Subscriber access provided by La Trobe University Library
Article
Water-Insoluble Hydrophilic Electrospun Fibrous Mat of Cyclodextrin-Epichlorohydrin Polymer as Highly Effective Sorbent Asli Celebioglu, Fuat Topuz, and Tamer Uyar ACS Appl. Polym. Mater., Just Accepted Manuscript • DOI: 10.1021/acsapm.8b00034 • Publication Date (Web): 29 Nov 2018 Downloaded from http://pubs.acs.org on December 2, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
1
Water-Insoluble Hydrophilic Electrospun Fibrous Mat
2
of Cyclodextrin-Epichlorohydrin Polymer
3
as Highly Effective Sorbent
4
Asli Celebioglu, Fuat Topuz and Tamer Uyar*
5
Institute of Materials Science & Nanotechnology, UNAM-National Nanotechnology Research
6
Center, Bilkent University, 06800 Ankara, Turkey
7 8
*
To whom correspondence should be addressed: Prof. T. Uyar (
[email protected]) Phone: +90 (312) 290 8987
9 10 11 12 13 14 15 16 17 18
1 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 2 of 27
19
ABSTRACT. The electrospinning of cyclodextrin (CD) functional fibers has emerged as a
20
promising strategy to develop high performance fibers with great promising applications in
21
many fields, including water treatment. Here, we report the fabrication of water-insoluble
22
hydrophilic poly(cyclodextrin-epichlorohydrin) (poly(CD-ECH)) fibers by the electrospinning
23
of an aqueous solution of hydroxypropyl--CD (HP--CD) and ECH, and their cross-linking
24
through heat treatment. The viscosity and time-dependent oscillatory deformation tests
25
revealed that the cross-linking reactions between CD and ECH are highly sensitive to
26
temperature, and main cross-linking takes place after the heat-treatment of the electrospun
27
mat, which was confirmed by FTIR and XPS analyses. The water contact-angle (WCA)
28
measurement showed the hydrophilicity of the poly(CD-ECH) mat, which could maintain its
29
fibrous structure in water. Furthermore, the poly(CD-ECH) fibers were stable in various
30
organic solvents, i.e., acetonitrile, ethanol, methanol, trichloromethane, dimethylformamide
31
and dimethyl sulfoxide. Thermal gravimetric analysis (TGA) showed the cross-linking
32
increased thermal stability of the poly(CD-ECH) fibers compared to the pristine CD, while
33
XRD analysis revealed the amorphous structure of the poly(CD-ECH) fibers. As a proof-of-
34
concept study, the fiber and granule forms of the poly(CD-ECH) were exploited for the
35
scavenging of an organic dye (i.e., phenolphthalein) and a polycyclic aromatic hydrocarbon
36
(PAH) (i.e., phenanthrene) from their aqueous solutions, and rapid removal was observed for
37
the poly(CD-ECH) fibers than its granule form. Given that the hydrophilic nature of the
38
poly(CD-ECH) electrospun mat, this high scavenging performance can be ascribed to the
39
presence of high active CD content in the poly(CD-ECH) fibers, along with their high specific
40
surface area.
41
Keywords.
42
Cyclodextrin,
electrospinning,
nanofibers,
inclusion-complexation,
phenolphthalein, phenanthrene, water treatment
43 2 ACS Paragon Plus Environment
Page 3 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
44
INTRODUCTION
45
Cyclodextrin (CD) is a cyclic oligomer of glucose with a unique torus-like shape with a
46
central hydrophobic cavity interior and a hydrophilic exterior.1 CDs are inherently nontoxic2
47
and edible molecules,3 and have been widely used as solubilization enhancers for poorly
48
soluble drug molecules,4 drug carriers,5-6 food3 and tissue engineering7, and textile industry8.
49
Likewise, materials derived from CDs have taken considerable interest in a wide spectrum of
50
applications, in which each CD molecule can involve in the removal of water
51
micropollutants.9-13 In one example, Alsbaiee et al. reported the synthesis of porous -CD
52
polymers for the removal of various organic micropollutants, i.e., 2, 4-dichlorophenol, 2-
53
naphthol, 1-napthylamine, metolachlor, bisphenol A, bisphenol S, ethinyl oestradiol,
54
propranolol hydrochloride, from water.14 The authors used tetrafluoroterephthalonitrile as a
55
linker for the production of porous CD polymers with a surface area as high as 263 m2 g-1,
56
which allowed rapid removal of organic pollutants. The same research group used
57
decafluorobiphenyl as a cross-linker of -CD moieties under nucleophilic aromatic
58
substitution conditions and exploited the CD networks for the scavenging of environmentally
59
persistent perfluorooctanoic acid (PFOA).15 The materials could sequester PFOA in a few
60
hours from aqueous solutions. Likewise, epichlorohydrin (ECH) cross-linked CD polymers
61
were exploited as sorbents for the removal of various types of pollutants.16-17 The sorption
62
performance of such materials can be enhanced with increasing their surface areas. In this
63
regard, the electrospinning of CD-functional nanofibers has been a focus of interest owing to
64
their high specific surface area (i.e., more active CD content) and highly porous structure,
65
which enable faster and efficient removal of organic micropollutants.
66
The embedment of CD molecules via blending with a polymeric carrier is a simple route to
67
produce CD-functional electrospun fibers. But, the possibility of leaching of CD molecules
68
from the fiber matrix restricts their reuse18 unless they are chemically attached to the fibrous 3 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 27
69
network19. Further, their embedment within the polymeric matrix can substantially block the
70
CD cavity to able to form inclusion-complexation. Many studies have been reported using this
71
strategy due to its simplicity. In this regard, Zhao et al. reported the preparation of CD-
72
functional fibers using the mixed solution of poly(acrylic acid), citric acid and -CD. The
73
electrospinning and thereafter, the heat-treatment of the resultant fibers led to CD-functional
74
fibers, which were exploited for the removal of methylene blue with a maximum adsorption
75
capacity of 826.45 mg/g.20 -CD was also loaded in the poly(ether sulfone) (PES) nanofibers
76
and implemented for water depollution from hormone estradiol and pesticide chlorpyrifos.21
77
The removal performance of the materials was compared with the CD-free PES fibers, and the
78
results revealed an enhanced sorption capacity with the incorporation of 10 wt.% CD. CD was
79
also used for the decoration of the fiber surface to enhance the sorption performance of fibers.
80
In this regard, Kayaci et al. reported the surface modification of polyester nanofibers with CD
81
motifs and exploited the fibers for the removal of phenanthrene.22 On the other hand, the use
82
of electrospun fibers made by only CDs would be a rational strategy with enhanced
83
performance for sorption applications.23-24 However, such fibers suffer from rapid dissolution
84
in water by reason of their uncross-linked structure.25-26 To address this problem, in our recent
85
study, we have reported the production of electrospun fibers of cross-linked CD polymers
86
using a multivalent carboxylic acid (i.e., 1,2,3,4-butanetetracarboxylic acid) functional linker
87
and their use in the efficient removal of methylene blue from water.27 Even though the
88
presence of their high potential applications, yet, there is not much strategy in the fabrication
89
of water-insoluble electrospun CD fibers. Therefore, there exists an increasing demand
90
towards the production of the insoluble CD fibers while maintaining their hydrophilic
91
structure for the snaring of pollutants from an aqueous environment through inclusion-
92
complexation.
4 ACS Paragon Plus Environment
Page 5 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
93
The proportion of active CD content in the fiber can be explored by means of inclusion-
94
complexation with phenolphthalein through UV-Vis measurements because of its color
95
change from pink to colorless with the formation of lactonoid dianion.28 Moreover, it can be
96
regarded as a water micropollutant due to its adverse health effects on animals. In this regard,
97
Dunnick et al. reported the continuous administration of phenolphthalein to mice over two
98
years using the concentrations of 0, 3 000, 6 000, and 12 000 ppm and observed multiple
99
carcinogenic effects associated with phenolphthalein uptake.29 Furthermore, Artymowicz et
100
al. reported phenolphthalein-induced toxic epidermal necrolysis in humans.30 Their findings
101
suggests that that phenolphthalein should be included in the list of drug-induced toxic
102
epidermal necrolysis (TEN). CD molecules can form ICs with phenolphthalein, and
103
particularly, -CD has shown good complexation with phenolphthalein with a rate constant of
104
3.7 x 10-7 M-1 s-1.31 Thus, the materials derived from -CD molecules would be rational
105
platforms for the removal of phenolphthalein from water. In this regard, poly(CD-ECH) fibers
106
can be used for the removal of phenanthrene, which is one of the most ubiquitous
107
environmental micropollutants. Unlike most polycyclic aromatic hydrocarbons (PAHs), the
108
water solubility of phenanthrene exceeds 1 ppm, and thus, it can be found in water at a larger
109
extent than other PAH molecules. Furthermore, the half-lives of phenanthrene in soil and
110
sediment were reported in the range of 16-126 days,32 and with time, phenanthrene can
111
contaminate water sources. Therefore, timely clean-up of PAH molecules, such as
112
phenanthrene from contaminated sites, particularly from water sources, is crucial. Like
113
phenolphthalein, CD molecules can also form IC with phenanthrene since CD presents a
114
suitable microcavity to able to host phenanthrene molecules.19, 22
115
In this study, poly(CD-ECH) fibers were produced by the electrospinning of CD molecules
116
in the presence of epichlorohydrin (ECH) as the cross-linker. Rheology was used to explore
117
the flow behavior of the electrospinning solution and their cross-linking at 25 and 50 oC over 5 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 27
118
time. Then, the electrospun fibrous mat was exposed to thermal treatment at 150 oC for the
119
cross-linking of hydroxyl moieties of CD molecules with ECH. The stability of the
120
electrospun poly(CD-ECH) fibers was explored in water and various organic solvents (i.e.,
121
trichloromethane (TCM), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), ethanol
122
(EtOH), methanol (MeOH), and acetonitrile (ACN)). As a proof-of-concept study, the
123
poly(CD-ECH) fibrous mats were used for the removal of phenolphthalein and phenanthrene
124
from aqueous solutions, and their performance was compared with the granule form of the
125
poly(CD-ECH).
126
EXPERIMENTAL SECTION
127
Materials and Methods. Hydroxypropyl--cyclodextrin (HP--CD, Cavasol® W7 HP))
128
was obtained as a gift from Wacker Chemie GmbH, Germany. Acetonitrile (ACN, ≥99.5%),
129
methanol (MeOH, ≥99.8%), ethanol (EtOH, ≥99.8%), dimethylformamide (DMF, ≥99.8%),
130
dimethyl sulfoxide (DMSO, ≥99.9%), and trichloromethane (TCM, ≥99%) were purchased
131
from Sigma Aldrich and used as received. Epichlorohydrin (ECH, 99%), phenolphthalein
132
(ACS reagent) and phenanthrene (98%) were received from Sigma Aldrich. The distilled
133
water was produced by a Millipore Milli-Q Ultrapure System.
134
Electrospinning and Cross-linking of CD-ECH Fibers. HP--CD molecules were
135
dissolved in an aqueous solution of NaOH (25% (w/v, g/mL)), and ECH (1:10 molar ratio of
136
HP--CD/ECH, nECH/HP--CD=10) was slowly added. The solution was mixed at 50 oC for few
137
minutes to increase viscosity due to partial cross-linking and thereafter, cooled down to room
138
temperature. The solution was transferred into 3 mL syringes having sharped edged metallic
139
needles of 0.6 mm inner diameter. The syringes were horizontally placed on a syringe pump,
140
and the flow rate was set to 1 mL/h for the electrospinning. A high voltage power supply
141
(Matsusada, AU series) was used to apply 15 kV. The fibers were deposited on a grounded
6 ACS Paragon Plus Environment
Page 7 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
142
stationary rectangular metal collector, which was covered by a piece of an aluminum foil. The
143
distance between needle and collector set to 10 cm. The electrospinning was performed at ~24
144
oC
145
and kept at 150
146
electrospinning of aqueous solutions of HP--CD and HP--CD/ECH was performed. After
147
thermal treatment, poly-CD fiber webs were washed with water and ethanol, respectively to
148
remove the unreacted reagents.
in an enclosed Plexiglas chamber. After the electrospinning, the fibrous mat put in an oven oC
for 5 h for the cross-linking reactions. As control fibers, the
149
Synthesis of Poly(CD-ECH) Granules. As a control material, poly(CD-ECH) granules
150
were produced using identical concentrations of the precursors: HP--CD (120% (w/v,
151
g/mL)) was dissolved in an aqueous solution of NaOH (25% (w/v, g/mL)), and thereafter,
152
ECH (nECH/HP--CD=10) was gradually added to the solution. The solution kept stirring at 50 oC
153
for few minutes, and then, left in oven at 150 oC for 5 h for cross-linking reactions.
154
Characterization. The morphology of the poly(CD-ECH) fibers and granules was explored
155
by scanning electron microscopy (SEM, Quanta 200 FEG, FEI). Prior to SEM analysis, the
156
samples were coated with 5 nm Au/Pd using a Gatan PECS 682 etching and coating system.
157
The mean diameter of the fibers was calculated from the SEM images of the fibers with
158
ImageJ software (US National Institutes of Health, USA) by analyzing 100 fibers for each
159
sample. The rheological analysis of the samples was performed with an Anton Paar Physica
160
MCR 301 rheometer. A cone-and-plate geometry was used with a gap size of 104 m and a
161
diameter of 50 mm (angle of 1o) during the experiments. Flow tests were performed in the
162
shear rate range of 10-3-103 s-1 at 50 oC. Afterwards, the solution was subjected to a dynamic
163
oscillatory deformation test at 50 oC for 90 min at the constant shear of 0.1% and frequency of
164
1 Hz. Fourier transform infrared spectroscopy (FTIR) analysis was performed using a Bruker-
165
VERTEX 70 spectrometer system. The samples were mixed with KBr and pressed to obtain
7 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 27
166
transparent pellets. The measurements were performed between 4000 and 400 cm-1 with a
167
resolution of 4 cm-1. An X-ray photoelectron spectrometer (XPS) (Thermo Scientific) was
168
used to study the chemical composition of the fiber surface. XPS was used by means of a
169
flood gun charge neutralizer system equipped with an Al K-α X-ray source (hυ=1486.6 eV).
170
High-resolution spectra were recorded for the spectral regions of C1s at a pass energy of 50
171
eV. The thermal analysis of the samples was performed using a thermogravimetric analyzer
172
(TGA, Q500, TA Instruments). The measurements were performed between 25 and 500 oC
173
with a heating rate of 20 oC under N2 atmosphere.
174
Removal of Phenolphthalein from Aqueous Solutions. Removal tests were performed
175
with a Varian Cary 5000 spectrophotometer. The measurements were performed in the
176
wavelength range of 400-800 nm to monitor changes in the concentration of phenolphthalein
177
during the treatment with the poly(CD-ECH) fibers and granules. In this regard, the fiber
178
sample (0.1 g and 6 cm * 6 cm dimensions) and granules (0.1 g) were separately transferred
179
into the bottom of quartz cuvettes containing phenolphthalein solution (0.4 mM) prepared
180
using a buffer solution (pH= 11). The reaction was performed at room temperature (25±2 oC)
181
by continuous stirring, and the spectra were collected in a fixed time interval up to 10 h.
182
Removal of Phenanthrene from Aqueous Solutions. The removal tests of phenanthrene
183
were performed using a HPLC system (Agilent 1200 Series). The separation of phenanthrene
184
molecules was performed with a Zorbax Eclipse XDB-C18 column (150 mm × 4.6 mm, 5 µm
185
particle size), and the concentration was detected at the wavelength of 254 nm. Acetonitrile
186
(100%) was used as a mobile phase at the flow rate of 0.3 mL/min, and the injection volume
187
was 10 L. Phenanthrene was dissolved in acetonitrile and afterwards, diluted in water to
188
perform filtration measurements. The fiber sample (~0.1 g and 6 cm * 6 cm dimensions) and
189
granules were treated with phenanthrene solutions (c= 1.8 ppm) at room temperature (25±2
190
oC)
up to 27 h. The calibration curve of phenanthrene was prepared using the stock solutions 8 ACS Paragon Plus Environment
Page 9 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
191
with different concentrations: 1.8, 0.9, 0.45, and 0.23 μg/ml. The curve showed a linearity
192
with R2≥0.99. The results were adapted to this calibration curve in terms of the peak area
193
under curves. Moreover, the reusability of the poly(CD-ECH) fibrous mat was explored at
194
room temperature (25±2 oC). In this regard, the poly(CD-ECH) mat was washed with
195
acetonitrile for 10 min, which led to the removal of 80% of the adsorbed phenanthrene from
196
the fibrous mats. The samples were retreated with phenanthrene solutions at room temperature
197
(25±2 oC) for 27 h, and the sorption performance was determined as previously reported.
198
RESULTS and DISCUSSION
199
The cross-linking between HP--CD and ECH takes place over primary and secondary
200
hydroxyl groups of HP--CD. A highly alkaline condition leads to the formation of alkoxide
201
groups. Bifunctional ECH reacts with the formed alkoxide groups, giving rise to water-
202
soluble CD macromolecules through polycondensation in highly branched structures.33 The
203
reaction between the hydroxyl groups of CD molecules with the epoxide ring of ECH results
204
in glyceryl bridges between neighboring CD molecules. However, ECH molecules can also
205
react themselves under alkaline conditions, leading to the homopolymers of ECH. As ECH
206
was added to the solution prior to the electrospinning, it may lead to changes on the solution
207
properties with time. In this regard, the solution viscosity becomes a critical factor for the
208
electrospinning of CD molecules due to their partial cross-linking with ECH. Further, the
209
cross-linking reactions are highly sensitive to temperature and therefore, the cross-linking
210
significantly rises with an increase in temperature. After the addition of ECH, the reaction
211
was stirred for a short time at 50 oC, and thereafter, cooled down to room temperature. Figure
212
1a shows the flow curve of the HP--CD solution containing ECH molecules (nECH/HP--
213
CD=10).
214
shear rate ( &) range of 10-3-103 Pa·s, where the solution showed a strong decrease in the
215
with increasing &. The solution did not reach to the infinite-shear viscosity (∞ range owing
The viscosity () of the electrospinning solution was explored by rheology in the
9 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 27
216
to the occurrence of the partial cross-linking reactions between precursors at the onset of the
217
measurement. While a dynamic oscillatory sweep test displays changes in shear moduli (i.e.,
218
elastic (G’) and loss (G’’)) over time at 50 oC because of cross-linking reactions (Figure 1b).
219
Initially, the loss modulus (G’’) was lower than the elastic modulus (G’), suggesting the sol-
220
state of the mixture. With time, G’ rapidly increased and could led to a densely cross-linked
221
network with a MPa level of G’, demonstrating the formation of a mechanically strong
222
network. The cross-over of G’ and G’’ was observed at 18 min, and thereafter, both moduli
223
drastically increased with time. This cross-over of both moduli can be considered as the
224
gelation point. Thus, the incubation time at 50 oC is highly critical and can lead to a cross-
225
linked network, which cannot be electrospun into fibers. The formation of a cross-linked
226
network can also be seen over the photos of the sample before and after heat treatment. Figure
227
1b (insets) shows the optical photos of the HP--CD/ECH solution before and after heat
228
treatment, where a color change to yellowish was observed. Further, the CD solution
229
transformed into a viscoelastic gel network at the inverted position. On the other hand, the
230
electrospinning solution did not lead to a gel network at 25 oC in (Figure S1). This is highly
231
critical since the electrospinning requires a steady-flow over time without any drastic changes
232
on the solution viscosity in a given time. With that, the electrospinnability of the system does
233
not significantly change over time throughout the electrospinning so that the proposed
234
concept is straightforward and reproducible.
235 10 ACS Paragon Plus Environment
Page 11 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
236
Figure 1. Rheological properties of an alkaline solution of HP--CD molecules in the
237
presence of ECH at 50 oC (nECH/HP--CD=10). (a) Viscosity () versus shear rate () and (b) the
238
respective shear elastic (G’) and loss (G’’) moduli of the solution as a function of time (t).
239
Inset photos show the CD solution before and after cross-linking at 50 oC for 90 min. cHP--CD=
240
120% (w/v, g/mL), NaOH (25% (w/v, g/mL)) and ECH ([ECH/HP--CD]=10).
241
When the viscosity of the electrospinning solution started to increase, the solution cooled
242
down to room temperature to prevent further cross-linking reactions and thereafter,
243
electrospun into fibers. The CD fibers were further kept in oven at 150 oC for 5 h for cross-
244
linking reactions, which led to the formation of the cross-linked poly(CD-ECH) fibers. The
245
optical photo of the poly(CD-ECH) fibers shows a free-standing electrospun mat whose SEM
246
analysis revealed the formation of bead-free fibers (Figure 2b-c). The cross-linking
247
mechanism was shown in Figure 2d, where neighboring CD molecules attached each other via
248
glyceryl bridges. The mats were stable in water due to the occurrence of highly efficient
249
cross-linking reactions between CD and ECH (Figure 2e), as revealed by rheological
250
characterization of the respective system. Further, water-contact angle (WCA) measurements
251
revealed the spreading of a water droplet on the fiber surface due to hydrophilic structure of
252
the fibrous mat owing to the hydrophilicity of both HP--CD and ECH and formed glyceryl
253
bridges (Figure 2f).
11 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 27
254 255
Figure 2. (a) An optical photo of the poly(CD-ECH) mat and inset photo (i) shows the
256
folded fiber mat. (b) Scanning electron micrograph of CD fibers before (b) and after (c) cross-
257
linking (cHP--CD= 120% (w/v, g/mL), NaOH (25% (w/v, g/mL)) and ECH ([ECH/HP--CD]=
258
10). (d) Cross-linking mechanism between CD and ECH, and (e) the poly(CD-ECH) mat
259
exposed to water, showing water-insoluble nature and structure stability of the poly(CD-ECH)
260
mat in water. (f) An optical photo shows the spreading of a water droplet on the poly(CD-
261
ECH) mat.
262
The electrospraying of the HP--CD molecules took place at the CD concentration of 50%
263
(w/v, g/mL) and [ECH/CD] of 8 and 10, while increasing the concentration of HP--CD to 75
264
and 100% (w/v, g/mL) led to beaded fibers (Figure S2, Supporting Information). On the other
265
hand, with increasing the CD concentration to 120% (w/v, g/mL), the electrospinning of the
266
HP--CD solution led to bead-free fibers with a mean diameter of 1.01 ±0.73 m, which is
267
higher than the ECH-free HP--CD fibers, demonstrating that the partial cross-linking of HP-
268
-CD molecules increased the viscosity and gave rise to the formation of larger fibers (Figure
269
3a). On the other hand, mean size of the fibers prior to the cross-linking was calculated as 12 ACS Paragon Plus Environment
Page 13 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
270
1.06 ±0.53 m, suggesting that cross-linking did not induce significant changes on the fiber
271
size (Figure 2b). The mean fiber diameter of the ECH-free CD system at the HP--CD
272
concentration of 160% (w/v, g/mL) was previously reported as 0.75 m25 while it increased to
273
1.01 ±0.73 m with the incorporation of ECH, suggesting that the occurrence of partial cross-
274
linking prior to the electrospinning process. This was also seen over the concentration of HP-
275
-CD needed to form bead-free fibers. Normally, the concentration of HP--CD should be
276
over 160% (w/v, g/mL) in water form to obtain bead-free fibers. While it decreased to 120%
277
(w/v, g/mL) when ECH was added to solution for the cross-linking. The partial cross-linking
278
of HP--CD molecules prior to the electrospinning led to higher viscosity, and therefore, the
279
lower concentration of HP--CDs was enough to produce bead-free fibers. After exposure to
280
water for 24 h, the fiber size remained nearly unchanged (Figure 3b).
281 282 283
Figure 3. Scanning electron micrographs of the cross-linked poly(CD-ECH) fibers before (a) and after (b) exposure to water for 24 h.
284
The stability of the poly(CD-ECH) fibers was also tested in various organic solvents (i.e.,
285
methanol, ethanol, acetonitrile, DMF, TCM and DMSO) for 24 h. The SEM photos of the
286
respective fibers showed different fiber morphologies depending on the solvent treated
13 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 27
287
(Figure 4). The poly(CD-ECH) fibers were stable in all solvents tested, and could preserve
288
their fibrous morphology. The thinnest fibers were observed after exposure to MeOH,
289
followed by EtOH, DMSO, DMF, and TCM, while the largest fibers were observed after
290
treatment with ACN. It is known that alcohols are bad solvents for CD systems and can lead
291
to the collapse of the fiber matrix. Thus, the smallest diameter in alcohols can be attributed to
292
their non-solvent character for CD molecules.
293 294
Figure 4. Scanning electron micrographs of the cross-linked poly(CD-ECH) fibers after
295
exposure to various solvents for 24 h. (a) TCM, (b) DMF, (c), DMSO, (d) EtOH, (e) MeOH
296
and (f) ACN.
297
The cross-linking of the HP--CD fibers with ECH was confirmed by XPS measurements
298
(Figure 5). The atomic composition of the HP--CD and poly(CD-ECH) fibers was shown in
299
Table S1 (Supporting Information). The XPS analysis of the poly(CD-ECH) fibers revealed
300
the presence of Na1s (4.27%) and Cl2p (3.28%) atoms at significant proportions. While no
14 ACS Paragon Plus Environment
Page 15 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
301
peaks related to these elements appeared for the pure HP--CD fibers since they were
302
electrospun from water in the absence of ECH. The deconvoluted C1s spectra show a broad
303
peak related to C atom, which can further be deconvoluted into three peaks as follows: the
304
peaks appeared at 284.8, 286, and 288 eV are respectively ascribed to C-C (or C-H), C-O and
305
O-C-O.34 The broader C peak centered at 286.4 eV was observed for the poly(CD-ECH)
306
fibers due to the formation of glyceryl bridges with ECH. On the other hand, the atomic
307
percentage of C-C drastically decreased from 10.16 to 3.6% with the incorporation of ECH,
308
which increased the ratio of C-O in overall composition from 45.6 to 50.45% by taking
309
account of C and O atoms (Table S1).
310 311
Figure 5. The deconvoluted C1s spectra of (a) HP--CD and (b) poly(CD-ECH) fibers.
312
The chemical analysis of the poly(CD-ECH) fibers was further explored by FT-IR analysis
313
(Figure 6a). The bands between 1035 and 1155 cm-1 are due to the stretching band of the
314
glycosidic links of CD molecules: the IR bands at 1155, 1082 and 1035 cm-1 can be attributed
315
to the stretching vibration of C-H and C-O bonds. Similar IR bands were also observed in
316
poly(CD-ECH) fibers. Here, the absorbance ratio (A1082/A1035) in this region of the IR
317
spectrum gives information about the degree of cross-linking and A1082/A1035 ratio of
318
poly(CD-ECH) fibers is 66% higher compared to HP--CD fibers. This ratio reveals the
319
partial cross-linking such that around 66% (approximately 66% of OH groups) of the primary 15 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 27
320
OH groups of HP--CD transformed into secondary OH forming the cross-link junction.27 For
321
the poly(CD-ECH) fibers, the peak intensity at 1456 cm-1 due to the bending of methylene
322
groups of the formed glyceryl links drastically increased, while the peaks at 948 and 1143 cm-
323
1
324
presence of unreacted epoxy groups. The thermal analysis of the fibers was carried out using
325
TGA, which revealed the enhanced stability of HP--CD fibers after cross-linking with ECH
326
(Figure 6b). The pyrolysis of HP--CD molecules starts over 300 oC, while it increased to 372
327
from 347 oC due to thermal stabilization of the CD fibers with the cross-linking by ECH. It is
328
known that the cross-linking of molecules generally rises the degradation temperature, and
329
thus, an increase in the degradation temperature can be attributed to the presence of a densely
330
cross-linked CD network, which stabilized the CD structure on the course of heating.
decreased for the poly(CD-ECH) fibers. The typical absorption band at 850 cm-1 shows the
331 332 333
Figure 6. (a) FTIR and (b) TGA of the pure HP--CD fibers, uncross-linked HP-CD/ECH fibers and poly(CD-ECH) fibers.
334
The structural properties of the pure HP--CD fibers and poly(CD-ECH) fibers were also
335
explored by wide-angle XRD measurements (Figure S3, Supporting Information). Unlike
336
native CD molecules (, and ), hydroxypropyl-substituted CD molecules are amorphous
337
and give a broad peak centered at 19o. Likewise, the XRD patterns of the pure HP--CD 16 ACS Paragon Plus Environment
Page 17 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
338
fibers and poly(CD-ECH) fibers displayed amorphous diffraction peaks. Interestingly, the
339
peak positions the HP--CD and poly(CD-ECH) fibers shifted to higher 2 and peak
340
intensities decreased with respect to the powder form of HP--CD (Figure S3). This shift and
341
decrease in the intensity after cross-linking may be attributed to the loss of structural
342
arrangement (i.e., an increase in the amorphous structure) of the HP--CD with heat
343
treatment.
344
The presence of active CD contents in the cross-linked (poly(CD-ECH) fibers was explored
345
using phenolphthalein over host-guest inclusion-complexation of accessible CD molecules.
346
Phenolphthalein is a model guest molecule, which is widely used for the exploration of active
347
CD contents in the CD-based materials.35 Furthermore, it is a dye molecule with some
348
toxicity.29 Thus, the removal of phenolphthalein from aqueous media is desired for water
349
treatment. It forms IC with CD molecules, which can easily be monitored through UV-Vis
350
measurements due to the change of its pink color to colorless, driven by the constrained
351
conformation of phenolphthalein in the CD cavity.28, 35 The removal performance was further
352
compared with the granule form of the poly(CD-ECH). Figure 7 shows the UV-Vis spectra of
353
phenolphthalein solutions exposed to the poly(CD-ECH) fibers and granules over time. The
354
maximum absorption intensity at 553 nm decreased with time, and after 120 min no peak
355
related to phenolphthalein was observable, suggesting about 80% phenolphthalein formed
356
inclusion complex with accessible CD molecules. The complete removal of phenolphthalein
357
was accomplished in 2h while 50% removal was reached in 25 min (Fig 7a-b), suggesting the
358
rapid removal of phenolphthalein molecules from water. On the other hand, the identical
359
concentration of phenolphthalein could be removed in 10 h using poly(CD-ECH) granules
360
(Figure 7b-d). The removal of phenolphthalein by the poly(CD-ECH) fibers was also shown
361
over the optical photos of the solutions over time (Figure 7b inset) with the decolorization of
362
the phenolphthalein solution. The faster removal of phenolphthalein by the poly(CD-ECH) 17 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 27
363
fibers can be attributed to their smaller size and the presence of a highly porous structure. The
364
morphology of the poly(CD-ECH) fibers could be preserved after the sorption tests,
365
suggesting their high potential for water treatment applications from organic micropollutants
366
(Figure S4).
367 368
Figure 7. Filtration performance of the electrospun poly(CD-ECH) fibrous mat over
369
phenolphthalein. (a) UV-Vis spectra of phenolphthalein solution treated with the poly(CD-
370
ECH) fibers as a function of time and (b) decrease in the absorbance (λ=553 nm) of the
371
phenolphthalein solution with time. (c) UV-Vis spectra of a phenolphthalein solution treated
372
with the poly(CD-ECH) granules with time and (d) decrease in the absorbance intensity
373
(λ=553 nm) over time.
374
The electrospun poly(CD-ECH) fibrous mat was also used for the removal of phenanthrene
375
from aqueous solutions with time (Figure 8). The concentration of phenanthrene was
376
measured over time by HPLC. The stock solutions of phenanthrene was prepared at the 18 ACS Paragon Plus Environment
Page 19 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
377
maximum solubility limits (i.e., 1.8 g/mL) in water/ACN mixtures (59 mL/10 L). Within
378
the first 40 min, 50% removal of the phenanthrene was accomplished, while after 350 min the
379
concentration of phenanthrene decreased to 0.2 g/mL. The removal performance of
380
poly(CD-ECH) fibrous mat was very high and could scavenge 88% of initial phenanthrene
381
content. On the other hand, poly(CD-ECH) granules could reach to an equilibrium sorption
382
level at ~900 min. Both fibrous mat and granules exhibited similar sorption levels, but in
383
different rate. The use of poly(CD-ECH) fibrous mat fastened the sorption rate by nearly 3-
384
fold, which can be attributed to the smaller size of the fibers and their highly porous structure.
385
Despite showing a similar sorption capacity, there are drastic differences in the sorption rate. This can
386
be attributed to the enhanced surface area for the nanofiber form of the poly(CD-ECH), which boosts
387
the sorption rate. For many applications, rapid removal of such pollutants is highly desired.
388
Furthermore, unlike granule form of the poly(CD-ECH), nanofibers are easy to use and do not require
389
any specific container during their use. Furthermore, after washing with ACN to remove
390
phenanthrene molecules from the poly(CD-ECH) mat, the poly(CD-ECH) mat was retreated
391
with phenanthrene solution containing an identical phenanthrene concentration of the first
392
solution. The poly(CD-ECH) mat could remove 70% of phenanthrene after second use
393
(Figure S5). The performance loss in removal capacity can be attributed to the presence of
394
remained phenanthrene molecules in CD cavities, which could not be washed away easily
395
after the first use. The SEM analysis of the poly(CD-ECH) fibers and poly(CD-ECH)
396
granules after sorption tests revealed no significant changes in their morphology (Figure S6).
397
The sorption capacity for phenanthrene was found to be 944 g per gram poly(CD-ECH)
398
fibers. This is higher than many sorbent materials used for phenanthrene removal from water
399
(Table S1, Supporting Information). Although the presence of some sorbent systems with
400
better sorption values, they used alcohols as co-solvent to increase the solubility of
401
phenanthrene. However, among water-based systems, poly(CD-ECH) fibers showed a good
19 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 27
402
sorption capacity, which is better than DNA-based nanogels (sorption capacity = 720 g/g)36
403
and CD-grafted cellulose acetate fibers (sorption capacity = 540 g/g)19 (Table S2).
404 405 406
Figure 8. Time-dependent removal of phenanthrene from aqueous solutions using poly(CDECH) fibers and granules.
407
The poly(CD-ECH) electrospun fibers are a novel type of materials with great promising
408
applications for water treatment. As we have shown here with the removal of phenolphthalein
409
and phenanthrene, they can be exploited as high-performance sorbent materials due to their
410
high specific surface area, along with a high active CD content. Given that their high stability
411
in aqueous and various organic solvent systems owing to their highly cross-linked network by
412
epichlorohydrin-based chemistry, these highly stable fibrous materials may find more
413
application area as highly effective sorbents in coming years. Unlike other methods used for
414
the cross-linking for CD molecules, epichlorohydrin-based cross-linking offers robust CD
415
networks, which are stable even in polar aprotic solvents, such as DMF. This allows their
416
reuse for sorption-based applications after removal of the adsorbed molecules with intense
417
washing with aprotic solvents.
20 ACS Paragon Plus Environment
Page 21 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
418 419
CONCLUSIONS
420
Insoluble poly(CD-ECH) fibers were produced by the electrospinning of the aqueous
421
solutions of HP--CD and ECH and their cross-linking by heat-treatment. The flow and
422
dynamic oscillatory deformation tests revealed partial cross-linking of CD molecules prior to
423
the electrospinning, however main cross-linking takes place after the heat-treatment of the
424
fibers at 150 oC. Due to highly efficient cross-linking reactions, poly(CD-ECH) fibers were
425
stable in water and various organic solvents (i.e., ACN, TCM, DMSO, DMF, MeOH and
426
EtOH) and could maintained their fibrous structure. The presence of high active CD content
427
in the fibers was revealed by removal tests of phenolphthalein and phenanthrene through
428
inclusion-complexation. The removal performance of poly(CD-ECH) fibers was compared
429
with poly(CD-ECH) granules, and the results showed that rapid removal of phenolphthalein
430
and phenanthrene by the fibers compared to the granule form of poly(CD-ECH) due to their
431
smaller size and high porous structure. The poly(CD-ECH) fibrous membrane with a high
432
specific surface area and structural stability in water and organic solvents are promising
433
materials in water treatment applications.
434
ASSOCIATED CONTENT
435
Supporting Information
436
The following files are available free of charge.
437
Dynamic oscillatory time sweep profile of an aqueous mixture of HP--CD and ECH. The
438
SEM images of the poly(CD-ECH) fibers and granules synthesized at various concentrations
439
and after their use in removal of phenolphthalein and phenanthrene. The atomic composition
21 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 27
440
of the fibers obtained by XPS analysis. The reuse of poly(CD-ECH) fibers in the removal of
441
phenanthrene.
442
AUTHOR INFORMATION
443
Corresponding Author
444
* E-mail:
[email protected] (T.U)
445
ORCID ID
446
F. T.: 0000-0002-9011-4495
447
T. U.: 0000-0002-3989-4481
448 449
Funding:
450
The Scientific and Technological Research Council of Turkey (TUBITAK, project number:
451
113Y348) is acknowledged for funding the research.
452
Author contributions:
453
A.C., F.T and T.U. conceived, built and carried out the experiment and analyzed the data. All
454
authors contributed to the preparation of the manuscript.
455
Notes:
456
The authors declare no competing financial interest.
457
REFERENCES:
458
(1)
10975.
459 460
(2)
Irie, T.; Uekama, K., Pharmaceutical Applications of Cyclodextrins. III. Toxicological Issues and Safety Evaluation. J. Pharm. Sci. 1997, 86 (2), 147-162.
461 462
Crini, G., Review: A History of Cyclodextrins. Chem. Rev. 2014, 114 (21), 10940-
(3)
Astray, G.; Gonzalez-Barreiro, C.; Mejuto, J. C.; Rial-Otero, R.; Simal-Gándara, J., A
463
review on the use of cyclodextrins in foods. Food Hydrocolloids 2009, 23 (7), 1631-
464
1640. 22 ACS Paragon Plus Environment
Page 23 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
465
ACS Applied Polymer Materials
(4)
solubilization and stabilization. J. Pharm. Sci. 1996, 85 (10), 1017-1025.
466 467
Loftsson, T.; Brewster, M. E., Pharmaceutical applications of cyclodextrins. 1. Drug
(5)
Li, J. J.; Zhao, F.; Li, J., Supramolecular Polymers Based on Cyclodextrins for Drug
468
and Gene Delivery. In Biofunctionalization of Polymers and their Applications,
469
Nyanhongo, G. S.; Steiner, W.; Gübitz, G., Eds. Springer Berlin Heidelberg: Berlin,
470
Heidelberg, 2011; pp 207-249.
471
(6)
Expert Opinion on Drug Delivery 2005, 2 (2), 335-351.
472 473
Loftsson, T.; Jarho, P.; Másson, M.; Järvinen, T., Cyclodextrins in drug delivery.
(7)
Prabaharan, M.; Jayakumar, R., Chitosan-graft-β-cyclodextrin scaffolds with
474
controlled drug release capability for tissue engineering applications. Int. J. Biol.
475
Macromol. 2009, 44 (4), 320-325.
476
(8)
Szejtli, J., Cyclodextrins in the Textile Industry. Starch - Stärke 2003, 55 (5), 191-196.
477
(9)
Topuz, F.; Uyar, T., Poly-cyclodextrin cryogels with aligned porous structure for
478
removal of polycyclic aromatic hydrocarbons (PAHs) from water. J. Hazard. Mater.
479
2017, 335, 108-116.
480
(10)
Topuz, F.; Uyar, T., Cyclodextrin-functionalized mesostructured silica nanoparticles
481
for removal of polycyclic aromatic hydrocarbons. J. Colloid Interface Sci. 2017, 497,
482
233-241.
483
(11)
Mhlanga, S. D.; Mamba, B. B.; Krause, R. W.; Malefetse, T. J., Removal of organic
484
contaminants from water using nanosponge cyclodextrin polyurethanes. J. Chem.
485
Technol. Biotechnol. 2007, 82 (4), 382-388.
486
(12)
Uyar, T.; Havelund, R.; Hacaloglu, J.; Besenbacher, F.; Kingshott, P., Functional
487
Electrospun Polystyrene Nanofibers Incorporating α-, β-, and γ-Cyclodextrins:
488
Comparison of Molecular Filter Performance. ACS Nano 2010, 4 (9), 5121-5130.
489
(13)
Zhao, F.; Repo, E.; Yin, D.; Chen, L.; Kalliola, S.; Tang, J.; Iakovleva, E.; Tam, K. C.;
490
Sillanpää, M., One-pot synthesis of trifunctional chitosan-EDTA-β-cyclodextrin
491
polymer for simultaneous removal of metals and organic micropollutants. Sci. Rep.
492
2017, 7 (1), 15811. 23 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
493
(14)
Page 24 of 27
Alsbaiee, A.; Smith, B. J.; Xiao, L.; Ling, Y.; Helbling, D. E.; Dichtel, W. R., Rapid
494
removal of organic micropollutants from water by a porous β-cyclodextrin polymer.
495
Nature 2015, 529, 190.
496
(15)
Xiao, L.; Ling, Y.; Alsbaiee, A.; Li, C.; Helbling, D. E.; Dichtel, W. R., β-
497
Cyclodextrin Polymer Network Sequesters Perfluorooctanoic Acid at Environmentally
498
Relevant Concentrations. J. Am. Chem. Soc. 2017, 139 (23), 7689-7692.
499
(16)
cyclodextrin–epichlorohydrin polymers. Prog. Polym. Sci. 2013, 38 (2), 344-368.
500 501
Morin-Crini, N.; Crini, G., Environmental applications of water-insoluble β-
(17)
Morin-Crini, N.; Winterton, P.; Fourmentin, S.; Wilson, L. D.; Fenyvesi, É.; Crini, G.,
502
Water-insoluble β-cyclodextrin–epichlorohydrin polymers for removal of pollutants
503
from aqueous solutions by sorption processes using batch studies: A review of
504
inclusion mechanisms. Prog. Polym. Sci. 2018, 78, 1-23.
505
(18)
Uyar, T.; Havelund, R.; Nur, Y.; Hacaloglu, J.; Besenbacher, F.; Kingshott, P.,
506
Molecular filters based on cyclodextrin functionalized electrospun fibers. J. Membr.
507
Sci. 2009, 332 (1), 129-137.
508
(19)
Celebioglu, A.; Demirci, S.; Uyar, T., Cyclodextrin-grafted electrospun cellulose
509
acetate nanofibers via “Click” reaction for removal of phenanthrene. Appl. Surf. Sci.
510
2014, 305, 581-588.
511
(20)
Zhao, R.; Wang, Y.; Li, X.; Sun, B.; Wang, C., Synthesis of β-Cyclodextrin-Based
512
Electrospun Nanofiber Membranes for Highly Efficient Adsorption and Separation of
513
Methylene Blue. ACS Applied Materials & Interfaces 2015, 7 (48), 26649-26657.
514
(21)
Schäfer, A. I.; Stelzl, K.; Faghih, M.; Sen Gupta, S.; Krishnadas, K. R.; Heißler, S.;
515
Pradeep, T., Poly(ether sulfone) Nanofibers Impregnated with β-Cyclodextrin for
516
Increased Micropollutant Removal from Water. ACS Sustainable Chemistry &
517
Engineering 2018, 6 (3), 2942-2953.
518
(22)
Kayaci, F.; Aytac, Z.; Uyar, T., Surface modification of electrospun polyester
519
nanofibers with cyclodextrin polymer for the removal of phenanthrene from aqueous
520
solution. J. Hazard. Mater. 2013, 261, 286-294.
24 ACS Paragon Plus Environment
Page 25 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
521
ACS Applied Polymer Materials
(23)
Zhang, W.; Chen, M.; Zha, B.; Diao, G., Correlation of polymer-like solution
522
behaviors with electrospun fiber formation of hydroxypropyl-β-cyclodextrin and the
523
adsorption study on the fiber. PCCP 2012, 14 (27), 9729-9737.
524
(24)
Celebioglu, A.; Sen, H. S.; Durgun, E.; Uyar, T., Molecular entrapment of volatile
525
organic compounds (VOCs) by electrospun cyclodextrin nanofibers. Chemosphere
526
2016, 144, 736-744.
527
(25)
Celebioglu, A.; Uyar, T., Electrospinning of nanofibers from non-polymeric systems:
528
polymer-free nanofibers from cyclodextrin derivatives. Nanoscale 2012, 4 (2), 621-
529
631.
530
(26)
2010, 46 (37), 6903-6905.
531 532
Celebioglu, A.; Uyar, T., Cyclodextrin nanofibers by electrospinning. Chem. Commun.
(27)
Celebioglu, A.; Yildiz, Z. I.; Uyar, T., Electrospun crosslinked poly-cyclodextrin
533
nanofibers:
534
complexation. Sci. Rep. 2017, 7 (1), 7369.
535
(28)
Highly
efficient
molecular
filtration
thru
host-guest
inclusion
Kuwabara, T.; Takamura, M.; Matsushita, A.; Ikeda, H.; Nakamura, A.; Ueno, A.;
536
Toda, F., Phenolphthalein-Modified β-Cyclodextrin as a Molecule-Responsive
537
Colorless-to-Color Change Indicator. The Journal of Organic Chemistry 1998, 63
538
(24), 8729-8735.
539
(29)
Effects in Experimental Model Systems. Cancer Res. 1996, 56 (21), 4922-4926.
540 541
(30)
Artymowicz, R. J.; Childs, A. L.; Paolini, L., Phenolphthalein-Induced Toxic Epidermal Necrolysis. Ann. Pharmacother. 1997, 31 (10), 1157-1159.
542 543
Dunnick, J. K.; Hailey, J. R., Phenolphthalein Exposure Causes Multiple Carcinogenic
(31)
Taguchi, K., Transient binding of phenolphthalein-.beta.-cyclodextrin complex: an
544
example of induced geometrical distortion. J. Am. Chem. Soc. 1986, 108 (10), 2705-
545
2709.
546 547
(32)
Shuttleworth, K. L.; Cerniglia, E., Environmental aspects of PAH biodegradation. Appl. Biochem. Biotechnol. 1995, 54 (1), 291-302.
25 ACS Paragon Plus Environment
ACS Applied Polymer Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
548
(33)
Page 26 of 27
Renard, E.; Deratani, A.; Volet, G.; Sebille, B., Preparation and characterization of
549
water soluble high molecular weight β-cyclodextrin-epichlorohydrin polymers. Eur.
550
Polym. J. 1997, 33 (1), 49-57.
551
(34)
Transport and Shape-Selective Permeability. Adv. Mater. 2017, 29 (26), 1606641.
552 553
Villalobos, L. F.; Huang, T.; Peinemann, K.-V., Cyclodextrin Films with Fast Solvent
(35)
Kettel, M. J.; Hildebrandt, H.; Schaefer, K.; Moeller, M.; Groll, J., Tenside-free
554
Preparation of Nanogels with High Functional β-Cyclodextrin Content. ACS Nano
555
2012, 6 (9), 8087-8093.
556
(36)
Topuz, F.; Singh, S.; Albrecht, K.; Möller, M.; Groll, J., DNA Nanogels To Snare
557
Carcinogens: A Bioinspired Generic Approach with High Efficiency. Angew. Chem.
558
Int. Ed. 2016, 55 (40), 12210-12213.
559 560 561 562 563 564 565 566 567 568 569 570 571
26 ACS Paragon Plus Environment
Page 27 of 27 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Polymer Materials
572 573
Table of Contents (ToC) Graphic
574
27 ACS Paragon Plus Environment