Thickness Effect on Structural Defect-Related Density of States and

1 day ago - We report on a study of thickness effect on the formation of structural defect-related density of states (DOS) in the band gap of poly(3-h...
0 downloads 7 Views 847KB Size
Subscriber access provided by UNIV OF SCIENCES PHILADELPHIA

Article

Thickness Effect on Structural Defect-Related Density of States and Crystallinity in P3HT Thin Films on ITO Substrates Vojtech Nádaždy, Katarína Gmucová, Peter Nadazdy, Peter Siffalovic, Karol Vegso, Matej Jergel, František (Franz) Schauer, and Eva Majkova J. Phys. Chem. C, Just Accepted Manuscript • DOI: 10.1021/acs.jpcc.7b11651 • Publication Date (Web): 02 Mar 2018 Downloaded from http://pubs.acs.org on March 4, 2018

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

The Journal of Physical Chemistry C is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Thickness Effect on Structural Defect-Related Density of States and Crystallinity in P3HT Thin Films on ITO Substrates Vojtech Nádaždy1, Katarína Gmucová1,*, Peter Nádaždy1, Peter Siffalovic1, Karol Vegso1, Matej Jergel1, František Schauer2, and Eva Majkova1 1

Institute of Physics, Slovak Academy of Sciences, Dúbravská cesta 9, 845 11 Bratislava, Slovak Republic 2

Faculty of Applied Informatics, Tomas Bata University in Zlín, Nad Stráněmi 4511, 760 05 Zlín, Czech Republic

*

Corresponding Author

E-mail: [email protected] Telephone number: +421220910762

1 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 26

ABSTRACT We report on a study of thickness effect on the formation of structural defect-related density of states (DOS) in the band gap of poly(3-hexylthiophene-2,5-diyl) (P3HT) thin films spincoated on ITO substrates. The energy-resolved electrochemical impedance spectroscopy and grazingincidence wide-angle X-ray scattering were used to correlate the DOS with the degree of crystallinity in P3HT thin films. We found an exponential increase of the defect DOS in the band gap with increasing fraction of the amorphous phase when decreasing the film thickness. The exponent increases abruptly when reducing the thickness down to 30 nm which indicates two thickness regions with different dynamics of the defect DOS formation driven by increasing fraction of the amorphous phase. Moreover, we observed co-existence of two P3HT polymorphic crystalline phases with different backbone spacings which results in the appearance of a peculiar DOS satellite peak above the HOMO. The volume of the minor, more dense, crystalline phase exhibits a thickness dependence with a maximum plateau around 40 nm. These results suggest an important effect of the substrate roughness on the crystallinity and polymorphism of P3HT thin films depending on the film thickness with general implications for polymer thin films.

2 ACS Paragon Plus Environment

Page 3 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

INTRODUCTION The defect-related electronic states in the band gap have a profound influence on efficiency of organic electronic devices such as solar cells1, organic field-effect transistors2, organic lightemitting diodes3, and recently electrochemical transistor4. Two classes of defects can be distinguished in organic semiconductors: extrinsic and intrinsic. The extrinsic defects are induced by chemical impurities in semiconductor while the intrinsic defects arise from structural disorder in semiconductor bulk and/or surface. The origin of chemical defects is attributed to the influence of ambient atmosphere and synthesis residues. The structural defects perturb surrounding energy levels and generate new electronic states in the band gap. As their effect is weak, no covalent bonds are altered1. Recently, we have reported on the changes arising in the fine band gap electronic structure of the regioregular P3HT as a consequence of the thin film exposure to the ambient air5. The oxygen and water-related defects have been identified by comparing the energy levels of the observed defect states with the data from literature that were obtained by a combination of optical and electrical spectroscopic methods or first-principles calculations. Preparation of samples in inert atmosphere prevents formation of oxygen and water-related defects. However, structural defects play an important role in the performance of organic electronic devices as well. The structure of solution-processed thin films of semiconducting conjugated polymers is characterized by ordered crystalline nano-domains embedded in an amorphous matrix6. The DOS related to the intrinsic structural defects may vary in these materials depending on the crystallinity7 that affects many microphysical properties8. For example, charge transport is typically limited by the hopping process resulting in low charge carrier mobilities ( 98%, the number average molecular weight Mn 45,000-65,000 gmol-1, and the polydispersity index PDI < 2 was purchased from Sigma Aldrich. The ITO coated glass substrates with sheet resistance of 7 ohm per square and the rms surface roughness of 7 nm were deliverd by Präzisions Glas & Optik, Germany. The ITO substrates were cleaned using ultrasonic bathing in acetone and isopropylalcohol. After drying out the substrates were treated with UV-ozone for 10 min. Then, P3HT thin films were deposited by spin-coating at the room temperature in the nitrogen atmosphere in the glove box. Before spin coating, all solutions were filtered using a 200 nm PTFE filter. The solvent annealing was performed in Petri dish with the volume of 18 cm3 for 30 min straight after the spin-coating. The samples were then immediately thermally annealed at 110 °C for 5 min with 30 s rise time from the room temperature. The cooling down took place spontaneously on the tissue-paper. The film thickness was measured with Dektak 150 surface profiler (Veeco, USA). The film thicknesses with determined experimental errors, solution concentrations, and spinning rates are summarized in Table 1.

6 ACS Paragon Plus Environment

Page 7 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Table 1. P3HT thin film preparation details. Film thickness (nm)

Concentration (wt %)

Spinning rate (rps)

7±2

0.3

30

10±2

0.3

28

16±2

0.5

30

30±3

1.0

60

40±3

1.0

45

50±3

1.0

30

60±3

1.0

28

90±4

1.5

35

120±5

1.5

30

Since the films were also electrochemically characterized in a liquid electrolyte, X-ray measurements of all samples were performed before and after wetting by the electrolyte to be sure that its penetration does not modify the polymer structure. This comparison experiment indicated a minor change of the diffraction intensity which did not affect the addressed correlation between the electronic structure and microstructure data (Supporting Information, section S3). Energy Resolved Electrochemical Impedance Spectroscopy. The ER-EIS is a spectroscopic method capable to map DOS in organic semiconductor materials in the entire energy range from HOMO to the lowest unoccupied molecular orbital (LUMO). This method recently introduced by us28 was used for elucidation of the chemical defect-related DOS in P3HT5 and UV irradiation induced defect states in polysilanes29-30. The DOS function g(E) in the semiconductor at the Fermi energy , = can be expressed in terms of the charge transfer resistance Rct measured at the applied potential E as28 7 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

d

s =  EF,redox =  = d

 et 

d d

= 

Page 8 of 26

 t ct

,

(1)

where S is the sample area. The charge transfer resistance Rct = dU/d(jS) corresponds to the real part of complex impedance measured by harmonic voltage at a given frequency f and an amplitude dE superimposed on the applied potential E. The DOS function g(eE) may be directly derived from the charge-transfer resistance Rct(E) measured at an instantaneous position of the Fermi energy given by the applied voltage E using eq (1). The impedance/gain-phase analyzer Solartron analytical, model 1260, was used in the configuration described in our previous paper28. The frequency, amplitude of AC voltage and the sweep rate of the DC voltage ramp were set to 0.5 Hz, 100 mV, and 10 mV/s, respectively. Electrochemical microcells of a volume of about ≈ 200 µL were formed on ITO substrates with deposited regioregular P3HT thin films by gluing the plastic cone5, 28. In this way, the disc working electrode area of 12 mm2 was defined. A solution of 0.1 M TBAPF6 in acetonitrile was employed as the supporting electrolyte. The potential of the working electrode with respect to the reference Ag/AgCl electrode was controlled via a potentiostat. A Pt wire was used as the counter electrode. Considering that the standard potential of the reference Ag/AgCl electrode is + 0.22 V31 relative to the standard hydrogen electrode (+ 4.44 V), the energy scale of DOS is recalculated to the local vacuum level with an Ag/AgCl energy vs. vacuum value of 4.66 eV. Grazing-Incidence Wide-Angle X-ray Scattering. The GIWAXS is a reciprocal-space mapping technique widely used for structural characterization of organic thin films. In this technique, a monochromatic and collimated X-ray beam impinges on the sample surface at a small angle of incidence (usually αinc = 0.2°-1°) with respect to the sample surface. The scattered X-ray photons are collected by a position-sensitive X-ray detector. The utilization of twodimensional (2D) X-ray detector allows simultaneous and fast acquisition of a large part of 8 ACS Paragon Plus Environment

Page 9 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

reciprocal space when compared to a point detector which scans reciprocal space along a particular trajectory. The application of GIWAXS technique to P3HT thin films was reviewed by P. Müller-Buschbaum32. The GIWAXS measurements of P3HT thin films were performed on a custom-designed Nanostar device (Bruker AXS, Germany) with a liquid Ga metal-jet X-ray source (Excillum, Sweden) dedicated to the small-angle and wide-angle X-ray scattering. The metal-jet X-ray source generates high-intense Ga Kα radiation with a photon energy of 9.25 keV (λ = 0.134 nm). The emitted X-ray photons were collected and collimated by a pair of multilayer mirrors arranged in Montel configuration. The photon flux behind Montel optics was 2×109 photons/s. The X-ray beam collimation was performed by two single-crystal Ge pinholes that were 550 cm in diameter and 50 cm apart each other. The photon flux behind the collimator was 3×108 photons/s. A vacuum compatible six-axis hexapod H-811 (Physik Instrumente, Germany) was employed to adjust the sample into the collimated X-ray beam. The angle of incidence was set to 0.2°. The GIWAXS pattern was recorded by a silicon-based 2D X-ray detector Pilatus 300K (Dectris, Switzerland) working in the single-photon counting regime. The reciprocal space of GIWAXS pattern was calibrated by a silver behenate standard. The sampleto-detector distance was 250 mm. The exposure time for a single measurement was set to 1500 s.

RESULTS AND DISCUSSION Structural Defect-related DOS. The DOS spectra measured with ER-EIS technique are shown in Figure 1. Considering the DOS maximum of the order of 1021 cm-3eV-1,33 the defect-related DOS can be estimated to vary between 1015 and 1018 cm-3 eV-1 which is in good agreement with the sub-band gap DOS reported by Nogueira et al.34 and Boix et al.35 The quantification of g(E) depends on the area of the bulk electrolyte/polymer interface, S (see eq. (1) and Supporting

9 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 10 of 26

Information, section S4). The spectra are therefore corrected with respect to the effective area of the thickest P3HT layer supposing a linear increase of the effective area with thickness. Unlike a previously reported DOS of chemical defects in P3HT5, a wide continuum of states between the LUMO and approximately – 0.25 V vs. Ag/AgCl (− 4.45 eV vs. vacuum energy) is recorded for the P3HT films thinner than 30 nm which grows with decreasing thickness. On the other hand, a systematic DOS decrease in the band gap of the P3HT films thicker than 30 nm is measured. To explain this evolution, the presence of oxygen-related defects may be excluded due to the inert nitrogen atmosphere. Hence, the DOS increase in the band gap with the thickness decrease can be attributed to intrinsic structural defects in the P3HT thin films. Besides, there is an apparent satellite peak above the HOMO whose amplitude varies with the film thickness.

Figure 1. The DOS of P3HT thin films of various thicknesses measured by the ER-EIS. The regions I. and II. are discussed in the text.

10 ACS Paragon Plus Environment

Page 11 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Microstructure. The molecular stacking in semiconducting polymers forms crystalline domains. In particular, the regioregular P3HT forms lamellar crystalline domains by a π-π stacking of the thiophene rings of the neighboring backbone chains which are separated by amorphous regions. The spin-coated P3HT thin films typically exhibit the edge-on configuration of crystalline domains with the π−π stacking direction parallel to the substrate surface. The lattice constant of this stacking is controlled by the crystallization of alkane side chains8, 36. The organic molecules in thin films tend to form multiple crystalline structures known as polymorphs. In the case of P3HT, polymorphic phases can be stimulated by solvent evaporation rate37, surface morphology38 or chemical additives39 used in the thin film processing. The most intense 100 diffraction in GIWAXS pattern suggests the edge-on configuration of π−π stacking with a strong preferential texture along the surface normal (Supporting Information, Figure S1). The intensity distribution of this diffraction along qz axis at qy = 0 nm-1 exhibits an asymmetry (Figure 2 and Supporting Information) which can be fully simulated by a contribution of two P3HT polymorphic phases labeled here as A and B. The dominant A phase has the backbone spacing 

≅ 1.65 nm ("# = 3.8 nm-1) which suggests a well-described bulk phase of P3HT8, 40. The

minor B phase has a smaller spacing $

≅ 1.51 nm ("#$ = 4.15 nm-1). Such a denser

polymorphic phase was found in the P3HT sample crystallized under extremely slow evaporation rate37. It was also shown that the packing density and structural perfection of P3HT is affected by the size of P3HT crystals38. The ratio of integral intensities RB/A of the overlapping 100 diffractions of the two P3HT crystalline phases exhibits a thickness dependence which can be correlated with the evolution of the satellite peak in DOS above the HOMO, as it will be shown later in the discussion. We also estimated a relative degree of crystallinity, xcr, in the P3HT thin films as41

11 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

%&' =

( )*+, )-) ( )*)-)

Page 12 of 26

(2)

Here, ." is the total scattered intensity including a contribution from the amorphous background and .&' " is the integral intensity of crystalline phase only (Supporting Information, Figure S2).

Figure 2. The intensity profile of 100 diffraction along qz axis at qy = 0 nm-1 for the 30 nm P3HT thin film measured by the GIWAXS. A decomposition into two polymorphic phases denoted as A and B is indicated.

Due to the restricted reciprocal space used for xcr evaluation (q = 1.4 - 4.7 nm-1), the calculated xcr values do not represent the absolute values of crystallinity degree but allow to quantify relative changes in a set of samples with different film thicknesses. A more profound analysis of the crystallinity degree employing the pole figures was published by Jimison et al.26. However, due to a high degree of texture in P3HT lamellar phase (see Figure S1 in Supporting Information), the approach used here is fully sufficient to describe the relative changes in P3HT 12 ACS Paragon Plus Environment

Page 13 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

crystallinity. These can be correlated with the DOS changes in the band gap as it is shown in the next section. Relation between Electronic Structure and Microstructure. To relate the thickness evolution of electronic structure probed by the ER-EIS method to that of microstructure probed by GIWAXS, the structural defect-related DOS in the band gap was compared with two structural parameters derived from GIWAXS. In particular, the relative amorphous volume fraction given as (1-xcr) and the RB/A ratio quantifying the relative amount of the two P3HT polymorphs were employed. The ER-EIS method shows that the DOS drops to a minimum close to 1015 cm-3eV-1 for the thickest film and increases with the reduction of film thickness in the whole band gap up to 1018 cm-3eV-1 (Figure 1). In addition, a satellite peak above the HOMO is recognized. Let ΣΙ and ΣΙΙ be numerically integrated values of DOS in the regions I and II, respectively, as indicated in Figure 1. The region I refers to the transport gap determined for each film thickness from the band edges in linear scale following a procedure used by Deibel et al.42. The region II refers to the satellite peak above the HOMO fitted with a Gaussian and an exponential background. Hence, ΣΙ is the integral value of DOS in the band gap without the satellite peak contribution while ΣΙΙ is the area under the Gaussian curve fit of the satellite peak. The ΣΙ dependence on the film thickness is shown in the semi-logarithmic scale in Figure 3a. The thinner the film, the higher ΣΙ is observed. The relative volume fraction of amorphous phase (1-xcr) exhibits a similar thickness dependence (Figure 3b). A relationship between these quantities is shown in Figure 4. The DOS in the band gap increases with the fraction of amorphous phase. In particular, two distinct line fits imply two different exponential dependences, ΣΙ ∝ exp[k × (1-xcr)], with remarkably different values of k coefficient, being 10 and 110 above and below the 30 nm film thickness, respectively. The amorphous volume

13 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 14 of 26

fraction at this crossover thickness is 80 %. In this regard, it is interesting to mention a paper by Jimison et al.20 who investigated the degree of crystallinity as a function of the P3HT film thickness by X-ray diffraction and found a steady increase with the film thickness before leveling off at around 30 nm.

Figure 3. (a) The integral value of DOS in the band gap and (b) the relative amorphous volume fraction as a function of the film thickness.

In our case, the existence of crossover thickness indicates different tendencies to the defect DOS formation induced by structural defects in the two thickness regions. Below 30 nm, the fraction of amorphous phase is higher and the thinner the films are, the easier various structural defects are formed and the faster the defect DOS are created. For very thin P3HT films, an amorphous-like phase with highly distorted lattice of P3HT molecular chains formed at the interface with substrate and occupying a major part of the film volume may be expected. In addition, the inter-chain and intra-chain disorder may be fostered by various structural defects

14 ACS Paragon Plus Environment

Page 15 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

inside the chains which also affect the DOS in the band gap. Theoretical calculations by Feng et al.17 showed that isolated rotation of the arene rings or loss of the π−π stacking either through tilting or lateral displacement of adjacent polymer chains results in the formation of defect states above the HOMO. Additional defect states below the LUMO were found after increasing the geometrical distorsion of arene rings. Such structural defects are presumably responsible for the steep increase of the integral value of DOS in the band gap below 30 nm. Above 30 nm, higher content of crystalline phase suggests less-defect molecular chains adopting energetically more favorable configurations which decelerates the defect DOS formation in the band gap with increasing the film thickness.

Figure 4. The integral value of DOS in the band gap as a function of the relative amorphous volume fraction. The respective film thicknesses are those in Figure 3.

The thickness dependences of ΣΙΙ (integral DOS of the satellite peak above the HOMO) and RB/A (intensity ratio of the two P3HT polymorphs) are shown in Figure 5. They exhibit similar shapes with a broad maximum centered around 40 nm. A linear dependence of ΣΙΙ on RB/A in the 15 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 16 of 26

semi-log scale (Figure 6) shows a correlation between the occurrence of B phase and the satellite peak above the HOMO. As mentioned above, the dominant A phase with the spacing 

≅ 1.65 nm is equivalent to the bulk phase of P3HT8, 40. This phase is typically observed as

the only phase in the P3HT thin films deposited on smooth polished substrates with rms roughness below 1 nm, such as silicon wafers, being manifested by a symmetric 100 diffraction peak at qz ≅ 3.8 nm-1. In our case, the substrate was a glass plate covered with ITO layer (used e.g. as the front transparent electrode in organic solar cell) and has a much larger rms roughness of about 7 nm. Such a large roughness acts adversely on the mobility of P3HT molecular chains during the solvent and thermal annealings to adopt energetically the most favorable configurations and is responsible for the appearance of the minor B phase with $

≅ 1.51 nm.

It is noteworthy that a similar co-existence of two polymorphic phases with the backbone spacings of 1.64 nm and 1.55 nm was observed in the P3HT films deposited on mesoporous titania electrodes with a particular pore size of 40 nm38. This compares well with the P3HT film thickness corresponding to the maximum content of B phase (Figure 5b). In contrast, only the regular 1.64 nm spacing was found in the electrodes with 12 nm pore size. In our case, the formation of B phase is suppressed at both small and large film thicknesses with respect to the 40 nm thick film. Small film thicknesses nearly approach the ITO substrate roughness. This may affect unfavorably the film morphology and continuity, impeding the formation of B phase over larger volumes during the solvent and thermal annealings. On the other hand, the effect of substrate roughness becomes weaker at larger film thicknesses and the film structure is more akin to bulk material.

16 ACS Paragon Plus Environment

Page 17 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Figure 5. (a) The integral DOS of the satellite peak above the HOMO and (b) the ratio of integral intensities of the 100 diffractions of the two P3HT polymorphs as a function of the P3HT film thickness.

Figure 6. The integral DOS of the satellite peak above the HOMO as a function of the ratio of integral intensities of the 100 diffractions of the two P3HT polymorphs.

17 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 18 of 26

SUMMARY The ER-EIS and GIWAXS techniques were applied to investigate the relationship between the electronic and molecular structures in P3HT thin films. An exponential increase of the DOS in the band gap with increasing fraction of the amorphous phase when decreasing the film thickness was found. The exponent increases abruptly by one order of magnitude when reducing the film thickness down to 30 nm (Figure 4), where the relative volume fraction of amorphous phase reaches 80 %. Hence, the films thinner than 30 nm exhibit a much faster formation of the defect DOS with increasing fraction of the amorphous phase than those thicker than 30 nm. The existence of crossover thickness is important for application of P3HT films on ITO substrate in electronic devices. The presence of two polymorphic crystalline A and B phases with different backbone spacings was found by the GIWAXS. The minor B phase content has a maximum plateau around 40 nm and decays at both small and large film thicknesses. The integral DOS of the satellite peak located above the HOMO shows an exponential increase with the volume ratio RB/A, suggesting a principal role of the minor B phase in the occurrence of the satellite peak. Our results show that in the case of rough substrates such as ITO, the DOS in the band gap of P3HT thin films is strongly dependent on the film thickness as the substrate roughness induces various structural defects and leads to the formation of polymorphic crystalline phases. The implications for applications of polymers in high-performance organic electronics are straightforward.

ASSOCIATED CONTENT

18 ACS Paragon Plus Environment

Page 19 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Supporting Information. Quantification of P3HT polymorphs, Degree of crystallinity in P3HT thin films, Influence of electrolyte on P3HT microstructure, and Determination of the diffusion coefficient of electrolyte penetration into P3HT.

ACKNOWLEDGMENTS The authors gratefully thank to P. Kalinay (Institute of Physics SAS, Bratislava) for the model of electrolyte penetration into P3HT given in the Supporting Information. This research was supported by the Slovak Research and Development Agency, project no. APVV-0096-11, the Scientific Grant Agency VEGA, projects nos. 1/0501/15, 2/0163/17, 2/0092/18, and the project Applied Research of Advanced Photovoltaic Cells, ITMS code 26240220047, supported by the Research and Development Operational Programme funded by ERDF.

REFERENCES (1)

Carr, J. A.; Chaudhary, S. The Identification, Characterization and Mitigation of Defect

States in Organic Photovoltaic Devices: A Review and Outlook. Energ. Environ. Sci. 2013, 6, 3414-3438. (2)

Diemer, P. J.; Hayes, J.; Welchman, E.; Hallani, R.; Pookpanratana, S. J.; Hacker, C. A.;

Richter, C. A.; Anthony, J. E.; Thonhauser, T.; Jurchescu, O. D. The Influence of Isomer Purity on Trap States and Performance of Organic Thin-Film Transistors. Adv. Electron. Mater. 2017, 3, 1600294. (3)

Ingram, G. L.; Zhao, Y.-B.; Lu, Z.-H. Exciton Dynamics of Luminescent Defects in

Aging Organic Light-Emitting Diodes. J. Appl. Phys. 2017, 122, 245501.

19 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

(4)

Page 20 of 26

Nielsen, C. B.; Giovannitti, A.; Sbircea, D.-T.; Bandiello, E.; Niazi, M. R.; Hanifi, D. A.;

Sessolo, M.; Amassian, A.; Malliaras, G. G.; Rivnay, J.; et al. Molecular Design of Semiconducting Polymers for High-Performance Organic Electrochemical Transistors. J. Am. Chem. Soc. 2016, 138, 10252-10259. (5)

Gmucová, K.; Nádaždy, V.; Schauer, F.; Kaiser, M.; Majkova, E. Electrochemical

Spectroscopic Methods for the Fine Band Gap Electronic Structure Mapping in Organic Semiconductors. J. Phys. Chem. C 2015, 119, 15926-15934. (6)

Nalwa, H. S. Handbook of Organic Conductive Molecules and Polymers; John Wiley and

Sons Ltd: Chichester, U.K.,1997. (7)

Spoltore, D.; Oosterbaan, W. D.; Khelifi, S.; Clifford, J. N.; Viterisi, A.; Palomares, E.;

Burgelman, M.; Lutsen, L.; Vanderzande, D.; Manca, J. Effect of Polymer Crystallinity in P3HT:PCBM Solar Cells on Band Gap Trap States and Apparent Recombination Order. Adv. Energy Mater. 2013, 3, 466-471. (8)

Prosa, T. J.; Winokur, M. J.; Moulton, J.; Smith, P.; Heeger, A. J. X-Ray Structural

Studies of Poly(3-Alkylthiophenes) - an Example of an Inverse Comb. Macromolecules 1992, 25, 4364-4372. (9)

Kobashi, M.; Takeuchi, H. Inhomogeneity of Spin-Coated and Cast Non-Regioregular

Poly(3-Hexylthiophene) Films. Structures and Electrical and Photophysical Properties. Macromolecules 1998, 31, 7273-7278.

20 ACS Paragon Plus Environment

Page 21 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

(10) Luo, C.; Kyaw, A. K. K.; Perez, L. A.; Patel, S.; Wang, M.; Grimm, B.; Bazan, G. C.; Kramer, E. J.; Heeger, A. J. General Strategy for Self-Assembly of Highly Oriented Nanocrystalline Semiconducting Polymers with High Mobility. Nano Lett. 2014, 14, 2764-2771. (11) Wang, G.; Swensen, J.; Moses, D.; Heeger, A. J. Increased Mobility from Regioregular Poly(3-Hexylthiophene) Field-Effect Transistors. J. Appl. Phys. 2003, 93, 6137-6141. (12) Skrypnychuk, V.; Wetzelaer, G.-J. A. H.; Gordiichuk, P. I.; Mannsfeld, S. C. B.; Herrmann, A.; Toney, M. F.; Barbero, D. R. Ultrahigh Mobility in an Organic Semiconductor by Vertical Chain Alignment. Adv. Mater. 2016, 28, 2359-2366. (13) Sirringhaus, H.; Brown, P. J.; Friend, R. H.; Nielsen, M. M.; Bechgaard, K.; LangeveldVoss, B. M. W.; Spiering, A. J. H.; Janssen, R. A. J.; Meijer, E. W.; Herwig, P.; et al. M. TwoDimensional Charge Transport in Self-Organized, High-Mobility Conjugated Polymers. Nature 1999, 401, 685-688. (14) Rivnay, J.; Noriega, R.; Northrup, J. E.; Kline, R. J.; Toney, M. F.; Salleo, A. Structural Origin of Gap States in Semicrystalline Polymers and the Implications for Charge Transport. Phys. Rev. B 2011, 83, 121306(R). (15) Street, R. A.; Song, K. W.; Northrup, J. E.; Cowan, S. Photoconductivity Measurements of the Electronic Structure of Organic Solar Cells. Phys. Rev. B 2011, 83, 165207. (16) Frost, J. M.; Kirkpatrick, J.; Kirchartz, T.; Nelson, J. Parameter Free Calculation of the Subgap Density of States in Poly(3-Hexylthiophene). Faraday Discuss. 2014, 174, 255-266.

21 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 22 of 26

(17) Feng, D. Q.; Caruso, A. N.; Losovyj, Y. B.; Shulz, D. L.; Dowben, P. A. Identification of the Possible in Poly(3-Hexylthiophene) Thin Defect States Films. Polym. Eng. Sci. 2007, 47, 1359-1364. (18) Poelking,

C.;

Andrienko,

D.

Effect

of

Polymorphism,

Regioregularity

and

Paracrystallinity on Charge Transport in Poly(3-Hexylthiophene) [P3HT] Nanofibers. Macromolecules 2013, 46, 8941-8956. (19) Maillard, A.; Rochefort, A. Structural and Electronic Properties of Poly(3Hexylthiophene) π-Stacked Crystals. Phys. Rev. B 2009, 79, 115207. (20) Lucke, A.; Schmidt, W. G.; Rauls, E.; Ortmann, F.; Gerstmann, U. Influence of Structural Defects and Oxidation onto Hole Conductivity in P3HT. J. Phys. Chem. B 2015, 119, 64816491. (21) DeLongchamp, D. M.; Kline, R. J.; Fischer, D. A.; Richter, L. J.; Toney, M. F., Molecular Characterization of Organic Electronic Films. Adv. Mater. 2011, 23, 319-337. (22) Botiz, I.; Stingelin, N. Influence of Molecular Conformations and Microstructure on the Optoelectronic Properties of Conjugated Polymers. Materials 2014, 7, 2273-2300. (23) Tremel, K.; Ludwigs, S. Morphology of P3HT in Thin Films in Relation to Optical and Electrical Properties. Adv. Polym. Sci. 2014, 265, 39-82. (24) Porzio, W.; Scavia, G.; Arnautov, S.; Conzatti, L.; Charmet, J.; Laux, E.; Keppner, H.; Zerbi, G.; Brambilla, L.; Bolognesi, A. Nanoscale Structure and Morphology of Thin Films of Poly(2-Chloroxylylene) Synthesized by the CVD Method on Different Liquids. Eur Polym J 2011, 47, 1725-1735. 22 ACS Paragon Plus Environment

Page 23 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

(25) Scavia, G.; Barba, L.; Arrighetti, G.; Milita, S.; Porzio, W. Structure and Morphology Optimization of Poly(3-Hexylthiophene) Thin Films onto Silanized Silicon Oxide. Eur. Polym. J. 2012, 48, 1050-1061. (26) Jimison, L. H.; Himmelberger, S.; Duong, D. T.; Rivnay, J.; Toney, M. F.; Salleo, A. Vertical Confinement and Interface Effects on the Microstructure and Charge Transport of P3HT Thin Films. J. Polym. Sci., Part B: Polym. Phys. 2013, 51, 611-620. (27) Spano, F. C.; Silva, C. H- and J-Aggregate Behavior in Polymeric Semiconductors. Annu. Rev. Phys. Chem. 2014, 65, 477-500. (28) Nádaždy, V.; Schauer, F.; Gmucová, K. Energy Resolved Electrochemical Impedance Spectroscopy for Electronic Structure Mapping in Organic Semiconductors. Appl. Phys. Lett. 2014, 105, 142109. (29) Schauer, F.; Tkáčová, M.; Nádaždy, V.; Gmucová, K.; Ožvoldová, M.; Tkáč, L.; Chlpík, J. Electronic Structure of Uv Degradation Defects in Polysilanes Studied by Energy Resolved Electrochemical Impedance Spectroscopy. Polym. Degrad. Stab. 2016, 126, 204-208. (30) Schauer, F.; Tkáč, L.; Ožvoldová, M.; Nádaždy, V.; Gmucová, K.; Jergel, M.; Šiffalovič, P. Effect of Crystallinity on UV Degradability of Poly[Methyl(Phenyl)Silane] by EnergyResolved Electrochemical Impedance Spectroscopy. AIP Adv. 2017, 7, 055002. (31) Bates, R. G.; Macaskill, J. B. Standard Potential of the Silver-Silver Chloride Electrode. Pure Appl. Chem. 1978, 50, 1701-1706. (32) Muller-Buschbaum, P. The Active Layer Morphology of Organic Solar Cells Probed with Grazing Incidence Scattering Techniques. Adv. Mater. 2014, 26, 7692-7709. 23 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 24 of 26

(33) Vukmirović, N.; Wang, L. W. Density of States and Wave Function Localization in Disordered Conjugated Polymers: A Large Scale Computational Study. J. Phys. Chem. B 2011, 115, 1792-1797. (34) Nogueira, A. F.; Montanari, I.; Nelson, J.; Durrant, J. R.; Winder, C.; Sariciftci, N. S. Charge Recombination in Conjugated Polymer/Fullerene Blended Films Studied by Transient Absorption Spectroscopy. J. Phys. Chem. B 2003, 107, 1567-1573. (35) Boix, P. P.; Garcia-Belmonte, G.; Muñecas, U.; Neophytou, M.; Waldauf, C.; Pacios, R. Determination of Gap Defect States in Organic Bulk Heterojunction Solar Cells from Capacitance Measurements. Appl. Phys. Lett. 2009, 95. (36) Brinkmann, M.; Rannou, P. Effect of Molecular Weight on the Structure and Morphology of Oriented Thin Films of Regioregular Poly(3-Hexylthiophene) Grown by Directional Epitaxial Solidification. Adv. Funct. Mater. 2007, 17, 101-108. (37) Yuan, Y.; Zhang, J. M.; Sun, J. Q.; Hu, J.; Zhang, T. P.; Duan, Y. X. Polymorphism and Structural Transition around 54 Degrees C in Regioregular Poly(3-Hexylthiophene) with High Crystallinity as Revealed by Infrared Spectroscopy. Macromolecules 2011, 44, 9341-9350. (38) Song, L.; Wang, W.; Pröller, S.; González, D. M.; Schlipf, J.; Schaffer, C. J.; Peters, K.; Herzig, E. M.; Bernstorff, S.; Bein, T.; et al. In Situ Study of Degradation in P3HT-TitaniaBased Solid-State Dye-Sensitized Solar Cells. ACS Energy Lett. 2017, 2, 991-997. (39) Smith, B. H.; Clark Jr., M. B.; Kuang, H.; Grieco, C.; Larsen, A. V.; Zhu, C.; Wang, C.; Hexemer, A.; Asbury, J. B.; Janik, M. J.; et al. Controlling Polymorphism in Poly(3-

24 ACS Paragon Plus Environment

Page 25 of 26 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Hexylthiophene) through Addition of Ferrocene for Enhanced Charge Mobilities in Thin-Film Transistors. Adv. Funct. Mater. 2015, 25, 542-551. (40) Dudenko, D.; Kiersnowski, A.; Shu, J.; Pisula, W.; Sebastiani, D.; Spiess, H. W.; Hansen, M. R. A Strategy for Revealing the Packing in Semicrystalline π-Conjugated Polymers: Crystal Structure of Bulk Poly-3-Hexyl-Thiophene (P3HT). Angew. Chem., Int. Ed. 2012, 51, 1106811072. (41) Roe, R. J. Methods of X-Ray and Neutron Scattering in Polymer Science; Oxford University Press: New York, USA, 2000. (42) Deibel, C.; Mack, D.; Gorenflot, J.; Scholl, A.; Krause, S.; Reinert, F.; Rauh, D.; Dyakonov, V. Energetics of Excited States in the Conjugated Polymer Poly(3-Hexylthiophene). Phys. Rev. B 2010, 81, 085202.

25 ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 26 of 26

TOC Graphic

26 ACS Paragon Plus Environment