Ultrathin Zirconia Passivation and Stabilization of Aluminum Nanoparticles for Energetic Nanomaterials via Atomic Layer Deposition Rong Chen, Kai Qu, Jiawei Li, Penghui Zhu, Chenlong Duan, Jing Zhang, Xiwen Li, Xiao Liu, and Zhijian Yang ACS Appl. Nano Mater., Just Accepted Manuscript • DOI: 10.1021/acsanm.8b01005 • Publication Date (Web): 13 Sep 2018 Downloaded from http://pubs.acs.org on September 13, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
Ultrathin Zirconia Passivation and Stabilization of Aluminum Nanoparticles for Energetic Nanomaterials via Atomic Layer Deposition
Rong Chen,*,† Kai Qu,† Jiawei Li,† Penghui Zhu,† Chenlong Duan,† Jing Zhang,† Xiwen Li,† Xiao Liu,*,† and Zhijian Yang‡
†
State Key Laboratory of Digital Manufacturing Equipment and Technology, School
of Mechanical Science and Engineering, Huazhong University of Science and Technology, Wuhan 430074, Hubei, People’s Republic of China. ‡
Institute of Chemical Materials, China Academy of Engineering Physics, Mianyang,
621900, Sichuan, People’s Republic of China.
ABSTRACT:
The stability of aluminum (Al) nanoparticles is a key issue that
determines the energy performance of solid fuels, Al-based green propellants, and fuel cells.
The surface native oxide shell (Al2O3), nevertheless, cannot stabilize Al
nanoparticles under hot water conditions.
Herein, we report a passivation method
utilizing an ultrathin zirconia (ZrO2) coating via atomic layer deposition, where subnanometer coating layer could completely prevent the reactions between Al nanoparticles and hot water (80 ºC).
The weight percentage of metallic Al for
ultrathin ZrO2 coated Al nanoparticles can reach 82.2 wt%, which is close to that of original Al nanoparticles with Al2O3 native oxide (88 wt%).
The metallic Al’s
weight has been kept at 93.4 % for the ultrathin ZrO2 coated Al nanoparticles compared to the original Al nanoparticles.
As a comparison, the Al2O3 coated Al
nanoparticles results in the oxidation failure in 60 ºC water.
The proposed
passivation mechanism is attributed to ZrO2 coating’s structural stability and the enhanced hydrophobicity to water.
The ultrathin ZrO2 passivation offers a valuable
ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
tool for enhancing the stability of Al nanoparticles, and thereby enables their potential applications in energy field. KEYWORD: Al nanoparticles, stability, ZrO2, ultrathin coating, atomic layer deposition
ACS Paragon Plus Environment
Page 2 of 27
Page 3 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
1. INTRODUCTION Aluminum (Al) nanoparticles with large specific area and high energy release rate, have aroused wide attentions in the applications of solid fuels, Al-based green propellants and fuel cells.1-6 However, the major drawback for Al nanoparticles, especially when the size getting smaller and smaller, is its poor stability towards the easy oxidation under ambient conditions.7-9
The oxidation process will lead to the
decrease of the metallic core’s weight percentage and combustion efficiency of Al nanopaticles.10-12
Moreover, the stability of Al nanoparticles in hot water is of
practical engineering significance, as it is required for preparing the slurry during the Al-based green propellants fabrication.13-14
Therefore, improving the stability of Al
nanoparticles is of great significance for their practical applications in the energetic materials field. Surface passivation of Al nanoparticles is a common method to enhance the stability of Al nanoparticles.15-25
The passivation films can be classified into two
categories depending on the materials, both of which should have good oxidation resistance and thin enough to keep the weight percentage of metallic Al.15-16
The
first type is organic coating such as toluene, isopropyl alcohol, perfluorodecalin, alkyl-substituted epoxides and varieties of organic acids.16-23
These organic coatings
can effectively resist the humidity, however, they are still permeable to oxygen and water at high temperatures, which can lead to the oxidation of internal metallic Al.22 The second type involves inorganic passivation film represented by alumina (Al2O3) and silica (SiO2), which can be formed by either internal oxidation or external chemical coating.15,19,24-25
Although the Al2O3 coated Al nanoparticles exhibit good
stability at 60 ºC with the relative humidity of 90%, the thick Al2O3 coatings (≥ 5 nm) prepared by thermal oxidation process have greatly reduced the weight percentage of metallic Al.15,19
Moreover, the Al2O3 coatings has exhibited a limited resistance
under more harsh conditions, such as higher temperature and humidity, which will lead to the further loss of metallic Al.
The failure of Al2O3 coatings is usually
attributed to the continued reaction between the metallic Al and AlOOH formed by the reaction of Al2O3 coatings and water.
Overall, developing a new method of
ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 27
uniform coating and thin passivation with high oxidation resistance opens up opportunities to enhance the stability of Al nanoparticles. Based on the self-limiting half reactions, atomic layer deposition (ALD) has been widely used to prepare uniform films on the nanoscale, which is advantageous in precisely controlling composition and thickness of films.26-27
We have successfully
utilized ALD method to passivate nanoparticles for their applications in catalysis, energy and medical fields.28-32
In this work, we report the use of ultrathin zirconia
(ZrO2) coatings prepared by ALD method to passivate Al nanoparticles.
The ZrO2
passivated Al nanoparticles exhibited higher oxidation resistance than Al nanoparticles with Al2O3 native oxide or Al2O3 coatings prepared by ALD method. Moreover, less than 1 nm of ZrO2 coatings is required for complete oxidation resistance in water at 80 ºC, which keeps the weight percentage of metallic Al compared to that of pure Al nanoparticles.
At last, the passivation mechanism of
ultrathin ZrO2 film on Al nanoparticles is investigated.
2. EXPERIMENTAL METHODS Al nanoparticles (99.5%, Aladdin) with the size of 20 ~ 200 nm were used without any pretreatment.
The untreated Al nanoparticles is labeled as Al@Al2O3,
where Al2O3 indicates the native oxide on commercial Al nanoparticles.
As shown
in Figure 1, the formed core-shell structures are named as Al@Al2O3@Al2O3-n and Al@Al2O3@ZrO2-n after the Al2O3 and ZrO2 ALD coating, where n means the ALD cycles.
All ALD processes were performed in our designed fluidized bed reactor,
which was reported in our previous study.33 In detail, the deposition of ZrO2 was performed at 150 ºC using Tetrakis(dimethylamino)zirconium (Zr(NMe2)4) and H2O as precursors.
The steel bottle contained Zr precursors were heated to 80 ºC to
ensure sufficient vapor pressure of Zr precursors.
The connecting steel pipes were
heated to 120 ºC during ZrO2 deposition to avoid precursors condensation.
The
ALD of Al2O3 was performed at 120 ºC with trimethylaluminum (TMA) and water (H2O) as precursors.
For a typical ALD process, about 200 mg Al nanoparticles are
loaded in the designed powder holder with the top and bottom being sealed by ACS Paragon Plus Environment
Page 5 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
stainless steel mesh.
Prior to ALD, the Al nanoparticles are fluidized by 50 mL/min
of ultrahigh purity N2 for 20 min at the reaction temperature.
One ALD cycle for
Al2O3 or ZrO2 consists of the following four steps: (1) 90 s pulse of Al or Zr precursor; (2) a purging time of 120 s; (3) 90 s pulse of H2O; (4) a purging time of 120 s.
The mass of oxide coatings with different cycles was measured by analytical
balance.
Figure 1. Scheme of Al2O3 and ZrO2 ALD coating on Al nanoparticles. The specific surface area of oxide coated samples was measured by N2 adsorption (Micromeritics ASAP 2020) after degassing treatment in a vacuum oven at 80 ºC for 5 hours.
X-ray diffraction (XRD) patterns were collected on a PANalytical
X'Pert PRO diffractometer, using Cu Kα radiation with λ = 1.5406 Å.
The
morphologies of oxide coated Al nanoparticles were characterized by scanning electron microscopy (SEM, Quanta 200) and transmission electron microscopy (TEM, Tecnai G2 F30, FEI, Inc.). using TEM.
The thickness of oxide coating layers was measured
The weight percentage of metallic Al (Al wt%) is defined as: Al wt% =
M -mAl2O3 M +moxide-ALD
where mAl2O3 is the mass of native oxide, which is calculated by the thickness measured from the TEM images. coating
and
total
mass
moxide-ALD and M are the mass gain after ALD of
Al
nanoparticles,
respectively.
Thermogravimetry/differential thermal analyzer (TG/DTA, Diamond, PerkinElmer Instruments) was used to measure the metallic Al content and exothermic ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
performance of passivated Al nanoparticles.
Page 6 of 27
All TG/DTA measurements were
performed with the heating rate of 20 ºC/min in air ambient and a gas flow rate of 40 ml/min. In order to evaluate the stability of Al nanoparticles with oxide coatings, the accelerated aging test of oxide coated Al nanoparticles in hot water at different temperatures were conducted by monitoring the volume of released H2.34-35
All tests
were carried out in a round-bottom flask with its temperature controlled by water bath.
For each test, 100 mg Al nanoparticles and 4 mL deionized water were added
into the round-bottom flask.
The volume of released H2 gas was measured by a
graduated cylinder using the dehydration method.
The conversion yield (%) was
defined as the volume ratio of released H2 gas (V) and the theoretical volume after 100 mg pure Al nanoparticles being oxidized completely (V0).34-35
3. RESULT AND DISCUSSION 3.1 ALD growth of ZrO2 and Al2O3 The mass gains of oxides coated Al nanoparticles (Al@Al2O3@ZrO2 and Al@Al2O3@Al2O3) are shown in Figure 2(a), which exhibit linear increase with respect to ALD cycles of ZrO2 and Al2O3.
The mass gain rates of ZrO2 and Al2O3
coatings are about 1.76 mg/cycle and 1.10 mg/cycle, respectively.
According to the
specific surface area of Al nanoparticles (16.26 m2/g) and the densities of passivation films, the growth rates of ZrO2 and Al2O3 on Al nanoparticles can be estimated to be 0.93 ± 0.02 Å/cycle and 1.2 ± 0.05 Å/cycle, which are similar to that on planar substrates (Figure S1 in supporting information (SI)).36-38
The XRD patterns of Al
nanoparticles, as well as 50 cycles of ZrO2 and Al2O3 coated Al nanoparticles (Al@Al2O3@ZrO2-50 and Al@Al2O3@Al2O3-50) are shown in Figure 2(b).
All the
diffraction patterns can be well assigned to the characteristic reflection planes of standard Al metal phase (JCPDS No. 89-2837).
There are no typical crystalline
peaks of ZrO2 and Al2O3 observed in the XRD patterns of oxide coated Al nanoparticles, indicating the amorphous nature of coating layers.
The amorphous
coating, similar to corrosion resistance films, is of importance to avoid the grain ACS Paragon Plus Environment
Page 7 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
boundary defects.
The calculated average crystallite sizes of Al@Al2O3,
Al@Al2O3@Al2O3-50 and Al@Al2O3@ZrO2-50 from the XRD profile using the Scherrer equation are 32.6 nm, 35.2 nm and 35.7 nm, indicating that the ALD process has not altered the crystal structures of the metallic Al cores.
The weaker diffraction
peaks of Al@Al2O3@Al2O3-50 and Al@Al2O3@ZrO2-50 than that of pristine Al nanoparticles may be due to the mass ratio’s decrease of Al nanoparticles as shown in Figure 2(a).
Figure 2. (a) The mass gains and Al nanoparticles’ mass ratios of Al@Al2O3@Al2O3 and Al@Al2O3@ZrO2 as the function of ALD cycles, (b) XRD patterns of Al nanoparticles, Al@Al2O3@Al2O3-50 and Al@Al2O3@ZrO2-50.
The TEM images in Figure 3(a) show that Al nanoparticles are spherical in shape with a size of 20 ~ 200 nm.
Clearly, Al nanoparticles exhibit a core-shell structure
with the native oxide of amorphous Al2O3 as shown in Figure 3(b).
The measured d
spacing of 0.23 nm is assigned to the (111) surface of metallic Al. thickness of Al2O3 shell is about 5.7 ± 0.7 nm.
The average
According to the density of Al2O3,
the calculated weight percentage of metallic Al for Al nanoparticles without pretreatment is about 88%, which is close to that in previous studies.22,39
The TEM
images of Al@Al2O3@ZrO2-50 in Figure 3(c) and (d) exhibit two shells on the metallic Al cores, which are the Al2O3 native oxide and grown ZrO2.
Figure 3(e) and
(f) also exhibit the double shell structure for Al@Al2O3@Al2O3-50.
The XPS results
in Figure S2 show that the organic residues are limited in the coated oxide layer.
ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 27
Moreover, both Al2O3 and ZrO2 shells are amorphous phase, which agrees well with the XRD patterns.
The measured thicknesses of ZrO2 and Al2O3 shells are about 4.5
nm and 6.1 nm, respectively, which agree well with their linear growth rates estimated by the mass gains.
Figure 3. (a)(b) TEM images of Al nanoparticles, (c)(d) TEM images of Al@Al2O3@ZrO2-50, and (e)(f) TEM images of Al@Al2O3@Al2O3-50.
3.2 Stability tests of Al@Al2O3@ZrO2 and Al@Al2O3@Al2O3 The effectiveness of coated oxides passivation has been evaluated by performing the accelerated aging test in hot water at different temperatures, in which the yields of hydrogen gas are monitored.
As shown in Figure 4(a), no hydrogen gas is detected
when Al nanoparticles stay in water at 40 ºC, which is due to the resistance of Al2O3 native oxide.
When the temperature increases to 60 ºC, the Al nanoparticles start to
react with water after a stabilization period of 17.6 min.
The Al nanoparticles can be
completely oxidized at 60 ºC with the max hydrogen gas yield of 88.6%, which is consistent with the calculated weight percentage of metallic Al after considering the mass of Al2O3 native oxide.
Moreover, when the temperature increases to 80 ºC, the
reaction between Al nanoparticles and water is more rapid and violent with the ACS Paragon Plus Environment
Page 9 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
stabilization period of 3.8 min and completed reaction time of 4.2 min. Figure 4(b) shows the hydrogen gas yields for different ALD cycles of Al@Al2O3@Al2O3 samples at 60 ºC.
Although the stabilization periods are
lengthened with increasing of ALD cycles, the metallic Al can still be completely oxidized by water within 30 min for Al@Al2O3@Al2O3-100, indicating that both Al2O3 native oxide and coated oxide cannot resist the oxidation.
For the
Al@Al2O3@ZrO2 samples under the same tests at 60 ºC, it is interesting that the oxidation rate can be greatly decreased after only 1 cycle coating of ZrO2 as shown in Figure 4(c).
Moreover, 5 cycles of ZrO2 can completely resist the oxidation of
metallic Al by water at 60 ºC, which can be related to the formation of continuous film on Al nanoparticles.
When the temperature increases to 80 ºC, the oxidation
reaction can also be completely resisted by just increasing several ALD cycles of ZrO2 as shown in Figure 4(d).
Figure 4. The yields of hydrogen gas as the function of time for (a) Al nanoparticles in water at 40 ºC, 60 ºC and 80 ºC, (b) Al@Al2O3@Al2O3 in water at 60 ºC, (c) Al@Al2O3@ZrO2 in water at 60 ºC and (d) Al@Al2O3@ZrO2 in water at 80 ºC.
ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
The
TG/DTA
analysis
of
Al
nanoparticles,
Page 10 of 27
Al@Al2O3@ZrO2-8
Al@Al2O3@Al2O3-50 has been performed as shown in Figure 5.
and
The mass gain of
Al nanoparticles at about 550 ºC is assigned to the oxidation of metallic Al cores.40 The oxidation temperatures of Al nanoparticles after ZrO2 and Al2O3 coating will be increased due to the enhancement of their stability.
The mass gains of Al
nanoparticles, Al@Al2O3@ZrO2-8 and Al@Al2O3@Al2O3-50 are 78.3%, 72.5%, and 60.8%, respectively.
The mass gains due to the oxidation of metallic Al cores are
consistent with the calculated weight percentages of metallic Al after considering the mass of Al2O3 native oxide and coated oxides.
The DTA profiles exhibit the
exothermic process of Al@Al2O3, Al@Al2O3@ZrO2-8 and Al@Al2O3@Al2O3-50 at 544.2 ºC, 549.5 ºC and 588.7 ºC.
The released heat of Al@Al2O3@ZrO2-8
determined by measuring the area of the DTA peaks is slightly less than Al nanoparticles.
However, the released heat of Al@Al2O3@Al2O3-50 is greatly
decreased compared to Al nanoparticles.
The results indicate that the oxidation of Al
nanoparticles just has slightly been retarded after the ultrathin ZrO2 coating, which is important for the applications in solid fuels and Al-based green propellants.
The
similar areas of the exothermic peaks of Al@Al2O3 and Al@Al2O3@ZrO2-8 also agree well with the mostly remained weight percentage of metallic Al for Al@Al2O3@ZrO2-8 (82.2 wt%) compared to that of Al@Al2O3 (88 wt%).
ACS Paragon Plus Environment
Page 11 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
Figure 5. TG/DTA analysis of Al nanoparticles, Al@Al2O3@ZrO2-8 and Al@Al2O3@Al2O3-50.
3.3 Morphologies of oxide coated Al nanoparticles after stability tests Figure 6(a) and (b) show the morphologies of Al@Al2O3@ZrO2-8 before and after stability tests at 80 ºC. Clearly, the samples can keep the spherical shape well, which is consistent with the test of hydrogen gas yield in Figure 4(d).
TEM image in
Figure 6(c) shows the ZrO2 coatings on the surface of Al@Al2O3@ZrO2-8, in accordance with the element line scanning result in Figure 6(d).
The thickness of
ZrO2 is about 0.6 nm, agreeing well with the growth rate of ZrO2 as the previous discussion of Figure 2(a).
As a comparison, the SEM image of Al@Al2O3@ZrO2-6
after stability test presents the porous surface as shown in Figure S3, which indicates the water have broken the ZrO2 coatings and reacted with the metallic Al cores.
The
morphologies of Al@Al2O3@Al2O3-50 before and after stability test are also presented in Figure 6(e) and (f).
The particles with irregular morphology in Figure
6(f) can be attributed to the Al2O3 products after stability test, indicating the complete oxidation as the hydrogen gas yield in Figure 4(b).
Figure 6. SEM images of Al@Al2O3@ZrO2-8 (a) before and (b) after stability test at ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
80 ºC.
Page 12 of 27
(c) TEM image and (d) element line scanning of Al@Al2O3@ZrO2-8 after
stability test.
SEM images of Al@Al2O3@Al2O3-50 (e) before and (f) after stability
test at 60 ºC.
3.5 Proposed passivation mechanism The passivation mechanism of ZrO2 and Al2O3 coated Al nanoparticles has been discussed.
When the Al@Al2O3@Al2O3 samples stay into water at 60 ºC, the Al2O3
coatings on the surface can react with water and generate hydration products (AlOOH), which is reactive to the metallic Al core by forming hydrogen gas.41-42
As
shown in Figure 7(a), the generated hydrogen gas can break the Al2O3 coatings and escape from the surface, which results in the failure of Al2O3 passivation film. Therefore, Al2O3 coating could not completely block the reaction between Al2O3 and water no matter of its thickness.
On the other hand, the ultrathin ZrO2 coating can
greatly enhance the hydrophobicity of Al2O3 film as shown in Figure S4.
The
previous studies have also reported that the Al2O3/ZrO2 laminated film can exhibit high permeation barrier to water, which is due to the formation of ZrAlxOy phase at the interface between Al2O3 and ZrO2 films.43-44
Therefore, the continuously
ultrathin ZrO2 coatings on Al nanoparticles could completely resist the oxidation reaction as shown in Figure 7(b).
The ZrO2 coating should be thick enough to avoid
the formation of cracks due to the existence of tensile stress in the ZrO2 coating for Al@Al2O3@ZrO2, whose thermal expansion coefficient is smaller than that of Al nanoparticles.45-46
ACS Paragon Plus Environment
Page 13 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
Figure 7. The schematic diagram of passivation mechanism for (a) Al@Al2O3@Al2O3 and (b) Al@Al2O3@ZrO2.
4. CONCLUSION In this paper, ultrathin ZrO2 has been coated on Al nanoparticles to enhance the stability using ALD method.
The Al@Al2O3@ZrO2-8 exhibits excellent stability in
water at 80 ºC, with 82.2 wt% of metallic Al, maintaining about 93.4% of pure Al nanoparticles.
In comparison, the Al@Al2O3@Al2O3 cannot resist the oxidation by
water at 60 ºC due to the reactivity between Al2O3 and water.
The passivation
mechanism of ZrO2 coatings can be attributed to their structural stability and enhanced hydrophobicity to water.
Our work on the enhanced stability of Al
nanoparticles in hot water can enable their safe applications in energy field.
■ ASSOCIATED CONTENT Supporting Information Growth rates of ZrO2 and Al2O3 on planar substrate; XPS characterizations of Al nanoparticles, Al@Al2O3@Al2O3-50 and Al@Al2O3@ZrO2-8; SEM images of Al@Al2O3@ZrO2-6 before and after stability test at 80 ºC. Water contact angle characterizations of Al2O3 film and Al2O3/ZrO2 laminate film. This material is available free of charge via the Internet at http://pubs.acs.org.
ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 27
■ AUTHOR INFORMATION Corresponding Authors *E-mail:
[email protected] (R. C.). *E-mail:
[email protected] (X. L.).
Notes The authors declare no competing financial interest.
■ ACKNOWLEDGMENTS This work was supported by the National Natural Science Foundation of China (51575217) and the China Postdoctoral Science Foundation (2018M630856).
X. L.
gratefully acknowledges the support of Postdoctoral Innovation Talents Support Program (BX20180104).
We would also like to acknowledge the technology
supports from the Analytic Testing Center and Flexible Electronics Research Center of HUST.
REFERENCES (1) Jayaraman, K.; Anand, K. V.; Chakravarthy, S. R.; Sarathi, R., Effect of Nano-aluminium in Plateau-Burning and Catalyzed Composite Solid Propellant Combustion. Combust. Flame 2009, 156, 1662-1673. (2) Day, E. S.; Morton, J. G.; West, J. L., Nanoparticles for Thermal Cancer Therapy. J. Biomech. Eng. 2009, 131, 074001. (3) Newell, A.; Thampi, K. R., Novel Amorphous Aluminum Hydroxide Catalysts for Aluminum-water Reactions to Produce H2 on Demand. Int. J. Hydrogen Energy 2017, 42, 23446-23454. (4) Yavor, Y.; Goroshin, S.; Bergthorson, J. M.; Frost, D. L.; Stowe, R.; Ringuette, S., Enhanced Hydrogen Generation from Aluminum-water Reactions. Int. J. Hydrogen Energy 2013, 38, 14992-15002. (5) Epshteyn, A.; Weismiller, M.R.; Huba, Z.J.; Maling, E. L.; Chaimowitz, A.S., ACS Paragon Plus Environment
Page 15 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
Optimization of a high energy Ti-Al-B nanopowder fuel. Energy Fuel 2017, 31, 1811-1819. (6)
Yan,
N.;
Qin, L.;
Hao,
H.; Hui,
L.;
Zhao,
F.; Feng,
H.,
Iron
oxide/aluminum/graphene energetic nanocomposites synthesized by atomic layer deposition: Enhanced energy release and reduced electrostatic ignition hazard. Appl. Surf. Sci. 2017, 408, 51-59. (7) Li, Y.; Song, W.; Xie, C.; Zeng, D.; Wang, A.; Hu, M., Influence of Humidity on the Thermal Behavior of Aluminum Nanopowders. Mater. Chem. Phys. 2006, 97, 127-131. (8) Vlaskin, M. S.; Shkolnikov, E. I.; Bersh, A. V., Oxidation Kinetics of Micron-Sized Aluminum Powder in High-Temperature Boiling Water. Int. J. Hydrogen Energy 2011, 36, 6484-6495. (9) Pei, H. B.; Liu, Y.; Ren, H., Nano Aluminum Powders Oxidation in CO2 and O2 Environments. Adv. Mater. Res. 2013, 771, 113-117. (10) Sundaram, D. S.; Yang, V.; Zarko, V. E., Combustion of Nano Aluminum Particles (Review). Combust. Explos. Shock Waves 2015, 51, 173-196. (11) Litrico, G.; Proulx, P.; Gouriet, J. B.; Rambaud, P., Controlled Oxidation of Aluminum Nanoparticles. Adv. Powder Technol. 2015, 26, 1-7. (12) Rai, A.; Park, K.; Zhou, L.; Zachariah, M. R., Understanding the Mechanism of Aluminum Nanoparticle Oxidation. Combust. Theory Model. 2006, 10, 843-859. (13) Connell, J.; Terrence L.; Risha, G. A.; Yetter, R. A.; Yang, V.; Son, S. F., Combustion of Bimodal Aluminum Particles and Ice Mixtures. Int. J. Energ. Mater. Chem. Propul. 2012, 11, 259-273. (14) Jun, J. Y.; Lee, B.-J.; Song, D. J., Measurement of burning velocity for bare strand casted with a frozen mixture of nano/micro-aluminum particles and water. J. Mech. Sci. Technol. 2016, 30, 2409-2413. (15) Mathe, V. L.; Varma, V.; Raut, S.; Nandi, A. K.; Pant, A.; Prasanth, H.; Pandey, R. K.; Bhoraskar, S. V.; Das, A. K., Enhanced Active Aluminum Content and Thermal Behaviour of Nano-aluminum Particles Passivated during Synthesis using Thermal Plasma Route. Appl. Surf. Sci. 2016, 368, 16-26. ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
(16) Crouse, C. A.; Pierce, C. J.; Spowart, J. E., Influencing Solvent Miscibility and Aqueous Stability of Aluminum Nanoparticles through Surface Functionalization with Acrylic Monomers. ACS Appl. Mater. Interfaces 2010, 2, 2560-2569. (17) Shahravan, A.; Desai, T.; Matsoukas, T., Passivation of Aluminum Nanoparticles by Plasma-enhanced Chemical Vapor Deposition for Energetic Nanomaterials. ACS Appl. Mater. Interfaces 2014, 6, 7942-7947. (18) Jouet, R. J.; Warren, A. D.; Rosenberg, D. M.; Bellitto, V. J.; Park, K.; Zachariah, M. R., Surface Passivation of Bare Aluminum Nanoparticles Using Perfluoroalkyl Carboxylic Acids. Chem. Mater. 2005, 17, 2987-2996. (19) Kwon, Y.-S.; Gromov, A. A.; Ilyin, A. P.; Rim, G.-H., Passivation Process for Superfine Aluminum Powders Obtained by Electrical Explosion of Wires. Appl. Surf. Sci. 2003, 211, 57-67. (20) Chung, S. W.; Guliants, E. A.; Bunker, C. E.; Hammerstroem, D. W.; Deng, Y.; Burgers, M. A.; Jelliss, P. A.; Buckner, S. W., Capping and Passivation of Aluminum Nanoparticles Using Alkyl-Substituted Epoxides. Langmuir 2009, 25, 8883-8887. (21) Klaumünzer, Martin.; Hubner, Jakob.; Spitzer, Denis.; Kryschi, Carola., Surface Functionalization and Electrical Discharge Sensitivity of Passivated Al Nanoparticles. ACS Omega 2017, 2, 52-61. (22) Kwon, Y.-S.; Gromov, A. A.; Strokova, J. I., Passivation of the Surface of Aluminum Nanopowders by Protective Coatings of the Different Chemical Origin. Appl. Surf. Sci. 2007, 253, 5558-5564. (23) Flannery, M.; Desai, T. G.; Matsoukas, T.; Lotfizadeh, S.; Oehlschlaeger, M. A., Passivation and Stabilization of Aluminum Nanoparticles for Energetic Materials. J. Nanomater. 2015, 2015, 1-12. (24) Kotov, Yu. A.; Beketov, I. V.; Medvedev, A. I.; Timoshenkova, O. R. Synthesizing Aluminum Nanoparticles in an Oxide Shell. Nanotechnol. Russia 2009, 4, 354-358. (25) Cheng, Z.-P.; Yang, Y.; Li, F.-S.; Pan, Z.-H., Synthesis and Characterization of Aluminum Particles coated with Uniform Silica Shell. Trans. Nonferrous Metals Soc. China 2008,18,378-382. ACS Paragon Plus Environment
Page 16 of 27
Page 17 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
(26) George, S. M., Atomic Layer Deposition: An Overview. Chem. Rev. 2010, 110 ,111-131. (27) Knez, M.; Nielsch, K.; Niinisto, L., Synthesis and Surface Engineering of Complex Nanostructures by Atomic Layer Deposition. Adv. Mater. 2007, 19, 3425-3438. (28) Duan, C.-L.; Deng, Z.; Cao, K.; Yin, H.-F.; Shan, B.; Chen, R., Surface Passivation of Fe3O4 Nanoparticles with Al2O3 via Atomic Layer Deposition in a Rotating Fluidized Bed Reactor. J. Vac. Sci. Technol. A 2016, 34, 04C103. (29) Chen, R.; Duan, C.-L.; Liu, X.; Qu, K.; Tang, G.; Xu, X.-X.; Shan, B., Surface Passivation of Aluminum Hydride Particles via Atomic Layer Deposition. J. Vac. Sci. Technol. A 2017, 35, 03E111. (30) Cao, K.; Shi, L.; Gong, M.; Cai, J.; Liu, X.; Chu, S.; Lang, Y.; Shan, B.; Chen, R., Nanofence Stabilized Platinum Nanoparticles Catalyst via Facet-Selective Atomic Layer Deposition. Small 2017, 13, 1700648. (31) Liu, X.; Zhu, Q.-Q.; Lang, Y.; Cao, K.; Chu, S.-Q.; Shan, B.; Chen, R.,Oxide-Nanotrap-Anchored Platinum Nanoparticles with High Activity and Stintering Resistance by Area-Selective Atomic Layer Deposition. Angew. Chem. Int. Ed. 2017, 56, 1648-1652. (32) Cai, J.-M.; Zhang, J.; Cao, K.; Gong, M.; Lang, Y.; Liu, X.; Chu, S.-Q. ; Shan, B.; Chen, R., Selective Passivation of Pt Nanoparticles with Enhanced Sintering Resistance and Activity toward CO and Activity toward CO Oxidation via Atomic Layer Deposition. ACS Appl. Nano Mater. 2018, 1, 522-530. (33) Duan, C.-L.; Zhu, P.-H.; Deng, Z.; Li, Y.; Shan, B.; Fang, H.-S.; Feng, G.; Chen, R., Mechanistic Modeling Study of Atomic Layer Deposition Process Optimization in a Fluidized Bed Reactor. J. Vac. Sci. Technol. A 2017, 35, 01B102. (34) Rong, S.; Baozhong, Z.; Yunlan, S., The Effect of NiCl2 and Na2CO3 on Hydrogen Production by Al/H2O System. Int. J. Hydrogen Energy 2017, 42, 3586-3592. (35) Liu, Y.; Liu, X.; Chen, X.; Yang, S.; Wang, C., Hydrogen Generation from Hydrolysis of Activated Al-Bi, Al-Sn Powders Prepared by Gas Atomization Method. ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Int. J. Hydrogen Energy 2017, 42, 10943-10951. (36) Van Hemmen, J.; Heil, S.; Klootwijk, J.; Roozeboom, F.; Hodson, C.; Van de Sanden, M.; Kessels, W., Plasma and Thermal ALD of Al2O3 in a Commercial 200 mm ALD Reactor. J. Electrochem. Soc. 2007, 154, G165-G169. (37) Dingemans, G.; Van de Sanden, M.; Kessels, W., Influence of the Deposition Temperature on the c-Si Surface Passivation by Al2O3 Films Synthesized by ALD and PECVD. Electrochem. Solid-State Lett. 2010, 13, H76-H79. (38) Blanquart, T.; Niinisto, J.; Aslam, N.; Banerjee, M.; Tomczak, Y.; Gavagnin, M.; Longo, V.; Puukilainen, E.; Wanzenboeck, H. D.; Kessels, W. M. M.; Devi, A.; Hoffmann-Eifert, S.; Ritala, M.; Leskela, M., [Zr(NEtMe)2(guan-NEtMe)2] as a Novel Atomic Layer Deposition Precursor: ZrO2 Film Growth and Mechanistic Studies. Chem. Mater. 2013, 25, 3088-3095. (39) Gromov, A.; Ilyin, A.; Forter-Barth, U.; Teipel, U., Characterization of Aluminum Powders: II. Aluminum Nanopowders Passivated by Non-Inert Coatings. Propellants, Explos., Pyrotech. 2006, 31, 401-409. (40) Foley, T. J.; Johnson, C. E.; Higa, K.T., Inhibition of Oxide Formation on Aluminum Nanoparticles by Transition Metal Coating. Chem. Mater. 2005, 17, 4086-4091. (41) Deng, Z. Y.; Ferreira, J. M. F.; Yoshihisa, T.; Ye, J., Physicochemical Mechanism for the Continuous Reaction of γ-Al2O3-Modified Aluminum Powder with Water. J. Am. Ceram. Soc. 2007, 90, 1521-1526. (42) Bunker, B. C.; Nelson, G. C.; Zavadil, K.; Barbour, J. C.; Wall, F. D.; Sullivan, J. P.; Windisch, C. F.; Engelhard, M. H.; Baer, D. R., Hydration of Passive Oxide Films on Aluminum. J. Phys. Chem. B 2002, 106, 4705-4713. (43) Oh, J.; Shin, S.; Park, J.; Ham, G.; Jeon, H., Characteristics of Al2O3/ZrO2 Laminated Films Deposited by Ozone-Based Atomic Layer Deposition for Organic Device Encapsulation. Thin Solid Films 2016, 599, 119-124. (44) Lee, S.; Choi, H.; Shin, S.; Park, J.; Ham, G.; Jung, H.; Jeon, H., Permeation Barrier Properties of an Al2O3/ZrO2 Multilayer Deposited by Remote Plasma Atomic Layer Deposition. Curr. Appl. Phys. 2014, 14, 552-557. ACS Paragon Plus Environment
Page 18 of 27
Page 19 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
(45) Nix, F.C.; MacNair, D.; The Thermal Expansion of Pure Metals: Copper, Gold, Aluminum, Nickel, and Iron. Phys. Rev.1941, 60, 597-605. (46) Haggerty, R. P.; Sarin, P.; Apostolov, Z. D.; Driemeyer, P. E.; Kriven, W. M.; Gauckler, L., Thermal Expansion of HfO2 and ZrO2. J. Am. Ceram. Soc. 2014, 97, 2213-2222.
ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure1 215x126mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 20 of 27
Page 21 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
Figure2 215x84mm (300 x 300 DPI)
ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure3 215x143mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 22 of 27
Page 23 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
Figure4 195x171mm (300 x 300 DPI)
ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure5 273x213mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 24 of 27
Page 25 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
Figure6 215x141mm (300 x 300 DPI)
ACS Paragon Plus Environment
ACS Applied Nano Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure7 215x124mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 26 of 27
Page 27 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Nano Materials
TOC 1054x546mm (150 x 150 DPI)
ACS Paragon Plus Environment