experimental section
102
2.1. Materials
103
Dibutyl itaconate (96%) was bought from Sigma-Aldrich. Isoprene (99%) was
104
bought from Alfa Aesar and distilled before use. GMA (97%) was bought from
105
Sigma-Aldrich and passed through a neutral alumina column before use. Sodium dodecyl
106
benzene sulfonate (SDBS, 95%) was purchased from Aladdin. Ferric ethylene diamine
107
tetraacetic acid salt (Fe-EDTA), sodium hydroxymethanesulfinate (SHS), tert-butyl
108
hydroperoxide (TBH), and hydroxylamine (HA) were bought from Sigma-Aldrich and
109
used as received. The precipitated silica (Ultrasil VN3) with a BET specific surface of
110
175 m2/g and a particle size of 20–30 nm was bought from Degussa Chemical. Other
111
materials used were of analytical grade and commercially available.
112
2.2. Synthesis of PDBII and PDBIIG
6
ACS Paragon Plus Environment
Page 6 of 34
Page 7 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
113 114
Figure 2. Polymerization reaction of PDBIIG.
115
Bio-based PDBIIG was synthesized via free-radical emulsion polymerization under
116
20 °C based on the formula shown in Table S1. The polymerization reaction is shown in
117
Figure 2. In a three-neck glass flask, deionized water, SDBS solution, Fe-EDTA solution,
118
SHS solution, and a mixture of the monomers (dibutyl itaconate, isoprene, and GMA)
119
were added under nitrogen atmosphere, and the emulsion system was stirred at 400 rpm
120
for 1 h. The initiator TBH was then added, and the stirring rate was reduced to 250 rpm.
121
After 12 h, the polymerization reaction was terminated with HA, and the PDBIIG latex
122
was obtained. The PDBIIG latex was then flocculated with ethanol to acquire the wet
123
PDBIIG elastomer, which was dried in a vacuum oven for 24 h at 60 °C. The PDBII
124
elastomer was also synthesized in the same way except for the addition of GMA to
125
compare with the PDBIIG elastomer.
126
2.3. Preparation of nanocomposites
127
The compounding formulation for silica/PDBII and silica/PDBIIG is shown in Table
128
S2. First, silica was mixed with the elastomer in a Haake internal mixer at 30 °C for 10
129
min. The silica/PDBII (silica/PDBIIG) mixture was taken out and cooled down to room
130
temperature. Second, the other additives were mixed with the silica/PDBII 7
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
131
(silica/PDBIIG) mixture at 30 °C to obtain the silica/PDBII (silica/PDBIIG) compound.
132
Finally, the compound was vulcanized at 150 °C under 15 MPa to obtain the silica/PDBII
133
(silica/PDBIIG) nanocomposite. The optimum curing time of the compound was
134
determined using a disc vulkameter. A silica/PDBIIG-150 nanocomposite was also
135
prepared to investigate the reaction between PDBIIG and silica. The silica/PDBIIG
136
mixture obtained at the first step was added to the Haake internal mixer at 150 °C and
137
treated for 5 min to facilitate further reaction between PDBIIG and silica. The obtained
138
silica/PDBIIG-150 mixture was then taken out and cooled down to room temperature.
139
The subsequent steps were the same as those for silica/PDBIIG. The neat PDBII and
140
PDBIIG elastomers were also compounded and vulcanized in the same manner as the
141
silica/PDBII (silica/PDBIIG) nanocomposite except for the addition of silica.
142
2.4. Measurements and characterization
143
1
H nuclear magnetic resonance (1H NMR) measurements were obtained using a
144
Bruker AV400 spectrometer with CDCl3 as the solvent. Fourier transform infrared (FTIR)
145
spectra were collected on a Bruker Tensor 27 spectrometer. Differential scanning
146
calorimetry (DSC) was conducted with a Mettler-Toledo DSC instrument under nitrogen.
147
The sample was heated to 100 °C and kept isothermal for 3 min to remove the previous
148
history. Then, it was cooled to −100 °C and reheated to 100 °C. The heating (cooling)
149
rate was 10 °C/min. Gel permeation chromatography was performed with a Waters
150
Breeze instrument equipped with three columns (Styragel HT3_HT5_HT6E) and a 8
ACS Paragon Plus Environment
Page 8 of 34
Page 9 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
151
refractive index detector. Tetrahydrofuran was used as the eluent with a flowing rate of
152
1.0 mL/min, and polystyrene standards were used for calibration. The morphologies of
153
the nanocomposites were observed using a Tecnai G2 20 S-TWIN transmission electron
154
microscope (TEM) at an acceleration voltage of 200 KV, and the ultrathin sections were
155
cut with an EM UC7/FC7 microtome at −100 °C. The strain sweep measurements of the
156
compounds and the nanocomposites were analyzed with an RPA 2000 at 60 °C, and the
157
test frequency was 1 Hz. The dynamic mechanical thermal properties were implemented
158
on a 01dB-Metravib VA 3000 dynamic mechanical thermal analyzer at 10 Hz under the
159
strain amplitude of 0.1% in a tension mode. The temperature was scanned from −80 °C to
160
80 °C with a heating rate of 3 °C/min. The mechanical properties were implemented
161
using a SANS CMT 4104 electrical tensile instrument at 25 °C with a tensile rate of 500
162
mm/min according to ASTM D412. The bound rubber tests were measured based on the
163
previously reported methods 42.
164 165
3. Results and discussion
166
3.1. Structure and characterization of PDBIIG
167
168
Table 1 Yields, compositions, and molecular weights of PDBII and PDBIIG. Sample
Yield (%)
GMA content in feed (wt.%)
Actual GMA content in PDBIIG (wt.%)
Mn (g/mol)
PDI
PDBII
89
0
0
475000
2.5
PDBIIG
92
5
3.7
397000
2.2
The bio-based elastomer PDBIIG was successfully synthesized via a mild redox 9
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
169
free-radical emulsion polymerization. After polymerization for 12 h, the yields of PDBII
170
and PDBIIG reached 89% and 92%, respectively. Table 1 shows that the number-average
171
molecular weight (Mn) of PDBII is 475000 g/mol with a polydispersity index (PDI) of 2.5,
172
whereas the Mn of PDBIIG is 397000 g/mol with a PDI of 2.2. The actual GMA content
173
of PDBIIG was estimated by NMR. The result shows that the GMA content in the
174
elastomer is lower than that in the feed.
175 176
Figure 3. FTIR spectra of PDBII and PDBIIG.
177 178
The chemical structure of PDBIIG was determined by FTIR and 1H NMR. Figure 3
179
shows the FTIR spectra of PDBII and PDBIIG. The two spectra present similar
180
absorption peaks. The peaks at 1173 cm−1 and 1728 cm−1 belong to the C-O-C and C=O
181
stretching vibrations of dibutyl itaconate, respectively. The peak at 1663 cm−1 is
182
attributed to the C=C stretching vibration of isoprene. The peaks at 844 cm−1 and 1350
183
cm−1 are assigned to the C-H out-of-plane and in-plane deformation vibrations of the 10
ACS Paragon Plus Environment
Page 10 of 34
Page 11 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
184
double bonds of isoprene, respectively. The peaks at 739 cm−1 and 967 cm−1 correspond
185
to the C-H deformation vibration of the cis-1,4 structures and trans-1,4 structures of
186
isoprene, respectively. The small difference of the two spectra lies on the weak peak at
187
908 cm−1, which corresponds to the ring vibration of the epoxy group. The structure of
188
PDBIIG was further confirmed by 1H-NMR. The spectra and the detailed assignments of
189
each peak to the molecular structure are shown in Figure 4. The small peaks at 2.82, 3.20,
190
and 3.82 ppm originate from the protons of an epoxy group and its adjacent methylene.
191
The results of the FTIR and 1H-NMR verify that GMA has been successfully introduced
192
into the PDBII chains.
193 194
Figure 4. 1H-NMR spectra of PDBII and PDBIIG.
195
The glass transition temperature (Tg) of PDBII and PDBIIG was obtained using DSC
196
thermograms (Figure 5). The introduction of GMA increases the Tg of the elastomer.
197
Moreover, neither of the two curves shows any crystallization peak, which indicates that
198
the elastomers are amorphous. 11
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
199 200 201
Figure 5. DSC curves of PDBII and PDBIIG. 3.2. Characterization of nanocomposites
202 203 204 205
Figure 6. Bound rubber contents of silica/PDBII, silica/PDBIIG, and silica/PDBIIG-150 compounds.
206
Bound rubber is the rubber absorbed on the filler surfaces. The interaction between
207
the filler and the rubber leads to the formation of bound rubber; bound rubber
208
significantly affects filler reinforcement
209
silica/PDBIIG, and silica/PDBIIG-150 compounds were measured. Figure 6 shows that
210
the introduction of GMA considerably increases bound rubber content, and the additional
43
. The bound rubber contents of silica/PDBII,
12
ACS Paragon Plus Environment
Page 12 of 34
Page 13 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
211
heat treatment at 150 °C further increases bound rubber content. Bound rubber
212
measurements were conducted on unvulcanized compounds; hence, we can speculate a
213
ring-opening reaction between PDBIIG and silica during the mixing process, and the heat
214
treatment further facilitates the reaction. The results of the bound rubber content indicate
215
that the interfacial interaction in silica/PDBIIG is stronger than that in silica/PDBII
216
because of the introduction of covalent bonds between silica and the matrix. Moreover,
217
the shear force during mixing with a high temperature facilitates the ring-opening
218
reaction between silica and PDBIIG.
219 220 221 222 223 224 225 226
Figure 7. FTIR spectra of (a) PDBIIG, (b) silica/PDBIIG compound, (c) silica/PDBIIG nanocomposite, (d) silica/PDBIIG-150 compound, (e) silica/PDBIIG-150 nanocomposite, and (f) silica/PDBII compound. (All the test samples were prepared using an identical procedure, as described in Section 2.3, but without the addition of any rubber ingredient to avoid interference peaks.) The
FTIR
spectra the
of
the
silica/PDBIIG
silica/PDBIIG-150
compound,
compound,
and
silica/PDBIIG
227
nanocomposite,
228
nanocomposite were obtained to further investigate the reaction between silica and 13
ACS Paragon Plus Environment
the
the
silica/PDBIIG-150
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
229
PDBIIG during the preparation of the nanocomposites. The corresponding spectra are
230
shown in Figure 7. All the spectra were normalized with the peak of the C=O stretching
231
vibration at 1728 cm−1. The intensity variation of the peak of the epoxy group ring
232
vibration at 908 cm−1 was used to characterize the ring-opening reaction between the
233
epoxy groups of PDBIIG and the hydroxyl groups of silica. The intensity of the peak at
234
908 cm−1 for the silica/PDBIIG compound (b) is slightly lower than that for the neat
235
PDBIIG (a), thereby indicating the ring-opening reaction between PDBIIG and silica
236
during the mixing process. After vulcanization, the intensity of the peak at 908 cm−1 of
237
silica/PDBIIG (c) continuously decreases, which indicates that the ring-opening reaction
238
proceeds during the hot-press process at 150 °C. The comparison between (b) and (d)
239
shows that the intensity of the peak at 908 cm−1 of the silica/PDBIIG-150 compound is
240
lower than that of the silica/PDBIIG compound, thereby indicating that the additional hot
241
treatment with shear force and temperature effectively facilitates ring-opening reaction,
242
which is consistent with the result of the bound rubber content mentioned earlier. The
243
subsequent vulcanization further promotes the reaction, and the peak at 908 cm−1 of the
244
silica/PDBIIG-150 nanocomposite (e) nearly disappears similar to that of the
245
silica/PDBII compound (f), which indicates that the ring-opening reaction between silica
246
and PDBIIG is nearly complete. The FTIR results of all the compounds and the
247
nanocomposites manifest that the reaction between silica and PDBIIG occurs in the
248
mixing and vulcanization processes. The hot treatment at 150 °C will make the reaction 14
ACS Paragon Plus Environment
Page 14 of 34
Page 15 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
249
Industrial & Engineering Chemistry Research
comprehensive.
250
The dispersion of the filler in the matrix is an important factor for a composite to
251
achieve high performance. The TEM micrographs shown in Figure 8 exhibit the
252
dispersion of silica in PDBIIG and PDBII. The dark spots in the micrographs are silica
253
particles. Figure 8(a) shows that the dispersion of silica in PDBII is poor with a few
254
aggregates and voids. The introduction of GMA significantly improves the dispersion of
255
silica. Figures 8(b) and 8(c) show that silica disperses uniformly in PDBIIG without any
256
evident aggregates and voids. The significant improvement of dispersion is attributed to
257
the formation of covalent bonds between silica and PDBIIG in the silica-filled PDBIIG
258
nanocomposites.
15
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
259 260 261
262 263 264 265 266 267
Figure 8. TEM micrographs of (a) silica/PDBII, (b) silica/PDBIIG, and (c) silica/PDBIIG-150 nanocomposites.
Figure 9. Strain amplitude dependence of (a) G′ of unvulcanized PDBII, PDBIIG, silica/PDBII, silica/PDBIIG, and silica/PDBIIG-150; and (b) tan δ of vulcanized PDBII, PDBIIG, silica/PDBII, silica/PDBIIG, and silica/PDBIIG-150. RPA was used to investigate the effect of covalent bonding interfaces on the filler 16
ACS Paragon Plus Environment
Page 16 of 34
Page 17 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
268
network, which consists of the filler–filler network and the filler–rubber network, and the
269
interfacial interaction between silica and PDBIIG. Figure 9 shows the strain amplitude
270
dependence of the G′ of the unvulcanized compounds and the tan δ of the vulcanized
271
PDBII, PDBIIG, silica/PDBII, silica/PDBIIG, and silica/PDBIIG-150. Little difference
272
exists between PDBII and PDBIIG in the RPA results. In the filled elastomers, the
273
structure of the filler–filler networks can be reflected by the Payne effect
274
referred to as the strain dependence of G′. G′ decreases sharply when the filler–filler
275
networks are broken after the strain reaches a critical value.
276
initial G′ of the silica/PDBII compound is the highest, and the Payne effect is evident,
277
which indicates that the filler–filler networks are strong in silica/PDBII because of the
278
poor dispersion of silica. The introduction of GMA effectively reduces the Payne effect,
279
and silica/PDBIIG and silica/PDBIIG-150 are less strain-dependent than silica/PDBII,
280
thereby indicating the improved dispersion of silica. Although the shapes of the curves of
281
silica/PDBIIG and silica/PDBIIG-150 are similar with long plateau regions of G′, the G′
282
of silica/PDBIIG-150 is higher than that of silica/PDBIG. This finding can be attributed
283
to the presence of more covalent bonds between silica and PDBIIG in silica/PDBIIG-150;
284
hence, the interfacial interaction between silica and PDBIIG in silica/PDBIIG-150 is
285
stronger than that in silica/PDBIIG. The strong interfacial interaction strengthens the
286
filler–rubber networks and restrains the mobility of the macromolecular chains, which
287
leads to an increase in G′. The tan δ of the vulcanized nanocomposites is presented in 17
ACS Paragon Plus Environment
44
, which is
Figure 9(a) shows that the
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 34
288
Figure 9(b). The minimal difference is between the tan δ of silica/PDBII and
289
silica/PDBIIG at a low strain value (less than 1%). With increasing strain, the tan δ of
290
silica/PDBII increases sharply, whereas the tan δ of silica/PDBIIG increases gradually.
291
The different tendencies of tan δ with increasing strain between silica/PDBII and
292
silica/PDBIIG is attributed to the different filler network structures. The poor dispersion
293
of silica in silica/PDBII leads to strong filler–filler networks, which are easily destroyed
294
with increasing strain. The destruction of strong filler–filler networks increases filler–
295
filler friction, and the weak interfacial interaction increases filler–rubber friction
296
which leads to the high tan δ at high strain. The improved interfacial interaction and
297
dispersion of silica in silica/PDBIIG contribute to the strong filler–rubber networks and
298
few filler–filler networks. Thus, the tan δ of silica/PDBIIG is lower than that of
299
silica/PDBII at high strain. The interfacial interaction between silica and PDBIIG is
300
stronger in silica/PDBIIG-150 than in silica/PDBIIG. Hence, the filler–rubber friction in
301
silica/PDBIIG-150 is further decreased, and the value of tan δ is lower.
302
18
ACS Paragon Plus Environment
45
,
Page 19 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
303 304 305 306
Figure 10. Vulcanization curves of the PDBII, PDBIIG, silica/PDBII, silica/PDBIIG, and silica/PDBIIG-150 nanocomposites.
307
Figure 10 shows the vulcanization curves of the PDBII, PDBIIG, silica/PDBII,
308
silica/PDBIIG, and silica/PDBIIG-150 nanocomposites. The corresponding vulcanization
309
characteristics are summarized in Table S3. The minimum torque (ML) and the maximum
310
torque (MH) of the neat PDBIIG are nearly the same as those of the neat PDBII. However,
311
the curing time of PDBIIG is longer than that of PDBII. All the rubber additives and
312
operations are the same; therefore, the increase in curing time is attributed to the presence
313
of the epoxy groups, which may react with the rubber accelerators
314
their accelerating effect on vulcanization. The addition of silica evidently extends the
315
curing time. Delayed vulcanization results from the adsorption of the accelerators on the
316
silica surfaces. The curing time of silica/PDBIIG is longer than that of silica/PDBII
317
because of the probable reaction between the epoxy groups and the accelerators. The
318
curing time of silica/PDBIIG-150 is shorter than that of silica/PDBIIG. The decrease in
319
the curing time of silica/PDBIIG-150 is attributed to the additional mixing at 150 °C, 19
ACS Paragon Plus Environment
46, 47
, and thus, reduce
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
320
during which more epoxy groups in PDBIIG react with silica, such that fewer epoxy
321
groups react with the accelerators during the vulcanization process. The torque of
322
silica/PDBIIG is significantly lower than that of silica/PDBII because filler–filler
323
networks are less in silica/PDBIIG. The interfacial interaction in silica/PDBIIG-150 is
324
stronger; hence, its torque values are higher than those of silica/PDBIIG. The torque
325
difference (MH−ML) of the vulcanization curve is closely related to crosslink density. The
326
two neat elastomers exhibit similar crosslink densities. In the silica-filled nanocomposites,
327
crosslink densities increase with the increase in interfacial interaction.
328
3.3. Performance of the nanocomposites
329 330 331 332 333 334
Figure 11. Temperature dependence of (a) E′ of the PDBII, PDBIIG, silica/PDBII, silica/PDBIIG, silica/PDBIIG-150, and silica/PDBII-Si69 nanocomposites; and (b) tan δ of the PDBII, PDBIIG, silica/PDBII, silica/PDBIIG, silica/PDBIIG-150, and silica/PDBII-Si69 nanocomposites.
335
The dynamic mechanical thermal properties of the PDBII, PDBIIG, silica/PDBII,
336
silica/PDBIIG, and silica/PDBIIG-150 nanocomposites are shown in Figure 11. With the
337
exception of the slightly higher Tg and lower tan δ at Tg, minimal difference is observed 20
ACS Paragon Plus Environment
Page 20 of 34
Page 21 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
338
between the two neat elastomers in the temperature dependence of E′ and tan δ. The
339
curves change significantly after silica is added. Figure 11(a) represents the temperature
340
dependence of E′ of the PDBII, PDBIIG, silica/PDBII, silica/PDBIIG, and
341
silica/PDBIIG-150 nanocomposites. The high E′ of silica/PDBII at the rubbery region is
342
attributed to the strong filler–filler networks that result from the poor dispersion of silica.
343
The E′ of silica/PDBIIG-150 is higher than that of silica/PDBIIG because of the
344
improved interfacial interaction between silica and PDBIIG. This finding is consistent
345
with the RPA results. The temperature dependence of the tan δ of the PDBII, PDBIIG,
346
silica/PDBII, silica/PDBIIG, and silica/PDBIIG-150 nanocomposites is shown in Figure
347
11(b) and summarized in Table 2. The Tg and the highest tan δ at Tg increase significantly
348
after the introduction of GMA into PDBII. The increase in Tg is attributed to the
349
strengthened filler–rubber networks resulting from the improved dispersion of silica and
350
interfacial interaction, which confines the mobility of the polymer chains. The confined
351
mobility of the polymer chains also decreases the highest tan δ at Tg. However, the
352
improved dispersion of silica increases the rubber fraction that participates in chain
353
segment relaxation by decreasing the amount of macromolecular chains trapped in the
354
filler–filler networks 45, 48, thereby increasing the highest tan δ at Tg. In silica/PDBIIG, the
355
second factor is dominant, and the highest tan δ at Tg of silica/PDBIIG is higher than that
356
of silica/PDBII. The Tg of silica/PDBIIG-150 is nearly the same as that of silica/PDBIIG,
357
whereas the highest tan δ at Tg of silica/PDBIIG-150 is lower because of the improved 21
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
358
interfacial interaction between silica and PDBIIG in silica/PDBIIG-150. It is widely
359
accepted in tire industry that the high tan δ at 0 °C indicates good wet skid resistance, and
360
the low tan δ at 60 °C indicates low rolling resistance
361
silica/PDBIIG nanocomposite exhibits significantly better wet skid resistance and lower
362
rolling resistance than silica/PDBII. The wet skid resistance of silica/PDBIIG-150 is
363
slightly lower than that of silica/PDBIIG given the lower tan δ at Tg. Moreover, the
364
silica-filled PDBII nanocomposite which contains 5 phr of Si69 (silica/PDBII-Si69) is
365
also prepared. The Tg and tan δ values of silica/PDBII-Si69 are presented in Table 2. The
366
comparison shows that silica/PDBIIG performs better than silica/PDBII-Si69 in terms of
367
wet skid resistance and rolling resistance. It is worth mentioning that the silica/PDBIIG
368
nanocomposite exhibits excellent wet skid resistance property compared with other
369
silica-filled traditional rubber composites 42, 51-55.
370 371
49, 50
. Table 2 shows that the
Table 2 Tg and tan δ values of the silica/PDBII, silica/PDBIIG, and silica/PDBIIG-150 nanocomposites. Sample
Tg (°C) Tan δ at 0 °C Tan δ at 60 °C
Silica/PDBII
−16.5
0.553
0.155
Silica/PDBIIG
−5.3
1.035
0.123
Silica/PDBIIG-150
−5.4
0.954
0.122
Silica/PDBII-Si69
−12.4
0.546
0.152
22
ACS Paragon Plus Environment
Page 22 of 34
Page 23 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
372 373 374 375
Industrial & Engineering Chemistry Research
Figure 12. Stress–strain curves of the PDBII, PDBIIG, silica/PDBII, silica/PDBIIG, silica/PDBIIG-150, and silica/PDBII-Si69 nanocomposites.
376
The stress–strain curves of PDBII, PDBIIG, silica/PDBII, silica/PDBIIG,
377
silica/PDBIIG-150, and silica/PDBII-Si69 are displayed in Figure 12 and summarized in
378
Table S4. The mechanical properties of the neat PDBII and PDBIIG are similar and poor,
379
and the addition of silica significantly improves the mechanical properties of PDBII and
380
PDBIIG. Moreover, silica/PDBIIG exhibits better mechanical properties than
381
silica/PDBII because of the strong interfacial interaction and the good dispersion of silica.
382
With the same silica loading and procedure, the inclusion of 3.7 wt.% GMA increases the
383
modulus at 100% strain by 150% and the modulus at 300% strain by 152.3%. The low
384
elongation at break of silica/PDBIIG results from the strong interfacial interaction
385
because the slippage of the polymer chains is restricted. The interfacial interaction of
386
silica/PDBIIG-150 is stronger than that of silica/PDBIIG. Thus, the elongation at break of
387
silica/PDBIIG-150 is lower and the modulus of silica/PDBIIG-150 is higher. The 23
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
388
mechanical properties of silica/PDBII-Si69 were also measured. Silica/PDBIIG performs
389
better than silica/PDBII-Si69 in modulus at 100% strain. However, the tensile strength of
390
silica/PDBIIG is slightly lower compared with other traditional rubber composites 31, 42, 48,
391
51-55
.
392 393
4. Conclusions
394
Epoxy group-functionalized bio-based elastomer PDBIIG was synthesized via
395
free-radical redox emulsion polymerization, and silica/PDBIIG nanocomposite was
396
prepared without the addition of silane coupling agents. The dispersion of silica in the
397
elastomer matrix and the interfacial interaction between silica and the elastomer was
398
improved significantly after the introduction of epoxy groups into PDBII. The
399
improvements were attributed to the ring-opening reaction between the hydroxyl groups
400
of silica and the epoxy groups of PDBIIG. Heat treatment at 150 °C facilitated the
401
ring-opening reaction, which further improved the interfacial interaction between silica
402
and PDBIIG. Silica/PDBIIG demonstrated better wet skid resistance, lower rolling
403
resistance, and better mechanical properties than silica/PDBII because of the strong
404
covalent bonding interfacial interaction and the uniform dispersion of silica. Moreover,
405
silica/PDBIIG performed better than silica/PDBII-Si69 in dynamic and static mechanical
406
properties. Silica/PDBIIG nanocomposite may have great potential in tire application
407
after our effort to further improve its comprehensive properties in the future. 24
ACS Paragon Plus Environment
Page 24 of 34
Page 25 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
408
ASSOCIATED CONTENT
409
Supporting Information
410
The Supporting Information is available free of charge on the ACS Publications website
411
at DOI:
412
Formulation for the emulsion polymerization of PDBII and PDBIIG. Formulation for the
413
silica/PDBII and silica/PDBIIG nanocomposites. Vulcanization characteristics of the
414
PDBII, PDBIIG, silica/PDBII, silica/PDBIIG, and silica/PDBIIG-150 nanocomposites.
415
Mechanical
416
silica/PDBIIG-150, and silica/PDBII-Si69 nanocomposites (PDF)
417
AUTHOR INFORMATION
418
Corresponding Author
419
*
420
Wang)
421
Author Contributions
422
The manuscript was written through contributions of all authors. All authors have given
423
approval to the final version of the manuscript.
424
Funding Sources
425
This work was supported by the National Natural Science Foundation of China
426
(50933001 and 51221002), the Key Program of Beijing Municipal Science and
properties
of
the
PDBII,
PDBIIG,
silica/PDBII,
silica/PDBIIG,
E-mail:
[email protected] (Liqun Zhang),
[email protected] (Runguo
25
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 26 of 34
427
Technology Commission (D14110300230000), and the Joint Development Project of
428
Beijing Municipal Education Commission (JWGJ201602).
429
References
430
(1) Ragauskas, A. J.; Williams, C. K.; Davison, B. H.; Britovsek, G.; Cairney, J.; Eckert,
431
C. A.; Frederick, W. J.; Hallett, J. P.; Leak, D. J.; Liotta, C. L. The path forward for
432
biofuels and biomaterials. Science 2006, 311, 484-489.
433
(2) Hermann, B.; Blok, K.; Patel, M. K. Producing bio-based bulk chemicals using
434
industrial biotechnology saves energy and combats climate change. Environ. Sci. Technol.
435
2007, 41, 7915-7921.
436
(3) Gandini, A. Polymers from renewable resources: a challenge for the future of
437
macromolecular materials. Macromolecules 2008, 41, 9491-9504.
438
(4) Van Beilen, J. B.; Poirier, Y. Establishment of new crops for the production of natural
439
rubber. Trends Biotechnol. 2007, 25, 522-529.
440
(5) Wang, R.; Zhang, J.; Kang, H.; Zhang, L. Design, preparation and properties of
441
bio-based elastomer composites aiming at engineering applications. Compos. Sci. Technol.
442
2016, 133, 136-156.
443
(6) Wu,
444
poly(glycerol-sebacate-citrate)
445
adjustable degradability, and better biocompatibility. J. Appl. Polym. Sci. 2012, 123,
446
1612-1620.
Y.;
Shi,
R.;
Chen,
D.;
Zhang,
elastomers
with
L.;
Tian,
improved
26
ACS Paragon Plus Environment
W.
Nanosilica
mechanical
filled
properties,
Page 27 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
447
(7) Wei, T.; Lei, L.; Kang, H.; Qiao, B.; Wang, Z.; Zhang, L.; Coates, P.; Hua, K.-C.;
448
Kulig, J. Tough Bio-Based Elastomer Nanocomposites with High Performance for
449
Engineering Applications. Adv. Eng. Mater. 2012, 14, 112-118.
450
(8) Lei, L.; Li, L.; Zhang, L.; Chen, D.; Tian, W. Structure and performance of
451
nano-hydroxyapatite
452
elastomers. Polym. Degrad. Stab. 2009, 94, 1494-1502.
453
(9) Kang, H.; Li, X.; Xue, J.; Zhang, L.; Liu, L.; Xu, R.; Guo, B. Preparation and
454
characterization of high strength and noncytotoxic bioelastomers containing isosorbide.
455
RSC Adv. 2014, 4, 19462-19471.
456
(10) Hu, X.; Kang, H.; Li, Y.; Li, M.; Wang, R.; Xu, R.; Qiao, H.; Zhang, L. Direct
457
copolycondensation of biobased elastomers based on lactic acid with tunable and
458
versatile properties. Polym. Chem. 2015, 6, 8112-8123.
459
(11) Wang, R. G.; Ma, J.; Zhou, X. X.; Wang, Z.; Kang, H. L.; Zhang, L. Q.; Hua, K. C.;
460
Kulig, J. Design and Preparation of a Novel Cross-Linkable, High Molecular Weight, and
461
Bio-Based Elastomer by Emulsion Polymerization. Macromolecules 2012, 45,
462
6830-6839.
463
(12) Qiao, H.; Wang, R.; Yao, H.; Wu, X.; Lei, W.; Zhou, X.; Hu, X.; Zhang, L. Design
464
and preparation of natural layered silicate/bio-based elastomer nanocomposites with
465
improved dispersion and interfacial interaction. Polymer 2015, 79, 1-11.
466
(13) Zhou, X.; Wang, R.; Lei, W.; Qiao, H.; Ji, H.; Zhang, L.; Hua, K.-C.; Kulig, J.
filled
biodegradable
poly((1,2-propanediol-sebacate)-citrate)
27
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
467
Design and synthesis by redox polymerization of a bio-based carboxylic elastomer for
468
green tire. Sci. China: Chem. 2015, 58, 1561-1569.
469
(14) Qiao, H.; Wang, R.; Yao, H.; Zhou, X.; Lei, W.; Hu, X.; Zhang, L. Preparation of
470
graphene oxide/bio-based elastomer nanocomposites through polymer design and
471
interface tailoring. Polym. Chem. 2015, 6, 6140-6151.
472
(15) Lei, W.; Zhou, X.; Russell, T. P.; Hua, K.-c.; Yang, X.; Qiao, H.; Wang, W.; Li, F.;
473
Wang, R.; Zhang, L. High performance bio-based elastomers: energy efficient and
474
sustainable materials for tires. J. Mater. Chem. A 2016, 4, 13058-13062.
475
(16) Lei, W.; Wang, R.; Yang, D.; Hou, G.; Zhou, X.; Qiao, H.; Wang, W.; Tian, M.;
476
Zhang, L. Design and preparation of bio-based dielectric elastomer with polar and
477
plasticized side chains. RSC Adv. 2015, 5, 47429-47438.
478
(17) Satoh, K.; Lee, D. H.; Nagai, K.; Kamigaito, M. Precision Synthesis of Bio‐Based
479
Acrylic Thermoplastic Elastomer by RAFT Polymerization of Itaconic Acid Derivatives.
480
Macromol. Rapid Commun. 2014, 35, 161-167.
481
(18) Wang, W.; Ping, P.; Yu, H.; Chen, X.; Jing, X. Synthesis and characterization of a
482
novel biodegradable, thermoplastic polyurethane elastomer. J. Polym. Sci., Part A:
483
Polym. Chem. 2006, 44, 5505-5512.
484
(19) Skarja, G. A.; Woodhouse, K. A. Structure-property relationships of degradable
485
polyurethane elastomers containing an amino acid-based chain extender. J. Appl. Polym.
486
Sci. 2000, 75, 1522-1534. 28
ACS Paragon Plus Environment
Page 28 of 34
Page 29 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
487
(20) Petrović, Z. S. Polyurethanes from Vegetable Oils. Polym. Rev. 2008, 48, 109-155.
488
(21) Hojabri, L.; Kong, X.; Narine, S. S. Novel long chain unsaturated diisocyanate from
489
fatty acid: Synthesis, characterization, and application in bio-based polyurethane. J.
490
Polym. Sci., Part A: Polym. Chem. 2010, 48, 3302-3310.
491
(22) Whited, G. M.; Feher, F. J.; Benko, D. A.; Cervin, M. A.; Chotani, G. K.; McAuliffe,
492
J. C.; LaDuca, R. J.; Ben-Shoshan, E. A.; Sanford, K. J. Technology update:
493
Development of a gas-phase bioprocess for isoprene-monomer production using
494
metabolic pathway engineering. Ind. Biotechnol. 2010, 6, 152-163.
495
(23) Willke, T.; Vorlop, K. D. Biotechnological production of itaconic acid. Appl.
496
Microbiol. Biotechnol. 2001, 56, 289-295.
497
(24) Okabe, M.; Lies, D.; Kanamasa, S.; Park, E. Y. Biotechnological production of
498
itaconic acid and its biosynthesis in Aspergillus terreus. Appl. Microbiol. Biotechnol.
499
2009, 84, 597-606.
500
(25) Morais, A. R.; Dworakowska, S.; Reis, A.; Gouveia, L.; Matos, C. T.; Bogdał, D.;
501
Bogel-Łukasik, R. Chemical and biological-based isoprene production: Green metrics.
502
Catal. Today 2015, 239, 38-43.
503
(26) Bokobza, L. The reinforcement of elastomeric networks by fillers. Macromol. Mater.
504
Eng. 2004, 289, 607-621.
505
(27) Wang, Z.; Liu, J.; Wu, S.; Wang, W.; Zhang, L. Novel percolation phenomena and
506
mechanism of strengthening elastomers by nanofillers. Phys. Chem. Chem. Phys. 2010, 29
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
507
12, 3014-3030.
508
(28) Mouri, H.; Akutagawa, K. Improved tire wet traction through the use of mineral
509
fillers. Rubber Chem. Technol. 1999, 72, 960-968.
510
(29) Job, K. Trends in green tire manufacturing. Rubber World 2014, 249, 32-38.
511
(30) Yatsuyanagi, F.; Suzuki, N.; Ito, M.; Kaidou, H. Effects of secondary structure of
512
fillers on the mechanical properties of silica filled rubber systems. Polymer 2001, 42,
513
9523-9529.
514
(31) Gui, Y.; Zheng, J.; Ye, X.; Han, D.; Xi, M.; Zhang, L. Preparation and performance
515
of silica/SBR masterbatches with high silica loading by latex compounding method.
516
Composites Part B 2016, 85, 130-139.
517
(32) Reuvekamp, L.; Ten Brinke, J.; Van Swaaij, P.; Noordermeer, J. Effects of time and
518
temperature on the reaction of TESPT silane coupling agent during mixing with silica
519
filler and tire rubber. Rubber Chem. Technol. 2002, 75, 187-198.
520
(33) Ten Brinke, J.; Debnath, S.; Reuvekamp, L.; Noordermeer, J. Mechanistic aspects of
521
the role of coupling agents in silica–rubber composites. Compos. Sci. Technol. 2003, 63,
522
1165-1174.
523
(34) Park, S.-J.; Cho, K.-S. Filler–elastomer interactions: influence of silane coupling
524
agent on crosslink density and thermal stability of silica/rubber composites. J. Colloid
525
Interface Sci. 2003, 267, 86-91.
526
(35) Goerl, U.; Hunsche, A.; Mueller, A.; Koban, H. Investigations into the silica/silane 30
ACS Paragon Plus Environment
Page 30 of 34
Page 31 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
527
reaction system. Rubber Chem. Technol. 1997, 70, 608-623.
528
(36) Cataldo, F. Preparation of silica‐based rubber compounds without the use of a silane
529
coupling agent through the use of epoxidized natural rubber. Macromol. Mater. Eng. 2002,
530
287, 348-352.
531
(37) Xu, T.; Jia, Z.; Luo, Y.; Jia, D.; Peng, Z. Interfacial interaction between the
532
epoxidized natural rubber and silica in natural rubber/silica composites. Appl. Surf. Sci.
533
2015, 328, 306-313.
534
(38) Kaewsakul, W.; Sahakaro, K.; Dierkes, W.; Noordermeer, J. Verification of
535
Interactions between Silica and Epoxidized Squalene as a Model for Epoxidized Natural
536
Rubber. J. Rubber Res. 2014, 17, 129-142.
537
(39) Varughese, S.; Tripathy, D. K. Chemical interaction between epoxidized natural
538
rubber and silica: Studies on cure characteristics and low-temperature dynamic
539
mechanical properties. J. Appl. Polym. Sci. 1992, 44, 1847-1852.
540
(40) Sengloyluan, K.; Sahakaro, K.; Dierkes, W. K.; Noordermeer, J. W. M.
541
Silica-reinforced tire tread compounds compatibilized by using epoxidized natural rubber.
542
Eur. Polym. J. 2014, 51, 69-79.
543
(41) Ragosta, G.; Abbate, M.; Musto, P.; Scarinzi, G.; Mascia, L. Epoxy-silica particulate
544
nanocomposites: Chemical interactions, reinforcement and fracture toughness. Polymer
545
2005, 46, 10506-10516.
546
(42) Qu, L.; Yu, G.; Xie, X.; Wang, L.; Li, J.; Zhao, Q. Effect of silane coupling agent on 31
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
547
filler and rubber interaction of silica reinforced solution styrene butadiene rubber. Polym.
548
Compos. 2013, 34, 1575-1582.
549
(43) Choi, S.-S. Influence of storage time and temperature and silane coupling agent on
550
bound rubber formation in filled styrene–butadiene rubber compounds. Polym. Test. 2002,
551
21, 201-208.
552
(44) Payne, A. R. The dynamic properties of carbon black‐loaded natural rubber
553
vulcanizates. Part I. J. Appl. Polym. Sci. 1962, 6, 57-63.
554
(45) Wu, Y. P.; Zhao, Q. S.; Zhao, S. H.; Zhang, L. Q. The influence of in situ
555
modification of silica on filler network and dynamic mechanical properties of silica‐
556
filled solution styrene–butadiene rubber. J. Appl. Polym. Sci. 2008, 108, 112-118.
557
(46) Martin, P. J.; Brown, P.; Chapman, A. V.; Cook, S. Silica-reinforced epoxidized
558
natural rubber tire treads-performance and durability. Rubber Chem. Technol. 2015, 88,
559
390-411.
560
(47) Gelling, I. R.; Morrison, N. J. Sulfur Vulcanization and Oxidative Aging of
561
Epoxidized Natural Rubber. Rubber Chem. Technol. 1985, 58, 243-257.
562
(48) Li, Y.; Han, B.; Wen, S.; Lu, Y.; Yang, H.; Zhang, L.; Liu, L. Effect of the
563
temperature on surface modification of silica and properties of modified silica filled
564
rubber composites. Composites. Part A 2014, 62, 52-59.
565
(49) Wang, M.-J. Effect of polymer-filler and filler-filler interactions on dynamic
566
properties of filled vulcanizates. Rubber Chem. Technol. 1998, 71, 520-589. 32
ACS Paragon Plus Environment
Page 32 of 34
Page 33 of 34
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
567
(50) Takino, H.; Nakayama, R.; Yamada, Y.; Kohjiya, S.; Matsuo, T. Viscoelastic
568
properties of elastomers and tire wet skid resistance. Rubber Chem. Technol. 1997, 70,
569
584-594.
570
(51) Yan, H.; Tian, G.; Sun, K.; Zhang, Y.; Zhang, Y. Effect of silane coupling agent on
571
the polymer-filler interaction and mechanical properties of silica-filled NR. J. Polym. Sci.
572
Part B: Polym. Phys. 2005, 43, 573-584.
573
(52) Kim, K.; Lee, J.-Y.; Choi, B.-J.; Seo, B.; Kwag, G.-H.; Paik, H.-J.; Kim, W.
574
Styrene-butadiene-glycidyl methacrylate terpolymer/silica composites: dispersion of
575
silica particles and dynamic mechanical properties. Compos. Interfaces 2014, 21,
576
685-702.
577
(53) Kaewsakul, W.; Sahakaro, K.; Dierkes, W. K.; Noordermeer, J. W. M. Optimization
578
of mixing conditions for silica-reinforced natural rubber tire tread compounds. Rubber
579
Chem. Technol. 2012, 85, 277-294.
580
(54) Feng, W.; Tang, Z.; Weng, P.; Guo, B. Correlation of filler networking with
581
reinforcement and dynamic properties of ssbr/carbon black/silica composites. Rubber
582
Chem. Technol. 2015, 88, 676-689.
583
(55) Choi, S.-S.; Nah, C.; Jo, B.-W. Properties of natural rubber composites reinforced
584
with silica or carbon black: influence of cure accelerator content and filler dispersion.
585
Polym. Int. 2003, 52, 1382-1389.
586 587 33
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
588
Table of content
589 590
34
ACS Paragon Plus Environment
Page 34 of 34