Chemical Vapor Deposition Growth of Two ... - ACS Publications

Jul 16, 2018 - The highlighted green color region has an rms of 0.19 nm. (d) Height profile of a continuous GaS film measured across the black line in...
0 downloads 0 Views 9MB Size
This is an open access article published under an ACS AuthorChoice License, which permits copying and redistribution of the article or any adaptations for non-commercial purposes.

Article Cite This: ACS Omega 2018, 3, 7897−7903

Chemical Vapor Deposition Growth of Two-Dimensional Monolayer Gallium Sulfide Crystals Using Hydrogen Reduction of Ga2S3 Xiaochen Wang, Yuewen Sheng, Ren-Jie Chang, Ja Kyung Lee, Yingqiu Zhou, Sha Li, Tongxin Chen, Hefu Huang, Benjamin F. Porter, Harish Bhaskaran, and Jamie H. Warner* Department of Materials, University of Oxford, 16 Parks Road, Oxford OX1 3PH, U.K.

Downloaded via 185.101.71.40 on July 17, 2018 at 00:03:22 (UTC). See https://pubs.acs.org/sharingguidelines for options on how to legitimately share published articles.

S Supporting Information *

ABSTRACT: Two-dimensional gallium sulfide (GaS) crystals are synthesized by a simple and efficient ambient pressure chemical vapor deposition (CVD) method using a singlesource precursor of Ga2S3. The synthesized GaS structures involve triangular monolayer domains and multilayer flakes with thickness of 1 and 15 nm, respectively. Regions of continuous films of GaS are also achieved with about 0.7 cm2 uniform coverage. This is achieved by using hydrogen carrier gas and the horizontally placed SiO2/Si substrates. Electron microscopy and spectroscopic measurements are used to characteristic the CVD-grown materials. This provides important insights into novel approaches for enlarging the domain size of GaS crystals and understanding of the growth mechanism using this precursor system.



precursors, and the reaction took place at 1170 °C using a vapor−solid method.33 Kang et al. reported GaS1−xSex alloy multilayers and monolayers synthesized on a SiO2/Si substrate (with 1 nm thick Au deposited film) at 950 °C using Ga2S3 and Ga2Se3 as precursors by the chemical vapor transport method.34 Dravid et al. mechanically exfoliated a single layer of GaS at room temperature under ambient conditions from a bulk material onto a SiO2/Si substrate, and the typical flakes had dimensions of tens of micrometers.19 Colmen et al. demonstrated the large quantities production of GaS via liquid exfoliation with lateral sizes and thicknesses of 50−1000 nm and 3−80 layers, respectively.24 Meng et al. synthesized the amorphous and smooth gallium sulfide material via atomic layer deposition method using hexakis digallium and hydrogen sulfide as precursors in the temperature range of 125−225 °C.35 Recently, Kalantar-Zadeh et al. developed a screen printing method for the deposition of bilayer 2D GaS thin films, which utilized an atomically thin oxide layer and further sulfurization process to replace the oxygen atoms with sulfur atoms.18 The controllable production of continuous, large-scale, high-quality GaS films still remains a challenge, and further research is needed to improve the material quality and uniformity of the samples. In this work, we develop a method for the growth of 2D GaS on SiO2/Si substrates using the ambient pressure CVD method. The growth process of GaS includes the evaporation and reduction of Ga2S3 precursor and using hydrogen carrier gas. Both monolayer and continuous GaS film are achieved by controlling the growth temperature, substrate position, and the

INTRODUCTION Monolayer and continuous two-dimensional (2D) transitionmetal dichalcogenides (TMDs) have attracted great interest because of their unique physical properties and promising future applications.1−8 The intensively studied TMDs, such as MoS2 and WS2, have dichalcogenide form of MX2; similarly, the posttransition metals of group III and VI elements have the form of MX where M = Ga, In and X = S, Se with monochalcogenide form.9−14 Two bonded gallium metal atoms are between two layers of sulfur atoms, like a sandwich. The unit cell of gallium sulfide (GaS) is hexagonal crystal structure with a = b = 3.587 Å, c = 15.492 Å, where c is equal to two layers of GaS.15 The indirect band gap of 2D GaS is about 3.05 eV which lies between the semimetal graphene and insulating hexagonal boron nitride.16−20 Because of the strong surface effects, the firstprinciple calculated band gap of GaS nanosheets varies from 2.59 to 1.6 eV, when the number of layers is increased from monolayer to bulk, which makes it a promising material for applications in electronics and opto-electronics.21,22 Also, 2D GaS has been explored for applications in transistors, photodetectors, energy storage, gas sensing, and application as hydrogen evolution catalysts.14,17,22−24 Chemical vapor deposition (CVD) has been one of the most promising methods of producing large-area and high-quality 2D materials, as well as for the synthesis of 2D GaS materials.25−31 Other synthesis methods include mechanical exfoliation, chemically assisted exfoliation, atomic layer deposition, and screen printing deposition methods. Barron et al. demonstrated CVD-synthesized polycrystalline gallium sulfide thin films using a predesigned single-source precursor of gallium chalcogenide cubane [(t-Bu)GaS]4 in 1992.32 Zhou et al. synthesized various morphologies of GaS such as nanowires, nanobelts, and hexagonal microplates using mixtures of GaN and Bi2S3 © 2018 American Chemical Society

Received: April 18, 2018 Accepted: June 25, 2018 Published: July 16, 2018 7897

DOI: 10.1021/acsomega.8b00749 ACS Omega 2018, 3, 7897−7903

Article

ACS Omega

Figure 1. Atmosphere pressure CVD synthesis of large-area gallium sulfide (GaS) on the SiO2/Si substrate. (a) Schematic illustration of the CVD setup of the synthesis of Ga2S3 white precursor powder is placed in the middle of the growth furnace. (b) Temperature against time profiles of the substrate with three stages includes heating stage I, maintaining stage II, and the last cooling stage III. (c) Photograph showing the overall after growth morphology of GaS on the 2 cm by 2 cm SiO2/Si substrate. The various contrast difference results from the thickness of the grown GaS materials. Two optical images of two separated regions labeled on the overall photo (c). (d) Thicker region of GaS located near the center indicates that the various shaped crystallized GaS flakes are stacked together. (e) Two individual triangular GaS domains with about 4 μm size.

Figure 2. SEM morphology study of the U-shaped CVD-grown GaS on SiO2/Si substrates. (a) Schematic of the U-shaped region with number labels. Each number label represents the typical regions and the morphologies are shown in the corresponding SEM images.



carrier gas flow rate. The CVD-grown GaS is characterized by optical microscopy, scanning electron microscopy (SEM),

RESULTS AND DISCUSSION

Figure 1a shows a schematic illustration of the CVD method to grow GaS on SiO2/Si substrates. The chemical reaction takes place inside a 1 in. diameter quartz tube under ambient pressure. The Ga2S3 precursor is placed at the center of the growth furnace. The 2 cm by 2 cm substrate is placed at the downstream

atomic force microscopy (AFM), photoluminescence (PL) and Raman spectroscopy, and transmission electron microscopy (TEM). 7898

DOI: 10.1021/acsomega.8b00749 ACS Omega 2018, 3, 7897−7903

Article

ACS Omega

Figure 3. Surface morphology of monolayer GaS films. (a) SEM image of large-area monolayer GaS film with initial nucleation sites. (b) SEM image of selected uniform region of monolayer GaS film. (c) SEM image of monolayer GaS film with second layer nucleation sites.

Figure 4. EDX analysis of gallium and sulfur from CVD-grown GaS. (a,b) Typical EDX spectra of GaS flakes and the GaS monolayer region, respectively. Both insets show SEM images where the five EDX spot spectra were obtained. The scale bar is 8 μm. (c) Ratio of sulfur to gallium and five positions between CVD-grown GaS flakes and domains. The reference ratio 1.5 is used from the Ga2S3 precursor.

variation of Ga2S3 vapor concentration gradient. This U-shaped pattern is observed in the CVD growth of other 2D TMD growth such as WS2 and MoS2.25,26 Figure 1d,e are two zoomedin optical images of selective regions in Figure 1c; both show the multilayer GaS flakes stacked area and individual triangle-shaped GaS domains with the size of 4 μm, respectively. Several stages are observed during the GaS layered growth. To study the morphology of the CVD-grown gallium sulphide 2D materials, SEM is used to examine the SiO2/Si substrate area by area. Figure 2a presents a schematic illustration of six selected regions which are numbers labeled, where the SEM images are taken. These six regions clearly reveal the dependence of the shape change on the distance from the Ga2S3 precursor vapor concentration. Figure 2 with position 1 shows the morphology of the center and upstream region where multilayer gallium sulfide flakes are formed. Toward the edge of the substrate at positions 2, 3, 4, isolated triangle GaS domains with the size ranging from about 8 and 2 μm are observed. Positions 4-1 to 4-3 represent the growth morphology of position 4 with more details. Furthermore, at position 4-1, the transition between individual domain and continuous film of GaS is found, half of the region shows complete continuous film and the other half region shows the triangular domains with various sizes. Toward the center of the substrate, a uniform continuous film of GaS is observed, formed by the merger of GaS domains and the size of

of the growth furnace with a distance of 8.5 cm. Figure 1b represents the profiles of temperature against time employed for the growth of GaS and includes three stages. The whole system is flushed with 500 sccm argon gas for 30 min. After that, the temperature of the precursor was increased from room temperature to 800 °C with a mixture of 70 sccm of hydrogen gas and 150 sccm of argon gas. The reaction is conducted once the temperature is reached for a short period of time with only 70 sccm hydrogen gas flow. At last, fast cooling process is applied with only 150 sccm argon gas flow. By optimizing the reaction parameters, such as the growth time, growth temperature, the amounts of precursors, the positions of the substrate, and the amount of hydrogen gas flow rate, we are able to produce the monocrystalline GaS domains or large-area continuous polycrystalline GaS film and even control the chemical composition between the gallium and sulfur. Two modifications are made in stage II. The first modification involves placing the substrate horizontally which creates a precursor concentration gradient and an inhomogeneity of the precursor feed-stock on the substrate surface. The other modification involves increasing the hydrogen gas flow rate during the growth stage and tuning the Ga2S3 decomposition (the compared SEM images are in the Supporting Information). Figure 1c shows the deposition pattern of after CVD growth of 2D GaS on SiO2/Si substrate and this formation of U-shaped pattern is because of the 7899

DOI: 10.1021/acsomega.8b00749 ACS Omega 2018, 3, 7897−7903

Article

ACS Omega

Figure 5. (a−c) Series of AFM images on same region with different magnifications. The zoomed-in regions are labeled in green and blue dashed boxes. The highlighted green color region has an rms of 0.19 nm. (d) Height profile of a continuous GaS film measured across the black line in (c). (e) AFM image of as-grown GaS flakes. (f) Corresponding height profile of selected GaS flakes measured across the black line in (e). (g) AFM images of two GaS domains. Box 1 has an rms of 0.48 nm on the SiO2/Si substrate, the boxes 2 and 3 have the same rms of 0.16 nm on the GaS domains. (h) Corresponding height profile of the GaS domain measured across the black line in (g).

GaS triangular domains increase from 2 to 6 μm, as shown in 4-2, and 4-3 SEM images, respectively. At the downstream region of the substrate, there is a change in the size of GaS domains. At positions 5 and 6, the GaS domain size is reduced to less than 2 μm and rounded nucleation sites are observed, and eventually the size is too small to identify its shape at the end. It can be seen that, with the increase in the distance between the precursor and the growth locations, GaS domains experience a regular morphology transformation as well as size and shape changes. The continuous region of CVD grown 2D GaS is further investigated because these qualities such as large-area, uniform, and continuous qualities are vital for future applications. Figure 3a shows the SEM image of a large continuous GaS region on a SiO2/Si substrate, with the left corner having partially covered regions where the triangle GaS domains are. While complete continuous film coverage of GaS is shown in Figure 3b with the size of 700 μm. It is observed that the large white particles are first deposited onto the SiO2/Si substrate and then gradually enclosed regions. Next, small triangular domains are nucleated at preferred locations, such as substrates’ edges, scratches, dust particles or rough surfaces.36 More SEM images are shown in the Supporting Information. Then, the nucleation sites continued to grow and formed boundaries when two or more layered 2D GaS meet, resulting in a partially continuous film. This process eventually leads to domains being coalesced and merged into large-area single-layered GaS continuous film, if sufficient precursor supply and denser nucleation sites are provided. A further zoomed-in SEM image of the GaS film is shown in Figure 3c, and the small dark regions on the continuous films are secondary layers which are formed during CVD growth. The energy-dispersive X-ray (EDX) spectroscopy, AFM, Raman spectroscopy, PL spectroscopy, and TEM are all used to evaluate the CVD-grown GaS in terms of chemical compositional analysis, thickness, film quality, and crystallinity. The typical EDX spot spectra are in Figure 4a,b, where the five spots EDX results are from GaS flakes and the monolayer GaS film region and shown in the corresponding inserts, respectively. The intensity of Ga and S from GaS flakes is significantly strong than

the monolayer GaS. The atomic percentage and ratio of sulfur and gallium elements are obtained from the EDX. Figure 4c reveals the S/Ga ratio comparison among the CVD-synthesized GaS flakes, monolayer region, and the Ga2S3 precursor. The S/ Ga ratios of GaS flakes is close to 1 and is consistent to about 1.2 value, whereas the ratio in monolayer GaS has large variation between 1.9 and 1.4. The ratio of the Ga2S3 precursor is set to 1.5 as a reference. This might be due to the ultrathin property of the material, making it difficult to detect subtle variations using EDX. All this information is summarized in Table S1 in the Supporting Information. In this work, the shape of CVDsynthesized GaS domain is quite consistent with a truncated triangle shape. In previous reports, the shape of CVD-grown GaS domains were hexagonal and sharp triangle shapes, and the hexagon-shaped domain has three Ga- and S-terminated edges, and the triangle-shaped domain can only have either S- or Gaterminated edges.33,34 The exact ratio between Ga and S atoms on the substrate influences the energetic stability of Ga- and Sterminated edges. Because a single-source precursor Ga2S3 is used here, and it is reduced by the hydrogen carrier gas, it means that only slightly excessive S is present throughout the whole synthesis process. This explains why the resulted GaS domains are truncated, because of a similar Ga/S ratio in the precursor. If the stoichiometry was such that S was in vast excess, we would expect sharp triangular domains. Similar results are reported in the CVD synthesis of MoS2 and WS2 as well.26 The roughness and thickness of the CVD-grown GaS continuous film, flakes, and domains are characterized by AFM. The AFM measurements in the topological mode for an almost fully merged region with corresponding zoomed-in AFM scans, indicated by dashed green and blue boxes, are shown in Figure 5a−c. This scanned region is not fully covered on the substrate; it is densely covered by triangular GaS domains, which are close to coalescing into a continuous film. Both the merged grain boundaries and the second nuclei are observed under the AFM measurements and a 0.19 nm root mean squared (rms) is measured, indicated by the green box, shown in Figure 5c. The corresponding height profile of the GaS continuous film is 7900

DOI: 10.1021/acsomega.8b00749 ACS Omega 2018, 3, 7897−7903

Article

ACS Omega

Figure 6. Raman spectra and PL measurements of CVD-grown GaS flakes and monolayer domain on the SiO2/Si substrate. (a) Raman spectrum and (c) PL emission spectra of the multilayer stacked GaS flakes region. (b) Raman spectrum and (d) PL emission spectra of monolayer triangle-shaped GaS domain. Both inserts are the corresponding optical images, and the scale bar is 5 μm.

Figure 7. TEM images of GaS multilayer flake. (a) Low-magnification TEM image of GaS flake shows the layered structure. (b) HRTEM and corresponding FFT image of GaS monolayer region at the zone axis of [0001], indicating the single-crystalline nature. (c) The corresponding line intensity profile is taken form the yellow marked region in (b). It results the (100) planes of GaS are separated by a distance of 0.31 nm. (d) Zoomed-in HRTEM image of GaS flakes corresponding to the selective area from (b). (e) Schematic illustration of the top view GaS crystal from the [0001] zone axis.

The as-grown GaS flakes and monolayer domains are further investigated using Raman spectroscopy with a 532 nm excitation to determine the layer number and quality. GaS has three firstorder phonon modes in Raman spectroscopy, two out-of-plane A11g and A21g modes, and one in-plane E12g mode. Raman spectra are taken from spot positions on both GaS flakes and domains, as shown in Figure 6a,b, respectively. The GaS flakes show Raman peaks for modes A11g (188 cm−1), A21g (360 cm−1) and E12g (294 cm−1). The full width at half-maximum of A11g and A21g mode are 5 and 6 cm−1, respectively. However, the GaS monolayer domain shows A11g (179 cm−1), E12g (297 cm−1) which is

measured in Figure 5d and the 1 nm thickness is in agreement with the GaS monolayer flakes on SiO2/Si substrate.19 The GaS flakes are also measured along the black line indicated in Figure 5e and the corresponding height profile results in two steps with 25 and 10 nm thickness of the GaS flakes, as shown in Figure 5f. The individual triangular GaS domain has about 0.6 nm step height, although the measured rms on the after CVD-grown SiO2/Si substrate is 0.48 nm on the same scan; both are shown in Figure 5g,h, respectively. The rms on the triangle GaS domains closely match the monolayer film, with both measured to have values of ∼0.16 nm. 7901

DOI: 10.1021/acsomega.8b00749 ACS Omega 2018, 3, 7897−7903

ACS Omega



combined with the 303 cm−1 Raman peak from the SiO2/Si substrate. This results in a broadened peak, and the A21g is not shown on the spectra. As the thickness of GaS decreases from flakes to monolayer domain, the frequency of the E12g mode slightly increased and that of A11g mode decreased, and also, the overall intensities are observed to decrease as well. These results are in agreement with previous reports.17,19,22,37 The spectroscopy measurements of the GaS flakes with 532 nm excitation also show a very broad peak between 550 and 800 nm with centered position at 622 nm. This peak is associated with either indirect transitions or defects in GaS flakes that produce deep trap recombination states.38 However, the monolayer GaS domain does not show this peak at all. The 532 nm excitation is not sufficient to excite the indirect band gap of GaS, and thus, we do not expect to observe high-efficiency PL from recombination across the indirect gap. These two strong PL peaks observed in both samples and obtained by 523 nm excitation is associated with the SiO2/Si substrates. TEM is used to further characterize the CVD as-grown gallium sulfide layered structures after transfer onto TEM grids by a poly(methyl methacrylate)-assisted wet chemical transfer method. Figure 7a−c shows typical low-magnification and highresolution TEM (HRTEM) images of thin layered GaS sheet, which is on a lacey carbon TEM grid. Figure 7a shows the layered structures at a large scale. Figure 7b,d shows HRTEM images, and they reveal the single-crystalline nature of the CVDgrown GaS flakes. Intensity line profiles are plotted in Figure 7c, and the measured d-spacing between the neighboring (100) planes is 0.31 nm which is consistent with the values for β-GaS (a = 3.587 Å and c = 15.492 Å).14,33 The inset in (b) shows corresponding fast Fourier-transform (FFT) power spectrum indicating that GaS sheets are orientated along at the [0001] zone axis and confirm the hexagonal structure, compared with previous report.34 Further zoomed-in HRTEM images are shown in Figure 7d, which corresponds to the selected area in Figure 7b; and the schematic diagram of the top view of the GaS crystal is presented in Figure 7e. Both help to confirm the crystalline quality of CVD-grown GaS materials and are in good agreement with the mechanical exfoliated prepared GaS nanoflakes.14

AUTHOR INFORMATION

Corresponding Author

*E-mail: [email protected]. ORCID

Yuewen Sheng: 0000-0003-3067-9520 Ren-Jie Chang: 0000-0001-8215-9469 Harish Bhaskaran: 0000-0003-0774-8110 Jamie H. Warner: 0000-0002-1271-2019 Notes

The authors declare no competing financial interest.

■ ■

ACKNOWLEDGMENTS J.H.W. thanks the support from the European Research Council (grant 725258 LATO) and the Royal Society. REFERENCES

(1) Manzeli, S.; Ovchinnikov, D.; Pasquier, D.; Yazyev, O. V.; Kis, A. 2D Transition Metal Dichalcogenides. Nat. Rev. Mater. 2017, 2, 17033. (2) Wilson, J. A.; Yoffe, A. D. The Transition Metal Dichalcogenides Discussion and Interpretation of the Observed Optical, Electrical and Structural Properties. Adv. Phys. 1969, 18, 193−335. (3) Mak, K. F.; Lee, C.; Hone, J.; Shan, J.; Heinz, T. F. Atomically Thin MoS2: A New Direct-Gap Semiconductor. Phys. Rev. Lett. 2010, 105, 136805. (4) Gutiérrez, H. R.; Perea-López, N.; Elías, A. L.; Berkdemir, A.; Wang, B.; Lv, R.; López-Urías, F.; Crespi, V. H.; Terrones, H.; Terrones, M. Extraordinary Room-Temperature Photoluminescence in Triangular WS2 Monolayers. Nano Lett. 2013, 13, 3447−3454. (5) Coleman, J. N.; Lotya, M.; O’Neill, A.; Bergin, S. D.; King, P. J.; Khan, U.; Young, K.; Gaucher, A.; De, S.; Smith, R. J.; et al. TwoDimensional Nanosheets Produced by Liquid Exfoliation of Layered Materials. Science 2011, 331, 568−571. (6) Radisavljevic, B.; Radenovic, A.; Brivio, J.; Giacometti, V.; Kis, A. Single-layer MoS2 transistors. Nat. Nanotechnol. 2011, 6, 147−150. (7) Splendiani, A.; Sun, L.; Zhang, Y.; Li, T.; Kim, J.; Chim, C.-Y.; Galli, G.; Wang, F. Emerging Photoluminescence in Monolayer MoS2. Nano Lett. 2010, 10, 1271−1275. (8) Hill, H. M.; Rigosi, A. F.; Rim, K. T.; Flynn, G. W.; Heinz, T. F. Band Alignment in MoS2/WS2 Transition Metal Dichalcogenide Heterostructures Probed by Scanning Tunneling Microscopy and Spectroscopy. Nano Lett. 2016, 16, 4831−4837. (9) Pospischil, A.; Furchi, M. M.; Mueller, T. Solar-Energy Conversion and Light Emission in an Atomic Monolayer P-N Diode. Nat. Nanotechnol. 2014, 9, 257−261. (10) Tan, H.; Xu, W.; Sheng, Y.; Lau, C. S.; Fan, Y.; Chen, Q.; Tweedie, M.; Wang, X.; Zhou, Y.; Warner, J. H. Lateral GrapheneContacted Vertically Stacked WS2 /MoS2 Hybrid Photodetectors with Large Gain. Adv. Mater. 2017, 29, 1702917. (11) Sheng, Y.; Wang, X.; Fujisawa, K.; Ying, S.; Elias, A. L.; Lin, Z.; Xu, W.; Zhou, Y.; Korsunsky, A. M.; Bhaskaran, H.; et al. Photoluminescence Segmentation within Individual Hexagonal Monolayer Tungsten Disulfide Domains Grown by Chemical Vapor Deposition. ACS Appl. Mater. Interfaces 2017, 9, 15005−15014. (12) He, Z.; Wang, X.; Xu, W.; Zhou, Y.; Sheng, Y.; Rong, Y.; Smith, J. M.; Warner, J. H. Revealing Defect-State Photoluminescence in Monolayer WS2 by Cryogenic Laser Processing. ACS Nano 2016, 10, 5847−5855. (13) Li, S.; Wang, S.; Salamone, M. M.; Robertson, A. W.; Nayak, S.; Kim, H.; Tsang, S. C. E.; Pasta, M.; Warner, J. H. Edge Enriched 2D MoS2 Thin Films Grown by Chemical Vapor Deposition for Enhanced Catalytic Performance. ACS Catal. 2016, 7, 877. (14) Late, D. J.; Liu, B.; Luo, J.; Yan, A.; Matte, H. S. S. R.; Grayson, M.; Rao, C. N. R.; Dravid, V. P. GaS and GaSe Ultrathin Layer Transistors. Adv. Mater. 2012, 24, 3549−3554. (15) Barron, A. R. MOCVD of Group III Chalcogenides. Adv. Mater. Opt. Electron. 1995, 5, 245−258.



CONCLUSION In conclusion, we report a simple CVD approach for growing both monolayer and multilayer high-quality GaS films with large domain size on SiO2/Si substrate using hydrogen carrier gas to reduce a single-source precursor of Ga2S3 at atmospheric pressure. The film microstructure, thickness, homogeneity, and quality are characterized by optical microscopy, SEM with EDX, Raman spectra, PL spectra, and TEM. These results show how sensitive the growth of GaS is to minor variations in the CVD parameters and that drastic improvements can be easily achieved by simple optimizations. This approach has shown potential in scale-up and meets safety requirements for large-scale implementation and eventually toward the controllable number of layers CVD growth of 2D GaS.



Article

ASSOCIATED CONTENT

S Supporting Information *

The Supporting Information is available free of charge on the ACS Publications website at DOI: 10.1021/acsomega.8b00749. EDX analysis; further SEM imaging; and further TEM characterization (PDF) 7902

DOI: 10.1021/acsomega.8b00749 ACS Omega 2018, 3, 7897−7903

Article

ACS Omega (16) Novoselov, K. S.; Geim, A. K.; Morozov, S. V.; Jiang, D.; Zhang, Y.; Dubonos, S. V.; Grigorieva, I. V.; Firsov, A. A. Electric Field Effect in Atomically Thin Carbon Films. Science 2004, 306, 666−669. (17) Hu, P.; Wang, L.; Yoon, M.; Zhang, J.; Feng, W.; Wang, X.; Wen, Z.; Idrobo, J. C.; Miyamoto, Y.; Geohegan, D. B.; et al. Highly Responsive Ultrathin GaS Nanosheet Photodetectors on Rigid and Flexible Substrates. Nano Lett. 2013, 13, 1649−1654. (18) Carey, B. J.; Ou, J. Z.; Clark, R. M.; Berean, K. J.; Zavabeti, A.; Chesman, A. S. R.; Russo, S. P.; Lau, D. W. M.; Xu, Z.-Q.; Bao, Q.; et al. Wafer-Scale Two-Dimensional Semiconductors from Printed Oxide Skin of Liquid Metals. Nat. Commun. 2017, 8, 14482. (19) Late, D. J.; Liu, B.; Matte, H. S. S. R.; Rao, C. N. R.; Dravid, V. P. Rapid Characterization of Ultrathin Layers of Chalcogenides on SiO2/ Si Substrates. Adv. Funct. Mater. 2012, 22, 1894−1905. (20) Watanabe, K.; Taniguchi, T.; Kanda, H. Direct-Bandgap Properties and Evidence for Ultraviolet Lasing of Hexagonal Boron Nitride Single Crystal. Nat. Mater. 2004, 3, 404−409. (21) Ma, Y.; Dai, Y.; Guo, M.; Yu, L.; Huang, B. Tunable Electronic and Dielectric Behavior of GaS and GaSe Monolayers. Phys. Chem. Chem. Phys. 2013, 15, 7098. (22) Yang, S.; Li, Y.; Wang, X.; Huo, N.; Xia, J.-B.; Li, S.-S.; Li, J. High Performance Few-Layer GaS Photodetector and Its Unique PhotoResponse in Different Gas Environments. Nanoscale 2014, 6, 2582− 2587. (23) Meng, X.; He, K.; Su, D.; Zhang, X.; Sun, C.; Ren, Y.; Wang, H.H.; Weng, W.; Trahey, L.; Canlas, C. P.; et al. Gallium Sulfide-SingleWalled Carbon Nanotube Composites: High-Performance Anodes for Lithium-Ion Batteries. Adv. Funct. Mater. 2014, 24, 5435−5442. (24) Harvey, A.; Backes, C.; Gholamvand, Z.; Hanlon, D.; McAteer, D.; Nerl, H. C.; McGuire, E.; Seral-Ascaso, A.; Ramasse, Q. M.; McEvoy, N.; et al. Preparation of Gallium Sulfide Nanosheets by Liquid Exfoliation and Their Application as Hydrogen Evolution Catalysts. Chem. Mater. 2015, 27, 3483−3493. (25) Sheng, Y.; Tan, H.; Wang, X.; Warner, J. H. Hydrogen Addition for Centimeter-Sized Monolayer Tungsten Disulfide Continuous Films by Ambient Pressure Chemical Vapor Deposition. Chem. Mater. 2017, 29, 4904−4911. (26) Wang, S.; Rong, Y.; Fan, Y.; Pacios, M.; Bhaskaran, H.; He, K.; Warner, J. H. Shape Evolution of Monolayer MoS2 Crystals Grown by Chemical Vapor Deposition. Chem. Mater. 2014, 26, 6371−6379. (27) Wang, S.; Wang, X.; Warner, J. H. All Chemical Vapor Deposition Growth of MoS2:h-BN Vertical van der Waals Heterostructures. ACS Nano 2015, 9, 5246−5254. (28) Chang, R.-J.; Wang, X.; Wang, S.; Sheng, Y.; Porter, B.; Bhaskaran, H.; Warner, J. H. Growth of Large Single-Crystalline Monolayer Hexagonal Boron Nitride by Oxide-Assisted Chemical Vapor Deposition. Chem. Mater. 2017, 29, 6252−6260. (29) Wang, X.; Hooper, T. N.; Kumar, A.; Priest, I. K.; Sheng, Y.; Samuels, T. O. M.; Wang, S.; Robertson, A. W.; Pacios, M.; Bhaskaran, H.; et al. Oligomeric Aminoborane Precursors For the Chemical Vapour Deposition Growth of Few-Layer Hexagonal Boron Nitride. CrystEngComm 2016, 19, 285−294. (30) Fan, Y.; He, K.; Tan, H.; Speller, S.; Warner, J. H. Crack-Free Growth and Transfer of Continuous Monolayer Graphene Grown on Melted Copper. Chem. Mater. 2014, 26, 4984−4991. (31) Rong, Y.; Fan, Y.; Leen Koh, A.; Robertson, A. W.; He, K.; Wang, S.; Tan, H.; Sinclair, R.; Warner, J. H. Controlling sulphur precursor addition for large single crystal domains of WS2. Nanoscale 2014, 6, 12096−12103. (32) MacInnes, A. N.; Power, M. B.; Barron, A. R. Chemical Vapor Deposition of Cubic Gallium Sulfide Thin Films: A New Metastable Phase. Chem. Mater. 1992, 4, 11−14. (33) Shen, G.; Chen, D.; Chen, P.-C.; Zhou, C. Vapor−Solid Growth of One-Dimensional Layer-Structured Gallium Sulfide Nanostructures. ACS Nano 2009, 3, 1115−1120. (34) Jung, C. S.; Shojaei, F.; Park, K.; Oh, J. Y.; Im, H. S.; Jang, D. M.; Park, J.; Kang, H. S. Red-to-Ultraviolet Emission Tuning of TwoDimensional Gallium Sulfide/Selenide. ACS Nano 2015, 9, 9585− 9593.

(35) Meng, X.; Libera, J. A.; Fister, T. T.; Zhou, H.; Hedlund, J. K.; Fenter, P.; Elam, J. W. Atomic Layer Deposition of Gallium Sulfide Films Using Hexakis(dimethylamido)digallium and Hydrogen Sulfide. Chem. Mater. 2014, 26, 1029−1039. (36) Najmaei, S.; Liu, Z.; Zhou, W.; Zou, X.; Shi, G.; Lei, S.; Yakobson, B. I.; Idrobo, J.-C.; Ajayan, P. M.; Lou, J. Vapour Phase Growth and Grain Boundary Structure of Molybdenum Disulphide Atomic Layers. Nat. Mater. 2013, 12, 754−759. (37) Gasanly, N. M.; Aydınlı, A.; Ö zkan, H.; Kocabaş, C. Temperature Dependence of the First-Order Raman Scattering in GaS Layered Crystals. Solid State Commun. 2000, 116, 147−151. (38) Aydinli, A.; Gasanly, N. M.; Gökşen, K. Donor-acceptor pair recombination in gallium sulfide. J. Appl. Phys. 2000, 88, 7144−7149.

7903

DOI: 10.1021/acsomega.8b00749 ACS Omega 2018, 3, 7897−7903