Structural Evolution of LixNiyMnzCo1-y-zO2 ... - ACS Publications

Nov 8, 2017 - (LIBs) for small and portable devices, their demand for larger scale applications (such as electric .... for recovering the charge-induc...
6 downloads 14 Views 2MB Size
Subscriber access provided by University of Florida | Smathers Libraries

Letter

Structural Evolution of LixNiyMnzCo1-y-zO2 Cathode Materials During High-Rate Charge and Discharge Sooyeon Hwang, Eunmi Jo, Kyung Yoon Chung, Kyo Seon Hwang, Seung Min Kim, and Wonyoung Chang J. Phys. Chem. Lett., Just Accepted Manuscript • DOI: 10.1021/acs.jpclett.7b02579 • Publication Date (Web): 08 Nov 2017 Downloaded from http://pubs.acs.org on November 9, 2017

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

The Journal of Physical Chemistry Letters is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry Letters

1

Structural Evolution of LixNiyMnzCo1-y-zO2 Cathode

2

Materials during High-Rate Charge and Discharge

3

Sooyeon Hwang1,2, Eunmi Jo1, Kyung Yoon Chung1, Kyo Seon Hwang3, Seung Min Kim4,*,

4

Wonyoung Chang1,*

5

1

Center for Energy Convergence, Korea Institute of Science and Technology (KIST), Seoul

6 7

02792, Republic of Korea 2

Center for Functional Nanomaterials, Brookhaven National Laboratory, Upton, New York

8 9

11973, United States 3

Department of Clinical Pharmacology and Therapeutics, College of Medicine, Kyung Hee

10 11

University, Seoul 02447, Republic of Korea 4

Carbon Composite Materials Research Centre, Institute of Advanced Composite Materials,

12

KIST, Wanju-gun 55324, Republic of Korea

13

AUTHOR INFORMATION

14

Corresponding Author

15

*S. M. Kim ([email protected]) *W. Chang ([email protected])

16

ACS Paragon Plus Environment

1

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 22

1

Ni-rich lithium transition metal oxides have received significant attention due to their high

2

capacities and rate capabilities determined via theoretical calculations. Although the structural

3

properties of these materials are strongly correlated with the electrochemical performance, their

4

structural stability during the high-rate electrochemical reactions has not been fully evaluated

5

yet. In this work, transmission electron microscopy is used to investigate the crystallographic and

6

electronic structural modifications of Ni-based cathode materials at a high charge/discharge rate

7

of 10 C. It is found that the high-rate electrochemical reactions induce structural inhomogeneity

8

near the surface of Ni-rich cathode materials, which limits Li transport and reduces their

9

capacities. This study establishes a correlation between the high-rate electrochemical

10

performance of the Ni-based materials and their structural evolution, which can provide

11

profound insights for designing novel cathode materials having both high energy and power

12

densities.

13 14

TOC GRAPHICS

15 16

KEYWORDS lithium ion batteries, high rate, cathode, structural evolution, transmission

17

electron microscopy

ACS Paragon Plus Environment

2

Page 3 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry Letters

1

After the successful utilization of lithium ion batteries (LIBs) for small and portable devices,

2

their demand for larger scale applications (such as electric vehicles and smart grids) has been

3

steadily increasing.1,2 In particular, the use of LIBs in electric vehicles requires both high energy

4

density and power density, which would enable prolonged driving on a single battery charge,

5

sufficient acceleration, and relatively short charging times. High energy density can be achieved

6

by increasing the capacity of each battery cell or widening the operating voltage range. Since the

7

power density of LIBs is related to their ability to charge and discharge quickly, the transport of

8

Li ions and electrons during the electrochemical process should be fast enough for reaching a

9

satisfactory level of power density. Thus, to incorporate LIBs into electric vehicles, electrode

10

materials with both high energy density and Li ion diffusivity must be developed.

11

To improve the figure of merits of cathode materials, lithium transition metal oxides (described

12

by the formula LiTMO2, where TM is a transition metal such as Mn, Co, or Ni) with a layered

13

structure (space group R 3ത m) have received significant attention. During the extraction or

14

insertion of lithium ions from/into cathode materials, TMs are participating the redox for charge

15

neutrality; thus, controlling the TM content of LiTMO2 is critical for the optimization of their

16

properties. Generally, Ni incorporation can be used to increase the capacity by modifying the

17

electronic structure.3-5 In addition, the activation barrier of the Li-ion movement near Ni2+ or

18

Ni3+ ions is lower than that near Co3+ or Mn4+ ions;6-8 hence, Li transport is facilitated in the Ni-

19

rich environment. However, it is well known that Ni-rich cathode materials exhibit significant

20

structural instability and related safety issues.3-5,9-12 Nevertheless, Ni-rich LiTMO2 compounds

21

still remain highly promising cathode materials with potentially high energy density and power

22

density, which can be realized by improving their structural stability during electrochemical

ACS Paragon Plus Environment

3

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 22

1

processes. For this purpose, a detailed analysis of the structural evolution of Ni-rich LiTMO2

2

materials must be performed particularly at high-rates.

3

In this work, various transmission electron microscopy (TEM) techniques were used to

4

investigate the structural modification of Ni-based cathode materials (LiNi0.8Mn0.1Co0.1O2 and

5

LiNi0.4Mn0.3Co0.3O2, which are further referred to as NMC811 and NMC433, respectively) after

6

the charge and discharge processes conducted at a high rate of 10 C. In previous studies, the

7

reversibility of the structural modifications of NMC cathode materials was observed at a

8

moderate charge/discharge rate of 0.1 C;13 however, the structural changes of cathode materials

9

at high currents have not been investigated in sufficient detail. Yang et al. reported the formation

10

of an intermediate phase and structural modifications of Li1−xNi1/3Co1/3Mn1/3O2 after charging at

11

various rates ranging from 0.1 C to 60 C.14 In the real batteries, the discharge process is also

12

important for their successful operation; thereby, structural analysis must be performed both after

13

the charge and discharge steps. Here, by examining the changes in the crystallographic and

14

electronic structures of NMC433 and NMC811 materials observed both in the bulk and on their

15

surfaces at high charge/discharge rates, it is possible to determine the mechanism of their

16

structural modifications induced by electrochemical reactions, which can be subsequently used

17

for designing novel cathode materials for high-power applications.

18

The structural evolutions of NMC433 and NMC811 materials induced by their charge at a high

19

rate of 10 C are investigated by acquiring selected area electron diffraction (SAED) patterns for

20

five different particles (see Figure S1 in the Supporting Information section). We set a cutoff

21

voltage of 4.8 V to investigate the structural modification at a highly delithiated state. Because of

22

the high potential increase induced by a high charging rate at the beginning of the charging

23

process (see Figure S2 in Supporting Information), it was practically difficult to set a cutoff

ACS Paragon Plus Environment

4

Page 5 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry Letters

1

voltage below 4.5 V, especially for NMC811. High-rate electrochemical testing may lead to

2

inhomogeneous distribution of charges inside the active particles; thus, we specify the area of

3

interest as the bulk (the inside area) and the near surface (the outer area) with a selected area

4

aperture (size of 160 nm). The charge profiles of the studied NMC433 and NMC811 samples are

5

shown in Figure S2 of the Supporting Information section. Figures 1a and b show the SAED

6

patterns and electron energy loss spectra (EELS) of the representative samples obtained for each

7

composition. Despite the initial charge to the cutoff voltage of 4.8 V, the charging process with a

8

high current results in the modifications of the crystalline and electronic structures of NMC811

9

even at the bulk area. EELS, which demonstrates the unoccupied density of states,15 is employed

10

to characterize the chemical state of NMC cathode materials. Pre-edge of oxygen K-edge (~530

11

eV) is sensitive to the oxidation state of binding transition metals: it moves to higher energy loss

12

when the metal is reduced, and vice versa.13 Transition metal L2,3 edge itself also changes with

13

valence: the onset energy shifts to lower energy loss, and L3/L2 intensity ratio becomes higher

14

when the metal ion is reduced.13,16 Near the surface of NMC811, the SAED is similar to that

15

acquired in the bulk area, but we could notice a significant change in EELS, particularly for the

16

O K-edge, indicating a considerable reduction in transition metals and formation of the rocksalt

17

phase. More Detailed explanations are available at elsewhere.17 The presence of the diffraction

18

spots originated from the spinel structure indicates that structural modifications also occur near

19

the NMC433 surface. (See Figure S3 in the Supporting Information for detailed indexing of

20

SAEDs) Figure 1c summarizes the structural evolution observed at NMC433 and NMC811

21

particles after their initial high-rate charge to 4.8 V. To see the trend for structural changes after

22

electrochemical lithium extraction, information acquired from five different particles are

23

summarized in the Venn diagram in Figure 1c. Each box represents layered, spinel, and rocksalt

ACS Paragon Plus Environment

5

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 6 of 22

1

structures after charge, and the overlapped areas indicate mixed phases. Considering the phase

2

transformation takes place from the original layered R 3ത m structure to a disordered spinel

3

structure and eventually to the rock-salt structure, more severe structural modifications are

4

observed near the NMC811 surface as compared to those of NMC433 and in the bulk region.

5

Therefore, the high-rate initial charge leads to a structural evolution of NMC cathode materials,

6

and their degree of deformation depends on the TM composition. It is interesting to note that the

7

charge capacity of NMC811 is much smaller than that of NMC433 at high charging rates, despite

8

the well-known ability of Ni-rich compounds to exhibit relatively high capacities.

9

Since the operation of LIBs is based on the insertion and removal of lithium ions between the

10

cathode and the anode, structural changes of electrode materials observed during the discharge

11

process are as important as those detected during charging. To investigate the structural changes

12

that occur during the high-rate (10 C) discharge, the coin cells with NMC cathodes were first

13

charged to 4.3 V or 4.8 V at a rate of 0.1 C, then discharged at a 100 times higher current down

14

to 2.0 V. Structural issues of cathode materials under normal and abused conditions are of

15

practical importance; hence, we employed two different charged states of 4.3 V (maximum

16

normal operating potential) and 4.8 V (abused condition) for subsequence discharging

17

experiments down to 2.0 V. Figure S4 in the Supporting Information section displays the charge

18

and discharge curves obtained for the NMC433 and NMC811 cathode materials. Similar to the

19

charge capacity (Figure S2), the discharge capacity of NMC811 from the charged state to 4.8 V

20

is far lower than that of NMC433 measured at a high discharge rate of 10 C. Although the

21

NMC811 delivers higher capacity during a charge to 4.3 V than NMC433, discharge capacities

22

of these materials from the charged state to 4.3 V are comparable, indicating inferior rate

23

capability of NMC811 compared to NMC433. The SAED patterns acquired for the bulk and near

ACS Paragon Plus Environment

6

Page 7 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry Letters

1

surface areas of the five particles with different compositions are presented in Figures S5 and S6

2

of the Supporting Information section. Figures 2a and b display typical SAED patterns and EELS

3

of the NMC433 and NMC811 samples obtained after their high-rate discharge from 4.8 V. The

4

SAED patterns and EELS indicate that the near surface of NMC433 and both bulk and near

5

surface of NMC811 have mixed layered and spinel structures. The contribution of the spinel

6

structure to the near surface region is greater than that to the bulk region regardless of the TM

7

composition. In our previous work, it was demonstrated that partial phase transformations could

8

occur near the surfaces of NMC433 and NMC811 even after the initial charge to 4.8 V at a rate

9

of 0.1 C; however, the lithium insertion to the structures of these materials conducted at a slow

10

rate of 0.1 C can recover these structural deformations both in the bulk and near the surface

11

area.13 Thus, in contrast to the low or moderate discharge rates, high discharge rates are

12

unfavorable for recovering the charge-induced structural inhomogeneity. Figures 2c, d

13

summarize all the SAED patterns obtained for the NMC433 and NMC811 samples at a high

14

discharge rate in the Venn diagram, indicating that the inhomogeneity of their crystalline

15

structures still exists after the lithiation process regardless of the cut-off voltage. In addition, the

16

most significant particle-to-particle variations are observed near the surface of NMC811 where

17

the most severe structural changes occur during the delithiation process.

18

The structural and chemical modifications of the NMC433 and NMC811 surfaces after the

19

high-rate discharge were further investigated via high-resolution electron microscopy (HREM)

20

and scanning transmission electron microscopy (STEM)-EELS. Figure 3 shows the HREM

21

images and fast Fourier transform (FFT) results obtained for their selected regions and the

22

changes in the L3/L2 intensity ratios of the Ni, Co, and Mn L2,3 edges along the scanning paths of

23

NMC433 and NMC811 after the high-rate discharge from the charged state to 4.8 V. In the case

ACS Paragon Plus Environment

7

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 22

1

of NMC811 compound, the L2,3 Mn and Co edges cannot be clearly distinguished in the inner

2

particle regions because of high sample thickness and relatively small contents of Mn and Co

3

elements; thus, the L3/L2 ratios of Mn and Co are partially plotted in Figure 3b. The

4

corresponding raw EELS containing the Ni, Co, and Mn L2,3 edges are presented in Figure S7 of

5

the Supporting Information section. The L2,3 edge features of TMs such as the L3/L2 intensity

6

ratio are sensitive to their oxidation states;18,19 thus, in this work, the L3/L2 intensity ratio was

7

utilized to track the changes in the TM chemical state along the scanning route. Previously, it

8

was found that the L3/L2 ratios of the L2,3 edges of Ni, Mn, and Co increased during reduction

9

and decreased during oxidation.20-23 The HREM images and corresponding FFT results shown in

10

Figure 3 demonstrate that both the NMC433 and NMC811 samples undergo structural

11

transformations, leading to the formation of the spinel and rock-salt structures on their surfaces.

12

In particular, the presence of the rock-salt structure indicates that more severe phase

13

transformations occur at the edge of the NMC433 and NMC811 specimens rather than near their

14

surfaces, as indicated by the SAED patterns depicted in Figures 2, S5, and S6. These structural

15

modifications observed at a couple of tens of nanometers from the sample edge become

16

irreversible after a high-rate discharge. Since the phase transformations from the layered

17

structure to the spinel and rock-salt structures are accompanied by the reduction of TMs inside

18

the studied materials,13,24 the variations of the L3/L2 intensity ratio were also examined. During

19

the electron probe scanning from the edge to the inner area of the particles along a line, the

20

changes in the L3/L2 ratio become more distinct: a higher white line ratio of Mn on the NMC433

21

surface but higher L3/L2 ratio of Ni in the NMC811. The EELS results demonstrate that the

22

reduction of Mn ions is the main reason for local structural modifications of NMC433, while the

23

reduction of Ni ions drives the phase transformations on the NMC811 surface. It is interesting to

ACS Paragon Plus Environment

8

Page 9 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry Letters

1

note that in our previous work, 20 charge and discharge cycles performed at a rate 0.1 C induced

2

similar chemical evolutions corresponding to Mn and Ni reduction on the surfaces of NMC433

3

and NMC811, respectively.25 Therefore, it can be assumed that the mechanism of the surface

4

degradation at a high rate of 10 C is similar to that observed at a moderate rate of 0.1 C;

5

however, the high-rate discharge does not allow the surface of NMC cathode materials to recover

6

from structural and chemical modifications due to insufficient time, which results in more severe

7

structural degradation even after the first discharge process.

8

A comparison of the SAED patterns and EELS spectra recorded for the NMC cathode

9

materials after the charge and discharge processes (Reference 13, Figures 2, 3) shows that the

10

structural deformations induced by charging at various rates and cut-off voltages are usually

11

recovered during discharge. However, it is noteworthy that the high-rate discharge can also

12

induce partial structural variations of NMC811 particles. Figure 4 shows the SAED patterns of

13

the NMC811 particles obtained after high-rate discharge (they are marked with the symbols +

14

and # in Figure 2d). For these particles, the contribution of the diffraction intensity from the

15

spinel structure to the SAED patterns (indicated by white arrows in Figure 4) is much stronger in

16

the bulk area than near the surface region (regardless of the cut-off voltage). These SAED

17

patterns indicate that the original layered structure of NMC811 is partially recovered during the

18

high-rate discharge only in the areas close to the specimen edges while the transformed spinel

19

structure is retained in the bulk. Thus, it is possible that the discharge of some NMC811 samples

20

which a high current can be an additional factor contributing to their local structural evolution.

21

Pan et al. calculated the diffusion coefficients of NMC cathode materials via ab initio

22

simulations, which showed that the Li-ion diffusion coefficient generally tended to increase with

23

the Ni content.7 The diffusivity of Li species also strongly depends on the size of the Li layer

ACS Paragon Plus Environment

9

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 10 of 22

1

along the c-axis since the larger space reduces the activation energy of Li movement.6 Cation

2

mixing in a layered structure significantly reduces the Li slab opening, which limits Li-ion

3

diffusion. Since further Li/TM mixing causes phase transitions from the layered to the spinel and

4

even rock-salt structures, local phase transformations may considerably degrade the kinetic

5

properties of NMC materials. Ni-rich cathode materials (such as NMC811) may be inherently

6

favorable for fast lithium diffusion; however, a significant degree of cation mixing and the

7

subsequent phase transformations limit their lithium ion diffusivity. During the high-rate

8

discharge, the presence of spinel and rock-salt structures near the surface may impede the

9

diffusion of lithium ions to the particle bulk, resulting in only partial structural recovery of the

10

NMC811 surface. In addition, since it is hard for lithium ions to reach the bulk of active

11

materials, only a fraction of the NMC811 sample can participate in electrochemical reactions,

12

resulting in a considerable capacity loss during the high-rate discharge. Meanwhile, the cathode

13

materials with smaller Ni contents (such as NMC433) may originally exhibit lower Li ion bulk

14

diffusivity; however, their better structural stability ensures Li movement to the bulk area even at

15

high discharge rates, thus preventing additional local structural evolution and capacity loss. The

16

larger potential drop in the beginning of the high-rate discharge process observed for NMC811

17

material (as compared to that of NMC433) in Figure S4 of the Supporting Information section

18

results from its higher resistance, which is most likely caused by the structural transition during

19

the initial charge process.

20

In this work, we demonstrate that the high-rate charge-discharge performance of NMC811 is

21

inferior to that of NMC433: the high-rate charge and discharge capacities of NMC811 are much

22

lower than those measured at moderate rates, owing to the severe structural inhomogeneity. It

23

can be concluded that the structural imperfectness and instability of NMC811 observed during

ACS Paragon Plus Environment

10

Page 11 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry Letters

1

electrochemical reactions at high charge/discharge rates are the origin of the discrepancy

2

between the theoretical and experimental results. This study also reveals that the structural

3

degradation of Ni-rich cathode materials observed during the high-rate electrochemical processes

4

is mainly caused by the reduction of Ni ions, while the degradation of Mn-rich materials (with a

5

smaller Ni content) is caused by the reduction of Mn ions. In addition, slower Li diffusion inside

6

NMC811 due to the severe structural degradation during the high-rate discharge may lead to a

7

lower degree of structural recovery in the bulk area as compared to that near the material surface.

8

Therefore, the development of various methods for preventing surface phase transformations and

9

reducing the electrode resistance must be conducted to achieve both the high energy density and

10

power density of Ni-rich cathode materials.

ACS Paragon Plus Environment

11

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

1

Page 12 of 22

FIGURES

2 3

Figure 1. Bright field image, SAEDs and EELS of (a) NMC433 and (b) NMC811 after charging

4

to 4.8V at a rate of 10C. Circles with the dotted line denote the contribution from the spinel

5

structure in case of mixed phase. (c) Summary of structural evolutions of five different NMC

6

particles after high-rate charge to 4.8V.

ACS Paragon Plus Environment

12

Page 13 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry Letters

1 2

Figure 2. Bright field image, SAEDs and EELS of (a) NMC433 and (b) NMC811 after a

3

discharge at a rate of 10C from 4.8 V. Circles with the dotted line denotes the contribution from

4

the spinel structure in case of mixed phase. Summary of structural evolutions of five different (c)

5

NMC433 and (d) NMC811 particles after high-rate discharge from 4.3V or 4.8V to 2V. Signs of

6

+ and # are used to indicate the identical particles in bulk and near the surface, respectively.

7

These particles are shown in Figure 4 in more details.

ACS Paragon Plus Environment

13

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 14 of 22

1 2

Figure 3. HREM images, fast Fourier transformation results acquired from designated areas, and

3

L3/L2 ratios of EELS along scanning path of (a) NMC433 and (b) NMC811 after 10C discharge

4

from 4.8 V.

ACS Paragon Plus Environment

14

Page 15 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry Letters

1 2

Figure 4. Bright field images and SAEDs of NMC811 after high-rate discharge from (a) 4.3 V

3

and (b) 4.8 V (white arrows indicate the positions of diffraction spots from the spinel structure).

4 5

ACKNOWLEDGMENT

6

This work was supported by the Korea Institute of Science and Technology (KIST)

7

Institutional Programs (Project Nos. 2E27062). This research was also supported by the

8

Technology Development Program to Solve Climate Changes of the National Research

9

Foundation

(NRF)

funded

by

the

Ministry

of

Science

&

ICT

(grant

number:

10

2017M1A2A2044482). S.H. acknowledges the support from the Center for Functional

11

Nanomaterials, Brookhaven National Laboratory, which is supported by the U.S. Department of

12

Energy, Office of Basic Energy Sciences, under Contract No. DE- SC0012704.

13 14

ASSOCIATED CONTENT

15

Supporting Information. Experimental details, charge-discharge profiles, and further data

16

regarding SAEDs, and STEM-EELS line scans.

17

AUTHOR INFORMATION

ACS Paragon Plus Environment

15

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

1

Notes

2

The authors declare no competing financial interests.

Page 16 of 22

3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41

REFERENCES (1) (2) (3)

(4)

(5)

(6) (7)

(8) (9)

(10)

(11)

(12)

(13)

Armand, M.; Tarascon, J.-M. Building Better Batteries. Nature 2008, 451, 652–657. Dunn, B.; Kamath, H.; Tarascon, J.-M. Electrical Energy Storage for the Grid: a Battery of Choices. Science 2011, 334, 928–935. Noh, H.-J.; Youn, S.; Yoon, C. S.; Sun, Y.-K. Comparison of the Structural and Electrochemical Properties of Layered Li[NixCoyMnz]O2 (X=1/3, 0.5, 0.6, 0.7, 0.8 and 0.85) Cathode Material for Lithium-Ion Batteries. J. Power Sources 2013, 233, 121–130. Hwang, S.; Kim, S. M.; Bak, S.-M.; Kim, S. Y.; Cho, B.-W.; Chung, K. Y.; Lee, J. Y.; Stach, E. A.; Chang, W. Using Real-Time Electron Microscopy to Explore the Effects of Transition-Metal Composition on the Local Thermal Stability in Charged LixNiyMnzCo1– y– zO2 Cathode Materials. Chem. Mater. 2015, 27, 3927–3935. Liu, W.; Oh, P.; Liu, X.; Lee, M.-J.; Cho, W.; Chae, S.; Kim, Y.; Cho, J. Nickel-Rich Layered Lithium Transition-Metal Oxide for High-Energy Lithium-Ion Batteries. Angew. Chem. Int. Ed. 2015, 54, 4440–4457. Kang, K.; Meng, Y. S.; Bréger, J.; Grey, C. P.; Ceder, G. Electrodes with High Power and High Capacity for Rechargeable Lithium Batteries. Science 2006, 311, 977–980. Wei, Y.; Zheng, J.; Cui, S.; Song, X.; Su, Y.; Deng, W.; Wu, Z.; Wang, X.; Wang, W.; Rao, M.; Lin, Y.; Wang, C.; Amine, K.; Pan, F. Kinetics Tuning of Li-Ion Diffusion in Layered Li(NixMnyCoz)O2. J. Am. Chem. Soc. 2015, 137, 8364–8367. Kang, K.; Ceder, G. Factors That Affect Li Mobility in Layered Lithium Transition Metal Oxides. Phys. Rev. B 2006, 74, 094105. Zheng, S.; Huang, R.; Makimura, Y.; Ukyo, Y.; Fisher, C. A. J.; Hirayama, T.; Ikuhara, Y. Microstructural Changes in LiNi0.8Co0.15Al0.05O2 Positive Electrode Material During the First Cycle. J. Electrochem. Soc. 2011, 158, A357–A362. Bak, S.-M.; Hu, E.; Zhou, Y.; Yu, X.; Senanayake, S. D.; Cho, S.-J.; Kim, K.-B.; Chung, K. Y.; Yang, X.-Q.; Nam, K.-W. Structural Changes and Thermal Stability of Charged LiNixMnyCozO2 Cathode Materials Studied by Combined in Situ Time-Resolved XRD and Mass Spectroscopy. ACS Appl. Mater. Interfaces 2014, 6, 22594–22601. Jung, S.-K.; Gwon, H.; Hong, J.; Park, K.-Y.; Seo, D.-H.; Kim, H.; Hyun, J.; Yang, W.; Kang, K. Understanding the Degradation Mechanisms of LiNi0.5Co0.2Mn0.3O2 Cathode Material in Lithium Ion Batteries. Adv. Energy Mater. 2014, 4 (1), 1300787. Kojima, Y.; Muto, S.; Tatsumi, K.; Kondo, H.; Oka, H.; Horibuchi, K.; Ukyo, Y. Degradation Analysis of a Ni-Based Layered Positive-Electrode Active Material Cycled at Elevated Temperatures Studied by Scanning Transmission Electron Microscopy and Electron Energy-Loss Spectroscopy. J. Power Sources 2011, 196, 7721–7727. Hwang, S.; Kim, S. M.; Bak, S.-M.; Chung, K. Y.; Chang, W. Investigating the Reversibility of Structural Modifications of LixNiyMnzCo1– y– zO2 Cathode Materials During Initial Charge/Discharge, at Multiple Length Scales. Chem. Mater. 2015, 27,

ACS Paragon Plus Environment

16

Page 17 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41

The Journal of Physical Chemistry Letters

(14)

(15)

(16)

(17)

(18)

(19)

(20) (21)

(22)

(23)

(24)

(25)

6044–6052. Zhou, Y.-N.; Yue, J.-L.; Hu, E.; Li, H.; Gu, L.; Nam, K.-W.; Bak, S.-M.; Yu, X.; Liu, J.; Bai, J.; Dooryhee, E.; Fu, Z.-W.; Yang, X.-Q. High-Rate Charging Induced Intermediate Phases and Structural Changes of Layer-Structured Cathode for Lithium-Ion Batteries. Adv. Energy Mater. 2016, 6, 1600597–1600598. Keast, V.; Scott, A. J.; Brydson, R.; Williams, D. B.; Bruley, J. Electron Energy‐Loss Near‐Edge Structure–a Tool for the Investigation of Electronic Structure on the Nanometre Scale. J. Microsc. 2001, 203, 135–175. Yoon, W.-S.; Balasubramanian, M.; Chung, K. Y.; Yang, X.-Q.; McBreen, J.; Grey, C. P.; Fischer, D. A. Investigation of the Charge Compensation Mechanism on the Electrochemically Li-Ion Deintercalated Li1-xCo1/3Ni1/3Mn1/3O2 Electrode System by Combination of Soft and Hard X-Ray Absorption Spectroscopy. J. Am. Chem. Soc. 2005, 127, 17479–17487. Hwang, S.; Kim, D. H.; Chung, K. Y.; Chang, W. Understanding Local Degradation of Cycled Ni-Rich Cathode Materials at High Operating Temperature for Li-Ion Batteries. Appl. Phys. Lett. 2014, 105, 103901. Graetz, J.; Ahn, C. C.; Yazami, R.; Fultz, B. An Electron Energy-Loss Spectrometry Study of Charge Compensation in LiNi0.8Co0.2O2. J. Phys. Chem. B 2003, 107, 2887– 2891. Graetz, J.; Ahn, C. C.; Ouyang, H.; Rez, P.; Fultz, B. White Lines and D-Band Occupancy for the 3d Transition-Metal Oxides and Lithium Transition-Metal Oxides. Phys. Rev. B 2004, 69, 235103. Wang, Z. L.; Yin, J. S.; Jiang, Y. D. EELS Analysis of Cation Valence States and Oxygen Vacancies in Magnetic Oxides. Micron 2000, 31, 571–580. Koyama, Y.; Mizoguchi, T.; Ikeno, H.; Tanaka, I. Electronic Structure of Lithium Nickel Oxides by Electron Energy Loss Spectroscopy. J. Phys. Chem. B 2005, 109, 10749– 10755. Riedl, T.; Gemming, T.; Wetzig, K. Extraction of EELS White-Line Intensities of Manganese Compounds: Methods, Accuracy, and Valence Sensitivity. Ultramicroscopy 2006, 106, 284–291. Zhao, Y.; Feltes, T. E.; Regalbuto, J. R.; Meyer, R. J.; Klie, R. F. In Situ Electron Energy Loss Spectroscopy Study of Metallic Co and Co Oxides. J. Appl. Phys. 2010, 108, 063704. Muto, S.; Sasano, Y.; Tatsumi, K.; Sasaki, T.; Horibuchi, K.; Takeuchi, Y.; Ukyo, Y. Capacity-Fading Mechanisms of LiNiO2-Based Lithium-Ion Batteries. J. Electrochem. Soc. 2009, 156 (5), A371–A377. Hwang, S.; Kim, S. Y.; Chung, K. Y.; Stach, E. A.; Kim, S. M.; Chang, W. Determination of the Mechanism and Extent of Surface Degradation in Ni-Based Cathode Materials After Repeated Electrochemical Cycling. APL Mater. 2016, 4, 096105–096108.

ACS Paragon Plus Environment

17

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 1. Bright field image, SAEDs and EELS of (a) NMC433 and (b) NMC811 after a charge to 4.8V at a rate of 10C. Circles with dotted line denotes the contribution from spinel structure at mixed phase. (c) Summary of structural evolutions of five different NMC particles after high-rate charge to 4.8V.

84x109mm (300 x 300 DPI)

ACS Paragon Plus Environment

Page 18 of 22

Page 19 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry Letters

Figure 2. Bright field image, SAEDs and EELS of (a) NMC433 and (b) NMC811 after a discharge at a rate of 10C from 4.8 V. Circles with dotted line denotes the contribution from spinel structure at mixed phase. Summary of structural evolutions of five different (c) NMC433 and (d) NMC811 particles after high-rate discharge from 4.3V or 4.8V to 2V. Signs of + and # is used for indicating an identical particle at bulk and at near surface.

84x142mm (300 x 300 DPI)

ACS Paragon Plus Environment

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 3. HREM images, fast Fourier transformation results acquired from designated areas, and L3/L2 ratios of EELS along scanning path of (a) NMC433 and (b) NMC811 after 10C discharge from 4.8 V.

84x217mm (300 x 300 DPI)

ACS Paragon Plus Environment

Page 20 of 22

Page 21 of 22

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry Letters

Figure 4. Bright field images and SAEDs of NMC811 after high-rate discharge from (a) 4.3 V and (b) 4.8 V (white arrows indicate the positions of diffraction spots from the spinel structure).

84x56mm (300 x 300 DPI)

ACS Paragon Plus Environment

The Journal of Physical Chemistry Letters

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Table of Contents 50x50mm (300 x 300 DPI)

ACS Paragon Plus Environment

Page 22 of 22