Subscriber access provided by Binghamton University | Libraries
Article
Wet-Laid Formation and Strength Enhancement of Alkaline Battery Separators Using Polypropylene Fibers and Polyethylene/ Polypropylene Bicomponent Fibers as Raw Materials Bingxu Zhang, Qingxi Hou, Wei Liu, Zhihui Liang, Bing Wang, and Honglei Zhang Ind. Eng. Chem. Res., Just Accepted Manuscript • DOI: 10.1021/acs.iecr.7b01664 • Publication Date (Web): 20 Jun 2017 Downloaded from http://pubs.acs.org on June 25, 2017
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Industrial & Engineering Chemistry Research is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1
Wet-Laid Formation and Strength Enhancement of
2
Alkaline Battery Separators Using Polypropylene Fibers
3
and Polyethylene/Polypropylene Bicomponent Fibers as
4
Raw Materials
5
Bingxu Zhang, Qingxi Hou*, Wei Liu, Zhihui Liang, Wang Bing, Honglei Zhang
6
Tianjin Key Laboratory of Pulp and Paper, Tianjin University of Science & Technology, Tianjin
7
300457, P. R. China
8
ABSTRACT: The handsheets of alkaline battery separator were made of
9
polypropylene
(PP)
fibers
and
polyethylene/polypropylene
bicomponent
10
sheath-core structure (EP) fibers in the wet-laid process followed by a hot-pressing
11
treatment. The effects of the process parameters in making the separator
12
handsheets on the formation and the resultant tensile strength, maximum pore
13
size, porosity and alkali resistance were investigated. The results showed that a
14
favorable formation could be obtained at the EP fibers addition level of not less
15
than 20%. In addition, the tensile strength, maximum pore size, porosity and alkali
16
resistance of the separator handsheets made of 60% PP fibers and 40% EP fibers
17
could meet the needs required in QB/T 4173 (2011), under the conditions of 1.5%
18
PEO and 4.0% PVA additions (on oven-dry fibers), the hot-pressing pressure of
19
0.5 MPa, and hot-pressing temperature of 135 °C for 90 s.
20
Key words: :Polypropylene fiber; Polyethylene/polypropylene bicomponent fiber;
21
Wet-laid process; Alkaline battery separator; Hot-pressing
22
■ INTRODUCTION
*
Corresponding author. E-mail address:
[email protected] (Q.X. Hou) 1
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
23
The main cause for developing various types of clean cars such as fuel-cell
24
and electric vehicles is an environmental issue. Among clean cars, a hybrid electric
25
vehicle (HEV) with a rechargeable battery is considered to be the most promising
26
and, therefore, has been receiving much attention.1 For these attractive HEVs,
27
however, high performance rechargeable batteries are necessary. So far almost all
28
commercial HEVs have been equipped with alkaline batteries because of their
29
better combination of output power, capacity, long life, reliability and cost.2-3 The
30
function of an alkaline battery separator, which plays a vital role in the application
31
of alkaline batteries, is to separate the positive and negative electrodes in the
32
batteries from direct contact so as to avoid a short circuit, load the electrolyte
33
solution, and allow the conductive ions to pass through the cell. Therefore, the
34
quality of the battery separator has a great effect on discharge behavior,
35
self-discharge rate and cycle life of an alkaline battery.4-5 It is necessary for an
36
alkaline battery separator not only to possess a fairly good chemical stability and
37
affinity with the electrolyte but also to have certain properties such as a high
38
mechanical strength, suitable pore size and porosity.6
39
One of the core technologies of an alkaline battery is the use of a synthetic
40
fiber-based separator, which possesses the properties of high porosity, high
41
strength, and solvent and corrosion resistance, and so on. Furthermore, the
42
synthetic fiber-based separator especially adapts alkaline batteries to large
43
capacity, low resistance, large output power and long period of storage, therefore,
44
synthetic fibers have become the important raw materials in production of alkaline
45
battery separators.7-9
46
Currently widely used alkaline battery separators are typically manufactured
47
from polyolefin, predominantly polyethylene (PE) or polypropylene (PP).10-12 U.S. 2
ACS Paragon Plus Environment
Page 2 of 33
Page 3 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
48
Pat. No. 3,615,865 to Wetherill discloses a battery separator comprising a
49
nonwoven mat of polypropylene fibers bonded with polyacrylic acid.12 J.P. Pat. No.
50
5,311,059 to Kubo discloses alkaline manganese batteries comprising a fibrous
51
web having mixing rayon 1.5-denier and synthetic fiber 1.0-denier.13 When being
52
used as raw material to make the separators by means of the traditional
53
papermaking method used for plant fibers, PP fibers can only be interlaced with
54
one another due to the absence of hydrogen bonding between the fibers. That is to
55
say, there is no bonding force between PP fibers in the separator, resulting in a
56
very low separator’s strength and a poor formation due to the lower density of PP
57
fibers than that of water. However, PP fibers can be mixed with the low-melt fibers
58
to make alkaline battery separators. When a separator made of PE and PP fibers
59
is heated, the totally or partially melted PE fibers could act as binding ones to
60
improve the separator’s strength.14 However, the totally melted PE fibers can lead
61
to reducing in the separator’s porosity and subsequent battery quality. Among the
62
low-melt fibers, polyethylene/polypropylene bicomponent sheath-core structure
63
(EP) fibers with a PP core and a PE sheath are thought to be most promising.15
64
Heating these fibers to the temperature above the PE melting point can make the
65
fibers surface sticky, so that the bonding points between the fibers can be formed,
66
resulting in an enhancement in the separator’s strength.14,16 The battery separator
67
made of polyamide and EP fibers has a poor resistance to oxidation and may
68
cause the self-discharge of the cells.15
69
So far, a number of forming technologies to make alkaline battery separators
70
using synthetic fibers as raw materials have involved the wet-laid process,14,17-19
71
dry-laid process,20-22 and melt-blown process.23-24 The melt-blown process among
72
them has been suggested as the best way of using the fibers with a small diameter 3
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
73
and low strength, and the dry-laid one can be applied in making the separators
74
with a relatively low quality. The wet-laid process to be applied in making alkaline
75
battery separators has many advantages, such as a relative high tightness, better
76
formation, and low production cost. However, due to the severe flocculation and
77
poor dispersibility, only using low-density PP fibers to make the battery separators
78
in the wet-laid process could lead to a very poor formation of the resultant
79
separators. In addition, using PP and EP fibers simultaneously to make alkaline
80
battery separators in the wet-laid process has been rarely reported.
81
In this work, PP and EP fibers were selected to prepare alkaline battery
82
separators by using the wet-laid process. The addition of EP fibers was mainly
83
used to well disperse PP fibers in water and consequently to improve the
84
separator’s formation as well as to increase the mechanical strength of the
85
separator handsheets by hot-pressing treatment. In addition, PEO and PVA were
86
also selected to add in the fiber suspension for further enhancing the tensile
87
strength of the separator handsheets. The aim of this work is to improve the
88
separator formation in the wet-laid process and the properties such as tensile
89
strength, maximum pore size and porosity of the separator handsheet.
90
■ MATERIALS AND METHODS
91
Materials and chemicals. PP fibers (density of 0.91 g/cm3, alkali resistance
92
of 0.88%, mean fiber length of 6.56 mm and mean fiber diameter of 2.06 µm) was
93
obtained from an electronic ceramics company in Guangdong Province, China. EP
94
fibers (PE/PP biocomponent sheath-core structure, Superior grade, density of 0.95
95
g/cm3, alkali resistance of 0.32%, mean fiber length of 2.55 mm and mean fiber
96
diameter of 14.1 µm) was obtained from the Complex New Material Technology
97
(Shanghai, China) Co., Ltd. 4
ACS Paragon Plus Environment
Page 4 of 33
Page 5 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
98
Polyethylene oxide (PEO, Mw = 5000000) was purchased from Sigma Aldrich
99
Co., and polyvinyl alcohol (PVA) with a polymerization degree of 1700 and
100
alcoholysis degree of 88% was supplied by Aladdin Reagent (Shanghai) Co., Ltd.
101
N-butanol and potassium hydroxide were purchased from Sinopharm Chemical
102
Reagent Co., Ltd. All chemicals used in the experiments were analytical-grade
103
products.
104
Fiber morphology. The mean diameter and length of PP fibers were
105
determined by using the Image-Pro Plus (IPP) software and the images of a SEM
106
(JSM-IT300LV, JEOL, Japan) according to the method described in literature.25
107
The EP fiber’s morphology was analyzed by using a Fiber Tester (Model 912,
108
Lorentzen & Wettre Co. Ltd., Sweden).
109
Determination of sedimentation volume. 400 mg fibers were added into
110
800 mL deionized water to make a 0.05% fiber suspension. After being stirred for
111
15 min, the fiber suspension was poured into a 1000 mL graduated cylinder. The
112
sedimentation volume was determined according to the upper suspended volume
113
of the fiber suspension.
114
Preparation of alkaline battery separator handsheets. A series of 0.5%
115
fiber suspensions with different proportions of the PP and EP fibers, i.e., the
116
addition levels of the EP fibers were 0%, 10%, 20%, 25%, 30% and 40%,
117
respectively, were firstly made, and then the fiber suspensions were disintegrated
118
for 20000 revolutions using a standard desintegrator (970154, Lorentzen & Wettre
119
Co. Ltd., Sweden). After pouring PEO (0.5%, 1.0%, 1.5%, 2.0%, 2.5%, and 3.0%
120
on oven-dry fibers, respectively) and/or PVA (1.0%, 2.0%, 3.0%, 4.0%, 5.0%, 6.0%,
121
and 7.0% on oven-dry fibers, respectively) into the fiber suspension, stirring for 10
122
min was required. The handsheets of alkaline battery separator with a basis weight 5
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
123
of 50 g/m2 (over-dry) were made by using a sheet former (RK-ZA-KWT, PTI,
124
Austria) according to the standard method of ISO 5269–1(1998), then further
125
dehydrated in a wet paper press machine (KRK SE0808098, MAVIS, UK) and
126
subsequently dried in a drum dryer (2110, AMC, USA). Finally, the hot-pressing
127
treatment of the separator handsheets was conducted by using a hot press
128
machine (LX101-63, Lizhengxin Mechanical Equipment Co., China). The
129
hot-pressing conditions were as follows: the pressure of 0.1 MPa, 0.2 MPa, 0.3
130
MPa, 0.4 MPa, 0.5 MPa, 0.55 MPa, and 0.6 MPa, respectively; the temperature of
131
130 °C, 135 °C, 140 °C, 145 °C, 150 °C, 155 °C, and 160 °C, respectively; and the
132
hot-pressing time of 90 s.
133
Sulfonation treatment of alkaline battery separator handsheets. The
134
alkaline battery separator handsheets were soaked with concentrated sulfuric acid
135
(mass fraction of 98%) at room temperature for 5 min, 10 min, 15 min, 20 min, and
136
25 min, respectively. Then the sulfonated handsheets were taken out and
137
thoroughly washed with deionized water until the pH of the filtrate was neutral.
138
Finally, the sulfonated separator handsheets were dried in an electric heating
139
air-blowing drier (DGG-101-1, Tianjin Tianyu Experimental Instrument Co., China).
140
DSC determination. The DSC determination of the separator handsheets
141
was conducted by using a DSC (200F3, NETZSCH, Germany) under a nitrogen
142
atmosphere from 20 °C to 200 °C at a heating rate of 10 °C/min.
143
Determination of the separators performance. Physical properties. The
144
basis weight, thickness and tensile index of the separator handsheets were
145
determined according to ISO 536 (1995), ISO 534 (1998) and ISO1924–2 (1994),
146
respectively. The pore size of the separator handsheet was detected by using a
147
Capillary Flow Porometer (Porolux 100, porometer NV, Germany) according to 6
ACS Paragon Plus Environment
Page 6 of 33
Page 7 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
148
SJ/T 10171.10 (1991). The porosity of the separator handsheet was determined by
149
using the n-butanol uptake test according to the literature method,26-27 as
150
calculated by the following equation:
Porosity(%) = ( W 2 − W 1 ) / ρbV ×100
151
(1)
152
where W2 and W1 are the weights of the wet and dry separator handsheet,
153
respectively, ρb is the density of n-butanol, and V is the geometric volume of the
154
separator handsheet.
155
Alkali resistance, alkali absorption rate and alkali absorption height. The
156
alkali resistance, alkali absorption rate and alkali absorption height of the separator
157
handsheet were detected according to SJ/T 10171.6 (1991), SJ/T 10171.7 (1991)
158
and ISO 8787 (1991), respectively.
159
SEM observation. The morphologies of the separator handsheets were
160
observed by using a SEM (JSM-IT300LV, JEOL, Japan). Before observation, the
161
test samples were oven-dried in a vacuum oven at 50 °C for 4 h, and then sputter
162
coated with gold.
163
■ RESULTS AND DISCUSSION
164
Effect of the addition level of EP fibers on the handsheet formation of
165
alkaline battery separator. The effect of the addition level of EP fibers on the
166
handsheet formation of alkaline battery separator was investigated, and the result
167
is shown in Figure 1. In Figure 1, a better formation can be found as the addition
168
level of the EP fibers was 20% or more, which is accordant with the result of about
169
65% PP fibers observed by other researchers.16,28 This is because the EP fibers
170
were shorter in length and had a higher density and larger diameter than the PP
171
fibers, which effectively inhibited flocculation of the PP fibers in water. Therefore,
172
from a better formation point of view, 20% or more addition level of the EP fibers 7
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
173
was necessary to make alkaline battery separator handsheets.
174
Selection of the temperature in the hot-pressing treatment of the
175
separator handsheets. The DSC curves of the separator handsheets were shown
176
in Figure 2. It can be found in Figure 2 that the melting temperature ranged from
177
130 °C to 170 °C. According to previous studies,14,16,29 the PE sheath of the EP
178
fibers would melt slightly beyond 130 °C, which is the main reason why the tensile
179
index of the separator handsheet would increase after hot-pressing. That is
180
because the bonding points between the fibers in the separator handsheet
181
increased with an increase in the addition level of the EP fibers, resulting in an
182
enhancement in the bonding strength of the separator handsheet. Furthermore,
183
the EP fibers had a larger diameter and a shorter length than the PP fibers,
184
resulting in an increment in the porosity and pore size of the separator handsheet,
185
which can be confirmed according to the effect of the addition level of the EP fibers
186
on the porosity and maximum pore size of the separator handsheets (Figure 3).
187
However, as the hot-pressing temperature rose, the melting amount of the fibers
188
increased, leading to a decrease in the porosity of the separator handsheet.
189
Considering the porosity requirement for alkaline battery separators, the
190
hot-pressing temperature ranging from 130 °C to 150 °C would be appropriate.
191
Effect of hot-pressing temperature on the tensile strength, maximum
192
pore size and porosity of the separator handsheets. The effect of hot-pressing
193
temperature on the tensile strength, maximum pore size and porosity of the
194
separator handsheets were explored, as shown in Figure 4. It can be found in
195
Figure 4a that with the increase in hot-pressing temperature the tensile strength of
196
the separator handsheets had an overall raising trend. When the hot-pressing
197
temperature exceeded 130 °C, the PE sheath of the EP fibers might begin melting 8
ACS Paragon Plus Environment
Page 8 of 33
Page 9 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
198
and the PP fibers were then adhered to the EP fibers, resulting in an increased
199
tensile index of the separator handsheets, which is consistent with the previous
200
study.14 Actually, there is no bonding strength between the PP fibers, thus the
201
moderate melting of the PE sheath of the EP fibers becomes the main source of
202
producing the bonding strength between the PP fibers. In other words, at that time
203
the EP fibers acted as a binder between the PP fibers. However, as the
204
hot-pressing temperature exceeded 135 °C, the PE sheath of the EP fibers could
205
have completely melted, which led to changing the bonding mode between the
206
fibers in the separator handsheets from ‘contact bonding’ to ‘layered-structure
207
bonding’. Because the stress withstood by a layered-structure bonding is much
208
smaller than that by a contact bonding,30 the tensile strength of the separator
209
handsheets declined until the hot-pressing temperature reached 140 °C. As the
210
hot-pressing temperature was over 140 °C, the ‘layered-structure bonding’ could
211
have been improved greatly, leading to an ascendant trend of the tensile strength
212
once again.
213
The
hot-pressing
decreased
the
diameter
of
the
EP
fibers
and
214
correspondingly increased the tightness of the separator handsheets, as a result,
215
the maximum pore size and porosity of the handsheets were both decreased
216
(Figures 4b and c). Moreover, it can be clearly seen from Figure 4 that the
217
maximum pore size had a rapid decrease as hot-pressing temperature exceeded
218
150 °C.
219
Effect of hot-pressing pressure on the tensile strength, maximum pore
220
size and porosity of the separator handsheets. Figure 5 shows the effect of
221
hot-pressing pressure on the tensile strength, maximum pore size and porosity of
222
the separator handsheets. It can be found in Figure 5a that the tensile index had a 9
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
223
rapid increase at a hot-pressing pressure of lower than 0.5 MPa and a
224
subsequently flat trend beyond 0.5 MPa. Contrary to the trend of tensile index, the
225
maximum pore size and porosity had a rapid decrease at a hot-pressing pressure
226
of lower than 0.5 MPa and a subsequently flat trend beyond 0.5 MPa (Figures 5b
227
and c). In addition, the tensile index, maximum pore size and porosity all rose as
228
the addition level of the EP fibers in the separator handsheets increased at the
229
same hot-pressing pressures. When the proportion of the EP fibers was 40%, the
230
tensile index, maximum pore size and porosity of the resultant separator
231
handsheets reached 33.00 Nm/g, 40.91 µm and 45.71%, respectively. When the
232
pressure rose to 0.5 MPa or more, almost no changes happened to the tensile
233
index, maximum pore size, and porosity. The events above can be explained as
234
follows: under a certain addition level of the EP fibers, high hot-pressing pressure
235
could result in a large contact area and a consequently strong bonding between
236
the fibers in the separator handsheets; as a result, the pore size and porosity
237
declined. The explanation above can be also confirmed by the SEM observation
238
shown in Figure 6. It can be found from Figures 6a to c that more coating which
239
came from the melted PE sheath of the EP fibers appeared on the surface of the
240
separators handsheets, leading to the gradually decreased porosity and pore size
241
of the handsheets. Meanwhile, the bonding between the fibers in the separator
242
handsheets could be enhanced, resulting in the improved tensile strength of the
243
separator handsheets.
244
Optimization of the hot-pressing temperature and pressure for the
245
separator handsheets. Figure 7 further shows the changes of the surface and
246
cross section of the separator handsheets at a hot-pressing pressure of 0.5 MPa
247
and temperatures of 135 °C and 150 °C as follows: on the surface of the separator 10
ACS Paragon Plus Environment
Page 10 of 33
Page 11 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
248
handsheets, both the melting amount of the EP fibers and consequently the
249
binding area at a hot-pressing temperature of 150 °C (Figure 7b) were obviously
250
larger than that at 135 °C (Figure 7a); on the cross section of the separator
251
handsheets, almost all the fibers were more tightly closed with each other at
252
150 °C (Figure 7d) than that at 135 °C (Figure 7c), both leading to the decreased
253
porosity and maximum pore size.
254
In general, the requirements of the maximum pore size and porosity for
255
alkaline battery separators are less than 50 µm (QB/T 4173 (2011)) and 40% or
256
more,26,31 respectively. Based on the discussions above, the appropriate
257
hot-pressing pressure and temperature were 0.5 MPa and 135 °C, respectively.
258
Effect of PEO addition on fiber dispersion. It can be found in Figure 8 that
259
with the increase in sedimentation time the sedimentation volume of fibers in the
260
fiber suspension has a reducing trend. The sedimentation volume decreased
261
rapidly when the sedimentation time was less than 225 s, and then went flatly
262
beyond 225 s. The above can be explained as follows: the PP fibers flocculated
263
constantly before 225 s, and flocculated completely over 225 s, which is consistent
264
with the fact that the tensile index reduced with increasing the PEO dosage.
265
Figure 9 shows the effect of adding PEO on the sedimentation volume of
266
fibers in the fiber suspension. It can be seen from this figure that the sedimentation
267
volume had an increasing trend, especially when the PEO dosage was lower than
268
1.5%. This can be attributed to that the addition of PEO might increase the
269
viscosity of the fiber suspension and therefore prevented the PP fibers from
270
flocculating, thus making PP fibers and EP fibers uniformly mixed in the
271
suspension.16
272
Effects of PEO and PVA additions on tensile strength of the separator 11
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
273
handsheets. It can be found in Figure 10a that the tensile index of the separator
274
handsheets made of 60% PP fibers and 40% EP fibers just reached 33.00 Nm/g
275
at a hot-pressing pressure of 0.5 MPa and temperature of 135 °C for 90 s,
276
suggesting that it did not meet the needs of more than 40.00 Nm/g required in
277
QB/T 4173 (2011). Consequently, PEO and PVA were selected as dispersant and
278
reinforcing agent, respectively, to add to the fiber suspension for further enhancing
279
the tensile strength of the resultant separator handsheets in this work. Figure 1h
280
shows the formation of the resultant separator handsheets, seemingly no obvious
281
change compared to that shown in Figure 1g.
282
Figure 10a shows the effect of the PEO dosage on the tensile index of the
283
separator handsheets. It can be seen that the tensile index had a sharp increase
284
until the PEO dosage reached 1.5% (on oven-dry fibers) and that the maximal
285
tensile index of 40.29 Nm/g could be got at the PEO dosage of 1.5%. This is
286
because with an increase in the PEO dosage the viscosity of the fiber suspension
287
rose and the movement of the PP fibers in the fiber suspension was blocked,
288
resulting in the improved formation and resultant tensile index, which is consistent
289
with the previous report.32 However, when the PEO dosage exceeded 1.5% in the
290
handsheet-making process, the drainage time of the fiber suspension on the
291
formation web was so prolonged that the PP fibers could flocculate again,28 which
292
led to a poor formation and consequently decreased tensile strength of the
293
resultant separator handsheets.
294
Figure 10b shows the effect of the PVA dosage on the tensile index and
295
maximum pore size of the separator handsheets at the PEO dosage of 1.5% (on
296
oven-dry fibers). It can be clearly seen in Figure 10b that the tensile index
297
increased obviously until the addition level of PVA was up to 4.0% (on oven-dry 12
ACS Paragon Plus Environment
Page 12 of 33
Page 13 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
298
fibers) and then went slowly, in which the tensile index increased from 40.29 Nm/g
299
to 45.16 Nm/g, an increment of 12.1%. That can be attributed to the good bonding
300
property of the PVA between the fibers in the separator handsheets in the
301
hot-pressing treatment. However, the maximum pore size went completely
302
opposite to the tensile index, because the existence of PVA improved the bonding
303
area between the fibers, resulting in a decrease in the pore size of the separator
304
handsheet. When the PEO and PVA dosages were 1.5% and 4.0%, respectively,
305
the maximum pore size decreased from 40.31 µm to 34.19 µm, a decrement of
306
15.2%. As the addition level of PVA was further raised, the maximum pore size did
307
not meet the needs (30-50 µm) required in QB/T 4173 (2011). Therefore, at the
308
addition level of 1.5% PEO, the appropriate dosage of PVA was 4.0% on oven-dry
309
fibers.
310
Performance of the separator handsheets under the optimal conditions.
311
Based on all discussions above, the separator handsheets were also made of 60%
312
PP fibers and 40% EP fibers under the optimum conditions as follows: 1.5% PEO;
313
4.0% PVA; hot-pressing pressure of 0.5 MPa; and hot-pressing temperature of
314
135 °C for 90 s. The performance of the separator handsheets was then tested,
315
and the results are listed in Table 1. It can be seen in Table 1 that the tensile
316
strength, maximum pore size, porosity and alkali resistance of the separator
317
handsheets were qualified compared to the standard values set in QB/T 4173
318
(2011). In order to further compare the performance of the separator handsheets
319
to that of some commercial separators available in the market and the standard
320
values in QB/T 4173 (2011), the above separator handsheets were then
321
experienced a sulphonation treatment to increase their absorbing capability. The
322
result of the corresponding comparison is listed in Table 2, in which the data for 13
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
323
two commercial separators are cited in literatures.18,33 It can be seen in Table 2
324
that the tensile index and alkali absorption rate of the separator handsheets were
325
lower than those of the American product but met the needs of QB/T 4173 (2011),
326
and the alkali resistance of the separator handsheets was the highest among the
327
three samples.
328
■ CONCLUSIONS
329
The handsheets of alkaline battery separators were successfully made of PP
330
fibers and EP fibers in the wet-laid process followed by a hot-pressing treatment.
331
Both the formation issue that exists in the wet-laid process and the poor
332
corresponding tensile strength of the resultant alkaline battery separators can be
333
solved. A better formation of the separator handsheet could be obtained when the
334
addition of the EP fibers was not less than 20%. The properties such as tensile
335
strength, maximum pore size, porosity and alkali resistance of the separator
336
handsheets made of 60% PP fibers and 40% EP fibers could meet the needs
337
required in QB/T 4173 (2011) under the conditions of 1.5% PEO and 4.0% PVA
338
additions (on oven-dry fibers), the hot-pressing pressure of 0.5 MPa, and
339
hot-pressing temperature of 135 °C for 90 s.
340
■ AUTHOR INFORMATION
341
Corresponding Author
342
343 344 345 346
*Email:
[email protected] (Q. X. Hou) ■ REFERENCES
(1) Bitsche, O.; Gutmann, G. Systems for hybrid cars. J. Power Sources. 2004, 127, 8–15. (2) Verbrugge, M.; Tate, E. Adaptive state of charge algorithm for nickel metal 14
ACS Paragon Plus Environment
Page 14 of 33
Page 15 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
347
hydride batteries including hysteresis phenomena. J. Power Sources. 2004, 126,
348
236–249.
349
(3) Taniguchi, A.; Fujioka, N.; Ikoma, M.; Ohta, A. Development of
350
nickel/metal-hydride batteries for EVs and HEVs. J. Power Sources. 2001, 100,
351
117–124.
352
(4) Shinyama, K.; Harada, Y.; Maeda, R.; Nakamura, H.; Matsute, S.; Nohma, T.;
353
Yonezu, I. Effect of separators on the self-discharge reaction in nickel-metal
354
hydride batteries. Res. Chem. Intermed. 2006, 32, 447–452.
355
(5) Li, X.; Song, Y.; Wang, L.; Xia, T.; Li, S. Self-discharge mechanism of Ni-MH
356
battery by using acrylic acid grafted polypropylene separator. Int. J. Hydrogen
357
Energy. 2010, 35, 3798–3801.
358 359
(6) Jiao, X. N.; Yang, W. J. Nonwoven separator for Ni-MH battery. China Text. Leader. 2005, 12, 71–74.
360
(7) Ciszewski, A.; Kunicki, J.; Gancarz, I. Usefulness of microporous
361
hydrophobic polypropylene membranes after plasma-induced graft polymerization
362
of acrylic acid for high-power nickel-cadmium batteries. Electrochim. Acta. 2007,
363
52, 5207–5212.
364
(8) Jiao, X. N.; Cheng, B.; Kang, W. M.; Yang, W. J. Nickel–metal hydride
365
battery separators fabricated from sulfonated nonwovens. J. Appl. Polym. Sci.,
366
2008, 109, 272–275.
367
(9) Gancarz, I.; Bryjak, M.; Kunicki, J.; Ciszewski, A. Microwave plasma-initiated
368
grafting of acrylic acid on Celgard 2500 membrane to prepare alkaline battery
369
separators—Characteristics of process and product. J. Appl. Polym. Sci. 2010, 116,
370
868-875.
371
(10) Ciszewski, A.; Gancarz, I.; Kunicki, J.; Bryjak, M. Plasma-modified 15
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
372
polypropylene membranes as separators in high-power alkaline batteries. Coat.
373
Technol. 2006, 201, 3676–3684.
374
(11) Ming, X.; Tang, H. L.; Wang, Y. D.; Mu, P. Ethylcellulose-coated polyolefin
375
separators for lithium-ion batteries with improved safety performance. Carbohydr.
376
Polym. 2014, 101, 1140–1146.
377 378 379 380 381 382
(12) Williams, R. C.; Goettmann, J. A.; Funk, G, L.; Gee, L. M. Wet-laid nonwoven polyolefin battery separator substrate, 6174826 US Patent, 2001. (13) Kubo, Y. Separator paper for alkaline-battery, 5,311,059 JP 1959 Patent, 1959. (14) Kritzer, P.; Cook, J. A. Nonwovens as separators for alkaline batteries an overview. J. Electrochem. Soc. 2007, 154, A481–A494.
383
(15) Kritzer, P. Separators for nickel metal hydride and nickel cadmium
384
batteries designed to reduce self-discharge rates. J. Power Sources. 2004, 137,
385
317–321.
386 387
(16) Liu, X. Y.; Chen, J. Z.; Ren, B. L. Study on polyolefin fiber battery separator paper. China Pulp Pap. 2007, 26, 15–17.
388
(17) Chen, W. J.; Shi, L. Y.; Wang, Z. Y.; Zhu, J. F.; Yang, H. J.; Mao, X. F.; Chi,
389
M. M.; Sun, L. N.; Yuan, S. Porous cellulose diacetate-SiO2 composite coating on
390
polyethylene separator for high-performance lithium-ion battery. Carbohydr. Polym.
391
2016, 147, 517–524.
392
(18) Tian, Y. C.; Gao, H. P.; Wang, J. C.; Jin, X. Y.; Wang, H. W. Preparation of
393
hydroentangled CMC composite nonwoven fabrics as high performance separator
394
for nickel metal hydride battery. Electrochim. Acta. 2015, 177, 321–326.
395
(19) Tadokoro, Y.; Uesaka, M.; Takata, Y.; Goto, F. Wet-laid nonwoven fabric for
396
battery separator, its production method and sealed type secondary battery, 16
ACS Paragon Plus Environment
Page 16 of 33
Page 17 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
397 398 399
Industrial & Engineering Chemistry Research
5888916 US Patent, 1999. (20) Tabatabaei, S. H.; Carreau, P. J.; Ajji, A. Microporous membranes obtained from PP/HDPE multilayer films by stretching. J. Membr. Sci. 2009, 345, 148–159.
400
(21) Wu, H. L.; Li, K.; Sun. T.; Liu, B.; Kou, F.; Jia, F.; Yuan, J. K.; Bai, Y.
401
Synthesis, Crystal Structure, and DNA-Binding Studies of a Ni(II) Complex with the
402
Tris (N-methylbenzimidazol -2-ylmethyl)amine Ligand. J. Chem. Sci. 2010, 65,
403
1474–1480.
404 405 406 407
(22) Kurauchi, H.; Akazawa, T. Process for producing microporous film having breakage resistance when melted, 5258156A US Patent, 1993. (23) Wang, H.; Sha, C. H.; Jin, X. Y. Hydrophilic polypropylene melt-blown nonwoven as Ni/MN battery separator. Battery Bimon. 2013, 43. 166–169.
408
(24) Wang, H.; Jin, X. Y.; Mao, N. T.; Russell, S. J. Differences in the Tensile
409
Properties and Failure Mechanism of PP/PE Core/Sheath Bicomponent and PP
410
Spunbond Fabrics in Uniaxial Conditions. Text. Res. J. 2010, 80, 1759-1767.
411
(25) Kapłonek, W.; Nadolny, K. Assessment of the grinding wheel active surface
412
condition using SEM and image analysis techniques. J. Braz. Soc. Mech. Sci. Eng.
413
2013, 35, 207–215.
414
(26) Yanilmaz, M.; Lu, Y.; Li, Y.; Zhang, X. W. SiO2/polyacrylonitrile membranes
415
via centrifugal spinning as a separator for li-ion batteries. J. Power Sources. 2015,
416
273, 1114–1119.
417
(27) Liu, Q. Z.; Xia, M.; Chen, J. H.; Tao, Y. F.; Wang, Y. D.; Liu, K.; Li, M. F.;
418
Wang,
419
alcohol-co-ethylene) nanofibrous membrane for lithium-ion battery separator.
420
Electrochim. Acta. 2015, 176, 949–955.
421
W.
W.;
Wang,
D.
High
performance
hybrid
Al2O3/poly(vinyl
(28) Shen, F. Y.; Zhang, X. F. Study of making alkaline battery separator paper 17
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
422 423 424 425 426 427 428
by wet papermaking. J. Membr. Sci. Technol. 2013, 33, 24–119. (29) Zhao, L. J.; Liu, W.; Zhou, L. C. Effect of hot press on physical properties of battery separator paper-base. China Pulp Pap. Ind. 2016, 22, 34–38. (30) Wang, Y. X. Non-woven fabric production technologies; China textile University Press: Shanghai, 1998. (31) Hu, J. W.; Xu, K.; Shen, J. R. Research and development of separators for lithium-ion batteries. Polym. Mater.: Sci. Eng. 2003, 19, 215–219.
429
(32) Gaudreault, R.; Ven, T. G. M. V. D.; Whitehead, M. A. Mechanisms of
430
flocculation with poly (ethylene oxide) and novel cofactors. Colloids Surf., A. 2005,
431
268, 131–146.
432
(33) Zhang, W. N. Preliminary research on high performance battery separator
433
of alkaline-manganese battery. M.S. Thesis, South China Univ. Technol.,
434
Guangdong, 2010.
435 436 437 438 439 440 441 442 443
18
ACS Paragon Plus Environment
Page 18 of 33
Page 19 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Captions of Figures Figure 1. Images of the handsheet formation of alkaline battery separator with different addition levels of the EP fibers: (a) 100% PP; (b) 10% EP + 90% PP; (c) 15% EP + 85% PP; (d) 20% EP + 80% PP; (e) 30% EP + 70% PP; (f) 35% EP + 65% PP; (g) 40% EP + 60% PP;(h) (40% EP + 60% PP)/(1.5% PEO + 4.0% PVA). Figure 2. DSC curves of the separator handsheets: T1 was the initial melting temperature of PE sheath of the EP fibers; T2 was the initial melting temperature of the PP fibers and PP core of the EP fibers. Figure 3. Effect of the addition level of the EP fibers on the porosity and maximum pore size of the separator handsheets at hot-pressing pressure of 0.5 MPa and temperature of 135 °C for 90 s. Figure 4. Effect of hot-pressing temperature on the tensile index (a), maximum pore size (b) and porosity (c) of the separator handsheets at hot-pressing pressure of 0.5 MPa for 90 s. Figure 5. Effect of hot-pressing pressure on the tensile index (a), maximum pore size (b) and porosity (c) of the separator handsheets at hot-pressing temperature of 135 °C for 90 s. Figure 6. SEM images of the separator handsheets made of 60% PP fibers and 40% EP fibers under the conditions of hot-pressing pressure of 0.1 MPa (a), 0.3 MPa (b) and, 0.5 MPa (c) and hot-pressing temperature of 135 °C for 90 s. Figure 7. SEM images of the surfaces (a, 135 °C; b, 150 °C) and cross sections (c, 135 °C; d, 150 °C) of the separator handsheets made of 60% PP fibers and 40% EP fibers under the conditions of a pressure of 0.5 MPa and 19
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
temperatures of 135 °C and 150 °C for 90 s. Figure 8. Relationship of the sedimentation volume of the fibers in the fiber suspension with time. Figure 9. Effect of adding PEO on the sedimentation volume of fibers in the fiber suspension. Figure 10. Effects of PEO (a) and PVA (b) dosages on the tensile index and/or maximum pore size of the separator handsheets at hot-pressing pressure of 0.5 MPa and temperature of 135 °C for 90 s.
Captions of Tables Table 1. Performance of the separator handsheets. Table 2. The performance comparison of commercial separators and the separator handsheets expericed a sulphonation treatment.
20
ACS Paragon Plus Environment
Page 20 of 33
Page 21 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Figure 1.
a
b
c
d
e
f
g
h
21
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
Figure 2.
Heat Flow Endo Up
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 33
20% EP + 80% PP 30% EP + 70% PP 40% EP + 60% PP (40% EP + 60% PP)/1.5% PEO (40% EP + 60% PP)/1.5% PEO/4% PVA
T1=130 oC
20
40
60
80
100
120
140
T2=170 oC
160
Temperature, oC
22
ACS Paragon Plus Environment
180
200
Page 23 of 33
Figure 3.
60 55 40% EP + 60 %PP 1.5% PEO
50
50
45 45
40
40
35 Maximum pore size Porosity
30 25
35 30
20
30
40
50
60
ES fiber dosage, %(on oven-dry fibers)
23
ACS Paragon Plus Environment
Maximum pore size, µm
55
Porosity, %
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Industrial & Engineering Chemistry Research
a
48
b
50
Maximum pore size, µm
Figure 4.
45
45 30% EP + 70% PP 35% EP + 65% PP 40% EP + 60% PP
42 39 36 33 30 130
135
140
145
150
155
30% EP + 70% PP 35% EP + 65% PP 40% EP + 60% PP
40 35 30
27
25
160
130
135
o
c
140
52 30% EP + 70% PP 35% EP + 65% PP 40% EP + 60% PP
48 44 40 36 32 130
145
150
155
Hot-pressing tempeture, oC
Hot-pressing temperature, C
Porosity, %
Tensile index, N·m/g
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 24 of 33
135
140
145
150
155
160
Hot-pressing tempeture, oC
24
ACS Paragon Plus Environment
160
Page 25 of 33
34
b
32 30 28 30% EP + 70% PP 35% EP + 65% PP 40% EP + 60% PP
26 24 22
80 30% EP + 70% PP 35% EP + 65% PP 40% EP + 60% PP
70 60 50 40 30
0.1
0.2
0.3
0.4
0.5
0.6
0.1
c
0.2
65 30% EP + 70% PP 35% EP + 65% PP 40% EP + 40% PP
60 55 50 45 40 35 0.1
0.3
0.4
0.5
Hot-pressing pressure, MPa
Hot-pressing pressure, MPa
Porosity, %
a
Maximum pore size, µ m
Figure 5.
Tensile index, N·m/g
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
0.2
0.3
0.4
0.5
0.6
Hot-pressing pressure, MPa
25
ACS Paragon Plus Environment
0.6
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 6.
26
ACS Paragon Plus Environment
Page 26 of 33
Page 27 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Figure 7.
27
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
Figure 8.
700
Sedimentation volume, mL
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 28 of 33
650 1.5% PEO 3.0% PEO
600 550
40% EP + 60% PP
500 450 0
100
200
300
400
Sedimentation time, s
28
ACS Paragon Plus Environment
500
600
Page 29 of 33
Figure 9.
560
Sedimentation volume, mL
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
540 40% EP + 60% PP sedimentation time of 2 min
520 500 480 460 440 420 0.0
0.5
1.0
1.5
2.0
2.5
PEO dosage, % (on oven-dry fibers)
29
ACS Paragon Plus Environment
3.0
Industrial & Engineering Chemistry Research
Figure 10.
42 40% EP + 60% PP
b Tensile index, N·m/g
40 38 36 34 32
42 46 39
45 40% EP + 60% PP 1.5% PEO
44
36 33
43 42
30 Tensile index Maximum pore size
41
27
40 24 0.0
0.5
1.0
1.5
2.0
2.5
3.0
0
1
2
3
4
5
6
7
PVA dosage, % (on oven-dry fibers)
PEO dosage, % (on oven-dry fibers)
30
ACS Paragon Plus Environment
8
Maximum pore size, µ m
a Tensile index, N·m/g
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 30 of 33
Page 31 of 33
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Table 1
2
Basis weight (g/cm ) Maximum pore size (µm) Porosity (%) Tensile index (Nm/g) Alkali resistance (%) *
Standard valuea
Test sample*
30 ~ 50 30 ~ 50 ≥ 40 ≥ 40