The reduction of ferric oxide to iron

mel-alumel thermocouple. ... more slowly, just began to turn gray. ... to gray. These directions apply to a 0.5 g. sample of oxide. Several tests were...
61 downloads 0 Views 912KB Size
The Reduction of Ferric Oxide to Iron JANE N A S H Northwestern University, Evanston, Illinois

OF THE most familiar experiments1 in general 0NEchem~stry . is. the determination of the equivalent weight of a metal by reduction of its oxide in hydrogen. At Northwestern the metal oxides are issued to the students in the form of unknowns. Very satisfactory results have been obtained with the oxides of copper and of nickel, but students often make large errors in the reduction of ferric oxide. This has led to the supposition that there must be some ambiguity in the laboratory directions. The purposes of this work were to find directions which would give results with a minimum of error, and a t the same time to examine the products formed during the course of the reduction. It is well known that the reduction of femc oxide passes through several stages, involving, perhaps, solid solutions of the various reduction products. Emphasis was, therefore, placed on the time and temperature of heating of the femc oxide. C. p. femc oxide was first weighed, strongly heated, then weighed again to determine its moisture content, which proved to be negligible. A sample of the oxide was then weighed in a porcelain boat which could be strongly heated in an atmosphere of hydrogen. Temperatures were determined by a single junction chromel-alumel thermocouple. Final weighing of the porcelain boat and reduction product was sometimes doue in a hydrogen-filled test tube because i t was discovered that when the oxide had reached certain stages of reduction it reoxidized immediately on exposure to air. In the first test to be described, the oxide was reduced under conditions paralleling as closely as possible the standard laboratory directions for this experiment. About 0.5 g. of ferric oxide was heated in a stream of hydrogen a t about 500°C. for five minutes. During this time the oxide quickly turned black and then, more slowly, just began to turn gray. It was cooled in hydrogen, then removed for weighing. The moment that the boat was removed from the hydrogen atmosphere the material began to change color to a brownish orange. The boat became very hot. This material weighed almost the same as the original ferric oxide. One important source of error in this experiment now becomes clear. At certain stages of reduction the material suffers spontaneous reoxidation in air. Students SELWOOD, THIS JOURNAL, 19,375 (1942).

in a hurry to complete this experiment have sometimes been criticized for trying to weigh the porcelain boat and contents while they are still warm. In a t least some cases, i t now becomes evident, the boat was cool before being removed from the hydrogen but spontaneous reoxidation took place immediately on exposure to air. In the next experiment the oxide was heated twice as long a t the same temperature. During the first few minutes the powder turned a deep black. Then it gradually changed to a fairly light gray. The loss of oxygen was 30.8 per cent, compared with a theoretical oxygen content of 30.06 per cent in FelOa. The reduction product, which must have been practically pure iron, did not change in the least when i t was gently heated in air. The main purpose of this work had, therefore, been achieved. The complete reduction of ferric oxide may he obtained by extending the reduction period to about ten minutes a t about 500°C. It is essential that the first black reduct~onproduct be completely converted to gray. These directions apply to a 0.5 g. sample of oxide. Several tests were now made in an effort to learn more of the compositmn of the pyrophoric and partially reduced oxide. The products were weighed in hydrogen. The results are summarized in Table 1. TABLE 1

TI>, 1

% Lor9

Of

7.47

3

1.02 21.6

4 5

14.0

2

8.87

0%

Color

Slizhtly gray Black Sl8ghfly gray Black Hiack

Adi.il? loward R.orid.l;o?i in Air Spontaneous on gentle heating S~ont~neourat180~C. Spomtsneous on geotlc heatin. Spontaneousat lUOaC. Spontrncousnt 8U0C.

It is clear that act~vitytoward reoxidation is found over widely differingoxygen content. All the partially rrvluced oxides were attracted to a magnet, and in some 'cases the reoxidized product was also ferromagnetic. We are unable to state precisely what condition leads to maximum pyrophoricity. Metallic iron appears not to be responsible. Possibly femous oxide is the pyrophoric substance and this starts the oxidation of FesO, which must also be present. The ferromagnetism of the final reoxidation product may be due to y-Fez03. This work was doue a t the suggestion, and under the direction, of Professor P. W. Selwood.