Amine-functionalized mesoporous silica as a support for on-demand release of copper in the A3-coupling reaction: ultra-low concentration catalysis and confinement effect Julio Cesar S. Terra, Audrey Moores, and Flávia Cristina Camilo Moura ACS Sustainable Chem. Eng., Just Accepted Manuscript • DOI: 10.1021/ acssuschemeng.9b00576 • Publication Date (Web): 08 Apr 2019 Downloaded from http://pubs.acs.org on April 8, 2019
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
Amine-functionalized mesoporous silica as a support for on-demand release of copper in the A3-coupling reaction: ultra-low concentration catalysis and confinement effect Julio C. S. Terra†, Audrey Moores†,*, Flavia C. C. Moura#,* † Centre for Green Chemistry and Catalysis, Department of Chemistry, McGill University, 801 Sherbrooke Street West, Montreal, QC, H3A 0B8, Canada. *
[email protected] # Departamento de Química, ICEx, Universidade Federal de Minas Gerais, Av. Antônio Carlos, 6627, Pampulha, Belo Horizonte, MG, 31270-901, Brazil. *
[email protected] Keywords MCM-41, supported catalyst, confinement effect, A3-coupling.
Abstract
ACS Paragon Plus Environment
1
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 2 of 45
The study of catalysts activity at ultra-low concentration is a
prime
importance
for
the
development
of
more
sustainable
catalytic processes. In this work, we designed mesoporous MCM-41 silica
with
covalent
functionalization
with
amine
groups
at
different levels of coverage. This material as used as a support to immobilize small quantities of Cu (I) species to be used as a catalyst in the A3-coupling reaction. The support design allowed the controlled release of the catalytically active species, as well
as
its
scavenging
after
reaction.
This
system
achieved
excellent catalytic performance, leading to 95% yield of the desired propargylamine within 2 hours of reaction at 100ºC under microwave conditions, using only 0.02 mol% of catalyst, the lowest catalyst amount ever reported for this reaction and high TON (4750) and TOF (2375 h-1). An interesting effect was noticed, where the catalyst on the support yielded improved reaction rates as compared to unsupported catalysts in solution, under the same concentration conditions. We discuss the possibility of a confinement of metal species inside the mesoporous structure of the support, which made the
immobilized
system
more
effective
than
the
homogenous
counterpart. The present study pushes the limits of A3-coupling reaction
conditions
and
the
potential
of
supported
metal
catalysis. Introduction
ACS Paragon Plus Environment
2
Page 3 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
Propargylamines are versatile compounds, frequently used as intermediates for building nitrogen-containing heterocycles1 such as natural products and biologically-active molecules.2 They can be
atom-economically
obtained
from
a
one-pot
three-component
condensation between an aldehyde, an amine and an alkyne, known as A3-coupling.3 In this Mannich-type reaction, the alkyne C-H bond needs
to
be
activated
for
the
process
to
happen,
hence
the
importance of an adequate catalyst choice.4 This reaction has been extensively studied in the context of homogeneous catalysis, since
the 2000s and the seminal work of
the Li group with the use of inorganic salts of various metals, including systems
gold,3 were
silver5
developed
and to
copper.6–9 improve
Thereafter,
the
different
process,
including
transition metal complexes as homogeneous catalysts.10–16 Despite the high efficiency of the homogenous version of this reaction, difficulties in reusability and product purification led to
the
development
of
heterogeneous
catalysts,17
18
with
a
particular focus on copper systems, thanks to the abundance and low cost of this metal.19,20 Copper nanoparticles, for instance, have been used in their suspended form21–23 and on several different supports such as montmorillonite24, graphene25, carbon nanotubes26 and activated carbon.27 Another common strategy is the grafting of copper
ions
on
functionalized
surfaces,
enabling
means
to
ACS Paragon Plus Environment
3
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 45
hetereogenize such species. This is achieved by covalently binding organic ligands on the surface of selected organic or inorganic supports, which will then coordinate to the metal species.
Many
examples can be found in the literature using complex multidentate ligands
to
graft
metal
species
onto
solid
supports,
mainly
polymers,28–32 silica beads33–35 and mesoporous silica.36–39 Although
heterogeneous
catalysts
are
meant
to
avoid
the
presence of metal species in the final product, many do typically suffer
from
leaching
issues.40
Copper
can
be
toxic
beyond
a
threshold concentration and its content in products is strictly regulated.41,42 This significant drawback causes many pharmaceutical processes to necessitate the use of expensive scavengers column. But
leaching
also
leads
to
mechanistic
uncertainties.
As
an
example, Moaddeli and coworkers38 used functionalized mesoporous silica with a super paramagnetic core to immobilize copper and successfully catalyzed the formation of propargylamines. Leaching studies evidenced that 38% of the initial copper content in the catalyst was lost after one cycle (~811 ppm metal/product) and 65% after three reaction cycles, along with moderate decrease in the catalytic
activities.
polymer-supported
In
copper
another species
study, to
Rus
catalyze
et the
coll.28
used
A3-coupling
reaction. The authors reported a decrease of about 15% in the copper content of the catalyst (~350 ppm metal/product) after
ACS Paragon Plus Environment
4
Page 5 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
running the reaction for one cycle. These leached copper species often have the ability to homogeneously catalyze the process as well. In fact, many catalysts, although designed as heterogeneous, actually worked as providers of active – yet often uncredited – homogeneous species,43 especially given the fact that A3-coupling reactions copper.
can
proceed
Another
with
impressively
Cu-catalyzed
reaction
small
quantities
relying
on
of
alkyne
activation, the Huisgen condensation, has been shown by the Yamada and Uozumi group44 to work with copper levels as low as 4.5 ppm using
a
self-assembled
Following the same
polymeric
imidazole
copper
principle, some groups have
catalyst.
been
able
to
significantly lower the catalytic charge for A3-coupling. For example, copper-impregnated magnetite has been used to effectively catalyze
A3-coupling
at
a
0.1
mol%
copper
load45
(~230
ppm
metal/product) and montmorinollite-supported copper nanoparticles have been able to catalyze the process at a catalyst load as low as 0.05 mol%24 (~120 ppm metal/product). Yet at very low charge, any leaching will quickly cause the loss of a significant portion of the heterogenized phase of copper. Catalytic
systems
where
dynamic
exchanges
between
nanoparticles and soluble species play a role in activity have been known and studied for several decades, but remain an active area
of
research
due
to
the
difficulties
to
unambiguously
ACS Paragon Plus Environment
5
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 45
characterize the active species. Suzuki-Miyaura and Mizoroki-Heck are excellent examples, where soluble Pd(II) and Pd (0) species are the active catalytic species which may exist in equilibrium with nanoparticulate systems.46 An interesting strategy developed by Crudden and coworkers40 is the use of thiol-functionalized mesoporous silica to deliver and subsequently trap catalytically active Pd(II), relying on the high affinity between sulfur and palladium atoms. Mesoporous
silica
materials
are
attractive
and
highly
versatile because these highly porous inorganic networks feature large surface areas and hydroxylated surfaces which are prone to functionalization.47,48 The easily tunable functionalization of such materials
has
chromatographic
given
them
stationary
diverse
applications,
phases49
immobilization of different molecules
to 50,51
ranging
supports
for
from the
and metal species for
both environmental remediation52,53 and catalytic interests.35,40 In particular, amine-grafted mesoporous silica have been extensively researched.54–58 Amine grafted mesoporous silica are particularly attractive for the adsorption of copper species, as rationalized in terms of Pearson’s hard-soft acid-base theory. For instance, Lam et al.59 have previously reported the high affinity of silver to
thiol-functionalized
materials,
whereas
adsorbed on amine-functionalized supports.
copper
was
better
Similar strategies
ACS Paragon Plus Environment
6
Page 7 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
have been reported for the A3-coupling reaction
33–39
using large
ligands with multiple complexation sites. Such ligands are great in
immobilizing
exchanges
the
between
metal
the
species,
but
heterogeneous
also
and
prevent
homogeneous
dynamic media,
potentially leading to catalytic systems that suffer from poor diffusion. Based on this state of the art, we took the appraoch of embracing the role of leaching in the heterogeneous catalyzed A3 coupling
and
designed
a
system
able
to
deliver
on-demand
homogeneous copper species and also recover them at the end of the process. Herein, we report the use of aminopropyl-functionalized MCM-41 as a multifunctional support, which not only provides copper for catalyzing the A3-coupling reaction inside its own pores, but also scavenges eventually leached metal species from the resulting propargylamine. In addition, we discovered that mesopores were able to confine species and provided nanoenvironments enhancing catalytic activity as compared to the homogenous blank. This allowed the use of unprecedently low catalyst loads. The use of simple ligands and low metal loading on the support ensures the ability of the ions to be freed and furtherly trapped by the highly available adsorption sites, providing an interesting system that works
on
the
frontier
between
homogeneous
and
heterogeneous
catalysis.
ACS Paragon Plus Environment
7
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 45
Results and discussion Catalyst support characterization The catalyst synthesis process is summarized on Figure 1 and detailed in the experimental section. The methodology for making MCM-41 has been previously reported by us (the Moura Group60) and is an adaptation of the Grün method,61 which is a modification of the original method reported by Kresge and Beck in 1992.62,63 The modification of silica with silane coupling agents was inspired by the method reported by the Resasco Group,64 which is carried out in
room
temperature,
simpler
than
reflux
methods
previously
reported in the literature.40,59 Post-synthetic functionalization was chosen to assure the shape and size homogeneity of the pores, but there are other methods where the organosilane reagent is added during the synthesis of the material and co-condensed within the inorganic
network.
The
co-condensation
method
gives
a
more
homogeneous distribution of the organic groups through the surface of the support, but it compromises the regularity of the porous structure.48
MCM-41
was
functionalized
with
APTMS
[(3-
aminopropyl)trimethoxysilane] in different APTMS to MCM-41 ratios X (X = 1.5, 3.0, 4.5 and 6.0 mmol.g-1), leading to four different amine grafted materials labeled NH2_X/MCM-41, using a slightly modified reported method.64
ACS Paragon Plus Environment
8
Page 9 of 45
SCHEME OF MCM-41 FUNCTIONALIZATION AND COPPER IMMOBILIZATION O SUPPORT FUNCTIONALIZATION AND COPPER IMMOBILIZATION Si OH
O
Si
Si
CuI
Si O O
O Si
O
O Si
H2N APTMS/MCM-41 1.5 mmol.g-1
O Si
O
Si O O O
MCM-41
O
NH2
(H3CO)3Si
O
Si O
CuI 0.4
H 2N
MCM-41
O
Si O O O
OO Si OH OH H2N Si O O Si OH O Si OH Si OH H3CO SiOO OCH H3CO SiSi 3OH OH OO APTMS/MCM-41: APTES/MCM-41: Si OH 1.5, 3.0, 4.5Oand 6.0 mmol.g-1
H 2N
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
Cu +
H2N O
NH2
mmol.L-1
24h, RT
Si
O
NH
NH 2 2
Cu+ O
Si O O
(from NH-MCM-41_1.5)
(1.5, 3.0, 4.5, 6.0)
O O
NH 2
Cu-NH-MCM-41
NH-MCM-41
O
O Si
NH2/MCM-41
Si O
NH2
O Si O
O Si O
Si
O
Cu/NH2/MCM-41
Pore size around 3 nm, structures not drawn in scale.
Figure 1. Scheme of catalyst synthetic procedure, which consists of support functionalization and copper immobilization.
Initially,
functionalization
of
the
materials
investigated by solid state nuclear magnetic resonance (NMR). Cross-Polarization spectra
were
Magic
registered
Angle for
Spinning
both
NMR
starting
(29Si and
CPMAS
was 29Si
NMR)
functionalized
silica materials (Figure 2).
ACS Paragon Plus Environment
9
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
NH2_6.0/MCM-41 NH-MCM-41_6.0
5
NH2_4.5/MCM-41 NH-MCM-41_4.5
4
NH2_3.0/MCM-41 NH-MCM-41_3.0
3
T3
T2
NH2_1.5/MCM-41 NH-MCM-41_1.5
-25
-30
Q4
Q2 -35
-40
-45
-50
-55
-60
2
Q3
MCM-41 MCM-41
-20
Page 10 of 45
-65
-70 -75 f1 (ppm)
-80
-85
-90
-95
-100
-105
-110
-115
1
-120
-125
(ppm)
T2 O
O OH Si
NH2
T3 O
Q2
O O Si
NH2
OH Si O OH O
Q3
Q4
OH Si O O O
O Si O O O
Geminal silanol Free Silanol [SiO2(OH)2] [SiO3OH]
Siloxane [SiO4]
Figure 2. Top: 29Si CPMAS NMR spectra for parent MCM-41 and functionalized silica materials NH2_X/MCM-41 (X=1.5, 3.0, 4.5 and 6.0). Below: List of functionalities assigned to 29Si CPMAS NMR peaks observed for these materials. [O] fragments represent oxygen atoms connected to the silica matrix via O-Si bonds.
ACS Paragon Plus Environment
10
Page 11 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
Unfunctionalized MCM-41 afforded a typical spectrum featuring the three possible chemical environments for Si atoms depicted in figure 2,65 labeled Q2, around -93 ppm, Q3, around -102 ppm and Q4
,
around -112 ppm (Q standing for 4 bound O atoms, quattuor in latin).66 Spectra of the functionalized materials featured not only Q signals, as parent MCM-41 does, but also T2, from -60 to -56 ppm, and T3 peaks, from -68 to -64 ppm (T standing for 3 bound O atoms), which reflect the introduction of Si atoms from the grafting of ATPMS. The presence of signals T2 and T3 was a firm evidence that organic groups are indeed covalently bonded to the support matrix rather than simply adsorbed onto its surface.67 Another feature noticeable in Figure 2 is the increase in the intensity of the Q4 signal
when
compared
to
the
intensity
of
Q3
peaks
for
functionalized materials. This is expected since Q3 are converted into T3 sites in the functionalized materials, while Q4 sites, lacking OH groups, are not prone to functionalization and remain unchanged.
ACS Paragon Plus Environment
11
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
MCM-41
ACS Sustainable Chemistry & Engineering
11
O O Si O
2 1
3
22
3
Page 12 of 45
NH2 33
1
2
4
NH2_6.0/MCM-41 NH-MCM-41_6.0 N6.0
NH2 3
N4.5 NH2_4.5/MCM-41 NH-MCM-41_4.5
3
2 1
N3.0
4
NH2_3.0/MCM-41 NH-MCM-41_3.0
2
MCM-41
N1.5 1
NH-MCM-41_1.5 NH2_1.5/MCM-41 50
50
Si OOO
45
30
40
40
35
30
10
20
f1 (ppm)
25
20
15
10
MCM-41
(ppm)
5
(ppm)
Figure 3. 13C CPMAS NMR spectra for the four functionalized materials.
13C
CPMAS
NMR
further
confirmed
the
successful
functionalization of MCM-41 (Figure 3). The three major signals present for each material correspond to the three carbon atoms of the aminopropyl functionality. The peaks around 11 ppm, 20-30 ppm, and 44 ppm, correspond respectively to carbons 1, 2 and 3 as depicted on figure 3. The peaks were assigned in accordance with the
shielding
effect
provided
by
the
siloxane
and
amino
functionalities. The broader peak from carbon 2 could be attributed to conformational changes within the ligand. Signals around 16 ppm (peak 4) from materials NH2_1.5/MCM-41 and NH2_3.0/MCM-41 were attributed to adsorbed residual silane coupling agent, since such
ACS Paragon Plus Environment
12
Page 13 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
signals
were
not
found
in
the
parent
material
and
do
not
corroborate with previous literature.68 Interestingly, in both
29Si
and
13C
CPMAS NMR spectra, the
signals corresponding to propylsiloxane were consistently shifted downfield as the degree of functionalization increased, except for sample
NH2_6.0/MCM-41,
which
features
similar
displacement
to
NH2_4.5/MCM-41. This indicated that functionalization reached a plateau for APTMS initial loading of 4.5 mmol.g-1 (vide infra). Overall,
29Si
and
13C
CPMAS NMR confirmed the covalent grafting of
APTMS and the preservation of the propylamine structure. Following,
TGA
and
XPS
were
performed
to
quantify
the
effective grafting of the aminopropyl groups onto the supports (Table 1, further details in SI, sections 1 and 2). TGA allowed to access the degrees of functionalization, based on the premise that organic matter mass loss was coming from grafted propylamines and gave values of 1.7, 2.5, 3.3 and 3.2 mmol.g-1 for materials of theoretical functionalization 1.5, 3.0, 4.5 and 6.0, respectively. TGA confirmed complete loading at low charge, and then saturation of the loading at 3.3 mmol.g-1 at higher charge. As NMR results already suggested, functionalization reached a maximum for the initial APTMS load of 4.5 mmol.g-1, and plateaued thereafter. XPS functionalization degrees were obtained from Si/N atomic ratios and gave values of 2.3, 3.2, 4.2, and 4.0 mmol.g-1 for the initially added 1.5, 3.0, 4.5 and 6.0 mmol.g-1, respectively. Although this
ACS Paragon Plus Environment
13
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 45
data follows the same trend as the data obtained by TGA, XPS systematically led to slightly higher anchoring rates. This can be understood by the fact that XPS is a surface technique, evaluating only the first few nm of the studied material. Hence it is known that grafting in mesoporous silica is usually more efficient in the outer surfaces and regions close to the pore openings.
Table 1. Degree of aminopropyl functionalization for materials NH2_X/MCM-41 (X=1.5, 3.0, 4.5 and 6.0) obtained by TGA and the XPS Si/N atomic ratios, in mmol of aminopropyl group per gram of MCM-41 and BET specific surface areas for pure MCM-41 and the four functionalized materials. Figures in parenthesis carry the calculation uncertainties.
Entry
1 2 3 4 5
Material
NH2_1.5/MCM41 NH2_3.0/MCM41 NH2_4.5/MCM41 NH2_6.0/MCM41 MCM-41
TGA effective
XPS effective
BET
degree of
degree of
Surface
functionalization functionalization Area (m2 (mmol.g-1)
(mmol.g-1)
g-1)
1,72(9)
2,3(3)
865
2,46(6)
3,2(2)
469
3,33(7)
4,1(7)
66
3,19(8)
3,9(6)
125
N/A
N/A
1271
In order to acquire information on the morphology and porosity of the materials, parent MCM-41 and aminopropyl-functionalized
ACS Paragon Plus Environment
14
Page 15 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
supports were characterized by N2-sorption and TEM (Figures S2 and S3). BET specific surface areas are shown in Table 1. As expected, specific surface area decreases as grafting load increases due to the possible obstruction of pores caused by the functionalization process.48
Samples
NH2_1.5/MCM-41
and
NH2_3.0/MCM-41
featured
relatively good specific surface areas of 865 and 469 m2 g-1 when compared to 1271 m2 g-1 for the parent MCM-41 (Table 1, entries 12 &5). We observed isotherm profiles (Figure S2) of the I(b) type, as proposed to Thommes et al.,69 associated with micropores or tiny mesopores, whose diameter lie just above the microporous threshold (2 nm). Transmission electron microscopy (TEM, Figure S3) confirms this point with pore sizes of about 3.3 nm. Materials NH-MCM41_4.5 and 6.0 were found to have surface areas as low as less than 10% of the surface of the original MCM-41 (Table 1, entries 3 and 4) and presented isotherm profiles of type II isotherm,69 typical of microporous or non-porous adsorbents, confirming that high functionalization degree leads to blocking most of pore entrances, essentially eliminating porous properties. Catalyst immobilization and catalytic activity study Once
we
have
established
that
the
materials
were
functionalized and learnt about their surface areas and porosity profiles, NH2_1.5/MCM-41 was chosen to be used to immobilize copper (I) species. The choice was made because such material has the highest surface area among the prepared supports and preserved
ACS Paragon Plus Environment
15
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 45
most of its porous structure which is essential for improving diffusion
rates
featured
a
during
good
catalysis.
propylamine
The
chosen
loading,
material
essential
for
also Cu
stabilization. Therefore, that material was used to immobilize copper
species,
leading
to
the
catalyst
Cu
over
NH2/MCM-41
(Cu/NH2/MCM-41). NH2_1.5/MCM-41 was suspended in a CuI solution in acetonitrile and stirred for 24h. The amount of copper provided was chosen so that, in the case of adsorption on all the available metal, only half of the available sites would be occupied on the support, so that leached copper could be readsorbed onto the support after the reaction had been catalyzed. The previously white material turned light green upon Cu exposure and subsequent washing with acetonitrile. In order to evaluate the amount of immobilized copper in the hybrid material, it was digested in hot HNO3. The Cu content was then measured by ICP-OES analysis to be 0.0954 mmol g-1, which corresponds to occupation of about 10% of the available adsorption sites on the material (assuming each cation coordinates with two amine groups59). The
copper-loaded
materials
were
also
subjected
to
XPS
analysis in order to study the oxidation state of the metal. Figure 4 presents the Cu 2p spectra for Cu/NH2/MCM-41 and CuI and two important pieces of information can be obtained from them. First, the absence of satellite peaks around 945 eV means that there are
ACS Paragon Plus Environment
16
Page 17 of 45
no Cu(II) species in the materials,70 so the metal was not oxidized in the immobilization process. This is a desirable feature since Cu(I)
species
are
recognized
to
be
essential
for
catalytic
activity.4 Choi & Jang71 carried out comparative studies with both Cu(I) and Cu(II) salts and found the former to be more active in A3-coupling. Second, the binding energies slightly shifted to higher values when the Cu species were grafted on functionalized silica, as compared to CuI. Such a shift is consistent with Cu atoms coordination with a more electronegative atom, such as nitrogen in the amine functionality, and confirms the expected bonding scheme.
932.9 eV
Cu 2p
Intensity Intensity
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
932.0 eV
951.7 eV 952.9 eV
Cu/NH Cu-NH-MCM-41 2/MCM-41 970 970
960 960
CuI 950 950
940 940
930 930
920 920
Binding Binding Energy energy (eV) (eV)
Figure 4. Cu 2p XPS spectra of CuI (green) and Cu/NH2/MCM-41 (black).
ACS Paragon Plus Environment
17
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 45
The functionalized material was tested for the A3-coupling of the model reagents: cyclohexanecarboxyaldehyde, piperidine and phenylacetylene (Scheme 1). The reaction conditions were initially chosen according to previous experience from our group. Initially, the reaction was carried out in a solvent-free fashion at 100oC for 5 minutes in a microwave reactor and a catalyst load of 0.4 mol% (Table 2, entries 1). This provided moderate yields of 42%. Interestingly, upon reducing the load incrementally all the way to 0.02 mol%, this yield level remained remarkably stable. In order to push the reaction yield, the reaction time was varied.
the At
the low charge of 0.02 mol%, excellent yield of 95% in 2h were measured. 0.02 mol% was the minimum feasible charge at our reaction scale (0.5 mL). We thus increased the scale of the reaction to 1 mL, which enabled the use of 0.01 mol% of catalyst. This lower catalyst load provided a good yield of 85% after 2h of reaction (Table 2, entry 11). We set the optimized reaction conditions at 0.02 mol% of catalyst for 2h.
Cu-NH-MCM-41 0.02 mol% Cu o 100 C (MW), 2h, neat
N H H
O
N
- H 2O
Scheme 1. A3-coupling reaction scheme between cyclohexanecarboxyaldehyde, piperidine and phenylacetylene.
ACS Paragon Plus Environment
18
Page 19 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
Table 2. Catalyst load and reaction time optimization. All the reactions were carried out with the selected model substrates, under solvent-free conditions and 100oC microwave heating. Entry
Catalyst load (mol%)
1 2 3 4 6 7 8 9 10 11
0.4 0.2 0.1 0.05 0.02 0.02 0.02 0.02 0.02 0.01
Reaction time (min) 5 5 5 5 5 15 30 60 120 120
NMR yield (%) 42 41 42 48 43 79 85 92 95 85
A comparative kinetic study was carried out with 0.02 mol% of catalyst for the reaction catalyzed with either immobilized copper on Cu/NH2/MCM-41 or CuI alone as catalyst, using the exact same amount
of
copper
in both
cases.
The
recovered products were
systematically digested and submitted to ICP-OES Cu analysis, leading to a measure of the quantity of released Cu into the reaction mixture over time. Figure 5 summarizes the kinetic data obtained
for
product
formation
(solid
lines)
and
copper
concentration in solution (dotted lines).
ACS Paragon Plus Environment
19
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 45
Figure 5. Kinetic study of the A3-coupling reaction of cyclohexanecarboxaldehyde, piperidine and phenylacetylene catalyzed by CuI or Cu/NH2/MCM-41 (solid lines – left ordinate) and Cu leaching into products (dotted lines – right ordinate). Reactions carried out with 0.02 mol% catalyst and 100°C under microwave heating.
With
the
supported
Cu/NH2/MCM-41
catalyst,
the
reaction
proceeded very fast, reaching a yield of 79% after 15 min and 95% after 2h, under microwave heating at 100°C with a catalyst load of 0.02 mol%. Using ICP-OES, we noticed that about 55 to 60% of the Cu species were released during the reaction. This value remained fairly stable over the reaction period. Homogeneous CuI however
ACS Paragon Plus Environment
20
Page 21 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
had a slower start, with a conversion of 47% at 15 min of reaction and 74% yield at 2 h, all other experimental conditions being identical. Intuitively, 100% of the Cu from CuI present was in solution. These measurements show two aspects. First, this proves that our system could keep at least a part of the Cu species immobilized, thus limiting contamination of the product. Secondly, the reaction was accelerated and overall more efficient across the reaction period for the heterogeneous system compared to the homogenous one. This is counter intuitive since in most systems, mass
transfer
causes
homogeneous
systems
to
outperform
heterogeneous ones.72 In order to rationalize this reactivity, we considered
the
possibility
of
having
a
confinement
effect,
affording accelerated rates in the pores of our catalyst.73 The
reactants
were
also
submitted
to
the
same
reaction
conditions, but this time replacing Cu/NH2/MCM-41 for a combination of homogeneous CuI plus NH2/MCM-41 or homogeneous CuI plus MCM-41. Both blanks gave the same results as the homogeneous catalyst itself (Supporting Information, Figure S6), indicating that the support does not play a role in the system unless copper species are effectively immobilized on the surface and allowed to permeate the pores of the material. Therefore, the immobilization of metal within the porous structure was demonstrated to be the key step for the observed catalytic activity increase.
ACS Paragon Plus Environment
21
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 45
Indeed, porous materials are known for having a special sorption equilibrium caused by the curvature of the pores, which leads to an increased concentration of specific reagents inside the nanostructures. Such confinement effect has long been known on zeolites, the microporous relatives of mesoporous silicas, having Derouane and coworkers investigated the subject decades ago.74–76 In fact, the confinement effect on zeolites is considered one of the most interesting features of such materials.77 Although a solid literature exists on the confinement effect for zeolites, the knowledge of such phenomenon in materials with larger pores is still being built.78 The Kim group, for example, has shown that dyes
confined
properties
in
that
the
mesopores
differ
of
MOFs
significantly
from
have the
photophysical non-confined
molecules.79 Another interesting work was published by the Goswami group, in which the authors were able to conduct polyol metal nanoparticles synthesis inside the pores of polystyrene and silica gel
particles.80
conditions.
In
Such
methods
addition,
are
Herrmann
not &
possible Iglesias
under
ambient
studied
the
condensation of acetone in aluminosilicates with different types of pores using DFT calculations.81 By studying the transition states, the authors demonstrated that the rate constants greatly depend on the size and shape of the confining voids. There is also a study by Bereckzi et al.72 that found similar results to ours. The authors immobilized a Cu (II) complex on mesoporous silica
ACS Paragon Plus Environment
22
Page 23 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
aerogel and used it to catalyze the oxidation of phenol. They found that the immobilized catalyst had up to 15 times higher TOFs than the purely homogeneous complex and attributed this fact to the confinement of species inside the mesopores. Porous structures can, thus, concentrate catalytic species in their interiors, which allows the reagents to experience a local higher catalyst concentration. This enabled us to use of such a low catalyst amount, which is, the lowest ever reported in the literature for A3-coupling. The small scale of the reaction made the effective reutilization of the material impossible, which is an open avenue for further improving this system in the future. Nevertheless, the low catalyst load still gives our system maximum TON
and
TOF
of
4750
and
2375
h-1,
respectively,
which
are
competitive with the best values encountered in the literature for this reaction. Such systems often require multiple recycling steps to
achieve
high
TONs.
Montmorillonite-stabilized
copper
nanoparticles, for example, afforded a TON of 5640 over three runs24 and a catalyst based on copper supported on organosilica and ionic liquid framework gave a TON of
4526 over 7 runs.32 Most
works
the
found
in
the
literature
for
same
process
have
significantly lower TONs (i.e. below 1000), even after multiple cycles of reuse.25,27,28,30,36–38,82,83 The low catalyst load limits the copper contamination in the product to a maximum of about 50 ppm (in the extreme case of total
ACS Paragon Plus Environment
23
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 24 of 45
leaching), which is already below the limits for oral exposure stablished by both the U.S. Food and Drugs Administration42 and the European Medicines Agency41 (300 and 250 ppm respectively), being good for most applications. ICP-OES measurements on the products showed that the system was able to scavenge about 40% of the total copper species used (Figure 5). Given the known ability of amine groups of coordinating to copper, it is reasonable to assume that the functionalized materials would be able to retrieve the metals from the reaction mixture, but it must be also taken into account the presence of other amines in the reaction mixture (reagents and products) that could compete with the support for the copper ions, being a possible cause of leaching. Despite such leaching, our system
remains
competitive
with
other
known
catalysts,
which
typically lead to more leaching. The combination of low metal load with the retention of part of it on the support led to final contamination in the product as low as only 30 ppm. In order to prove the versatility of the system, different aldehydes, amines and alkynes were used to build a substrate scope (Table 3, expanded on Table S2). A3-coupling is a well-known reaction and a range of different propargylamines were obtained in good to excellent yields. Aromatic aldehydes (entries 2-3) were less
active
than
the
aliphatic
model
substrate
and
required
slightly higher reaction temperatures. Product was observed with both cyclic and non-cyclic secondary amines (entries 4-6) and
ACS Paragon Plus Environment
24
Page 25 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
morpholine (entry 6) was slightly less reactive than the other ones due to the presence of the oxygen atom in the ring, which is electron-withdrawing
and
reduces
the
basicity
of
the
amine.
Aromatic and non-aromatic alkynes were also used (entries 7-8) and the former provided slightly higher yield since the resonance structures contribute to make the terminal hydrogen more acidic and the C-H bond more easily activated. The system proved to be selective
to
the
propargylamine,
having
all
the
additional
functional groups used in the scope remained untouched in the final product. Table 3. A3-coupling substrate scope using Cu/NH2/MCM-41.a Entr y
Aldehyde O
1
O
2
O
3
Amine
Alkyne
Product
H N
N
H N
N
H N
H3CO
Yield (%) 95
68b
N
79b
H3CO O
O
4
H N
N
87
O
ACS Paragon Plus Environment
25
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
O
5
Page 26 of 45
N
H N
91
N
O H N
6
O
7
59
H N
N
91 Br Br
O
8
H N
N
79
aReaction
conditions as described in the typical procedure.
bAromatic
aldehydes were reacted at 120oC.
Experimental All the reagents used were purchased from Sigma-Aldrich and used as provided, unless specified. Synthesis of catalysts: MCM-41 was synthesized according to a procedure described by us (Moura) in a previous report.60 The functionalization was carried out by modifying a method used by Zapata et al.64 Initially, a suspension containing 0.5 g of parent MCM-41 in 10 mL of dry toluene was prepared in a polypropylene tube
and
sonicated
for
1h.
Then,
25
mL
of
a
(3-
aminopropyl)trimethoxysilane (APTMS) solution in dry toluene was added to the suspension, being the amount of APTMS calculated according to the desired degree of functionalization. In this work,
ACS Paragon Plus Environment
26
Page 27 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
the loadings were 1.5, 3.0, 4.5 and 6.0 mmol g-1. The suspensions containing both MCM-41 and APTMS were magnetically stirred at 1600 rpm and 30°C for 24h. Each of the functionalized materials was, then, vacuum filtered and washed with 300 mL of ethanol P.A., ovendried for 18h at 115°C and washed with dry toluene in a soxhlet extractor for 3h, followed by extra rinsing with ethanol P.A. and oven-dried for extra 18h at 100°C. The four functionalized fine white powders obtained were named after their nitrogen loading: N1.5, N3.0, N4.5 and N6.0. Once the materials were obtained, N1.5 was used to immobilize copper (I) species by suspending 200 mg of N1.5 in 200 mL of a 0.4 mmol L-1 CuI solution in acetonitrile. The suspension of stirred at 800 rpm for 24h at room temperature. The greenish powder obtained was vigorously washed with approximately 300 mL of acetonitrile, then dried in vacuum oven at 50°C for 18h, maintaining its greenish color. Characterization of the catalysts: Parent MCM-41 and the four functionalized materials were characterized by N2 sorption, solid state
29Si
analysis
and (TGA),
13C
CPMAS X-ray
NMR
spectroscopy,
photoelectron
thermogravimetric
spectroscopy
(XPS),
inductively coupled plasma atomic emission spectroscopy (ICP-OES), and transmission electron microscopy. N2 sorption isotherms were obtained on a Micrometric TriStar 3000, 55 points scan at 77.35 K, having the samples being previously degassed at 100°C for 10 hours; the isotherms were analyzed by Brunauer, Emmett and Teller (BET)
ACS Paragon Plus Environment
27
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 28 of 45
and Barrett, Joyner and Halenda (BJH) methods. Solid state NMR was performed on a 400 MHz Varian VNMRS equipment using 7.5 mm zirconia rotors spinning at 5 kHz with cross polarization and magical angle spinning (CPMAS), 20 ms acquisition time, 4 s recycle delay on 1024 scans, operating at Larmor frequencies of 100.53 MHz for and 79.42 MHz for in
concentrated
concentration
29Si.
trace
measured
13C
The copper-loaded materials were digested metal by
grade
HNO3
inductively
and
had
coupled
their
copper
plasma
atomic
emission spectroscopy (ICP-OES) on a Thermo iCap 6500 Duo Series spectrometer. Catalytic tests: The amine was chosen as the limiting reagent and the A3-coupling reaction reagents were added in a molar ration 1.6:1.3:1.6 of aldehyde:amine:alkyne and a catalyst load of 0.02 mol%.
A
typical
procedure
cylohexanecarboxaldehyde,
128
would L
of
take
piperidine,
200 180
L L
of of
phenylacetylene and 2.7 mg of Cu/NH2/MCM-41 (0.0954 mmol g-1 of Cu). The reagents and catalyst were added to a V-shaped microwave tube (0.5-2 mL) with a magnetic stir bar, sealed and set in a Biotage microwave reactor for 2h at 100oC and low frequency, 5s of pre-stirring. Following, 100 L of diphenylmethane 99% were added to the crude product along with around 5 mL of ethyl acetate. The mixture was homogenized and filtered on celite, then the solvent was removed and the absolute yield was calculated by proton NMR using diphenylmethane as internal standard. Products
ACS Paragon Plus Environment
28
Page 29 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
were
also
qualitatively
analyzed
by
GC-MS.
The
proton
NMR
experiments were performed with 16 scans on a 500 MHz AVIIIHD Bruker
spectrometer. Additionally, the products
were properly
digested and the leached copper amount was also measured by ICPOES. The digestion was carried out in a multi-step procedure consisted by wet ashing with concentrated sulfuric acid, followed by an open digestion step with concentrated nitric acid. Conclusion Our
results
position
amine-functionalized
MCM-41
in
a
strategic position as a non-innocent support for copper (I) species in the A3-coupling reaction. The support did not only deliver the catalytic species, but also enabled their confinement inside the pores, which made possible the use of the lowest catalyst loads ever reported for this reaction, working better than the purely homogeneous catalyst itself. Furthermore, even though leaching of the metal species was observed at the end of the reaction, the support is still able to scavenge part of those leached species, leading to a product contamination as low as 30 ppm, which is one order of magnitude lower than the concentration permitted by regulatory agencies. The products were, therefore, obtained from minimum metal usage and dispense costly and energy-consuming metal purification steps. This work showcases the power of mesoporous silica as a catalytic support by challenging current boundary
ACS Paragon Plus Environment
29
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
conditions
exploits
one
of
the
multiple
Page 30 of 45
possibilities
for
improving supported metal catalysis.
Acknowledgements We thank the Natural Science and Engineering Research Council of Canada
(NSERC)
Discovery
Grant
and
accelerator
programs,
the
Canada Foundation for Innovation (CFI), the Canada Research Chairs (CRC), the Centre for Green Chemistry and Catalysis (CGCC) and McGill University for their financial support. We also thank Dr. Robin Stein for the precious help with Solid State NMR, Andrew Golsztajn for the dedication on ICP Analysis and Alain Y. Li for his priceless help and advice. Supporting information TGA
profiles
description
and of
XPS the
atomic
percentage
calculation
of
tables,
effective
as
well
degrees
as of
functionalization by both methods. Full N2 sorption isotherms for all materials and TEM image depicting the porous structure of the synthesized MCM-41. Information on the identification of the main product, including detailed
1H
NMR and mass spectra. Also results
of catalytic control experiments and an expanded scope table.
References (1) Querard, P.; Girard, S. A.; Uhlig, N.; Li, C.J. Gold-Catalyzed Tandem
Reactions
of
Amide–aldehyde–alkyne
Coupling
and
Cyclization-Synthesis of 2,4,5-Trisubstituted Oxazoles. Chem. Sci.
2015,
6
(12),
7332–7335.
ACS Paragon Plus Environment
30
Page 31 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
https://doi.org/10.1039/C5SC02933C. (2) Wei, C.; Li, Z.; Li, C.J. The Development of A
3
-Coupling
(Aldehyde-Alkyne-Amine) and A3-Coupling (Asymmetric AldehydeAlkyne-Amine).
Synlett
2004,
No.
9,
1472–1483.
https://doi.org/10.1055/s-2004-829531. (3) Wei, C.; Li, C. J. A Highly Efficient Three-Component Coupling of Aldehyde, Alkyne, and Amines via C-H Activation Catalyzed by Gold in Water. J. Am. Chem. Soc. 2003, 125 (32), 9584–9585. https://doi.org/10.1021/ja0359299. (4) Peshkov, V. a.; Pereshivko, O. P.; Van der Eycken, E. V. A Walk around the A3-Coupling. Chem. Soc. Rev. 2012, 41 (10), 3790. https://doi.org/10.1039/c2cs15356d. (5) Wei, C.; Li, Z.; Li, C. J. The First Silver-Catalyzed ThreeComponent Coupling of Aldehyde, Alkyne, and Amine. Org. Lett. 2003, 5 (23), 4473–4475. https://doi.org/10.1021/ol035781y. (6) Li,
C.J.;
Wei,
C.
Highly
Efficient
Grignard-Type
Imine
Additions via C–H Activation in Water and under Solvent-Free Conditions.
Chem.
Commun.
2002,
No.
3,
268–269.
https://doi.org/10.1039/b108851n. (7) Leadbeater, N. E.; Torenius, H. M.; Tye, H. Microwave-Assisted Mannich-Type Three-Component Reactions. Mol. Divers. 2003, 7, 135–144. https://doi.org/10.1023/B:MODI.0000006822.51884.e6. (8) Shi, L.; Tu, Y. Q.; Wang, M.; Zhang, F. M.; Fan, C. A. Microwave-Promoted
Three-Component
Coupling
of
Aldehyde,
Alkyne, and Amine via C-H Activation Catalyzed by Copper in Water.
Org.
Lett.
2004,
6
(6),
1001–1003.
https://doi.org/10.1021/ol049936t. (9) Ju, Y.; Li, C. J.; Varma, R. S. Microwave-Assisted Cu (I)
ACS Paragon Plus Environment
31
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 32 of 45
Catalyzed Solvent-Free Three Component Coupling of Aldehyde, Alkyne and Amine. QSAR Comb. Sci. 2004, 23 (10), 891–894. https://doi.org/10.1002/qsar.200420034. (10)
Grirrane,
A.;
Álvarez,
E.;
García,
H.;
Corma,
A.
Cationic copper(I) Complexes as Highly Efficient Catalysts for Single and Double A3-Coupling Mannich Reactions of Terminal Alkynes: Mechanistic Insights and Comparative Studies with Analogous gold(I) Complexes. Chem. - A Eur. J. 2014, 20 (44), 14317–14328. https://doi.org/10.1002/chem.201403927. (11)
Rosales, J.; Garcia, J. M.; Ávila, E.; González, T.; Coll, D. S.; Ocando-Mavárez, E. A Novel Tetramer copper (I) Complex
Containing
Characterization
and
Diallylphosphine Catalytic
(Aldehyde-Amine-Alkyne) 2017,
Ligands:
Application
Reactions.
in
Inorganica
Synthesis, A3-Coupling Chim.
467,
Acta
155–162.
https://doi.org/10.1016/j.ica.2017.07.038. (12)
Cammarata, J. R.; Rivera, R.; Fuentes, F.; Otero, Y.; Ocando-Mavárez, E.; Arce, A.; Garcia, J. M. Single and Double A3-Coupling (Aldehyde-Amine-Alkyne) Reaction Catalyzed by an Air
Stable
2017,
copper(I)-Phosphole 58
Complex.
Tetrahedron
(43),
Lett.
4078–4081.
https://doi.org/10.1016/j.tetlet.2017.09.031. (13)
Kashid, V. S.; Balakrishna, M. S. Microwave-Assisted copper(I)
Catalyzed
A3-Coupling
Reaction:
Reactivity,
Substrate Scope and the Structural Characterization of Two Coupling Products. Catal. Commun. 2018, 103 (September 2017), 78–82. https://doi.org/10.1016/j.catcom.2017.09.020. (14)
Rasheed, O. M.; Bawn, C.; Davies, D.; Raftery, J.; Vitorica-Yrezabal, I.; Pritchard, R.; Zhou, H.; Quayle, P. The
ACS Paragon Plus Environment
32
Page 33 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
Synthesis of Group 10 and 11 Metal Complexes of 3,6,9-Trithia1-(2,6)-Pyridinacyclodecaphane and Their Use in A3-Coupling Reactions.
European
J.
Org.
Chem.
2017,
5252–5261.
https://doi.org/10.1002/ejoc.201701033. (15)
Beillard, A.; Métro, T.-X.; Bantreil, X.; Martinez, J.; Lamaty,
A3-Coupling
F.
Reaction
and
[Ag(IPr)2]PF6 :
A
Successful Couple. European J. Org. Chem. 2017, 2017 (31), 4642–4647. https://doi.org/10.1002/ejoc.201700985. (16)
Price, G. A.; Brisdon, A. K.; Randall, S.; Lewis, E.; Whittaker, D. M.; Pritchard, R. G.; Muryn, C. A.; Flower, K. R.; Quayle, P. Some Insights into the Gold-Catalysed A3Coupling Reaction. J. Organomet. Chem. 2017, 846, 251–262. https://doi.org/10.1016/j.jorganchem.2017.06.019.
(17)
Zeng, T.; Chen, W.-W.; Cirtiu, C. M.; Moores, A.; Song, G.; Li, C.J. Fe3O4 Nanoparticles: A Robust and Magnetically Recoverable Catalyst for Three-Component Coupling of Aldehyde, Alkyne
and
Amine.
Green
Chem.
2010,
12
(4),
570.
https://doi.org/10.1039/b920000b. (18)
Nasrollahzadeh,
M.;
Mohammad
Sajadi,
S.;
Rostami-
Vartooni, A. Green Synthesis of CuO Nanoparticles by Aqueous Extract
of
Anthemis
Nobilis
Flowers
and
Their
Catalytic
Activity for the A3 Coupling Reaction. J. Colloid Interface Sci.
2015,
459,
183–188.
https://doi.org/10.1016/j.jcis.2015.08.020. (19)
Wang, D.; Astruc, D. The Recent Development of Efficient Earth-Abundant Rev.
Transition-Metal
2017,
Nanocatalysts.
46
(3),
Chem.
Soc.
816–854.
https://doi.org/10.1039/C6CS00629A. (20)
Kaushik,
M.;
Moores,
A.
New
Trends
in
Sustainable
ACS Paragon Plus Environment
33
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 34 of 45
Nanocatalysis: Emerging Use of Earth Abundant Metals. Curr. Opin.
Green
Sustain.
Chem.
2017,
7,
39–45.
https://doi.org/10.1016/j.cogsc.2017.07.002. (21)
Kidwai,
M.;
Bansal,
V.;
Mishra,
N.
K.;
Kumar,
A.;
Mozumdar, S. Copper Nanoparticle Catalyzed A3-Coupling via C-H Activation.
Synlett
2007,
No.
10,
1581–1584.
https://doi.org/10.1055/s-2007-980365. (22)
Kantam, M. L.; Yadav, J.; Laha, S.; Jha, S. Synthesis of Propargylamines
by
Three-Component
Coupling
of
Aldehydes,
Amines and Alkynes Catalyzed by Magnetically Separable Copper Ferrite
Nanoparticles.
Synlett
2009,
No.
11,
1791–1794.
https://doi.org/10.1055/s-0029-1217362. (23)
Lakshmi Kantam, M.; Laha, S.; Yadav, J.; Bhargava, S. An Efficient Synthesis of Propargylamines via Three-Component Coupling
of
Aldehydes,
Amines
and
Alkynes
Catalyzed
by
Nanocrystalline copper(II) Oxide. Tetrahedron Lett. 2008, 49 (19),
3083–3086.
https://doi.org/10.1016/j.tetlet.2008.03.053. (24)
Borah, B. J.; Borah, S. J.; Saikia, L.; Dutta, D. K. Efficient Three-Component Coupling Reactions Catalyzed by Cu0Nanoparticles Stabilized on Modified Montmorillonite. Catal. Sci.
Technol.
2014,
4
(4),
1047–1054.
https://doi.org/10.1039/C3CY00639E. (25)
Frindy, S.; El Kadib, A.; Lahcini, M.; Primo, A.; García, H. Copper Nanoparticles Supported on Graphene as an Efficient Catalyst Technol.
for
A3-Coupling 2016,
of
Benzaldehydes.
6
(12),
Catal.
Sci.
4306–4317.
https://doi.org/10.1039/C5CY01414J. (26)
Ramu, V. G.; Bordoloi, A.; Nagaiah, T. C.; Schuhmann,
ACS Paragon Plus Environment
34
Page 35 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
W.; Muhler, M.; Cabrele, C. Copper Nanoparticles Stabilized on Nitrogen-Doped Carbon Nanotubes as Efficient and Recyclable Catalysts for Alkyne/aldehyde/cyclic Amine A 3-Type Coupling Reactions.
Appl.
Catal.
A
Gen.
2012,
431–432,
88–94.
https://doi.org/10.1016/j.apcata.2012.04.019. (27)
Cheng, S.; Shang, N.; Feng, C.; Gao, S.; Wang, C.; Wang, Z.
Efficient
Multicomponent
Synthesis
of
Propargylamines
Catalyzed by Copper Nanoparticles Supported on Metal-Organic Framework Derived Nanoporous Carbon. Catal. Commun. 2017, 89, 91–95. https://doi.org/10.1016/j.catcom.2016.10.030. (28)
Bukowska, A.; Bukowski, W.; Bester, K.; Hus, K. Polymer Supported copper(II) Amine-Imine Complexes in the C-N and A3coupling Reactions. Appl. Organomet. Chem. 2017, 31 (12), 1–15. https://doi.org/10.1002/aoc.3847.
(29)
Kodicherla,
B.;
Perumgani,
P.
C.;
Mandapati,
M.
R.
Polymer-Anchored copper(II) Complex: An Efficient Reusable Catalyst Organomet.
for
the
Synthesis
Chem.
of
2014,
Propargylamines. 28
(10),
Appl.
756–759.
https://doi.org/10.1002/aoc.3193. (30)
Liu, X.; Lin, B.; Zhang, Z.; Lei, H.; Li, Y. Copper(II) Carboxymethylcellulose (CMC-CuII) as an Efficient Catalyst for Aldehyde-Alkyne-Amine Coupling under Solvent-Free Conditions. RSC
Adv.
2016,
6,
94399–94407.
https://doi.org/10.1039/C6RA18742K. (31)
Islam, M. M.; Roy, A. S.; Islam, S. M. Functionalized Polystyrene Supported Copper(I) Complex as an Effective and Reusable Catalyst for Propargylamines Synthesis in Aqueous Medium.
Catal.
Letters
2016,
146
(6),
1128–1138.
https://doi.org/10.1007/s10562-016-1728-3.
ACS Paragon Plus Environment
35
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
(32)
Gholinejad,
M.;
Saadati,
F.;
Page 36 of 45
Shaybanizadeh,
S.;
Pullithadathil, B. Copper Nanoparticles Supported on Starch Micro Particles as a Degradable Heterogeneous Catalyst for Three-Component Coupling Synthesis of Propargylamines. RSC Adv.
2016,
6
(6),
4983–4991.
https://doi.org/10.1039/C5RA22292C. (33)
Li, P.; Wang, L. A Highly Efficient Three-Component Coupling of Aldehyde, Terminal Alkyne, and Amine via C-H Activation
Catalyzed
Organic-Inorganic
by
Reusable
Hybrid
Immobilized
Materials
under
Copper
in
Solvent-Free
Reaction Conditions. Tetrahedron 2007, 63 (25), 5455–5459. https://doi.org/10.1016/j.tet.2007.04.032. (34)
Sreedhar, B.; Surendra Reddy, P.; Vamsi Krishna, C. S.; Vijaya Babu, P. An Efficient Synthesis of Propargylamines Using a Silica Gel Anchored Copper Chloride Catalyst in an Aqueous Medium. Tetrahedron Lett. 2007, 48 (44), 7882–7886. https://doi.org/10.1016/j.tetlet.2007.08.116.
(35)
Wang, M.; Li, P.; Wang, L. Silica-Immobilized NHC-CuI Complex: An Efficient and Reusable Catalyst for A3-Coupling (Aldehyde-Alkyne-Amine)
under
Solventless
Reaction
Conditions. European J. Org. Chem. 2008, No. 13, 2255–2261. https://doi.org/10.1002/ejoc.200800006. (36)
Sadjadi, S.; Heravi, M. M.; Ebrahimizadeh, M. Synthesis of
Cu@Fur-SBA-15
Catalyst Reaction
for
as
a
Promoting
Conditions.
Novel
Efficient
A3-Coupling J.
Porous
and
under Mater.
Heterogeneous
Green
and
2017,
Mild 1–10.
https://doi.org/10.1007/s10934-017-0491-1. (37)
Naeimi,
H.;
Moradian,
M.
Copper(I)-N2S2-Salen
Type
Complex Covalently Anchored onto MCM-41 Silica: An Efficient
ACS Paragon Plus Environment
36
Page 37 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
and Reusable Catalyst for the A3-Coupling Reaction toward Propargylamines. Appl. Organomet. Chem. 2013, 27 (5), 300– 306. https://doi.org/10.1002/aoc.2976. (38)
Gharibpour, Super
N.;
Paramagnetic,
Complexed
Dendrimer:
Propargylamine
Abdollahi-Alibeik, MCM-41-Supported, A
Novel
Synthesis
ChemistrySelect
M.;
Moaddeli,
Recyclable
Nanostructured
Under
2017,
2
Copper-
Catalyst
Solvent-Free
A. for
Conditions.
(10),
3137–3146.
https://doi.org/10.1002/slct.201700180. (39)
Gholinejad, M.; Karimi, B.; Aminianfar, A.; Khorasani, M.
One-Pot
Preparation
of
Propargylamines
Catalyzed
by
Heterogeneous Copper Catalyst Supported on Periodic Mesoporous Organosilica with Ionic Liquid Framework. Chempluschem 2015, 80 (10), 1573–1579. https://doi.org/10.1002/cplu.201500167. (40)
Crudden, C. M.; Sateesh, M.; Lewis, R. MercaptopropylModified Mesoporous Silica: A Remarkable Support for the Preparation of a Reusable, Heterogeneous Palladium Catalyst for Coupling Reactions. J. Am. Chem. Soc. 2005, 127 (28), 10045–10050. https://doi.org/10.1021/ja0430954.
(41)
Guideline on the Specification Limits for Residues of Metal Catalysts or Metal Reagents. EMEA European Medicines Agency: London, 2007.
(42)
Q3D
Elemental
Impurities
Guidance
for
Industry.
International Conference on Harmonisation, U.S. Food and Drug Administration, 2015. (43)
Eremin, D. B.; Ananikov, V. P. Understanding Active Species in Catalytic Transformations: From Molecular Catalysis to
Nanoparticles,
Dynamic
Leaching,
Systems.
“Cocktails”
Coord.
Chem.
of
Catalysts Rev.
and
2017.
ACS Paragon Plus Environment
37
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 38 of 45
https://doi.org/10.1016/j.ccr.2016.12.021. (44)
Yamada, Y. M. A.; Sarkar, S. M.; Uozumi, Y. Amphiphilic Self-Assembled Polymeric Copper Catalyst to Parts per Million Levels: Click Chemistry. J. Am. Chem. Soc. 2012, 134 (22), 9285–9290. https://doi.org/10.1021/ja3036543.
(45)
Aliaga, M. J.; Ramón, D. J.; Yus, M. Impregnated Copper on
Magnetite:
An
Efficient
and
Green
Catalyst
for
the
Multicomponent Preparation of Propargylamines under Solvent Free
Conditions.
Org.
Biomol.
Chem.
2010,
8
(1),
43–46.
https://doi.org/10.1039/b917923b. (46)
Gaikwad, A. V.; Holuigue, A.; Thathagar, M. B.; Ten Elshof,
J.
E.;
Mechanisms
from
Reactions.
Chem.
Rothenberg, Palladium -
A
G.
Ion-
Nanoparticles
Eur.
J.
2007,
and
Atom-Leaching
in
Cross-Coupling
13
(24),
6908–6913.
https://doi.org/10.1002/chem.200700105. (47)
Sahoo,
D.
P.;
Rath,
D.;
Nanda,
B.;
Parida,
K.
M.
Transition Metal/metal Oxide Modified MCM-41 for Pollutant Degradation and Hydrogen Energy Production: A Review. RSC Adv. 2015,
5
(102),
83707–83724.
https://doi.org/10.1039/C5RA14555D. (48)
Brühwiler, Mesoporous
D.
Silica.
Postsynthetic Nanoscale
Functionalization
2010,
2
(6),
of
887–892.
https://doi.org/10.1039/c0nr00039f. (49)
Zhang, L.; Dai, Q.; Qiao, X.; Yu, C.; Qin, X.; Yan, H. Mixed-Mode
Chromatographic
Stationary
Phases:
Recent
Advancements and Its Applications for High-Performance Liquid Chromatography. TrAC - Trends Anal. Chem. 2016, 82, 143–163. https://doi.org/10.1016/j.trac.2016.05.011.
ACS Paragon Plus Environment
38
Page 39 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
(50)
Berger, E.; Hahn, M. W.; Przybilla, T.; Winter, B.; Spiecker, E.; Jentys, A.; Lercher, J. A. Impact of Solvents and Surfactants on the Self-Assembly of Nanostructured Amine Functionalized Silica Spheres for CO2 Capture. J. Energy Chem. 2016,
25
(2),
327–335.
https://doi.org/10.1016/j.jechem.2016.02.005. (51)
Chen, J.; Lyu, Q.; Yang, M.; Chen, Z.; He, J. Selective Elimination of the Free Fatty Acid Fraction from Esterified Fatty Acids in Rat Plasma through Chemical Derivatization and Immobilization on Amino Functionalized Silica Nano-Particles. J.
Chromatogr.
A
2016,
1431,
197–204.
https://doi.org/10.1016/j.chroma.2015.12.078. (52)
Aguado, J.; Arsuaga, J. M.; Arencibia, A.; Lindo, M.; Gascón, V. Aqueous Heavy Metals Removal by Adsorption on Amine-Functionalized 2009,
Mesoporous
163
Silica.
J.
Hazard.
(1),
Mater.
213–221.
https://doi.org/10.1016/j.jhazmat.2008.06.080. (53)
Bois, L.; Bonhommé, A.; Ribes, A.; Pais, B.; Raffin, G.; Tessier,
F.
Functionalized
Silica
for
Heavy
Metal
Ions
Adsorption. Colloids Surfaces A Physicochem. Eng. Asp. 2003, 221
(1–3),
221–230.
https://doi.org/10.1016/S0927-
7757(03)00138-9. (54)
Sadjadi, S.; Heravi, M. M. Current Advances in the Utility of Functionalized SBA Mesoporous Silica for Developing Encapsulated Nanocatalysts: State of the Art. RSC Adv. 2017, 7 (49), 30815–30838. https://doi.org/10.1039/C7RA04833E.
(55)
Rath,
D.;
Rana,
S.;
Parida,
K.
M.
Organic
Amine-
Functionalized Silica-Based Mesoporous Materials: An Update of Syntheses and Catalytic Applications. RSC Adv. 2014, 4
ACS Paragon Plus Environment
39
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 40 of 45
(100), 57111–57124. https://doi.org/10.1039/C4RA08005J. (56)
Jiao, J.; Cao, J.; Xia, Y.; Zhao, L. Improvement of Adsorbent Materials for CO2capture by Amine Functionalized Mesoporous Silica with Worm-Hole Framework Structure. Chem. Eng.
J.
2016,
306,
9–16.
https://doi.org/10.1016/j.cej.2016.07.041. (57)
Min, K.; Choi, W.; Kim, C.; Choi, M. Oxidation-Stable Amine-Containing Adsorbents for Carbon Dioxide Capture. Nat. Commun. 2018, 9 (1), 726. https://doi.org/10.1038/s41467-01803123-0.
(58)
Mafra, L.; Čendak, T.; Schneider, S.; Wiper, P. V.; Pires, J.; Gomes, J. R. B.; Pinto, M. L. Amine Functionalized Porous Silica for CO 2 /CH 4 Separation by Adsorption: Which Amine and Why. Chem. Eng. J. 2018, 336 (October 2017), 612– 621. https://doi.org/10.1016/j.cej.2017.12.061.
(59)
Lam, K. F.; Yeung, K. L.; Mckay, G. A Rational Approach in the Design of Selective Mesoporous Adsorbents. Langmuir 2006, 4 (17), 9632–9641.
(60)
Martins, A. R.; Salviano, A. B.; Oliveira, A. A. S.; Mambrini,
R.
V.;
Characterization Partially
of
Moura, Catalysts
Hydrophobized
Environ.
Sci.
for
Pollut.
F.
C.
Based
C. on
Synthesis
Mesoporous
Technological Res.
and
Silica
Applications.
2016,
1–11.
https://doi.org/10.1007/s11356-016-6692-3. (61)
Grün, M.; Unger, K. K.; Matsumoto, A.; Tsutsumi, K. Novel Pathways for the Preparation of Mesoporous MCM-41 Materials : Control of Porosity and Morphology. Microporous Mesoporous Mater.
1999,
27,
207–216.
https://doi.org/10.1016/S1387-
1811(98)00255-8.
ACS Paragon Plus Environment
40
Page 41 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
(62)
Kresge, C. T.; Leonowicz, M. E.; Roth, W. J.; Vartuli, J.
C.;
Beck,
J.
S.
Ordered
mesoporous
molecular
sieves
synthesized by a liquid-crystal template mechanism. Nature 1992, 359, 710–712. https://doi.org/10.1038/359710a0. (63)
Beck, J. S.; Schmitt, K. D.; Higgins, J. B.; Schlenkert, J. L. A New Family of Mesoporous Molecular Sieves Prepared with Liquid Crystal Templates. J. Am. Chem. Soc. 1992, 114, 10834–10843. https:/doi.org/ 10.1021/ja00053a020.
(64)
Zapata,
P.
A.;
Huang,
Y.;
Gonzalez-Borja,
M.
A.;
Resasco, D. E. Silylated Hydrophobic Zeolites with Enhanced Tolerance to Hot Liquid Water. J. Catal. 2013, 308, 82–97. https://doi.org/10.1016/j.jcat.2013.05.024. (65)
Cerveny, S.; Schwartz, G. a.; Otegui, J.; Colmenero, J.; Loichen, J.; Westermann, S. Dielectric Study of Hydration Water in Silica Nanoparticles. J. Phys. Chem. C 2012, 116 (45), 24340–24349. https://doi.org/10.1021/jp307826s.
(66)
Smith, M. E.; MacKenzie, K. Silicon-29 NMR. Multinucl. Solid-state
NMR
Inorg.
Mater.
2002,
6
(C),
201–268.
https://doi.org/10.1016/S1470-1804(02)80005-0. (67)
Babonneau, F.; Baccile, N.; Laurent, G.; Maquet, J.; Azaïs, T.; Gervais, C.; Bonhomme, C. Solid-State Nuclear Magnetic
Resonance:
A
Valuable
Tool
to
Explore
Organic-
Inorganic Interfaces in Silica-Based Hybrid Materials. Comptes Rendus
Chim.
2010,
13
(1–2),
58–68.
https://doi.org/10.1016/j.crci.2009.08.001. (68)
de Lima, C.
M.;
Mota,
a L.; Mbengue, C.
J.
a.
a; San Gil, R. a S.; Ronconi,
Synthesis
of
Amine-Functionalized
Mesoporous Silica Basic Catalysts for Biodiesel Production. Catal.
Today
2014,
226,
210–216.
https://doi.org/DOI
ACS Paragon Plus Environment
41
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 42 of 45
10.1016/j.cattod.2014.01.017. (69)
Thommes, M.; Kaneko, K.; Neimark, A. V.; Olivier, J. P.; Rodriguez-Reinoso, Physisorption
of
F.;
Rouquerol,
Gases,
with
J.;
Special
Sing,
K.
Reference
S. to
W. the
Evaluation of Surface Area and Pore Size Distribution (IUPAC Technical Report). Pure Appl. Chem. 2015, 87 (9–10), 1051– 1069. https://doi.org/10.1515/pac-2014-1117. (70)
Moulder, J. F.; Stickle, W. F.; Sobol, P. E.; Bomben, K. D. Handbook of X-Ray Photoelectron Spectroscopy; Chastain, J.; King, R.C. Physical Electronics: Eden Prairie, MN, 1995.
(71)
Choi, Y. J.; Jang, H. Y. Copper-Catalyzed A3-Coupling: Synthesis of 3-Amino-1,4-Diynes. European J. Org. Chem. 2016, 18, 3047–3050. https://doi.org/10.1002/ejoc.201600343.
(72)
Bereczki, H. F.; Daróczi, L.; Fábián, I.; Lázár, I. SolGel Synthesis, Characterization and Catalytic Activity of Silica Aerogels Functionalized with copper(II) Complexes of Cyclen and Cyclam. Microporous Mesoporous Mater. 2016, 234, 392–400. https://doi.org/10.1016/j.micromeso.2016.07.026.
(73)
Yu, C.; He, J. Synergic Catalytic Effects in Confined Spaces.
Chem.
Commun.
2012,
48
(41),
4933–4940.
https://doi.org/10.1039/c2cc31585h. (74)
Derouane, E. G. The Energetics of Sorption by Molecular Sieves: Surface Curvature Effects. Chem. Phys. Lett. 1987, 142 (3–4), 200–204. https://doi.org/10.1016/0009-2614(87)80922-3.
(75)
Derouane, E. G.; Nagy, J. B. Reply To “comments on Diffusion
of
Alkanes
in
Molecular
Sieves:
Evidence
for
Confinement Effects.” Appl. Catal. 1989, 52 (1), 169–170. https://doi.org/10.1016/S0166-9834(00)83381-3.
ACS Paragon Plus Environment
42
Page 43 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
(76)
Derycke, I.; Vigneron, J. P.; Lambin, P.; Lucas, A. A.; Derouane, E. G. Physisorption in Confined Geometry. J. Chem. Phys.
1991,
94
(6),
4620–4627.
https://doi.org/10.1063/1.460590. (77)
Sastre, Zeolites.
J.
G.;
Corma,
A.
Mol.
Catal.
A
The
Confinement
Chem.
2009,
305
Effect (1–2),
in 3–7.
https://doi.org/10.1016/j.molcata.2008.10.042. (78)
Goettmann, F.; Sanchez, C. How Does Confinement Affect the Catalytic Activity of Mesoporous Materials? J. Mater. Chem. 2007, 17 (1), 24. https://doi.org/10.1039/b608748p.
(79)
Choi, I. H.; Bin Yoon, S.; Huh, S.; Kim, S. J.; Kim, Y. Photophysical Properties of Cationic Dyes Captured in the Mesoscale Channels of Micron-Sized Metal-Organic Framework Crystals.
Sci.
Rep.
2018,
8
(1),
1–12.
https://doi.org/10.1038/s41598-018-28080-y. (80)
Patra, S.; Pandey, A. K.; Sarkar, S. K.; Goswami, A. Wonderful
Nanoconfinement
Equilibrium.
RSC
Adv.
Effect 2014,
on 4
Redox
(63),
Reaction
33366–33369.
https://doi.org/10.1039/c4ra05104a. (81)
Herrmann, S.; Iglesia, E. Elementary Steps in Acetone Condensation Diverse
Void
Reactions
Catalyzed
Structures.
J.
by
Catal.
Aluminosilicates 2017,
346,
with
134–153.
https://doi.org/10.1016/j.jcat.2016.12.011. (82)
Bosica,
G.;
Gabarretta,
J.
Unprecedented
One-Pot
Multicomponent Synthesis of Propargylamines Using Amberlyst A-21 Supported CuI under Solvent-Free Conditions. RSC Adv. 2015,
5
(57),
46074–46087.
https://doi.org/10.1039/C5RA05546F.
ACS Paragon Plus Environment
43
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
(83)
Page 44 of 45
Xiong, X.; Chen, H.; Zhu, R. Highly Efficient and Scaleup Synthesis of Propargylamines Catalyzed by Graphene OxideSupported CuCl2 catalyst under Microwave Condition. Catal. Commun.
2014,
54,
94–99.
https://doi.org/10.1016/j.catcom.2014.05.030.
ACS Paragon Plus Environment
44
Page 45 of 45 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
FOR TABLE OF CONTENTS USE ONLY
A3-coupling reaction happens with low catalyst load and yields lowcontaminated product, limiting the use of metal and eliminating the need for product purification.