Closed-Loop Electrochemical Recycling of Spent Copper(II) from

4 days ago - Facile On-site Aqueous Pollutant Monitoring Using a Flexible, Ultra-light and Robust SERS Substrate: Interface Self-Assembly of Au@Ag Nan...
1 downloads 6 Views 2MB Size
Subscriber access provided by - Access paid by the | UCSB Libraries

Sustainability Engineering and Green Chemistry

Closed-Loop Electrochemical Recycling of Spent Copper(II) from Etchant Wastewater Using a Carbon Nanotube Modified Graphite Felt Anode Yan Chang, LIN DENG, Xiaoyang Meng, Wen Zhang, Chunzhen Wang, Yuxin Wang, Song Zhao, Li Lin, and John C. Crittenden Environ. Sci. Technol., Just Accepted Manuscript • DOI: 10.1021/acs.est.7b06298 • Publication Date (Web): 16 Apr 2018 Downloaded from http://pubs.acs.org on April 16, 2018

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 35

Environmental Science & Technology

1

Closed-Loop Electrochemical Recycling of Spent

2

Copper(II) from Etchant Wastewater Using a Carbon

3

Nanotube Modified Graphite Felt Anode

4

Yan Chang1, Lin Deng2,3, Xiaoyang Meng2, Wen Zhang1, 2*, Chunzhen Wang1, Yuxin Wang1,

5

Song Zhao1, Li Lin2,4, John C. Crittenden2

6

1 State Key Laboratory of Chemical Engineering, Co-Innovation Center of Chemical Science &

7

Engineering, Tianjin Key Laboratory of Membrane Science & Desalination Technology and

8

School of Chemical Engineering and Technology, Tianjin University, Tianjin 300350, China.

9

2 Brook Byer Institute for Sustainable Systems and School of Civil and Environmental

10

Engineering, Georgia Institute of Technology, Atlanta, Georgia 30332, United States.

11

3 Key Laboratory of Building Safety & Energy Efficiency and Department of Water Engineering

12

and Science, College of Civil Engineering, Hunan University, Changsha 410082, China.

13

4 Basin Water Environmental Research Department, Changjiang River Scientific Research

14

Institute, Wuhan, 430010, China.

15

* To whom correspondence should be addressed (W. Z.)

16

E-mail: [email protected].

ACS Paragon Plus Environment

1

Environmental Science & Technology

17

Page 2 of 35

ABSTRACT

18

Developing effective technologies for treatment of spent etchant in printed circuit boards

19

industries is of paramount for sustainable copper reuse and reducing copper discharge. We

20

developed a novel closed-loop electrochemical cell for on-site regeneration of spent acidic cupric

21

chloride etchant. It does not have any emissions and recycles all the copper using a three-

22

dimensional graphite felt anode decorated with carbon nanotube (CNT/GF). The CNT/GF anode

23

oxidizes Cu(I) to Cu(II) so that the spent cuprous chloride can be converted to cupric chloride

24

and reused. The decorated CNT layer with abundant oxygen-containing functional groups

25

significantly enhanced the electrocatalytic activity for Cu(II)/Cu(I) redox. The CuCl 32 - is

26

oxidized to CuCl + at the anode and the CuCl + is reduced to Cu(0) at the cathode. The closed-

27

loop cycle system converts the catholyte into the anolyte. On average, the energy consumption of

28

Cu(I) oxidation by CNT/GF is decreased by 12%, comparing to that by untreated graphite felt.

29

The oxidation rate of Cu(I) is determined by the current density, and there is no delay for the

30

mass transport of Cu(I). This study highlights the outstanding electrocatalytic performance, the

31

rapid mass-transfer kinetics and the excellent stability of the CNT/GF electrode, and provides an

32

energy-efficient and zero-emission strategy for the regeneration of etchant waste.

ACS Paragon Plus Environment

2

Page 3 of 35

33

Environmental Science & Technology

INTRODUCTION

34

Because of the rapid increasing market demand for electronic and electrical equipment, the

35

printed circuit boards (PCB) industry has expanded sharply in the past decade.1 Current PCB

36

industries involve diverse toxic chemicals during different manufacturing processes including

37

board preparation, circuit pattern transfer, etching and plating processes. These processes pose a

38

serious potential hazard to the environmental and human health.2-4 In particular, about 70% of

39

copper is removed from copper covered PCB in the etching step, and it generates a spent etchant

40

with a high concentration of copper ion. The quantity of spent etchant produced by 1 m2 of PCB

41

is between 1.5 to 3.5 liters, and the total spent etchant yield is about 1 billion cubic meters in the

42

world annually.5 Accordingly, developing an efficient regeneration process for spent etchant is a

43

crucial issue to minimize copper wastes originating from PCB industries and recovery of copper.

44

Since acidic cupric chloride (CuCl2) solution has the advantages of high etch rate, high

45

dissolved copper capacity and excellent operating controllability, and it is the dominant etchant

46

in PCB industries.6 When removing of the exposed copper to create desired circuit patterns using

47

acidic CuCl2 etchant, a comproportionation takes place, as shown in Equation (1).7

48

Cu(II)Cl 2 + Cu(0) → 2Cu(I)Cl

(1)

49

In this reaction, the cupric ion (Cu(II)) responsible for etching is consumed, and cuprous ion

50

(Cu(I)) is produced. With the accumulation of dissolved Cu(I) in CuCl2 etchant, a sparingly

51

insoluble passivation CuCl film will be formed on the etching surface, and the rate of etching

52

will decrease dramatically.8, 9 Therefore, developing effective technologies for removal of Cu(I)

53

is of paramount for recycling of spent CuCl2 etchant.

ACS Paragon Plus Environment

3

Environmental Science & Technology

Page 4 of 35

Several methods have been used to treat spent etchant, including chemical precipitation,10-12

54 55

flocculation,13 ultrasonic treatment,14 solvent extraction,15,

16

electrochemical regeneration17-21

56

and membrane technology.22 Among these methods, the electrochemical regeneration has

57

advantages of good reuse, no secondary contamination, high removal rate and purified recovery,

58

and the environment values of electrochemical method is greater than the others.5 In the

59

electrolytic process, Cu(I) is oxidized at the anode and some Cu(0) is deposited at the cathode.

60

However, chloride gas (Cl2) evolves from the anode at high anode potential and causes safety

61

issues.18 To avoid Cl2 evolution, Oxley et al.23 developed a complicated electrochemical system

62

with a flow-through carbon anode and two electrolytic cells. However, the two cells may raise the

63

equipment cost and complicate the recovery operation. In our previous study, a simple anion

64

exchange separated electrolytic cell was designed using a graphite felt (GF) anode.17 Overall,

65

these flow-through electrode materials and electrolytic regeneration processes are encouraging,

66

but they still suffer from low energy efficiency for Cu(I) oxidation and secondary waste.

67

Therefore, efforts are still required to seek out more efficient electrodes and electrolytic

68

strategies to reduce energy use and discharge of secondary waste.

69

Heretofore, because of the excellent electrical conductivity, distinguished stability and low

70

cost, GF electrode has been successfully applied in microbial fuel cells,24-27 vanadium flow redox

71

cells28, 29 and electrochemical decontamination.30 However, it still suffers from hydrophilicity

72

and poor electrocatalytic activity. To enhance its electrolyte accessibility and active sites, these

73

methods have been used: (1) noble metals deposition,25, 30, 31 (2) acid/alkali/plasma treatment28, 32,

74

33

75

electrode has not been reported as electrocatalysts for the Cu(II)/Cu(I) redox couple before. As

76

the strongest carbon nanomaterial, CNT is not altered by strong acidic etchant, due to its high

and (3) carbon nanomaterials deposition34-36. To our knowledge, the use of composite GF

ACS Paragon Plus Environment

4

Page 5 of 35

Environmental Science & Technology

77

chemical/mechanical stability.37 Compared with other modified layers, CNT also has the

78

advantages of low synthesis cost, high electrical conductivity, large surface area for

79

accommodating more active sites.38, 39 Therefore, a composite GF decorated with CNT is an

80

ideal electrode for electro-oxidation of Cu(I) in PCB etchant.

81

In this study, we developed a novel electrolytic regeneration technology for acidic spent CuCl2

82

etchant to recycle copper, eliminate waste water production and save energy, using a composite

83

GF electrode in a closed-loop electrolytic cell. For one thing, we developed a CNT modified GF

84

anode (CNT/GF) for enhancing Cu(I) electro-oxidation performance. For another, we elaborated

85

an electrochemical strategy converting the catholyte into the anolyte to create a zero-emission

86

regeneration process. The CNT/GF electrodes were characterized by their structure, composition,

87

wettability, and the electroactivity for the Cu(II)/Cu(I) redox couple. The reaction mechanism

88

was studied by thermodynamic analysis and DFT calculation. The mass transfer of reactants was

89

evaluated to clarify the kinetic impact from the decoration of CNT on the GF surface.40-42 The

90

operating parameters were optimized on the basis of thermodynamics and kinetics analyses. The

91

energy consumption of Cu(I) oxidation and Cu(0) deposition are estimated. The long-term

92

stability of the composite anode was also investigated. We believe these results will be useful for

93

the further engineering application of this regenerative electrolytic cell, as well as the similar

94

electrochemical systems using composite GF electrodes.

95

MATERIALS AND METHODS

96

Growth of carbon nanotubes on graphite felt. The graphite felt (GF, Beijing Sanye Carbon

97

Co.), was tailored into cylinders with the diameter of 14 mm and height of 5 mm, and subjected

98

to ultrasonic treatment in alcohol to remove microfiber fragments. Then they were immersed in

ACS Paragon Plus Environment

5

Environmental Science & Technology

Page 6 of 35

99

Pluronic F127 (2.5 wt. %, EO106PO70EO106 , Sigma-Aldrich) aqueous solution for 2 h and dried

100

at 50 °C for 12 h. The nickel was deposited onto these GF cylinders using incipient impregnation

101

with a 0.1 mol/L Ni(NO3)2 ethanol solution. After drying at 50 °C for 3 h, they were decorated

102

by growing of carbon nanotubes (CNT) using chemical vapor deposition (CVD).43

103

The Ni deposited GF cylinders were calcined under a N2 atmosphere (300 cm3/min flow rate)

104

at 450 °C for 1.5 h. Then they were reduced in a mixture of H2 (60 cm3/min)/N2 (100 cm3/min)

105

at 500 °C for 1 h. Then, the furnace was heated to 900 °C, 1000 °C, or 1100 °C under N2

106

atmosphere (100 cm3/min), respectively. Then a stream of toluene gas (heated to 80 °C) was

107

introduced for 40 min to grow CNT. Finally, the furnace was allowed to cool to room

108

temperature. As-grown CNT modified GF (CNT/GF) samples were refluxed in 2 mol/L HNO3 at

109

90 °C for 1 h to remove metal impurities and introduce the surface oxygen-containing groups.

110

After that, the samples were washed with distilled water and dried at 100 °C in air for 12 h. For a

111

clear description, CNT/GF grown in 900 °C, 1000 °C and 1100 °C were denoted as CNT900/GF,

112

CNT1000/GF and CNT1100/GF, respectively.

113

Electrode characterization. The surface morphology of the CNT on GF was examined by

114

scanning electron microscopy (SEM, Nova Nanosem 430), transmission electron microscopy

115

(TEM, JEOL JEM2100) and Raman spectroscopy (DXR Microscope, Excitation wavelength 532

116

nm). The functional groups of the CNT on GF were analyzed via an X-ray photoelectron

117

spectroscope (XPS, Thermo Electron PHI-5000 II, C1s at 285 eV).

118

The cyclic voltammogram (CV) was measured by an electrochemical workstation

119

(PARSTAT4000) with a three-electrode arrangement at 25 °C. The GF working electrode was

120

connected to platinum wire with a Ag/AgCl reference electrode and a Pt plate auxiliary electrode

ACS Paragon Plus Environment

6

Page 7 of 35

Environmental Science & Technology

121

(30 mm

╳ 30

mm). The test was performed in 0.1 mol/L CuCl + 2 mol/L HCl + 2 mol/L NaCl

122

solution at different scan rates range from 1 to 10 mV/s under N2 atmosphere.

123

Regeneration of acidic CuCl2 etchant. A small-scale flow electrolytic system was

124

constructed as shown in Figure 1. The two electrode compartments, with the same size of 2 cm

125

length

126

AMI-7001, Membranes International Inc.). This AEM was pretreated by immersion in the

127

etchant for 24 hours before use. UGF or CNT1100/GF was used as the anode and copper foil (99

128

wt. %) was the cathode. The composition of spent CuCl2 etchant was provided by Tianjin

129

Printronics Circuit Corp., and it was 1.70 mol/L CuCl2 + 0.10 mol/L CuCl + 2 mol/L HCl + 2

130

mol/L NaCl (50 °C). This etchant, was fed to the anode compartment directly as the anolyte. The

131

catholyte (0.50 mol/L CuCl2 + 0.03 mol/L CuCl + 2 mol/L HCl + 2 mol/L NaCl, 50 °C) was a

132

diluted etchant obtained by mixing the pristine etchant with 2 mol/L HCl + 2 mol/L NaCl

133

solution. Peristaltic pumps and thermostats were used to keep the electrolytes at constant rates

134

and temperatures (50 ± 1 °C), respectively. The flow rates were calibrated by weighing the

135

anolyte or catholyte. After 1 hour’s regeneration test, the concentration of Cu(I) in the

136

electrolytes was determined via redox titrimetry,17 while the Cu(II) was measured by a

137

spectrophotometer at 630 nm.44

138

RESULTS AND DISCUSSION



1 cm width



2 cm height, were segregated by an anion exchange membrane (AEM,

139

Characterization of CNT/GF Composite Anode. Figure 2a and 2b exhibit the SEM images

140

of the UCF with a diameter of 15 µm. The slightly uneven fine-grained surface of UCF can

141

provide abundant impregnation sites for development of Ni catalyst, which can initiate CNT

142

growth. From the representative TEM images shown in Figure S1, the diameter and the wall

ACS Paragon Plus Environment

7

Environmental Science & Technology

Page 8 of 35

143

thickness of CNT increase as the temperature increases. The morphology of CNT is directly

144

relevant to the nucleation rate and growth rate of Ni catalyst, which are mainly controlled by

145

temperature.45,

146

nucleation rate of Ni catalyst is fast and the growth rate of it is slow. As a result, the slim CNT

147

fiber is agglomerated into three-dimensional nanotube fibrous ‘silk flower’ architectures (Figure

148

2c and 2d), and the growth stops due interference between the nanotubes. CNT900/GF has a

149

specific surface area of 22.2 m2/g (Figure S2) and abundant 2-5 nm mesoporous structures

150

(Figure S3). For CNT1000/GF, SEM images (Figure 2e and 2f) show that a dense CNT fibers,

151

with the diameter of 100-300 nm and length of 10-50 µm covers the GF surface. As the

152

temperature rises to 1100 °C, the CNT fibers become thicker and straighter, and interwoven into

153

a three-dimensional network microstructure (Figure 2g and 2h). The N2 adsorption and

154

desorption curves for CNF1000/CF and CNF1100/CF are almost overlapping (Figure S2),

155

suggesting a similar pore structure.47 The specific surface area of CNF1000/CF and

156

CNF1100/CF are 16.4 m2/g and 7.6 m2/g, respectively, which are much larger than that of

157

untreated GF (UGF) (0.4 m2/g). Compared with UCF, the weights of CNT900/GF, CNT1000/GF

158

and CNT1100/GF increase by 6.1 %, 22.9 % and 61.4 %, respectively.

46

At a low temperature (900 °C), a fine Ni cluster is developed because the

159

XPS Analyses. From XPS survey scan spectra (Figure S4), the oxygen content (atom.%) in

160

UGF, CNT900/GF, CNT1000/GF and CNT1100/GF samples are 4.04%, 5.79%, 5.2% and

161

11.23%, respectively. Figure 3a and 3b shows the C1s and O1s narrow scan spectra of the four

162

samples. The deconvolution of the C1s main peak (284.5 eV) suggests five carbon bonding

163

configurations, namely, ―COOH (C1, 289.2 eV), C=O (C2, 287.0 eV), C―O (C3, 285.9 eV), C

164

― C (C4, 285.2 eV) and C=C (C5, 284.4 eV). Compared with CNT, the percentages of all

165

oxygen functional groups on the surfaces of CNT/GF are increased (Figure 3c). In particular, the

ACS Paragon Plus Environment

8

Page 9 of 35

Environmental Science & Technology

166

amount of C=O, COOH and C ― O of CNT1100/GF are increased by106%. Consistent with

167

previous studies,48, 49 there are three types of oxygen bonding configurations on the surfaces of

168

samples, including C―O―C (O1, 533.5 eV), C―OH (O2, 532.6 eV) and C=O (O3, 531.4 eV)

169

functional groups. Compared with UGF, the CNT/GF samples have more C=O oxygen, which is

170

contributed by carbonyl/lactone groups (C=O) and carboxyl groups (O=C―OH) on the CNT

171

surfaces (Figure 3d).

172

Raman characterization. The amount of defects of UGF and CNT/GF samples was

173

characterized by Raman spectroscopy, as shown in Figure 4. The Raman spectra are fitted by

174

four peaks, G band (1580 cm-1, ideal graphitic lattice), D band (1350 cm-1, disordered graphitic

175

lattice (edges)), A band (1520 cm-1, amorphous carbon) and I band (1200 cm-1, polyenes and

176

ionic impurities).50 The intensity ratio of the G and D bands (IG/ID) can be used as an indicator of

177

the amount of defects sites presented in the graphite fibers of GF. The IG/ID decreases

178

remarkably in the sequence of UGF < CNT1000/GF < CNT900/GF < CNT1100/GF, which is in

179

good agreement of oxygen content measured by XPS.

180

Electrochemical measurement. Before the electrochemical experiments, all the samples

181

were pretreated by immersion in the etchant for 48 hours to eliminate the interfacial gas layer

182

between the electrode and etchant electrolyte (Text SI4). The SI videos also show that GF and

183

CNT/GF materials have an excellent wettability after immersion.

184

Cyclic voltammetry (CV) was conducted to evaluate the electrochemical activity of UGF and

185

CNT/GF electrodes toward the Cu(II)/Cu(I) redox reaction. Figure 5a―5d illustrate CV results

186

for UGF and CNT/GF electrodes at different scan rates. For all the electrodes, the peak

187

separation (∆Ep) between anodic peak potential (Ep,a) and cathodic peak potential (Ep,c) increase

ACS Paragon Plus Environment

9

Environmental Science & Technology

Page 10 of 35

188

with increasing scan rates, while the average peak potential ((Ep,a + Ep,c)/2) remains constant.

189

These results indicate that the Cu(II)/Cu(I) redox reaction on UGF and CNT/GF electrodes are

190

quasi-reversible, and this is controlled by both diffusion and charge transfer processes.51 As

191

shown in Figure 5e, for all electrodes, the anodic peak currents (Ip,a) are proportional to the

192

square root of the scan rates (v). The increasing of the slopes follow this order: UGF (2.91)