Carbon Nanotubes Enhanced Fluorinated Polyurethane Macroporous

Jun 3, 2015 - Waterproof and breathable macroporous membranes that are both completely resistant to liquid water penetration and easily allowable to v...
0 downloads 7 Views 1MB Size
Subscriber access provided by NEW YORK UNIV

Article

Carbon Nanotubes Enhanced Fluorinated Polyurethane Macroporous Membranes for Waterproof and Breathable Application Yang Li, Zhigao Zhu, Jianyong Yu, and Bin Ding ACS Appl. Mater. Interfaces, Just Accepted Manuscript • DOI: 10.1021/acsami.5b02848 • Publication Date (Web): 03 Jun 2015 Downloaded from http://pubs.acs.org on June 7, 2015

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

ACS Applied Materials & Interfaces is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

1

Carbon Nanotubes Enhanced Fluorinated Polyurethane Macroporous

2

Membranes for Waterproof and Breathable Application

3

Yang Li,†,§ Zhigao Zhu,†,§ Jianyong Yu,‡,§ and Bin Ding*,†,‡,§

4



5

of Material Science and Engineering, Donghua University, Shanghai 201620, China

6



7

Textiles, Donghua University, Shanghai 201620, China

8

§

9

200051, China

State Key Laboratory for Modification of Chemical Fibers and Polymer Materials, College

Key Laboratory of Textile Science & Technology, Ministry of Education, College of

Nanomaterials Research Center, Modern Textile Institute, Donghua University, Shanghai

10 11 12 13 14 15 16 17

*

Corresponding author: Prof. Bin Ding (E-mail: [email protected])

ACS Paragon Plus Environment

1

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 28

18

ABSTRACT: Waterproof and breathable macroporous membranes that are both completely

19

resistant to liquid water penetration and easily allowable to vapor transmission would have

20

significant implication for numerous applications, however, fabrication of such materials has

21

proved to be tremendously challenging. Herein, we reported novel electrospun composite

22

fibrous membranes with high waterproof and breathable performance, which consisted of

23

polyurethane (PU), terminal fluorinated polyurethane (FPU) and carbon nanotubes (CNTs).

24

Benefiting from the utilization of FPU and CNTs, the fibrous membranes were endowed with

25

superhydrophobic surface, optimized pores size and porosity, along with enhanced fibers,

26

which resulted in excellent waterproof, breathable and mechanical properties. Significantly,

27

the relationship among waterproofness, pore structure and surface wettability has been

28

confirmed finely accordance with Young-Laplace equation. Ultimately, the resultant

29

membranes presented high waterproofness with hydrostatic pressure up to 108 kPa, good

30

breathability with water vapor transmission rate over 9.2 kg m-2 d-1, as well as robust

31

mechanical properties with bursting strength of 47.6 kPa and tensile strength of 12.5 MPa,

32

suggesting them as promising alternatives for a number of potential applications such as

33

protective clothing.

34 35

KEYWORDS: electrospinning, terminal fluorinated polyurethane, carbon nanotubes,

36

macroporous membrane, waterproof and breathable

37 38 39 40

ACS Paragon Plus Environment

2

Page 3 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

41

ACS Applied Materials & Interfaces

1. INTRODUCTION

42

Macroporous membranes that could strictly resist the penetration of liquid water while

43

easily transmitting water vapor molecules have brought a revolution in a number of practical

44

applications, including protective clothing and shoes, filter and separator media, and medical

45

supplies.1-4 In general, the fascinating properties of resistance to water droplets penetration

46

and the admittance to water vapor and gases transmission of these membranes are generated

47

from the utilization of hydrophobic raw materials, which turns the porous structure into

48

interconnected passageway with hydrophobic walls.5-6 Accordingly, the waterproof and

49

breathable performance could be improved not only by minimization of pore size to

50

withstand water penetration, but also maximization of porosity to transmit more water

51

vapor.7-8

52

Up to now, various conventional techniques have been employed to fabricate macroporous

53

membranes with waterproofness and breathability, including mechanical fibrillation,9

54

template methods10 and melt blown.11 Nevertheless, these methods are considered to be

55

complicated in controlling, time-consuming and high cost, as well as inappropriate in

56

regulating pore size and porosity to meet the requirement of better waterproof and breathable

57

performance.

58

Recently, electrospinning has proved to be an alternative to these methods, which could

59

facilely fabricate macroporous membranes by accumulating of fibers, moreover, the porous

60

structure could be controlled simply by regulating fiber diameter and packing density.12-14

61

Owing to these advantageous features, a lot of research efforts have been made to fabricate

62

waterproof and breathable macroporous membranes. In 2007, polyurethane (PU) was first

63

used to prepare waterproof and breathable fibrous membranes with macroporous structure,

64

which exhibited limited waterproofness with hydrostatic pressure of 3.7 kPa but good

65

breathability with water vapor transmission (WVT) rate of 9 kg m-2 d-1.15 Further

ACS Paragon Plus Environment

3

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 28

66

investigation had been done by utilizing thinner fibers, which resulted in higher hydrostatic

67

pressure of 80 kPa but depressed WVT rate of 4.3 kg m-2 d-1.16 In our previous study, we

68

reported a strategy for fabricating electrospun fibrous membranes with waterproof and

69

breathable properties by introducing low surface energy materials, which exhibited medium

70

hydrostatic pressure of 39.3 kPa along with high WVT rate of 9.2 kg m-2 d-1.17 Also reported

71

in our recent study is that by modifying polyacrylonitrile fibrous membranes with waterborne

72

polyurethane (WFPU) emulsion, we obtained waterproof and breathable fibrous membranes

73

with hydrostatic pressure of 83.4 kPa and WVT rate of 9.2 kg m-2 d-1, however, this strategy

74

suffered from the complicated modification procedure with WFPU emulsion.18 Therefore, in

75

order to satisfy the requirement of practical application, waterproof and breathable fibrous

76

membranes with improved performance and easy fabrication method are still in urgent

77

demand.

78

Intending to obtain electrospun fibrous membranes with better waterproof and breathable

79

performance, the fibrous membranes should be promoted by other stimulative additive,

80

besides the low surface energy component. Carbon nanotubes (CNTs) has been used as a

81

promising nanofiller to prepare electrospun composite fibers and fibrous membranes, due to

82

the extraordinary ability to improve mechanical, antifouling and electrical properties,19 as

83

well as obtainment of uniform fibers and pores,20 which could result in improvement of

84

waterproof and breathable performance of eleetrospun fibrous membranes.

85

On the other hand, the resistance of water penetration of macroporous membranes has

86

already known to be related to the capillary force which is generated from hydrophobic

87

feature and small pore size of the porous structure.21-22 However, the electrospun

88

macroporous membranes are constructed via accumulating of fibers during electrospinning

89

process, which result in torturous interconnected porous structures and complex situation for

90

liquid water flow through the membranes.23-24 Therefore, accurate investigation of the

ACS Paragon Plus Environment

4

Page 5 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

91

dependence of waterproof and breathable properties on the intrinsic structure characteristic is

92

significant and complicated, scarce efforts have focus on this problem.

93

In this study, we have designed and fabricated a kind of composite fibrous membranes

94

with waterproof and breathable performance via electrospinning. The composite fibrous

95

membranes consist of PU as substrate polymer, terminal fluorinated polyurethane (FPU) as

96

low surface energy content and CNTs as inspiring additive. Significantly, waterproof,

97

breathable and mechanical properties of the fibrous membranes were thoroughly investigated

98

basing on surface wettability, fibers construction and porous structure, which were regulated

99

be tuning the concentrations of polymers solutions and the contents of CNTs. Furthermore,

100

Young-Laplace equation was employed to estimate the dependence of hydrostatic pressure on

101

the pore structure and surface wettability. Ultimately, FPU/PU/CNTs fibrous membranes

102

with superhydrophobic surface, optimized porous structure and reinforced fibers were

103

obtained, which exhibited robust waterproof, breathable and mechanical performance.

104 105

2. EXPERIMENTAL SECTION

106

2.1. Materials. PU (Elastollan® 2280A10, Mw=180 000 g mol-1, density = 1.13 g cm-3) was

107

purchased from BASF Polyurethane Specialties Co., Ltd., China. Multi-wall carbon

108

nanotubes (CNTs, average diameter = 8 nm, length = 1-30 µm, purity > 95 wt%) were bought

109

from

110

(CF3(CF2)7CH2CH2OH, TEOH-8) was obtained from Hengtong Fluorine CO., Ltd., China.

111

4.4’-methylenebisphenylisocyanate (MDI), Polytetramethylene ether glycol (PTMEG, Mn =

112

1000 g mol-1), triethylene glycol (TEG), N,N-dimethylformamide (DMF), dimethylacetamide

113

(DMAc), Tetrahydrofuran (THF), anhydrous calcium chloride (CaCl2) and methanol were

114

provided by Aladdin Chemical Reagent Co., Ltd., China. All chemicals were of analytical

115

grade and were used as received without further purification.

Chengdu

Organic

Chemicals

Co.,

Ltd.,

China.

Perfluoro-1-decanol

ACS Paragon Plus Environment

5

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 6 of 28

116

2.2. Synthesis of terminal fluorinated polyurethane. The FPU was synthesized

117

according to a three-step polymerization route (as shown in Figure S1, Supporting

118

Information) described in our previous works.25 Typically, a mixture of TEOH-8 (9.28 g) and

119

DMF (8 g) was added dropwise into a flask containing 12.5 g MDI and 12 g of DMF. After

120

stirring at 50 oC for 2 h, PTMEG (7.5 g) was added slowly to the above solution as soft

121

segment to give a chain extending reaction at 60 oC for 2 h. Subsequently, TEG (2 g) as a

122

chain extender was poured into the flask and stirred at 70 oC for 2 h, then the mixture was

123

heated to 80 oC, followed by the addition of 2.32 g TEOH-8 and 2 g DMF to obtain FPU. The

124

resultant polymers were precipitated in excess water and dried in a vacuum oven at 60 oC,

125

then re-dissolved in DMAc and precipitated in an excess methanol/water mixture (1/1, w/w)

126

to remove low molecular weight products. The calculated mass fraction of perfluoroalkyl

127

species to FPU is 31.2%. The purified polymer was washed with methanol and water, and

128

dried in a vacuum oven at 60 oC to get the final FPU. The molecular weight of the final FPU

129

was measured by gel permeation chromatography, and Mw is 33 741 g mol-1. The structural

130

confirmation by 1H and

131

affirmations by Fourier transform infrared (FT-IR) spectrograph were presented in Figure S2,

132

S3 and S4 (Supporting Information).

19

F nuclear magnetic resonance (NMR) spectroscopy and group

133

2.3. Preparation of polymers solutions. The FPU/PU solutions were prepared by

134

dissolving FPU and PU in the mixture solvent of DMF/THF (1/1, w/w) with vigorous stirring

135

for 12 h at ambient temperature. The polymers concentrations of the solutions were 1.0, 1.5,

136

2.5, 3.5, and 4.5 wt%, respectively, and the FPU/PU weight ratio was kept 1:8 in all samples.

137

Additionally, the FPU/PU/CNTs solutions were prepared by dispersing CNTs in the 1.5 wt%

138

FPU/PU solution with ultrasonic treatment for 12 h. The contents of CNTs with respect to the

139

polymers weight were 0.25, 0.5, 0.75, and 1.0 %, respectively.

ACS Paragon Plus Environment

6

Page 7 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

140

2.4. Solutions properties. Electrical conductivity was measured using a conductivity

141

meter (FE30, Mettler-Toledo Group, Switzerland). Viscosity was tested using a viscometer

142

(SNB-1A, Shanghai Fangrui Instrument Co., Ltd., China) with spindle No. 21 at 50 rpm, and

143

surface tension was determined with tensiometer (QBZY, Shanghai Fangrui Instrument Co.,

144

Ltd., China) at ambient temperature.

145

2.5. Fabrication of the membranes. The fibrous membranes were fabricated via

146

electrospinning using the DXES-1 spinning equipment (Shanghai Oriental Flying

147

Nanotechnology Co., Ltd., China). Typically, the solution was loaded into a syringe and

148

injected through a metal needle with a controlled feed rate of 5 mL/h. A high voltage of 25

149

kV was applied to the needle tip, resulting in the generation of a continuous jet stream. The

150

fibrous membranes were deposited on a grounded metallic rotating roller at a 20 cm tip-to-

151

collector distance, and then dried in vacuum oven for 2 h at 80 oC to remove the residual

152

solvent. The electrospinning chamber was kept at a constant temperature (25 oC) and relative

153

humidity (50%). All the membranes were fabricated within an identical thickness of 30 ± 2

154

µm. The obtained membranes from the FPU/PU solutions were denoted as FPU/PU fibrous

155

membranes, and the ones fabricated from the 1.5 wt% FPU/PU solutions containing different

156

CNTs contents were denoted as FPU/PU/CNTs fibrous membranes. Nonporous membranes

157

with smooth surface were prepared using the dry-casting method. Typically, the polymers

158

solutions were cast uniformly on a glass plate, and were dried in a vacuum oven at 80 oC.

159

2.6. Characterization of the membranes. The morphology of the fibrous membranes was

160

observed by field emission scanning electron microscopy (FE-SEM, S-4800, Hitachi Ltd.,

161

Japan), all samples were coated with gold for 2min before analysis. The tensile mechanical

162

property was measured on a tensile tester (XQ-1C, Shanghai New Fiber Instrument Co., Ltd.,

163

China) with a crosshead speed of 10 mm min-1. The membranes were cut into strips with

164

width of 3 mm as testing samples, and the results were average value of ten samples from

ACS Paragon Plus Environment

7

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 28

165

each fibrous membrane. The bursting mechanical property was tested on a materials testing

166

machine (H10K-S, Tiniius Olsen Co., Ltd., USA) according to ISO 3303. Circular samples

167

with diameter of 4.5 cm fixed on the machine, and a steel ball was perpendicularly pressed on

168

the membrane with an advancing speed of 300 mm min-1, the results were average value of

169

five samples for each fibrous membrane. Advancing water contact angle (θadv, 5 µL) of the

170

membranes were measured by a contact angle goniometer Kino SL200B using the increment

171

method. Thickness was measured by a thickness gauge (CHY-C2, Labthink Instruments Co.,

172

Ltd., China). The pore size was characterized via bubble point method using a capillary flow

173

porometer (CFP-1100AI, Porous Materials Inc., USA). Porosity of the fibrous membranes

174

were calculated as: porosity =

175

( D 0 − D1) ×100% D0

(1)

176

where D0 was the density of the raw PU materials, D1 was the density of the obtained fibrous

177

membranes.26

178

2.7. Measurements of waterproof and breathable performance. The waterproofness of

179

the membranes were investigated by examining hydrostatic pressure of water penetration,

180

according to AATCC 127 standard test method for water penetration by using a hydrostatic

181

pressure tester (YG812C, Nantong Hongda Experiment Instruments Co., Ltd., China). The

182

samples were covered by a Nylon woven fabric to avoid deformation, and the water pressure

183

increasing rate is 6 kPa/min. The breathable performance was evaluated by measuring the

184

WVT rate according to ASTM E96-CaCl2 standards desiccant method by using a water vapor

185

transmission tester (YG 601H, Ningbo Textile Instruments Co., Ltd., China), under constant

186

temperature of 38 oC and relative humidity of 90%.

187 188

3. RESULTS AND DISCUSSION

ACS Paragon Plus Environment

8

Page 9 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

189

3.1. FPU/PU fibrous membranes. In order to obtain membranes with waterproof and

190

breathable properties, in the present work we designed hydrophobic fibrous membranes using

191

FPU and PU mixed solutions with different polymers concentrations (1.0-4.5 wt%). The

192

representative FE-SEM images of FPU/PU fibrous membranes obtained by varying the

193

polymers concentrations of FPU/PU solutions are presented in Figure 1 and S5 (Supporting

194

Information), revealing that the fibers oriented randomly to form three-dimensional

195

macroporous structures, which could serve as interconnected passageway for water and

196

vapor. When FPU/PU fibrous membrane was fabricated from 1.0 wt% polymers solution,

197

bead-on-string structures could be clearly observed (as shown in Figure 1a), which

198

constructed with thin fibers (average diameter of 162 nm, Table S1, Supporting Information)

199

and numerous micro-sized elliptical beads (average diameter of 1.46 µm) along the fiber axis.

200

This structure could be caused by the employment of solutions with low polymers

201

concentration and low viscosity (as shown in Table S1, Supporting Information), which

202

induced the instable whipping of solution jet during electrospinning.27-28 However, affected

203

by the solutions viscosity, the increase of polymers concentrations from 1.0 to 1.5 wt% led to

204

disappearance of beads and increased fiber diameter (272 nm), as presented in Figure 1b.

205

Further increase of polymers concentration from 2.5 to 4.5 wt% resulted in gradual increase

206

of fiber diameter from 757 to 3124 nm (shown in Figure 1c-d and Figure S5, Supporting

207

Information). Meanwhile, adhesion structures among the adjacent fibers could be observed

208

obviously in all the samples, which could be formed due to the incomplete evaporation of

209

DMF used as good solvent for both FPU and PU.29-30 The formation of adhesion structure

210

made the electrospun fibers into a dimensionally stable network, which would improve the

211

mechanical properties of the membranes.

ACS Paragon Plus Environment

9

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 10 of 28

212 213

Figure 1. Morphology, mechanical properties and pore structure of FPU/PU fibrous

214

membranes. FE-SEM images of FPU/PU fibrous membranes fabricated from polymers

215

solutions with different concentrations: (a) 1.0 wt%, (b) 1.5 wt%, (c) 2.5 wt%, and (d) 3.5

216

wt%, respectively. (e) Bursting strength and elongation, (f) tensile strength and elongation at

217

break, (g) dmax and porosity of FPU/PU fibrous membranes fabricated from polymers

218

solutions with different concentrations. The FPU/PU weight ratio was kept 1:8.

219

Owing to the structure transformation of the fibers and the existence of adhesion structures,

220

mechanical properties of the fibrous membranes would be affected distinctly, which were

221

evaluated by measuring bursting strength normal to the long axis and tensile strength along

222

the long axis of the membranes.31 As shown in Figure 1e, the FPU/PU fibrous membrane

223

formed from 1.0 wt% polymers solution exhibits the minimum bursting strength (15.6 kPa)

224

and elongation (15.6 mm), which is mainly due to the bead-on-string structures and small

225

fiber diameter that could not afford high external stress.2, 31 However, with the disappearance

226

of beads and the increase of fiber diameter, the membranes fabricated from higher polymers

227

concentrations exhibit enhanced bursting strength up to 65.2 kPa and increased elongation up

228

to 40.3 mm (details are presented in Table S2, Supporting Information). Similarly, the

229

minimum tensile strength (4.1 MPa) and elongation (129.1%) was observed at the polymers

ACS Paragon Plus Environment

10

Page 11 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

230

concentrations of 1.0 wt%, as shown in Figure 1f. Moreover, a sharp increase of tensile

231

mechanical properties could be observed with the polymers concentration increasing to 1.5

232

wt% according to the transformation of fibers structure, wherein, the tensile strength at break

233

is 7.8 MPa and the elongation is 255.1%. Further increase of polymers concentrations to 4.5

234

wt% resulted in sizable increased tensile strength up to 12.7 MPa and elongation up to

235

469.8% (details are presented in Table S2, Supporting Information). These results

236

demonstrate that the mechanical properties could be improved with the increasing of

237

concentrations of polymers solutions, which would attributed to the increase of fiber diameter

238

that provided stronger individual fibers, as well as the existence of adhesion structures that

239

prevented the randomly oriented fibers from pulling apart.32

240

In the meantime, the porous structure of FPU/PU fibrous membranes had been changed

241

remarkably along with the transformation of fibers structure. Since liquid water would

242

preferentially penetrate into a porous media under relative low external pressure through the

243

pore with maximum diameter,33-34 maximum pore diameters (dmax) of the FPU/PU fibrous

244

membranes were measured via bubble point method. As presented in Figure 1g, with the

245

polymers concentrations increased from 1.0 to 4.5 wt%, the dmax of the FPU/PU fibrous

246

membranes increased from 1.57 to 5.39 µm (details are shown in Table S3, Supporting

247

Information), which could be attributed to the accumulating of thicker fibers that formed

248

larger space among the adjacent fibers.35 Additionally, the porosity of the membranes were

249

calculated as well, which would stand for the capacity of interconnected passageway. As

250

shown in Figure 1g, the porosity of FPU/PU fibrous membranes decreased from 45.8% to

251

35.2% (details are shown in Table S3, Supporting Information)with the of polymers

252

concentrations increasing from 1.0 to 4.5 wt%. These transmission of porosity could be

253

related to the thicker fibers and higher adhesion rate that took over more space among fibers,

254

which is consistent well with the precious studies.36-37

ACS Paragon Plus Environment

11

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 12 of 28

255

More interestingly, it also should be noticed that hierarchical surface structures with

256

micro/nanoscale wrinkles are clearly visible in the close observations of all samples (insets in

257

Figure 1a-d). The formation of these structures would be attributed to the low surface tension

258

and electrical repulsion of solution jet containing FPU as low surface energy content, which

259

generated collapse on the fluid jet surface during fast phase separation, similar to our

260

previous reports.17, 38 It is noteworthy that the cooperation of low surface energy additive and

261

hierarchical surface structure is considered to be strategic factor for surface hydrophobicity,

262

attributing to the entrapped air among the wrinkles like a repulsive cushion to water droplets,

263

as stated previously. As expected, all the FPU/PU fibrous membranes exhibited hydrophobic

264

surface with θadv reached up to 146 ± 2o (as shown in Table S4, Supporting Information),

265

which would contribute to the resistance to liquid water penetration.17, 39 Furthermore, θadv of

266

dry-casting membranes were also tested, which could exclude the effect of macro-sized

267

surface morphology of the membranes and represent the surface properties of the inner pores.

268

As shown in Table S4, the θadv of the all the dry-casting membranes were 117o, which colud

269

be propitious to stimulate the flow process of liquid water in the pores.40

ACS Paragon Plus Environment

12

Page 13 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

270 271

Figure 2. Waterproof and breathable properties of FPU/PU fibrous membranes. (a)

272

Hydrostatic pressure and (b) WVT rate of FPU/PU fibrous membranes fabricated from

273

polymers solutions with various concentrations. The inset in (a) showing the relationship

274

among hydrostatic pressure, dmax and θadv.

275

Benefiting from hydrophobic properties, FPU/PU fibrous membranes were endowed with

276

waterproofness, which was evaluated by measuring the hydrostatic pressure for water

277

penetration. As presented in Figure 2a, FPU/PU fibrous membrane obtained from 1.0 wt%

278

polymers solution exhibits the best waterproofness with hydrostatic pressure of 84.2 kPa.

279

Subsequently, with the increase of polymers concentration to 1.5 wt%, the hydrostatic

280

pressure goes down slightly to 81.1 kPa. And further increase of polymers concentrations

281

resulted in dramatically decrease of hydrostatic pressure. Since all the membranes exhibit

282

similar wettability, the decreased hydrostatic pressure of membranes obtained from higher

ACS Paragon Plus Environment

13

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 14 of 28

283

polymers concentrations should be mainly attributed to the enormous increased dmax, which

284

would be penetrated under lower external water pressure.41 Further investigation of the

285

relationship among hydrostatic pressure, hydrophobicity and pore size was carried out by

286

employing the Young-Laplace equation, which is commonly used to express the liquid enter

287

pressure of a cylindrical capillary:

288

4γ ⋅ cosθ adv d max

289

where P is the hydrostatic pressure, γ is the surface tension of water, θadv is the advancing

290

water contact angle of dry-casting membranes, and dmax is the diameter of the maximum

291

pores.42-43 Significantly, as shown in the inset in Figure 2a, the relationship among

292

hydrostatic pressure, dmax and θadv has been confirmed finely accordance with the Young-

293

Laplace equation.

P=−

(2)

294

On the other hand, the macroporous structure in FPU/PU fibrous membranes would play a

295

role as interconnected passageway for water vapor transmitting across the membranes, which

296

perform as breathability of membranes. Therefore, WVT rate of FPU/PU fibrous membranes

297

obtained from different polymers concentrations had been measured to estimate the

298

breathability. As shown in Figure 2b, the WVT rate of the fibrous membranes decreased from

299

9.2 to 7.3 kg m-2 d-1 gradually with the increase of polymers concentrations, revealing

300

impaired breathability. This would be attributed to that membranes with lower porosity

301

possess less interconnected passageway for water vapor transmission.36, 44 Considering the

302

practical application, the membranes should not only possess good mechanical properties, but

303

also exhibit high waterproof and breathable performance. Since lower polymers

304

concentration (1.5 wt%) could lead to

306

inappropriate porous structure and remarkable reduction of waterproof and breathable

ACS Paragon Plus Environment

14

Page 15 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

307

performance, the FPU/PU fibrous membranes fabricated from 1.5 wt% polymers solution

308

would be carried out in the following study.

309

3.2. FPU/PU/CNTs fibrous membranes. To further explore the applicability of the

310

fibrous membranes for waterproof and breathable application, herein, FPU/PU/CNTs fibrous

311

membranes containing various CNTs contents (0-1.0% with respect to polymers weight) were

312

investigated, the polymers concentration of the solutions were kept 1.5 wt%. In order to study

313

the morphology transformation generated from the addition of CNTs, a comparison between

314

FPU/PU/CNTs fibrous membranes containing 0% and 0.75% CNTs was investigated by FE-

315

SEM images and cross section images, as shown in Figure 3a-d. The FPU/PU/CNTs fibrous

316

membranes without CNTs loading exhibits fiber diameter of 272 nm (as described above)

317

and broad fiber diameter distribution ranging from 140 to 440 nm (as shown in Figure 3e),

318

which could be attributed to the conductivity and viscosity of 1.5 wt% polymers solutions

319

that is appropriate for the disappearance of beads but not adequate for effective stretching of

320

solution jet to provide uniform fibers.28 However, the FPU/PU/CNTs fibrous membranes

321

containing 0.75% CNTs reveals thinner fiber diameter of 180 nm (Figure 3b) and narrower

322

fiber diameter distribution ranging from 100 to 310 nm (as shown in Figure 3e). This would

323

be related to the increased conductivity that could inspired the stretching effect during

324

electrospinning process, as well as the slightly increased viscosity that could afford more

325

intense whipping.45-46

ACS Paragon Plus Environment

15

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 16 of 28

326 327

Figure 3. Structure of FPU/PU/CNTs fibrous membranes. FE-SEM images of FPU/PU/CNTs

328

fibrous membranes containing different CNTs contents: (a) 0% and (b) 0.75%. Cross section

329

images of FPU/PU/CNTs fibrous membranes containing different CNTs contents: (c) 0% and

330

(d) 0.75%. (e) Fiber diameter distribution of FPU/PU/CNTs fibrous membranes containing

331

0% and 0.75% CNTs. (f) Pore size distribution, (g) dmax and porosity of FPU/PU/CNTs

332

fibrous membranes containing various contents of CNTs. The FPU/PU concentration of all

333

the solutions was kept 1.5 wt%, and the FPU/PU weight ratio was kept 1:8.

334

At the meantime, the macroporous structure FPU/PU/CNTs fibrous membranes containing

335

0% and 0.75% CNTs was investigated by FE-SEM cross section images, revealing that the

336

fibers accumulated layer-by-layer to construct interconnected porous structures, as shown in

337

Figure 3c and d. As can be seen in Figure 3c, the fibrous membranes containing 0% CNTs

338

exhibits irregular porous structure with pore size distribution from 0.40 to 1.77 µm (as shown

339

in Figure 3f), which is related to the accumulation of fibers with un-uniformed diameter.

340

However, more regular porous structure with pore size distribution from 0.58 to 1.40 µm (as

341

shown in Figure 3f) would be observed in the membranes containing 0.75% CNTs. It is

342

mainly due to the increased solutions conductivity, which not only generated fibers with

343

uniform diameter, but also brought about densely accumulated fibers.47-48 Similar

ACS Paragon Plus Environment

16

Page 17 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

344

transformation also occurred in the other FPU/PU/CNTs fibrous membranes with various

345

CNTs concentrations (as shown in Figure S6, Supporting Information). Accordingly,

346

benefiting from the introduction of CNTs and the transformation of fiber diameter, the dmax of

347

FPU/PU/CNTs fibrous membranes decreased from 1.77to 1.40 µm gradually, and the

348

porosity increased slightly from 43.4% to 45.5% (as shown in Figure 5g and Table S3,

349

Supporting Information).

350

Moreover, with the addition of CNTs, more rough structure had been formed on the

351

surface of fibers (as can be seen in Figure 3d), which is similar to the previous studies and

352

would influence the hydrophobicity of the inner pores.49 As a result, θadv of the fibrous

353

membranes and the dry-casting membranes increased to 155o and 122o, respectively, as

354

shown in Table S4 and Figure S7 (Supporting Information), indicating an increased

355

hydrophobicity which would lead to higher resistance to water penetration.

356

ACS Paragon Plus Environment

17

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 18 of 28

357

Figure 4. Waterproof and breathable properties of FPU/PU fibrous membranes. (a)

358

Hydrostatic pressure and (b) WVT rate of FPU/PU/CNTs fibrous membranes containing

359

various contents of CNTs. The inset in (a) is the relationship among hydrostatic pressure, dmax

360

and θadv.

361

As expected, the optimized porous structure and improved surface hydrophobicity have led

362

to better waterproofness. As shown in Figure 4a, the hydrostatic pressure of FPU/PU/CNTs

363

fibrous membranes with 0.25%, 0.5%, 0.75%, and 1.0% CNTs were 98, 104, 108, and 109

364

kPa, respectively, which increased regularly with the decreasing of dmax and the increasing of

365

θadv. Furthermore, as can be seen in the inset of Figure 4a, the relationship among hydrostatic

366

pressure, dmax and θadv is finely conformed to the Young-Laplace equation.23-24 Meanwhile,

367

with the contents of CNTs increasing from 0% to 1.0%, the WVT rate increased from 8.8 to

368

9.3 kg m-2 d-1, as presented in Figure 4b. This would be attributed to that membranes with

369

higher porosity could provide more interconnected passageway for vapor transmission, which

370

exhibit better breathability. More interestingly, a demonstration of waterproofness and

371

breathable performances has been presented in Figure S8 (Supporting Information), wherein,

372

the FPU/PU/CNTs fibrous membrane was covered on a beaker with boiling water, and three

373

placed water droplets could not penetrate into the membrane while massive vapor transmitted

374

facilely through the membrane. Significantly, the optimized FPU/PU/CNTs fibrous

375

membranes exhibit better comprehensive performance in comparison of the conventional

376

waterproof and breathable materials, as presented in Figure S9 (Supporting Information).

ACS Paragon Plus Environment

18

Page 19 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

377 378

Figure 5. Mechanical properties of FPU/PU/CNTs fibrous membranes. (a) Bursting strength

379

and elongation, (b) tensile stress-strain curves of the FPU/PU/CNTs fibrous membranes

380

containing different contents of CNTs. (c) Proposed break mechanism of tensile fracture

381

process upon external stress. (d)-(g) In-situ SEM images of stretching process of the

382

FPU/PU/CNTs fibrous membranes containing 0.75% CNTs with different elongation: (d)

383

0%, (e) 50%, (f) 150% and (g) 300%, respectively.

384

Mechanical properties are important factors in practical application of waterproof and

385

breathable membranes, which would be notably influenced by the loading of CNTs. one of

386

the mechanical properties is bursting strength which would directly characterize the

387

resistance to external pressure perpendicular to the membranes. As shown in Figure 5a, with

388

the CNTs increasing to 0.75 %, the bursting strength increased to 47.6 kPa, which would

389

related to the reinforcement of CNTs (details are shown in Table S2, Supporting

390

Information).46,

391

strength of 30.0 kPa. This could mainly due to beads structure formed by the agglomeration

392

of CNTs at higher content (as shown in Figure S10, Supporting Information), which would

393

serve as stress concentrations that break prematurely.51-52 Meanwhile, the elongation of the

50

However, further increase of CNTs to 1.0% led to decreased bursting

ACS Paragon Plus Environment

19

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 20 of 28

394

membranes decreased gradually with higher loadings of CNTs, indicating that the membranes

395

would exhibit better dimensional stability under external water pressure.

396

At the same time, tensile strength is another mechanical property which would be

397

significant to the subsequent process of the membranes. Figure 5b presents the typical tensile

398

stress-strain curves of FPU/PU/CNTs fibrous membranes containing various CNTs contents.

399

Similar to the bursting mechanical property, the membranes demonstrated increased tensile

400

strength from 7.8 to 12.5 MPa with the content of CNTs increasing to 0.75%, which revealed

401

the reinforcement effect of CNTs46, 50. However, owing to the agglomeration of CNTs with

402

content of 1.0%, a reduction of tensile strength to 11.7 MPa could be observed. Moreover, all

403

samples reveal same nonlinear curve shape with little elongation under small stress loading

404

(Stage 1 in Figure 5b) and large elongation under little further increase of stress until broken

405

(Stage 2 in Figure 5b). This phenomenon could be illustrated by the two-step break

406

mechanism (as shown in Figure 5c), which has been demonstrated by in-situ FEM images of

407

the stretching process (Figure 5d-g). When a small external stress was loaded, nonaligned

408

fibers (Figure 5d) between bonding points started to orientate (Figure 5e), which led to little

409

elongation. With continual increasing of tensile stress, the nonbonding fibers slipping apart,

410

while the fibers between bonding points undertook the stress and became orientated and

411

thinner (Figure 5f), which resulted in rapid increase of elongation. Finally, the fibrous

412

membranes broke due to the fracture of fibers between bonding points, which was marked

413

with yellow circle (Figure 5g). Consequently, the above waterproof, breathable and

414

mechanical properties suggest the FPU/PU/CNTS fibrous membrane as a promising

415

candidate for a variety of potential applications, such as protective clothing, filter and

416

separator media, and medical supplies.

417

4. CONCLUSIONS

ACS Paragon Plus Environment

20

Page 21 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

418

In summary, we have described the fabrication of FPU/PU/CNTs fibrous membranes

419

exhibiting excellent waterproof and breathable performance. The introduction of FPU and

420

CNTs endowed the resultant membranes with hydrophobic surface properties. Uniform pore

421

structure and decreased maximum pore diameter were obtained with the addition of CNTs.

422

Significantly, the dependence of hydrostatic pressure on dmax and θadv was confirmed to be

423

finely accordance with the Young-Laplace equation. Consequently, the as-prepared

424

membranes containing 0.75% CNTs exhibited excellent waterproofness of 108 kPa, high

425

water vapor transmission rate of 9.2 kg m-2 d-1, as well as good mechanical properties with

426

bursting strength of 47.6 kPa and tensile strength of 12.5 MPa. These properties suggest the

427

FPU/PU/CNTS fibrous membrane as a promising candidate for a variety of potential

428

applications, such as protective clothing, filter and separator media.

429 430

ASSOCIATIED CONTENT

431

Supporting information. Schematic diagram illustrating the strategy for synthesis of FPU

432

(Figure S1), 1H NMR spectrum of FPU (Figure S2), 19F NMR spectrum of FPU (Figure S3),

433

FT-IR spectrum of FPU (Figure S4), FE-SEM image of FPU/PU fibrous membrane

434

fabricated from 4.5 wt% polymers solution (Figure S5), compositions and properties of the

435

polymers solutions (Table S1), mechanical properties of the fibrous membranes (Table S2),

436

dmax and porosity of the fibrous membranes (Table S3), θadv of fibrous membranes and dry-

437

casting membranes (Table S4), pore size distribution of FPU/PU/CNTs fibrous membranes

438

containing 0.25%, 0.5%, and 0.75% CNTs (Figure S6), θadv of the FPU/PU/CNTs dry-casting

439

membranes (Figure S7), a demonstration of waterproof and breathable performance (Figure

440

S8), a comparison of waterproof and breathable properties between current materials and

441

FPU/PU/CNTs fibrous membrane containing 0.75% CNTs (Figure S9), FE-SEM image of

ACS Paragon Plus Environment

21

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 22 of 28

442

FPU/PU/CNTs fibrous membrane containing 1.0 % CNTs (Figure S10). This material is

443

available free of charge via the Internet at http://pubs.acs.org.

444 445

AUTHOR INFORMATION

446

Corresponding Author

447 448 449 450

*

Prof. Bin Ding, Email: [email protected].

Author Contributions The manuscript was written through contributions of all authors. All authors have given approval to the final version of the manuscript.

451 452

ACKNOWLEDGEMENTS

453

This work is supported by the National Natural Science Foundation of China (No.

454

51473030 and 51322304), the Fundamental Research Funds for the Central Universities, and

455

the “DHU Distinguished Young Professor Program”.

456 457 458 459

ACS Paragon Plus Environment

22

Page 23 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

460

REFERENCES

461

(1) Lomax, G. R. Breathable Polyurethane Membranes for Textile and Related Industries. J.

462

Mater. Chem. 2007, 17, 2775.

463

(2) Wang, X. F.; Ding, B.; Yu, J. Y.; Wang, M. R. Engineering Biomimetic

464

Superhydrophobic Surfaces of Electrospun Nanomaterials. Nano Today 2011, 6, 510-

465

530.

466 467 468

(3) Gugliuzza, A.; Drioli, E. PVDF and HYFLON AD Membranes: Ideal Interfaces for Contactor Applications. J. Membr. Sci. 2007, 300, 51-62. (4) Lalia, B. S.; Guillen-Burrieza, E.; Arafat, H. A.; Hashaikeh, R. Fabrication and

469

Characterization

470

Electrospun Membranes for Direct Contact Membrane Distillation. J. Membr. Sci. 2013,

471

428, 104-115.

472 473 474 475

of

Polyvinylidenefluoride-co-Hexafluoropropylene

(PVDF-HFP)

(5) Gugliuzza, A.; Drioli, E. A Review on Membrane Engineering for Innovation in Wearable Fabrics and Protective Textiles. J. Membr. Sci. 2013, 446, 350-375. (6) Rivin, D.; Kendrick, C. E.; Gibson, P. W.; Schneider, N. S. Solubility and Transport Behavior of Water and Alcohols in Nafion™. Polymer 2001, 42, 623-635.

476

(7) Zhou, C.; Wang, Z.; Liang, Y. L.; Yao, J. M. Study on the Control of Pore Sizes of

477

Membranes Using Chemical Methods Part II. Optimization Factors for Preparation of

478

Membranes. Desalination 2008, 225, 123-138.

479

(8) Gugliuzza, A.; Drioli, E. New Performance of Hydrophobic Fluorinated Porous

480

Membranes Exhibiting Particulate-Like Morphology. Desalination 2009, 240, 14-20.

481

(9) Tabatabaei, S. H.; Carreau, P. J.; Ajji, A. Microporous Membranes Obtained from

482 483 484

Polypropylene Blend Films by Stretching. J. Membr. Sci. 2008, 325, 772-782. (10) Pan, J. H.; Dou, H.; Xiong, Z.; Xu, C.; Ma, J.; Zhao, X. S. Porous Photocatalysts for Advanced Water Purifications. J. Mater. Chem. 2010, 20, 4512-4528.

485

(11) Yu, B.; Han, J.; He, X. B.; Xu, G. P.; Ding, X. B. Effects of Tourmaline Particles on

486

Structure and Properties of Polypropylene Filtration Melt-Blown Nonwoven Electrets. J.

487

Macromol. Sci., Part B: Phys. 2012, 51, 619-629.

488

(12) Wang, X. F.; Ding, B.; Sun, G.; Wang, M. R.; Yu, J. Y. Electro-Spinning/Netting: A

489

Strategy for the Fabrication of Three-Dimensional Polymer Nano-Fiber/Nets. Prog.

490

Mater. Sci. 2013, 58, 1173-1243.

491 492

(13) Erisken, C.; Kalyon, D. M.; Wang, H. J. Functionally Graded Electrospun Polycaprolactone

and

Beta-Tricalcium

Phosphate

Nanocomposites

for

Tissue

ACS Paragon Plus Environment

23

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

493 494 495 496 497

Page 24 of 28

Engineering Applications. Biomaterials 2008, 29, 4065-4073. (14) Wang, X. F.; Ding, B.; Li, B. Y. Biomimetic Electrospun Nanofibrous Structures for Tissue Engineering. Mater. Today 2013, 16, 229-241. (15) Park, C. H.; Chung, S. E.; Yun, C. S. Effect of Drying Condition on the Electrostatic Characteristics of the Laundry. Fibers Polym. 2007, 8, 432-437.

498

(16) Yoon, B.; Lee, S. Designing Waterproof Breathable Materials Based on Electrospun

499

Nanofibers and Assessing the Performance Characteristics. Fibers Polym. 2011, 12, 57-

500

64.

501

(17) Ge, J. F.; Si, Y.; Fu, F.; Wang, J. L.; Yang, J. M.; Cui, L. X.; Ding, B.; Yu, J. Y.; Sun, G.

502

Amphiphobic fluorinated Polyurethane Composite Microfibrous Membranes with

503

Robust Waterproof and Breathable Performances. RSC Adv. 2013, 3, 2248-2255.

504

(18) Wang, J. Q.; Li, Y.; Tian, H. Y.; Sheng, J. L.; Yu, J. Y.; Ding, B. Waterproof and

505

Breathable Membranes of Waterborne Fluorinated Polyurethane Modified Electrospun

506

Polyacrylonitrile Fibers. RSC Adv. 2014, 4, 61068-61076.

507

(19) Ko, F.; Gogotsi, Y.; Ali, A.; Naguib, N.; Ye, H.; Yang, G. L.; Li, C.; Willis, P.

508

Electrospinning of Continuous Carbon Nanotube-Filled Nanofiber Yarns. Adv. Mater.

509

2003, 15, 1161-1165.

510

(20) Coleman, J. N.; Khan, U.; Blau, W. J.; Gun’ko, Y. K. Small but strong: A Review of the

511

Mechanical Properties of Carbon Nanotube-Polymer Composites. Carbon 2006, 44,

512

1624-1652.

513 514

(21) Kim, B. S.; Harriott, P. Critical Entry Pressure for Liquids in Hydrophobic Membranes. J. Colloid Interface Sci. 1987, 115, 1-8.

515

(22) Shirtcliffe, N. J.; McHale, G.; Newton, M. I.; Zhang, Y. Superhydrophobic Copper

516

Tubes with Possible Flow Enhancement and Drag Reduction. ACS Appl. Mater.

517

Interfaces 2009, 1, 1316-1323.

518

(23) Bui, N. N.; Lind, M. L.; Hoek, E. M. V.; McCutcheon, J. R. Electrospun Nanofiber

519

Supported Thin Film Composite Membranes for Engineered Osmosis. J. Membr. Sci.

520

2011, 385–386, 10-19.

521

(24) Zhou, W. P.; Wu, Y. L.; Wei, F.; Luo, G. H.; Qian, W. Z. Elastic Deformation of

522

Multiwalled Carbon Nanotubes in Electrospun MWCNTs-PEO and MWCNTs-PVA

523

Nanofibers. Polymer 2005, 46, 12689-12695.

524

(25) Wang, J. L.; Raza, A.; Si, Y.; Cui, L. X.; Ge, J. F.; Ding, B.; Yu, J. Y. Synthesis of

525

Superamphiphobic Breathable Membranes Utilizing SiO2 Nanoparticles Decorated

526

Fluorinated Polyurethane Nanofibers. Nanoscale 2012, 4, 7549-7556.

ACS Paragon Plus Environment

24

Page 25 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

527

(26) Mika, A. M.; Childs, R. F.; Dickson, J. M.; McCarry, B. E.; Gagnon, D. R. A New Class

528

of Polyelectrolyte-Filled Microfiltration Membranes with Environmentally Controlled

529

Porosity. J. Membr. Sci. 1995, 108, 37-56.

530 531 532 533

(27) Lin, J.; Ding, B.; Yu, J. Direct Fabrication of Highly Nanoporous Polystyrene Fibers via Electrospinning. ACS Appl Mater Interfaces 2010, 2, 521-528. (28) Greiner, A.; Wendorff, J. H. Electrospinning: A Fascinating Method for the Preparation of Ultrathin Fibers. Angew. Chem. Int. Ed. 2007, 46, 5670-5703.

534

(29) Khil, M. S.; Cha, D. I.; Kim, H. Y.; Kim, I. S.; Bhattarai, N. Electrospun Nanofibrous

535

Polyurethane Membrane as Wound Dressing. J. Biomed. Mater. Res., Part B 2003, 67B,

536

675-679.

537

(30) Mao, X.; Chen, Y. C.; Si, Y.; Li, Y.; Wan, H. G.; Yu, J. Y.; Sun, G.; Ding, B. Novel

538

Fluorinated Polyurethane Decorated Electrospun Silica Nanofibrous Membranes

539

Exhibiting Robust Waterproof and Breathable Performances. RSC Adv. 2013, 3, 7562-

540

7569.

541

(31) Yao, C.; Li, X. S.; Neoh, K. G.; Shi, Z. L.; Kang, E. T. Surface Modification and

542

Antibacterial Activity of Electrospun Polyurethane Fibrous Membranes with Quaternary

543

Ammonium Moieties. J. Membr. Sci. 2008, 320, 259-267.

544

(32) Lee, K. H.; Kim, H. Y.; Ryu, Y. J.; Kim, K. W.; Choi, S. W. Mechanical Behavior of

545

Electrospun Fiber Mats of Poly(vinyl chloride)/Polyurethane Polyblends. J. Polym. Sci.,

546

Part B: Polym. Phys. 2003, 41, 1256-1262.

547 548 549 550

(33) Hopkinson, D.; Zeh, M.; Luebke, D. The Bubble Point of Supported Ionic Liquid Membranes Using Flat Sheet Supports. J. Membr. Sci. 2014, 468, 155-162. (34) Wang, R.; Liu, Y.; Li, B.; Hsiao, B. S.; Chu, B. Electrospun Nanofibrous Membranes for High Flux Microfiltration. J. Membr. Sci. 2012, 392-393, 167-174.

551

(35) Li, X.; Wang, N.; Fan, G.; Yu, J. Y.; Gao, J.; Sun, G.; Ding, B. Electreted

552

Polyetherimide-Silica Fibrous Membranes for Enhanced Filtration of Fine Particles. J.

553

Colloid Interface Sci. 2015, 439, 12-20.

554 555 556 557 558 559 560

(36) Ryu, Y. J.; Kim, H. Y.; Lee, K. H.; Park, H. C.; Lee, D. R. Transport Properties of Electrospun Nylon 6 Nonwoven Mats. Eur. Polym. J. 2003, 39, 1883-1889. (37) Gibson, P.; Schreuder-Gibson, H.; Rivin, D. Transport Properties of Porous Membranes Based on Electrospun Nanofibers. Colloids Surf., A 2001, 187-188, 469-481. (38) Reneker, D. H.; Yarin, A. L. Electrospinning Jets and Polymer Nanofibers. Polymer

2008, 49, 2387-2425. (39) Manabe, K.; Nishizawa, S.; Kyung, K. H.; Shiratori, S. Optical Phenomena and

ACS Paragon Plus Environment

25

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 26 of 28

561

Antifrosting Property on Biomimetics Slippery Fluid-Infused Antireflective Films via

562

Layer-by-Layer Comparison with Superhydrophobic and Antireflective Films. ACS

563

Appl. Mater. Interfaces 2014, 6, 13985-13993.

564

(40) Si, Y.; Fu, Q. X.; Wang, X. Q.; Zhu, J.; Yu, J. Y.; Sun, G.; Ding, B. Superelastic and

565

Superhydrophobic Nanofiber-Assembled Cellular Aerogels for Effective Separation of

566

Oil/Water Emulsions. ACS Nano 2015, 9, 3791-3799.

567

(41) Manabe, K.; Nishizawa, S.; Shiratori, S. Porous Surface Structure Fabricated by Breath

568

Figures that Suppresses Pseudomonas Aeruginosa Biofilm Formation. ACS Appl. Mater.

569

Interfaces 2013, 5, 11900-11905.

570

(42) Saffarini, R. B.; Mansoor, B.; Thomas, R.; Arafat, H. A. Effect of Temperature-

571

Dependent Microstructure Evolution on Pore Wetting in PTFE Membranes Under

572

Membrane Distillation Conditions. J. Membr. Sci. 2013, 429, 282-294.

573 574

(43) Hu, H.; Larson, R. G. Evaporation of a Sessile Droplet on a Substrate. J. Phys. Chem. B

2002, 106, 1334-1344.

575

(44) Yuan, D.; Cheng, H.; Edwards, R. L.; Dykoski, C. A.; Kelly, M. J.; Zhang, M.; Qing, J.;

576

Lin, Y.; Wang, Y.; Wu, J.; Dorale, J. A.; An, Z.; Cai, Y. Timing, Duration, and Transitions

577

of the Last Interglacial Asian Monsoon. Science 2004, 304, 575-578.

578 579 580

(45) Xie, X. L.; Mai, Y. W.; Zhou, X. P. Dispersion and Alignment of Carbon Nanotubes in Polymer Matrix: A Review. Mater. Sci. Eng., R 2005, 49, 89-112. (46) Wang, X.; Si, Y.; Wang, X.; Yang, J.; Ding, B.; Chen, L.; Hu, Z.; Yu, J. Tuning

581

Hierarchically

Aligned

Structures

for

582

Nanofibers. Nanoscale 2013, 5, 886-889.

High-Strength

PMIA-MWCNT

Hybrid

583

(47) Zhu, Q.; Li, Y. Effects of Pore Size Distribution and Fiber Diameter on the Coupled

584

Heat and Liquid Moisture Transfer in Porous Textiles. Int. J. Heat Mass Transfer 2003,

585

46, 5099-5111.

586

(48) Lowery, J. L.; Datta, N.; Rutledge, G. C. Effect of Fiber Diameter, Pore Size and

587

Seeding Method on Growth of Human Dermal Fibroblasts in Electrospun Poly(ɛ-

588

caprolactone) Fibrous Mats. Biomaterials 2010, 31, 491-504.

589

(49) Mathew, G.; Hong, J. P.; Rhee, J. M.; Lee, H. S.; Nah, C. Preparation and

590

Characterization of Properties of Electrospun Poly(butylene terephthalate) Nanofibers

591

Filled with Carbon Nanotubes. Polym. Test. 2005, 24, 712-717.

592

(50) Dror, Y.; Salalha, W.; Khalfin, R. L.; Cohen, Y.; Yarin, A. L.; Zussman, E. Carbon

593

Nanotubes Embedded in Oriented Polymer Nanofibers by Electrospinning. Langmuir

594

2003, 19, 7012-7020.

ACS Paragon Plus Environment

26

Page 27 of 28

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

595

(51) Su, Z. Q.; Li, J. F.; Li, Q.; Ni, T. Y.; Wei, G. Chain Conformation, Crystallization

596

Behavior, Electrical and Mechanical Properties of Electrospun Polymer-Carbon

597

Nanotube Hybrid Nanofibers with Different Orientations. Carbon 2012, 50, 5605-5617.

598 599

(52) Coleman, J. N.; Khan, U.; Gun'ko, Y. K. Mechanical Reinforcement of Polymers Using Carbon Nanotubes. Adv. Mater. 2006, 18, 689-706.

600

ACS Paragon Plus Environment

27

ACS Applied Materials & Interfaces

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

601

Page 28 of 28

Table of Contents Graphic

602 603

ACS Paragon Plus Environment

28