Subscriber access provided by READING UNIV
Article
Bacterial Adhesion to Ultrafiltration Membranes: Role of Hydrophilicity, Natural Organic Matter, and Cell-Surface Macromolecules Sara BinAhmed, Anissa Hasane, Zhaoxing Wang, Aslan Mansurov, and Santiago Romero-Vargas Castrillón Environ. Sci. Technol., Just Accepted Manuscript • DOI: 10.1021/acs.est.7b03682 • Publication Date (Web): 28 Nov 2017 Downloaded from http://pubs.acs.org on December 1, 2017
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Environmental Science & Technology is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 35
1 2 3 4 5
Environmental Science & Technology
Bacterial Adhesion to Ultrafiltration Membranes: Role of Hydrophilicity, Natural Organic Matter, and Cell-Surface Macromolecules Sara BinAhmed1, Anissa Hasane2, Zhaoxing Wang1, Aslan Mansurov1, Santiago Romero-Vargas Castrillón* 1
6 7 8 9 10
1
11
Abstract
12
Insight into the mechanisms underlying bacterial adhesion is critical to the formulation of
13
membrane biofouling control strategies. Using AFM-based single-cell force spectroscopy, we
14
investigated the interaction between Pseudomonas fluorescens, a biofilm-forming bacterium,
15
and polysulfone (PSF) ultrafiltration (UF) membranes to unravel the mechanisms underlying
16
early-stage membrane biofouling. We show that hydrophilic polydopamine (PDA) coatings
17
decrease bacterial adhesion forces at short bacterium-membrane contact times. Further, we find
18
that adhesion forces are weakened by the presence of natural organic matter (NOM)
19
conditioning films, owing to the hydrophilicity of NOM. Investigation of the effect of adhesion
20
contact time revealed that PDA coatings are less effective at preventing bioadhesion when the
21
contact time is prolonged to 2 – 5 s, or when the membranes are exposed to bacterial
22
suspensions under stirring. These results therefore challenge the notion that simple hydrophilic
23
surface coatings are effective as a biofouling control strategy. Finally, we present evidence that
24
adhesion to the UF membrane surface is mediated by cell-surface macromolecules (likely to
25
be outer membrane proteins and pili) which, upon contacting the membrane, undergo surface-
26
induced unfolding.
27
Keywords. adhesion, biofouling, polydopamine, NOM, Pseudomonas fluorescens, single-cell
28
force spectroscopy, ultrafiltration.
Department of Civil, Environmental, and Geo- Engineering, University of Minnesota, 500 Pillsbury Dr SE, Minneapolis, MN 55455, United States 2 Department of Civil and Environmental Engineering, Norwegian University of Science and Technology, 7491 Trondheim, Norway
1 ACS Paragon Plus Environment
Environmental Science & Technology
29
1. Introduction
30
The presence of bacteria near interfaces is ubiquitous in natural and engineered aqueous
31
environments. Near most surfaces, adhered bacteria will aggregate in a hydrated matrix of
32
proteins and polysaccharides, known as biofilms1. These sessile communities are notoriously
33
resistant to removal by biocides and disinfectants due to the protection provided by a matrix of
34
predominantly self-produced extracellular polymeric substances (EPS)2–5. Consequently,
35
biofilm formation and biofouling constitute a major technical problem in membrane-based
36
water treatment, leading to decreased permeance, selectivity, and membrane useful life6–11. The
37
first step in biofilm formation and biofouling, termed bioadhesion, is the complex process of
38
bacterial attachment to a substrate12–14. A variety of nonspecific interactions drive
39
bioadhesion12,15,16 including long-range electrostatic forces14,17,18, and shorter ranged
40
hydrophobic14,van der Waals14,17, and hydrogen bond interactions17. These interactions come
41
into play through a host of bacterial cell membrane macromolecules (e.g., lipopolysaccharides,
42
proteins19), as well as cell-surface adhesins (e.g., pili and flagella) that often determine bacterial
43
adhesion to the substrate20–23. Cell appendages such as flagella and pili play a major role in
44
overcoming repulsive double layer surface forces, initiating bacterial attachment4,13,14, often at
45
several m from the substrate15.
46 47
Given that bioadhesion interactions are reversible24, insight into the mechanisms underlying
48
early-stage bacterial attachment is essential to the formulation of biofouling-resistant
49
membranes and biofouling prevention strategies. Nonetheless, given the myriad physical,
50
chemical, and biological factors intervening, bioadhesion remains a poorly understood
51
phenomenon, particularly for chemically heterogeneous interfaces such as membranes for
52
water separations, which exist in contact with complex solution matrices25. Earlier studies on
53
bioadhesion onto model polymeric (e.g., Teflon) and inorganic surfaces (glass, mica) have
2 ACS Paragon Plus Environment
Page 2 of 35
Page 3 of 35
Environmental Science & Technology
54
shown that attachment is enhanced by substrate hydrophobicity15,26. Several other interfacial
55
properties influence bacterial adhesion, including nanoscale roughness and surface charge (zeta
56
potential), as well as feed water composition (pH, ionic strength, presence of divalent cations,
57
organic matter properties), all of which are known to contribute to membrane fouling5,6,11–
58
14,27,28
.
59 60
In addition, transport and deposition of bacterial polymers, natural organic matter (NOM), and
61
other macromolecules at the substrate-water interface is thought to lead to the formation of a
62
conditioning film mainly composed of organic matter29 that may hinder29–31, or promote30,32,33
63
bacterial adhesion by providing support and nutrients for the foundation layer of a
64
biofilm13,14,20,34. The role of NOM in bacterial and biocolloid adhesion is poorly understood,
65
with previous studies reporting contradictory results31,35–39. Suwannee River (SR) NOM
66
conditioning films decrease the attachment efficiency of MS2 virus particles to silica surfaces,
67
possibly due to electrostatic repulsive forces that dominate at low ionic strength31. Conversely,
68
at low ionic strengths, SRNOM was shown to accelerate the deposition kinetics of C. parvum
69
oocysts on conditioned silica surfaces, compared to bare silica collectors35. Other studies
70
focused on the effect of humic acid (HA), the main hydrophobic36 constituent of NOM37 in
71
surface water38. HA had a minor influence on the attachment efficiency of E. coli cells to silica
72
particles36, while Suwannee River humic acid (SRHA) resulted in lower deposition of E. coli
73
on quartz sand when present in suspension or as a coating film37. On the other hand, the effect
74
of HA conditioning on Pseudomonas aeruginosa adhesion was found to be dependent on
75
lipopolysaccarride (LPS) structure. Adhesion of P. aeruginosa AK 1401, having an A-band
76
antigen in its LPS, exhibited similar adhesion forces to HA-coated silica particles as the bare
77
silica surfaces. Conversely, P. aeruginosa PAO1 possesses an additional long antigen (B-band)
78
that increased its adhesion to HA-coated silica39.
3 ACS Paragon Plus Environment
Environmental Science & Technology
79
Advanced surface analytical techniques, notably AFM-based single cell force spectroscopy
80
(SCFS), have emerged in recent years to investigate the mechanisms underlying bacterial
81
adhesion. In SCFS, an AFM cantilever is functionalized with a single bacterial cell, enabling
82
measurement of the nanoscale forces between individual cells and a substrate in native aqueous
83
environments16,40. In addition, SCFS can provide information on the mechanical response of
84
cell adhesins as they contact a substrate41,42.
85 86
In this study, we use SCFS to unravel the interactions between Pseudomonas fluorescens, a
87
biofilm-forming bacterium21,43, and polymeric ultrafiltration (UF) membranes. P. fluorescens
88
is an aerobic gram negative bacterium found in soil, drinking and river water, plants, in addition
89
to biomedical and industrial equipment25,44–46. We show that hydrophilic polydopamine (PDA)
90
surface coatings significantly weaken the adhesion forces of P. fluorescens. While this
91
observation underscores the importance of hydrophilicity in mitigating microbial adhesion, we
92
also show that the antifouling properties of hydrophilic coatings are less effective for prolonged
93
contact between the cell and the membrane surface. Further, we show that NOM conditioning
94
films weaken cell-substrate adhesion forces. Finally, a significant fraction of the force
95
measurements suggests that adhesion of P. fluorescens is mediated by cell surface appendages
96
whose elastic response can be modeled via the worm-like chain (WLC) model. Our WLC
97
analysis of adhesion forces suggests that unfolding of adhesins (pili and outer membrane
98
proteins) is a determinant of cell attachment to membrane surfaces.
99 100
2. Materials and Methods
101
2.1. Membrane Fabrication and Characterization
102
We investigate bioadhesion on polysulfone UF membranes fabricated by non-solvent induced
103
phase inversion47. Hydrophilic polydopamine48 (PDA) surface coatings, which have been
4 ACS Paragon Plus Environment
Page 4 of 35
Page 5 of 35
Environmental Science & Technology
104
shown to be effective in the control of membrane organic fouling49, are explored in this work
105
as a surface modification strategy to mitigate bioadhesion27. Polydopamine is formed by the
106
deposition of 3,4-dihydroxyphenylalanine (DOPA) from alkaline solution48. Hereinafter, we
107
refer to PDA-coated polysulfone UF membranes as PSF-PDA, while the unmodified
108
polysulfone control membranes are designated PSF membranes. In addition, the effect of NOM
109
conditioning films is investigated by depositing Upper Mississippi River NOM (International
110
Humic Substances Society, St. Paul, MN) on the membrane surfaces via pressure-driven
111
filtration of 10 ppm NOM solution.
112
The interfacial properties (wettability, surface charge and nanoscale roughness) and water
113
permeability coefficient of the PSF and PSF-PDA membranes were characterized. Detailed
114
experimental procedures and characterization data are presented in the Supporting Information
115
(SI).
116 117
2.2. Single-Cell Force Spectroscopy (SCFS) Experiments
118
2.2.1. Bacterial Strain and Growth Conditions
119
The strain of P. fluorescens used in our experiments, ATCC 13525, originates from pre-filter
120
tanks50. As with other bacteria in the Pseudomonas genus, P. fluorescens has a high
121
adaptation51 and biofilm formation potential43,52, possessing a variety of proteinaceous
122
adhesins53, such as flagella and pili, which are also fundamental to bacterial motility44,54. The
123
small radius of pili (1-5 nm55) is believed to help P. fluorescens overcome electrostatic
124
repulsive forces with the substrate13,55. Pili also promote P. fluorescens bioadhesion via
125
hydrophobic interactions with hydrophobic substrates55, due to the high content of hydrophobic
126
amino acids in the constituent pilin proteins56. LPS23,57,58 and outer membrane proteins
127
(OMP)14,39, such as LapA20,21, also contribute to adhesion of P. fluorescens. Experimental
128
details on bacterial culture preparation and growth conditions are provided in the SI.
5 ACS Paragon Plus Environment
Environmental Science & Technology
129
2.2.2. Membrane sample and cantilever preparation
130
A UF membrane coupon (~3×3 mm2) was glued using epoxy (3M Quick Set Epoxy Adhesive)
131
to a piranha-cleaned and UV/O3-treated glass disc, and allowed to set for 10 minutes.
132
Subsequently, a 20-µL droplet of bacterial suspension was deposited directly on the glass,
133
allowing the droplet to stand for 30 minutes to permit bacterial attachment to the glass surface.
134
The glass disk was rinsed with 2.5 mL PBS to remove unattached bacteria, avoiding contact
135
between the membrane surface and the bacterial suspension. Finally, the glass disk was inserted
136
in the fluid cell (Fluid Cell Lite, Asylum Research), and the cell was filled with 1.4 mL of test
137
solution. We conducted experiments in PBS or in 10 ppm NOM solution containing 156.4 mM
138
KCl and 0.5 mM CaCl2 (I = 158 mM, pH 7.2-7.4), i.e., conditions approximating those of PBS,
139
to perform experiments under comparable conditions.
140 141
Tipless SiN cantilevers (nominal k = 0.01 N/m, MLCT-O10 probe “C”, Bruker) were used.
142
Wet polydopamine (wPDA) was used as a wet adhesive to immobilize a single bacterial cell
143
on the cantilever, as done by others15,19,59,60. The adhesive properties of wPDA, which contrast
144
the antifouling properties of PDA explored in this work (and previously by others49,61,62), are
145
thought to depend on the degree of pH-induced oxidation of DOPA catechol groups to
146
quinones63–65, and the extent of crosslinking of DOPA monomers48,66. In our work, we observed
147
that longer deposition times on the membranes (~45 min) resulted in hydrophilic anti-fouling
148
coatings, whereas shorter (15 minutes) deposition times rendered adhesive cantilevers on
149
which bacterial cells could be robustly immobilized. We further observed that wPDA coatings
150
completely lost their adhesiveness after ~3 hours, possibly due to conversion to non-adhesive
151
(oxidized) PDA. Determination of the structures of adhesive wPDA and non-adhesive PDA,
152
as well as their formation mechanisms, are active areas of research67–69 that fall outside of the
153
scope of this study.
6 ACS Paragon Plus Environment
Page 6 of 35
Page 7 of 35
Environmental Science & Technology
154 155
To ensure adhesiveness of the wPDA, the AFM probes were coated immediately before each
156
experiment as follows: the UV/O3-cleaned AFM probe was immersed in 10 mL of 4 g/L PDA
157
solution (pH 8.5) prepared as described in the SI. After 15 minutes under shaking at 60 RPM,
158
the probe was rinsed with deionized (DI) water (18.2 M-cm, Barnstead) and dried under a
159
gentle nitrogen flow before mounting the probe on the AFM probe holder. The head was then
160
lowered into the fluid cell, immersing the probe in the solution (PBS or NOM) and allowing
161
the cantilever deflection to reach a stable deflection signal (which was typically observed
162
within 30-60 min).
163 164
2.2.3. Force Measurements
165
Single-cell force spectroscopy (SCFS) was performed at room temperature using an MFP-3D-
166
Bio atomic force microscope (Asylum Research, Santa Barbara, CA) integrated into a Zeiss
167
Axio Observer A.1 inverted optical microscope (IOM). The cantilever spring constant was
168
obtained using the thermal noise method70, and was always found to be within range specified
169
by the manufacturer. The optical lever sensitivity of the cantilever was determined from the
170
slope of the contact region of deflection signal (V) vs. piezo extension (nm) curves collected
171
over the bare glass. To immobilize a single bacterial cell on the cantilever, we adapted
172
previously reported experimental procedures15,19. Using the 60× objective of the IOM, the
173
wPDA-coated cantilever was directed towards a cell aligned parallel to the front edge of the
174
cantilever. The cantilever was engaged in contact mode over the cell for 5 minutes with a 1 nN
175
loading force15, after which the cantilever (functionalized with the bacterial cell) was
176
withdrawn.
177
7 ACS Paragon Plus Environment
Environmental Science & Technology
178
To begin force measurements, the cantilever was translated towards the membrane surface
179
using the AFM top view digital camera. Approach-retraction force cycles were recorded at a
180
400 nm/s cantilever speed and 4 µm ramp (8-µm ramps were used when long range interactions
181
were observed), with an approach (target loading) force of 600 pN. A dwell or contact time (0
182
≤ tContact ≤ 5 s), defined as the time in which the bacterial cell can remain in contact with the
183
membrane surface under a constant loading force, was investigated in a subset of the
184
experiments. Experiments in NOM solution and/or conditioning film were carried out at tContact
185
= 5 s only. Force curves were collected at multiple randomly chosen locations of the
186
membranes, measuring 3 force curves over each point, to minimize the deposition of cell-
187
surface macromolecules on the UF membrane (no systematic changes in adhesion force were
188
observed in sequential measurements on the same membrane location, or between locations).
189
A total of 100 force curves (minimum: 93, maximum: 129) were collected for each
190
combination of membrane type and experimental conditions, using at least 3 different bacterial
191
cells (i.e., at least 3 separate single-cell experiments). Both approach and pull-off force curves
192
were measured, but only pull-off force curves were considered to quantify adhesion. Raw data
193
in terms of cantilever deflection as a function of piezo Z position were first converted to force
194
versus cell-substrate separation curves using the method described by Senden71. The maximum
195
adhesion force and rupture separation (i.e., the separation at which cell-substrate forces vanish)
196
were extracted from each pull-off force curve using a Matlab code. A representative
197
approach/pull-off force cycle, showing the maximum adhesion force and rupture separation, is
198
shown in Figure S1.
199 200
Cell viability was assessed after each experiment using a live/dead assay (Baclight,
201
Thermofisher Scientific) consisting of SYTO 9 and propidium iodide (PI) fluorescent nucleic
202
acid stains. If the cell was dead (red fluorescence) or dislocated (i.e., if the cell position on the
8 ACS Paragon Plus Environment
Page 8 of 35
Page 9 of 35
Environmental Science & Technology
203
cantilever changed during the experiment), the collected data were discarded. Only data
204
collected with a live cell (green fluorescence) that remained at its initial location throughout
205
the experiment are reported herein.
206 207
3. Results and Discussion
208
3.1. Membrane Characterization
209
3.1.1. Contact Angle
210
Contact angle provides information about the hydrophilicity of the membranes, a well-known
211
attribute of fouling-resistant surfaces3,33,72,73. Contact angle measurements of an ultrapure water
212
droplet on various membrane surfaces are shown in Figure 1. The contact angle of PSF
213
membranes was θ = 62.7° ± 7.4°. A more hydrophilic surface results from PDA deposition,
214
which exhibits a contact angle θ = 51.5° ± 5.7°; the observed increase in hydrophilic character
215
of the PSF-PDA membrane is consistent with previous results of PSF-PDA-modified
216
membranes73 and other organic and inorganic63,66,74–76 substrates. Figure 1 also shows that both
217
the PSF and PSF-PDA membranes are rendered more hydrophilic after deposition of an NOM
218
conditioning film, when compared to their NOM-free counterparts. This can be attributed to
219
the hydrophilic components of NOM, which have been shown to render membrane surfaces
220
more hydrophilic after fouling experiments77. The hydrophilic components of NOM are
221
believed to be non-humic substances77 such as polysaccharides78,79 and proteins79. The
222
presence of polysaccharides on NOM-conditioned PSF and PSF-PDA membranes is supported
223
by FTIR data (Figures S2 and S3), showing an increase in the ~1078 cm-1 and 1105 cm-1 bands,
224
corresponding to polysaccharides and polysaccharide-like molecules78,80.
225
9 ACS Paragon Plus Environment
Environmental Science & Technology
Page 10 of 35
Contact Angle (deg.)
80 70
62.7 51.8 51.5
60 50
35.5
40 30 20 10 0
PSF
226 227 228 229 230 231 232 233
PSF -PDA
PSF -NOM
PSF-PDA -NOM
Figure 1: Sessile water drop contact angle measurements on PSF and PSF-PDA membranes, both pristine and coated with an NOM film (as described in the Supporting Text). For each membrane type, the reported contact angle is an average of at least 18 measurements, collected over 2 separately cast membrane samples of the same type; error bars indicate one standard deviation (p < 0.05 for all pairwise comparisons, except for PSF-PDA compared to PSF-NOM). 3.1.2. Zeta Potential
234
The charging behavior of a solid-water interface, as revealed by streaming potential
235
measurements, provides information about the functional groups present on the membrane
236
surface, as well as surface charges that influence cell deposition. The zeta potential () of PSF,
237
PSF-PDA, and NOM-conditioned membranes is shown in Figure S4 as a function of pH. PSF
238
membranes exhibited a negative over the entire pH range (4 to 10), due to OH- adsorption on
239
the PSF membrane surface49. In contrast, PSF-PDA membranes attained a positive zeta
240
potential at pH < 4.5, due to protonation of –NH– to –NH2+– in PDA. At basic pH,
241
deprotonation of hydroxyl groups in PDA results in negative zeta potential49. Figure S4 further
242
shows that the NOM conditioning film results in negative over the entire pH range
243
investigated for both PSF and PSF-PDA membranes. This is consistent with the presence of
244
polysaccharides and polysaccharide-like substances that increase the number of negatively
245
charged functional groups on the membrane surface78. The deposition of negatively charged
246
humic acid (HA), alginate (a polysaccharide), and a combination of HA and alginate has been
247
shown to decrease (i.e., render more negative) the zeta potential of polyethersulfone (PES) UF
248
membranes79. Comparing the four membrane types, Figure S4 shows that at low pH (pH < 5)
10 ACS Paragon Plus Environment
Page 11 of 35
Environmental Science & Technology
249
the zeta potential of NOM-conditioned membranes is lower (more negative) than that of
250
pristine PSF and PSF-PDA membranes. On the other hand, all membranes exhibit similar
251
surface charge at pH 7.2-7.4, the pH of our SCFS experiments (Section 3.2), irrespective of
252
NOM-conditioning or PDA surface modification.
253 254
We also measured the zeta potential of P. fluorescens cells (Figure S5, details in the SI).
255
Bacterial cells attain a negative surface charge at pH values corresponding to their normal
256
living environment2,81. As shown in Figure S5, bacteria exhibit a negative zeta potential at pH
257
7.2-7.4, becoming less negative with increasing ionic strength82–84 due to electrical double layer
258
compression82,83. Figure S5 also shows that the zeta potential of P. fluorescens was the same
259
when suspended in PBS or NOM solution, suggesting that both solutions yield similar
260
screening of bacterial surface charge at comparable ionic strength. This observation agrees with
261
the work of Yang et al.37, who found that the zeta potential of motile and nonmotile E. coli was
262
the same in the presence and absence of SRHA. Interestingly, the zeta potential of P.
263
fluorescens was approximately the same as that of the cell-free NOM solution, possibly due to
264
the presence of similar functional groups (e.g., carboxylates) in NOM and the surface of
265
bacteria.
266 267
In summary, Figures S4 and S5 show that both the bacterial and membrane surfaces possess
268
negative zeta potentials under the conditions of the SCFS experiments reported below,
269
irrespective of the presence of NOM or (for the membranes) PDA surface coating.
270 271
3.1.3. Roughness and Permeability
272
Figure S6 presents AFM images of PSF and PSF-PDA membranes. The root-mean-squared
273
(RMS) roughness, defined as the standard deviation of height z-values measured over the
11 ACS Paragon Plus Environment
Environmental Science & Technology
Page 12 of 35
274
scanned area85,86, was calculated from the AFM images. The RMS roughness of PSF and PSF-
275
PDA membranes was 2.45 ± 0.32 nm and 3.74 ± 1.44 nm, respectively. The slight increase in
276
roughness of PSF-PDA is presumed to be due to PDA nanoscale aggregates formed during
277
deposition49. The permeability coefficients of the membranes presented in Figure S7, are within
278
the range expected for UF membranes87,88. The slightly higher permeability of PSF-PDA
279
membranes can be attributed to the increased hydrophilicity of the PDA layer covering both
280
the membrane surface and the inner walls of the pores62.
281 282
3.2. Single-Cell Force Spectroscopy
283
In this section, we systematically investigate the effects of UF membrane hydrophilicity, cell-
284
substrate contact time, and NOM conditioning on the adhesion of P. fluorescens to polysulfone
285
UF membranes. Given the stochastic nature of microbial adhesion19,59, raw data (maximum
286
adhesion force and rupture separation, cf. Figure S1 for definition) are reported as histograms
287
(see SI).
288 289
3.2.1. Effect of Membrane Hydrophilicity and Contact Time
290
The adhesion of single P. fluorescens cells on polysulfone (PSF) and polydopamine-coated
291
polysulfone (PSF-PDA) membrane surfaces is investigated at contact times (tContact) of 0, 2 and
292
5 s in Figure 2 (A) and (B), which report the average maximum adhesion force and rupture
293
separation, respectively. All experiments were performed in PBS buffer, pH 7.4, at room
294
temperature. The histograms of the maximum adhesion force (Figure S8) and rupture
295
separation (Figure S9), from which Figure 2 was obtained, show broad distributions, derived
296
from complex interactions between the membrane and biopolymers present on the cell surface
297
(see Section 3.2.3). By contrast, cell-free control measurements (Figures S10-S15) between a
298
wPDA-coated cantilever and the membrane surface showed significantly higher average
12 ACS Paragon Plus Environment
Page 13 of 35
Environmental Science & Technology
299
adhesion forces (~1 nN, compared to forces < 1 nN with bacterial probes, cf. Figure S12) and
300
much shorter rupture distances (~100 nm, compared to rupture at > 1 m with bacterial probes,
301
cf. Figure S15), demonstrating that the forces presented in Figures 2 (A) and S8 are due to
302
bacterium-membrane interactions.
303 304
Figures 2 (A) and S8 show that the distribution of adhesion force measurements became
305
broader, i.e., the average adhesion force increased, as tContact increased from 0 to 5 s. Similarly,
306
Figure S8 shows that the fraction of predominantly repulsive forces (corresponding to the
307
column labeled “NO”) decreased with increasing contact time over both PSF and PSF-PDA
308
membranes. In these instances, attractive forces were too weak (on the order of 40 pN or less),
309
and could not be discriminated from the random fluctuations in the deflection of the cantilever
310
about zero force. Data on Figure 2 (A) thus show that adhesion of bacteria to membrane
311
surfaces is a time-dependent phenomenon15, irrespective of the membrane chemistry, with
312
bacterial cells adhering more strongly to a surface when a sufficiently prolonged contact time
313
is allowed. The higher mean adhesion force at longer tContact suggests that adhesins undergo
314
structural changes that strengthen attachment on contacting the membrane surface. The range
315
of tContact explored in Figure 2 (0 – 5 s) is shorter than the particle-substrate contact times
316
encountered in membrane filtration, which would exceed the hydraulic residence time of the
317
feed channel (> 10 s for typical module sizes and crossflow velocities of 10 cm s-1 89,90), but
318
nonetheless suffices to observe surface-induced conformational changes in bacterial adhesins,
319
which occur over times scales of ~100 – 700 ms 91. An important observation in Figure 2 (A)
320
is that average adhesion forces over PDA-coated membranes were always weaker than those
321
measured on PSF membranes at the same tContact. This is due to the interfacial properties of the
322
pristine and PDA-coated polysulfone membranes. The surface charge of both PSF and PSF-
323
PDA membranes is similar ( -25 mV at pH 7.4, Figure S4), and the bacterial zeta potential is
13 ACS Paragon Plus Environment
Environmental Science & Technology
Page 14 of 35
324
also weakly negative ( -5 mV, extrapolating data in Figure S5 to the ionic strength of PBS).
325
Further, both membranes have similarly low (< 4 nm) RMS surface roughness (Figure S6).
326
These results suggest that the weaker adhesion on PDA-coatings does not stem from surface
327
electrostatic interactions or nanoscale roughness, but rather from the increased hydrophilicity
328
of PSF-PDA membranes (= 51.5º ± 5.7º, compared to = 62.7º ± 7.4º for PSF, p < 0.05, cf.
329
Figure 1). Stronger bioadhesion on more hydrophobic substrates (PSF in this case) has been
330
reported by different studies using various bacterial strains13–15,26,59. Our results therefore
331
indicate that P. fluorescens uses adhesins (probably of proteinaceous nature, such as pili and
332
outer membrane proteins53) that depend on surface hydrophobicity for interaction.
333 334
Figure 2 (B) presents the mean rupture separation (defined as the distance at which the adhesion
335
force vanishes, cf. Figure S1), obtained from the distributions shown in Figure S9. Long rupture
336
separations, reaching up to 9 µm, were observed in some measurements (Figure S9), which can
337
be explained by the presence of long flagella and pili in P. fluorescens15,54,56,92,93. For both PSF
338
and PSF-PDA, longer rupture separations were recorded as tContact was increased from 0 to 2 s,
339
but remained unchanged (or increased slightly for PSF-PDA) on increasing tContact to 5 s. The
340
increase in average rupture separation as tContact was varied from 0 to 2 s indicates that at longer
341
tContact, longer adhesins (possibly pili) mediated attachment or more contact points along a
342
single pili were established. Beyond 2 seconds, the rupture separation did not vary significantly
343
but the adhesion became stronger (Figure 2 (A)), suggesting that more adhesins of similar
344
length were involved15. Additionally, we note that average rupture separation was always
345
smaller over PSF-PDA compared to PSF membranes for the same tContact (Figure 2 (B)). This
346
observation is analogous to the stronger adhesion observed on PSF compared to PSF-PDA
347
surfaces (Figure 2 (A)), suggesting that adhesins can engage more binding sites on the (more
348
hydrophobic) PSF membrane surface, resulting in longer rupture separation distances.
14 ACS Paragon Plus Environment
Page 15 of 35
Environmental Science & Technology
|Mean Adhesion Force| (nN)
349
1.0
tContact = 0 s tContact = 2 s tContact = 5 s
A
0.8
0.6
0.4
0.2
0.0
PSF-PDA
PSF
Mean Rupture Separation (m)
350
4.0
B
tContact = 0 s tContact = 2 s tContact = 5 s
3.5 3.0 2.5 2.0
*
*
1.5
*
1.0
*
0.5 0.0
PSF
PSF-PDA
351 352 353 354 355 356
Figure 2: Average maximum adhesion force (A) and mean rupture separation (B) of single P. fluorescens cells on PSF and PSF-PDA membranes investigated for different contact times (tContact) denoted in the inset. The histograms from which the reported means were computed are given in Figures S8 and S9 (p < 0.05, except for pairwise comparisons indicated by *).
357
3.2.2. Effect of NOM on Microbial Adhesion
358
To investigate the effect of NOM on microbial adhesion, we performed two types of
359
experiments at tContact = 5 seconds. In the first set, we investigated the effect of dissolved NOM
360
on bioadhesion by conducting SCFS in a 10 mg/L Upper Mississippi River NOM solution at
361
ionic strength (158 mM) and pH (7.2-7.4) that approximate those of PBS. The selected
362
concentration of NOM is a typical upper limit of the NOM concentration in surface waters (2-
363
10 mg/L)94. In the second set of experiments, NOM was deposited on the surface of the
15 ACS Paragon Plus Environment
Environmental Science & Technology
Page 16 of 35
membranes as a conditioning film (see SI). SCFS experiments with NOM-conditioned
365
membranes were also performed in 10 mg/L NOM solution at the ionic strength and pH
366
indicated above. The NOM conditioning film resulted in brown coloration of the membrane,
367
and its presence was verified by FTIR as explained in Section 3.1.1 (see also Figures S2 and
368
S3). Figure 3 summarizes the mean of the maximum adhesion force and mean rupture
369
separation computed from histograms presented in Figures S16 and S17 of the SI. Data for
370
experiments performed in PBS (tContact = 5 s) are also included in Figure 3 for comparison.
|Mean Adhesion Force| (nN)
364
PBS A NOM solution NOM solution & film
1.0
0.8
0.6
0.4
* *
* *
0.2
0.0
PSF-PDA
PSF
Mean Rupture Separation (m)
371
4.0
PBS B NOM solution NOM solution & film
3.5 3.0 2.5 2.0 1.5 1.0
*
0.5
*
0.0
PSF
PSF-PDA
372 373 374 375 376 377 378
Figure 3: Mean of the maximum adhesion force (A) and mean rupture separation (B) of single P. fluorescens cells on PSF and PSF-PDA membranes investigated in different solution chemistries, denoted in the inset: PBS, 10 ppm NOM solution, and NOM-conditioned membranes in 10 ppm NOM solution. The histograms from which the reported means were computed are given in Figures S16 and S17 (p < 0.05, except for pairwise comparisons indicated by *).
16 ACS Paragon Plus Environment
Page 17 of 35
Environmental Science & Technology
379 380
Figure 3 (A) shows that the presence of NOM simultaneously in solution and as a conditioning
381
film results in weaker adhesion, compared to experiments in NOM solution (without surface
382
conditioning) and PBS. Also, weaker adhesion forces are observed on the PSF membrane when
383
NOM is present only in solution compared to experiments performed in PBS. On the other
384
hand, the experiment performed on PSF-PDA membranes in NOM solution resulted in stronger
385
adhesion forces compared to PBS (-0.39 nN vs. -0.30 nN, respectively). Experiments with 3
386
different bacterial cell probes were conducted with the PSF-PDA membrane tested in NOM
387
solution, yielding mean adhesion forces (-0.48 nN, -0.65 nN and -0.08 nN) that varied by one
388
order of magnitude. We speculate that the large variation in adhesion – which may be due to
389
variations in bacterial surface hydrophobicity across different cells95 – may explain the stronger
390
adhesion observed in NOM solution with the PSF-PDA membrane. The effect of NOM on the
391
mean rupture separation is described in Figure 3 (B), showing smaller rupture separations in
392
NOM solution, which become shorter still for adhesion on NOM-conditioned membranes.
393
Figure 3 thus shows that NOM, when present simultaneously as a dissolved foulant and as an
394
adsorbed film, weakens, and shortens the range of, adhesive interactions between the microbe
395
and the membrane. A further observation from Figure 3 is that, for the same NOM solution
396
chemistry, adhesive forces are weaker and shorter-ranged over PSF-PDA membranes
397
compared to PSF membranes; this observation is consistent with findings in PBS, as depicted
398
in Figure 2, and are attributable to the more hydrophilic PSF-PDA surface.
399 400
The weaker adhesion of P. fluorescens in the presence of simultaneously dissolved and
401
adsorbed NOM is at odds with the notion that macromolecular adsorbed films promote
402
bacterial attachment20,30,96. Nevertheless, we note that observations of lower deposition of
403
biocolloidal particles on NOM-coated surfaces are not unprecedented; lower deposition rates
17 ACS Paragon Plus Environment
Environmental Science & Technology
Page 18 of 35
404
of oocysts on NOM-coated silica collectors have been reported35, while NOM was found to
405
decrease adhesion of Gram negative E. coli and Gram positive S. suis bacteria to soil colloidal
406
particles, possibly due to electrosteric repulsive forces83. In our experiments, the surface charge
407
of control and NOM-conditioned membranes was similar ( -25 mV, cf. Figure S4), while
408
bacteria suspended in NOM solution and PBS also exhibited similar values ( -5 mV,
409
extrapolating data in Figure S5 to the ionic strength of PBS). These measurements indicate that
410
NOM does not significantly modify the surface charge of the bacteria or the membranes.
411
Nonetheless, we note that the NOM-conditioned PSF membranes are as hydrophilic as the non-
412
conditioned PSF-PDA membranes, and that the NOM-coated PSF-PDA membrane exhibits
413
the lowest contact angle of all the systems measured (see Figure 1). Consequently, NOM
414
creates a hydrophilic coating on the membrane that weakens bacterial attachment, and reduces
415
the rupture separation through a reduction of binding sites available to adhesins. The
416
hydrophilic character of NOM films is expected given that NOM contains functional groups,
417
such as carboxylic acid and amine groups, that can form hydrogen bonds with water36. Further,
418
our FTIR data (Figures S2 and S3) show that NOM contains polysaccharides and
419
polysaccharide-like components, both of which are hydrophilic constituents of NOM. The
420
hydrophilicity of the NOM film can also be explained in terms of the high water content of the
421
NOM conditioning layer97. Steric repulsion, which acts at short distances (< 15 nm)26,83, may
422
also weaken adhesion on NOM-coated surfaces: cell-surface structures, such as
423
lipopolysaccharide chains, can introduce steric repulsive forces26,39 against macromolecular
424
polysaccharide chains that protrude from the NOM adsorbed on the membrane.
425 426
The weaker adhesion observed in PSF membranes when NOM is present only in solution can
427
be attributed to Ca2+-promoted complexation of NOM with sulfonyl functional groups on the
428
membrane surface98. Ca2+ ions, present in NOM solution, can adsorb to the UF membrane
18 ACS Paragon Plus Environment
Page 19 of 35
Environmental Science & Technology
429
surface99 reducing the electrostatic repulsion between NOM and the membrane79 and forming
430
a bridging complex with carboxyl groups in NOM100. The aromatic and aliphatic content of
431
NOM could also lead to the adsorption of NOM to hydrophobic PSF membrane surfaces via
432
hydrophobic interactions99,101. Since the NOM employed in this work is predominantly
433
hydrophilic (cf. Figure 1), its adsorption to PSF membranes decreases the magnitude of
434
bacterial adhesion forces and the rupture separation (cf. Figure 3 (A) and (B)). At the same
435
time, it is possible that NOM also adsorbs on the bacterial cell surface39,102, possibly due to
436
mediation of Ca2+ ions in solution. This would result in a more hydrophilic bacterial cell
437
surface, leading to weaker adhesion forces. Steric hindrance arising when a bacterial cell and
438
substrate are both coated with a macromolecule (e.g., NOM)102 may also be responsible for
439
weaker adhesion forces.
440 441
3.2.3. Molecular Basis of Microbial Adhesion to UF Membranes
442
A significant fraction (~30% at tContact = 5 s in PBS) of the pull-off force-separation
443
measurements collected over PSF and PSF-PDA membranes exhibited a series of consecutive
444
spring instabilities, resembling the “sawtooth” pattern characteristic of force unfolding of
445
biomolecule domains103. The representative force curve in Figure S1 shows that following
446
strong, unspecific adhesion at short separations, consecutive sawtooth peaks are observed,
447
which are usually ascribed to progressive unwinding of biomolecule domains42,104,105. In
448
agreement with previous work on protein unfolding106, we find that each peak is well fitted (R2
449
≥ 0.98) to the worm-like chain (WLC) model of polymer elasticity107 (cf. Figure S1). The WLC
450
model describes the polymer (in this case, the bacterial surface macromolecule) as a semi-
451
flexible chain that is randomly oriented at any point41,107,108.
452 453
The WLC fit to the force (F) – separation (z) profile along the sawtooth-like peaks (Figure S1)
19 ACS Paragon Plus Environment
Environmental Science & Technology
454
Page 20 of 35
is given by 𝐹(𝑧) =
455
𝑘𝐵 𝑇 1 𝐿𝑐 −𝑧 −2 𝐿𝑝
[4 (
𝐿𝑐
)
𝑧
1
+ 𝐿 − 4] 𝑐
(1)
456
where kB is Boltzmann’s constant, and T = 298 K is the absolute temperature41,106. Two fitting
457
parameters characterize a semi-flexible chain as described by the WLC model: the persistence
458
length (Lp) and the contour length (Lc). Lp is a property that reflects the flexibility of the chain
459
bonds109, and is thus a measure of the chain rigidity23; while Lc is the total length of the extended
460
polymer without stretching its backbone41,109,110. The WLC model conceptualizes the polymer
461
as an entropic chain: when undeformed, macromolecular chains are in a high entropy, random
462
coil configuration that resists stretching; an external force F must be applied to elongate the
463
polymer chain, i.e., to unfold the macromolecule107. Stretching results in a lower
464
configurational entropy due to alignment of the constituent segments along the direction of
465
load111.
466 467
Equation 1 was fitted to all the force curves exhibiting the sawtooth-like peaks. In all cases, we
468
excluded the unspecific, high-adhesion peak (cf. Figure S1), where the force-extension is not
469
well-defined, and excluded peaks resulting in Lp values < 0.15 nm (i.e., smaller than the length
470
of a C-C bond108) and > 1.0 nm107; persistence lengths exceeding 1 nm indicate that, in addition
471
to entropy, hydrophobic interactions which are not accounted for by the WLC model contribute
472
to protein extension112. The distribution of best-fit Lp values is presented in Figure 4 (A),
473
showing that the persistence length is narrowly distributed between 0.15 nm and 0.3 nm, with
474
an average Lp of 0.26 nm and 0.27 nm obtained for bacteria adhering on PSF and PSF-PDA,
475
respectively. The approximately equal values obtained over both membrane types reflect the
476
fact that Lp is an intrinsic property of the biopolymers intervening in bacterial adhesion, and is
477
thus independent of the chemistry of the substrate. A salient observation is that the mean
478
persistence length is consistent with that obtained from protein unfolding experiments (Lp =
20 ACS Paragon Plus Environment
Page 21 of 35
Environmental Science & Technology
479
0.36-0.4 nm21,106,107), i.e., with the persistence length of an unfolded polypeptide106,107. The
480
data in Figure 4 (A) therefore indicate that proteinaceous adhesins play a major role in
481
attachment of P. fluorescens on the UF membrane surfaces.
482 483
Figures 4 (B) and (C) present the distribution of forces measured at the spring instabilities in
484
each sawtooth-like peak (cf. Figure S1), and the number of sawtooth-like peaks per cell pull-
485
off, respectively. We refer to these quantities as the unfolding forces (FUnfolding, Figure 4 (B))
486
and number of unfolding events per cell pull-off (NUnfolding, Figure 4 (C)), respectively. We
487
observed that the distribution of unfolding forces is approximately Gaussian over both
488
membrane types, but a higher average unfolding force is observed over PSF compared to PSF-
489
PDA (-0.35 nN vs. -0.24 nN, respectively, cf. Figure 4 (B)). Moreover, we observed a broader
490
distribution of the number of unfolding events per cell pull-off over PSF membranes than over
491
PSF-PDA membranes (Figure 4 (C)), and, on average, fewer unfolding events over PSF-PDA
492
(5.3 ± 5.2) compared to PSF (6.4 ± 5.0).
493 494
We propose that data in Figures 4 (B) and (C) can be explained in terms of unfolding of cell-
495
surface proteins of P. fluorescens cells during bacterial adhesion. In support of this view, we
496
note the well-established observation that proteins lose conformational stability near
497
hydrophobic interfaces113, given that hydrophobic interactions between the hydrophobic
498
protein core and a hydrophobic substrate stabilize the unfolded state16,111,113,114. Protein
499
unfolding is more significant over PSF surfaces (note the higher average number of unfolding
500
events, cf. Figure 4 (C)) because PSF surfaces are more hydrophobic than PSF-PDA
501
membranes (cf. Figure 1). We surmise that adhesin proteins in P. fluorescens unfold, or
502
partially unfold to a “molten” globule state116 on the surface of the membrane, and that the
503
forces reported in Figure 4 (B) are those necessary to desorb the unfolded (or partially
21 ACS Paragon Plus Environment
Environmental Science & Technology
Page 22 of 35
504
unfolded) adhesin proteins from the membrane surface. On the surface of PSF membranes,
505
adhesin proteins can establish stronger hydrophobic interactions, hence the higher unfolding
506
forces shown in Figure 4 (B). These unfolding forces are in fair agreement with values (100 -
507
400 pN) observed during force-unfolding of proteins20,96,106,117,118. The observations made in
508
Figure 4 (B) are consistent with reported stronger adhesion forces of lysozyme on PSF
509
membranes compared to adhesion on the more hydrophilic 2-hydroxyethyl methacrylate
510
(HEMA)-grafted polysulfone114. Similarly, using AFM, adhesion forces of three different
511
proteins (bovine serum albumin (BSA), fibrinogen, and human FXII) were weaker over more
512
hydrophilic surfaces (contact angle less than 60°) than on more hydrophobic surfaces119. The
513
tendency of proteins to adhere more readily to hydrophobic surfaces was also shown using
514
lysozyme, fibrinogen, and BSA120.
515 516
We also obtained best-fit values of the contour length, finding that it ranged from 286 nm for
517
sawtooth-like peaks at short separations to 9950 nm at long separations. Further, we calculated
518
the increase in the contour length Lc between two consecutive unfolding peaks (work not
519
shown), as done by others20,110,121, finding that Lc was not constant, suggesting that the
520
adhesin proteins are partially unfolded upon contact with the surface20. In P. fluorescens,
521
proteins such as LapA are known to mediate adhesion 20,21,52. However, Lc for LapA does not
522
extend beyond 1875 nm20,21, whereas we observe contour lengths of several microns. It is
523
therefore likely that membrane proteins such as LapA are responsible for bacterial adhesion
524
when the observed rupture separation is 1 - 2 m. For longer rupture separations, adhesion is
525
likely due to pili, which are several-micrometer-long structures comprising pilin proteins122,123.
526
Finally, we examined the force-separation data collected on NOM-coated membranes (Figure
527
S18), finding that a significant fraction (39% for PSF, 24% for PSF-PDA) of the measurements
528
exhibit the signatures of force unfolding. The distribution of best-fit Lp values revealed mean
22 ACS Paragon Plus Environment
Page 23 of 35
Environmental Science & Technology
529
values (Figure S18 (A)) in close agreement with those obtained with NOM-free membranes
530
(Figure 4 (A)), suggesting that the sawtooth patterns are due to the elasticity of bacterial
531
adhesins, rather than stretching of adsorbed NOM. We also note that a smaller number of
532
unfolding events per pull-off was observed on NOM-coated membranes (Figure S18 (C))
533
compared to NOM-free membranes (Figure 4 (C)). It is possible that the NOM-conditioning
534
film, through a combination of hydrophilicity and steric repulsion, results in a smaller number
535
of adhesin proteins contacting and attaching to the substrate.
23 ACS Paragon Plus Environment
Environmental Science & Technology
Frequency (%)
75
Page 24 of 35
A PSF Avg. Lp = 0.26 0.18 nm
50 25 75
PSF-PDA Avg. Lp = 0.27 0.14 nm
50 25 0 0.15
0.30
0.45
0.60
0.75
0.90
1.05
Lp (nm) Frequency (%)
60
B
PSF Avg. Force=-0.35 0.12 nN
40 20 60
PSF-PDA Avg. Force=-0.24 0.08 nN
40
NO
20 0 -0.7
-0.6
-0.5
-0.4
-0.3
-0.2
-0.1
0.0
FUnfolding (nN) Frequency (%)
40
C
30
PSF Avg. Nunfolding = 6.4 5.0
20 10 40 30
PSF-PDA Avg. Nunfolding = 5.3 5.2
20 10 0
0
2
4
6
8
10
12
14
16
18
NUnfolding
536 537 538 539 540 541 542 543 544 545 546
Figure 4: (A) Distribution of best-fit persistence length values (Lp), obtained from WLC model fits to the pull-off force curve of single P. fluorescens cells. (B) Distribution of the unfolding forces (FUnfolding, the force measured at the sawtooth peak, cf. Figure S1), defined as the force necessary to unwind a macromolecular domain. (C) Distribution of the number of unfolding events (NUnfolding, the number of sawtooth-like peaks per cell pull-off). The mean of each histogram is shown in the inset. Data were collected with single bacterial cells over PSF membranes (upper panel in A, B and C), and PSF-PDA membranes in PBS buffer (pH 7.4) at tContact = 5 s. The histograms reflect 179 WLC fits to sawtooth-like unfolding events, identified in 28 retraction force curves over PSF membranes; and 221 sawtooth-like unfolding events observed in 42 retraction force curves over PSF-PDA membranes.
24 ACS Paragon Plus Environment
Page 25 of 35
Environmental Science & Technology
547
3.3. Environmental Implications
548
This work employed SCFS to understand bacterial adhesion to UF membrane surfaces, the first
549
stage in membrane biofouling. Using P. fluorescens as a model biofilm-forming bacterium, we
550
investigated the effect of PDA deposition on bioadhesion to polysulfone UF membranes.
551
Weaker adhesion forces were observed on the more hydrophilic PSF-PDA UF membranes
552
compared to the unmodified control PSF membranes. Nevertheless, we observed that the
553
adhesion force increased with bacterium-UF membrane contact time, with the PDA membrane
554
exhibiting an average adhesion force at tContact = 5 s that is greater than that of the unmodified
555
(and more hydrophobic) polysulfone at 0 s. When the membranes were challenged with
556
bacterial suspensions in batch deposition experiments (Figure S19, experimental details are
557
given in the SI), we observed that the difference in the number of deposited cells (PSF: 760 ±
558
720 mm-2; PSF-PDA: 340 ± 250 mm-2) was not statistically significant (p = 0.11, two sided,
559
unpaired t-test). The strong bioadhesion forces observed at long tContact, together with the data
560
in Figure S19, call into question the effectiveness of simple hydrophilic coatings in controlling
561
biofouling, considering that bacterium-membrane contact would be frequent and prolonged in
562
membrane filtration. Similar observations have been made by others27,124. On the other hand,
563
the combination of PDA surface modification with biocidal nanoparticles (e.g., Ag)61, appears
564
to be a promising strategy to slow down biofouling rates. Insights into molecular level
565
phenomena underlying bacterial adhesion to membrane surfaces also emerge from this study.
566
In bacteria which rely on hydrophobic adhesins for attachment, results pressented herein
567
suggest that surface-induced protein unfolding on hydrophobic membrane substrates (possibly
568
involving outer membrane proteins, or pilin proteins) promotes bacterial attachment.
569 570 571
Supporting Information
25 ACS Paragon Plus Environment
Environmental Science & Technology
Page 26 of 35
572
Additional materials and methods information (membrane fabrication and surface
573
modification; membrane characterization). Sample force curve (Figure S1); FTIR spectra
574
(Figures S2 and S3); zeta potential of membrane surfaces (Figure S4); zeta potential
575
measurements of P. fluorescens cells (Figure S5); AFM surface roughness (Figure S6); water
576
permeability coefficient (Figure S7); distribution of adhesion forces on PSF and PSF-PDA
577
membranes for 0, 2, and 5 s contact time (Figure S8); distribution of rupture separations on
578
PSF and PSF-PDA membranes for 0, 2, and 5 s contact time (Figure S9); distribution of
579
adhesion forces and rupture separations for control measurements (cell-free cantilever) over
580
PSF and PSF-PDA membranes (Figures S10 to S15); distribution of adhesion forces on PSF
581
and PSF-PDA membranes in the presence of NOM (Figure S16); distribution of rupture
582
separations on PSF and PSF-PDA membranes in the presence of NOM (Figure S17);
583
distribution of Lp, FUnfolding and NUnfolding observed with NOM-coated membranes (Figure S18);
584
results of bacterial deposition experiments (Figure S19). This material is available free of
585
charge via the Internet at http://pubs.acs.org.
586 587
Corresponding Author
588
Santiago Romero-Vargas Castrillón. E-mail:
[email protected] 589 590
Acknowledgments
591
We gratefully acknowledge funding from the United States Geological Survey through the
592
Minnesota Water Resources Center (grant no. MN WRC 2015MN362B), and from 3M Co.
593
(Non-Tenured Faculty Award Program). Parts of this work were carried out in the
594
Characterization Facility and Minnesota Nano Center at the University of Minnesota, which
595
receive partial support from NSF through the MRSEC and NNIN programs, respectively. S.
596
BA. acknowledges the support of a Ling Graduate Fellowship in Environmental Engineering.
26 ACS Paragon Plus Environment
Page 27 of 35
Environmental Science & Technology
597
A. H. acknowledges the support of the Norwegian Center for International Cooperation in
598
Education Partnership Program with North America. We also acknowledge Nathan Karp for
599
his contributions to the preliminary stages of this study. We thank the University Imaging
600
Centers at the University of Minnesota for support, and Dr. Guillermo Marqués for technical
601
assistance.
27 ACS Paragon Plus Environment
Environmental Science & Technology
602 603 604 605 606 607 608 609 610 611 612 613 614 615 616 617 618 619 620 621 622 623 624 625 626 627 628 629 630 631 632 633 634 635 636 637 638 639 640 641 642 643 644 645 646 647 648 649 650 651
Page 28 of 35
References 1. Costerton, J. W. Bacterial Biofilms: A Common Cause of Persistent Infections. Science (80-. ). 284, 1318–1322 (1999). 2. Busscher, H. J. & van der Mei, H. C. How do bacteria know they are on a surface and regulate their response to an adhering state? PLoS Pathog. 8, 1–3 (2012). 3. Matin, A., Khan, Z., Zaidi, S. M. J. & Boyce, M. C. Biofouling in reverse osmosis membranes for seawater desalination: Phenomena and prevention. Desalination 281, 1– 16 (2011). 4. Vlamakis, H., Chai, Y., Beauregard, P., Losick, R. & Kolter, R. Sticking together: building a biofilm the Bacillus subtilis way. Nat. Rev. Microbiol. 11, 157–168 (2013). 5. Bazaka, K., Jacob, M. V., Crawford, R. J. & Ivanova, E. P. Efficient surface modification of biomaterial to prevent biofilm formation and the attachment of microorganisms. Appl. Microbiol. Biotechnol. 95, 299–311 (2012). 6. Elimelech, M. & Phillip, W. a. The future of seawater desalination: energy, technology, and the environment. Science 333, 712–717 (2011). 7. Romero-Vargas Castrillón, S., Lu, X., Shaffer, D. L. & Elimelech, M. Amine enrichment and poly(ethylene glycol) (PEG) surface modification of thin-film composite forward osmosis membranes for organic fouling control. J. Memb. Sci. 450, 331–339 (2014). 8. Werber, J. R., Osuji, C. O. & Elimelech, M. Materials for next-generation desalination and water purification membranes. Nat. Rev. Mater. 1, 16018 (2016). 9. Characklis, W. G. & Bryers, J. D. Fouling biofilm development: a process analysis. Biotechnol. Bioeng. 102, 309–347 (2009). 10. Al-Ahmad, M., Abdul Aleem, F. A., Mutiri, A. & Ubaisy, A. Biofuoling in RO membrane systems Part 1: Fundamentals and control. Desalination 132, 173–179 (2000). 11. Allen, A. et al. Nanofiltration and reverse osmosis surface topographical heterogeneities: Do they matter for initial bacterial adhesion? J. Memb. Sci. 486, 10–20 (2015). 12. Friedlander, R. S., Vogel, N. & Aizenberg, J. Role of Flagella in Adhesion of Escherichia coli to Abiotic Surfaces. Langmuir 31, 6137–6144 (2015). 13. Garrett, T. R., Bhakoo, M. & Zhang, Z. Bacterial adhesion and biofilms on surfaces. Prog. Nat. Sci. 18, 1049–1056 (2008). 14. Araújo, E. A. et al. Control of microbial adhesion as a strategy for food and bioprocess technology. Food Bioprocess Technol. 3, 321–332 (2010). 15. Zeng, G., Müller, T. & Meyer, R. L. Single-cell force spectroscopy of bacteria enabled by naturally derived proteins. Langmuir 30, 4019–4025 (2014). 16. Beaussart, A. et al. Quantifying the forces guiding microbial cell adhesion using singlecell force spectroscopy. Nat. Protoc. 9, 1049–1055 (2014). 17. Quirynen, M., Dierickx, K. & van Steenberghe, D. in Handbook of Bacterial Adhesion Principles, Methods, and Applications (eds. An, Y. H. & Friedman, R. J.) 91–102 (Humana Press Inc., 2000). 18. An, Y. H., Dickinson, R. B. & Doyle, R. J. in Handbook of Bacterial Adhesion Principles, Methods, and Applications (eds. An, Y. H. & Friedman, R. J.) 1–27 (Humana Press Inc., 2000). 19. Thewes, N. et al. Stochastic binding of Staphylococcus aureus to hydrophobic surfaces. Soft Matter 11, 8913–8919 (2015). 20. El-Kirat-Chatel, S., Boyd, C. D., O’Toole, G. A. & Dufrêne, Y. F. Single-Molecule Analysis of Pseudomonas fluorescens Footprints. ACS Nano 8, 1690–1698 (2014). 21. El-Kirat-Chatel, S., Beaussart, A., Boyd, C. D., O’Toole, G. A. & Dufrêne, Y. F. Single-
28 ACS Paragon Plus Environment
Page 29 of 35
652 653 654 655 656 657 658 659 660 661 662 663 664 665 666 667 668 669 670 671 672 673 674 675 676 677 678 679 680 681 682 683 684 685 686 687 688 689 690 691 692 693 694 695 696 697 698 699 700 701
Environmental Science & Technology
22. 23.
24.
25.
26. 27.
28. 29. 30. 31.
32.
33.
34. 35.
36. 37. 38. 39.
40.
Cell and Single-Molecule Analysis Deciphers the Localization, Adhesion, and Mechanics of the Biofilm Adhesin LapA. ACS Chem. Biol. 9, 485–494 (2014). Sullan, R. M. A. et al. Single-cell force spectroscopy of pili-mediated adhesion. Nanoscale 6, 1134–1143 (2014). Camesano, T. A., Liu, Y. & Datta, M. Measuring bacterial adhesion at environmental interfaces with single-cell and single-molecule techniques. Adv. Water Resour. 30, 1470–1491 (2007). Van Loosdrecht, M. C. M., Lyklema, J., Norde, W., Zehnder, A. J. B. & Zehnder ’, A. J. B. Bacterial Adhesion: A Physicochemical Approach. Source Microb. Ecol. Microb Ecol Microb. Ecol. 17, 1–15 (1989). Donnarumma, G. et al. Effect of Temperature on the Shift of Pseudomonas Fluorescens from an Environmental Microorganism to a Potential Human Pathogen. Int. J. Immunopathol. Pharmacol. 3, 227–234 (2010). Ong, Y. L., Razatos, A., Georgiou, G. & Sharma, M. M. Adhesion forces between E. coli bacteria and biomaterial surfaces. Langmuir 15, 2719–2725 (1999). Miller, D. J. et al. Short-term adhesion and long-term biofouling testing of polydopamine and poly(ethylene glycol) surface modifications of membranes and feed spacers for biofouling control. Water Res. 46, 3737–3753 (2012). Howe, K. J. & Clark, M. M. Fouling of Microfiltration and Ultrafiltration Membranes by Natural Waters. Environ. Sci. Technol. 36, 3571–3576 (2002). Chamberlain, A. H. L. in Biofilms - Science and Technology 59–67 (Springer Netherlands, 1992). doi:10.1007/978-94-011-1824-8_6 Palmer, J., Flint, S. & Brooks, J. Bacterial cell attachment, the beginning of a biofilm. J. Ind. Microbiol. Biotechnol. 34, 577–588 (2007). Yuan, B., Pham, M. & Nguyen, T. H. Deposition kinetics of bacteriophage MS2 on a silica surface coated with natural organic matter in a radial stagnation point flow cell. Environ. Sci. Technol. 42, 7628–7633 (2008). de Kerchove, A. J., Weroński, P. & Elimelech, M. Adhesion of Nonmotile Pseudomonas aeruginosa on ‘Soft’ Polyelectrolyte Layer in a Radial Stagnation Point Flow System: Measurements and Model Predictions. Langmuir 23, 12301–12308 (2007). Habimana, O., Semião, A. J. C. & Casey, E. The role of cell-surface interactions in bacterial initial adhesion and consequent biofilm formation on nanofiltration/reverse osmosis membranes. J. Memb. Sci. 454, 82–96 (2014). Marshall, K. C., Stout, R. & Mitchell, R. Selective sorption of bacteria from seawater. Can. J. Microbiol. 17, 1413–1416 (1971). Liu, Y., Janjaroen, D., Kuhlenschmidt, M. S., Kuhlenschmidt, T. B. & Nguyen, T. H. Deposition of Cryptosporidium parvum Oocysts on Natural Organic Matter Surfaces: Microscopic Evidence for Secondary Minimum Deposition in a Radial Stagnation Point Flow Cell. Langmuir 25, 1594–1605 (2009). Parent, M. E. & Velegol, D. E. coli adhesion to silica in the presence of humic acid. Colloids Surfaces B Biointerfaces 39, 45–51 (2004). Yang, H., Kim, H. & Tong, M. Influence of humic acid on the transport behavior of bacteria in quartz sand. Colloids Surfaces B Biointerfaces 91, 122–129 (2012). Fein, J. B., Boily, J.-F., Güçlü, K. & Kaulbach, E. Experimental study of humic acid adsorption onto bacteria and Al-oxide mineral surfaces. Chem. Geol. 162, 33–45 (1999). Abu-Lail, L. I., Liu, Y., Atabek, A. & Camesano, T. A. Quantifying the Adhesion and Interaction Forces Between Pseudomonas aeruginosa and Natural Organic Matter. Environ. Sci. Technol. 41, 8031–8037 (2007). Gaboriaud, F. & Dufrêne, Y. F. Atomic force microscopy of microbial cells: Application to nanomechanical properties, surface forces and molecular recognition forces. Colloids
29 ACS Paragon Plus Environment
Environmental Science & Technology
702 703 704 705 706 707 708 709 710 711 712 713 714 715 716 717 718 719 720 721 722 723 724 725 726 727 728 729 730 731 732 733 734 735 736 737 738 739 740 741 742 743 744 745 746 747 748 749 750 751
41. 42. 43.
44. 45.
46.
47. 48. 49.
50.
51. 52.
53. 54. 55.
56. 57. 58. 59.
60.
Page 30 of 35
Surfaces B Biointerfaces 54, 10–19 (2007). Francius, G. et al. Stretching polysaccharides on live cells using single molecule force spectroscopy. Nat. Protoc. 4, 939–946 (2009). Dufrêne, Y. F. Sticky microbes: forces in microbial cell adhesion. Trends Microbiol. 23, 376–382 (2015). Hinsa, S. M., Espinosa-Urgel, M., Ramos, J. L. & O’Toole, G. A. Transition from reversible to irreversible attachment during biofilm formation by Pseudomonas fluorescens WCS365 requires an ABC transporter and a large secreted protein. Mol. Microbiol. 49, 905–918 (2003). Tolker-Nielsen, T. & Molin, S. The Biofilm Lifestyle of Pseudomonas. Pseudomonas, V1 547–571 (2004). Malheiro, J. et al. The Effects of Selected Brominated and Chlorinated Chemicals on Pseudomonas fluorescens Planktonic Cells and Flow-Generated Biofilms. J. Food Process. Preserv. 40, 316–328 (2016). Pereira, M. O. & Vieira, M. J. Effects of the interactions between glutaraldehyde and the polymeric matrix on the efficacy of the biocide against pseudomonas fluorescens biofilms. Biofouling 17, 93–101 (2001). Mulder, M. in Basic Principles of Membrane Technology 71–156 (Springer Netherlands, 1996). doi:10.1007/978-94-009-1766-8 Lee, H., Dellatore, S. M., Miller, W. M. & Messersmith, P. B. Mussel-inspired surface chemistry for multifunctional coatings. Science 318, 426–430 (2007). Kasemset, S., He, Z., Miller, D. J., Freeman, B. D. & Sharma, M. M. Effect of polydopamine deposition conditions on polysulfone ultrafiltration membrane properties and threshold flux during oil/water emulsion filtration. Polymer (Guildf). 97, 247–257 (2016). Elomari, M., Coroler, L., Izard, D. & Leclerc, H. A numerical taxonomic study of fluorescent Pseudomonas strains isolated from natural mineral waters. J. Appl. Bacteriol. 78, 71–81 (1995). Picot, L. et al. Pseudomonas fluorescens as a potential pathogen: adherence to nerve cells. Microbes Infect. 3, 985–995 (2001). Ivanov, I. E. et al. Atomic force and super-resolution microscopy support a role for LapA as a cell-surface biofilm adhesin of Pseudomonas fluorescens. Res. Microbiol. 163, 685–691 (2012). Tamber, S. & Hancock, R. E. W. The Outer Membranes of Pseudomonas. Pseudomonas, V1 575–601 (2004). Dasgupta, N., Arora, S. & Ramphal, R. The Flagellar System of Pseudomonas Aeruginosa. Pseudomonas, V1 675–698 (2004). Isaacson, R. E. in Bacterial Adhesion Mechanisms and Physiological Significance (eds. Savage, D. C. & Fletcher, M.) 307–336 (Plenum Press, 1985). at Vesper, S. J. Production of Pili (Fimbriae) by Pseudomonas fluorescens and Correlation with Attachment to Corn Roots. Appl. Environ. Microbiol. 53, 1397–405 (1987). Kim, D., Jung, S., Sohn, J., Kim, H. & Lee, S. Biocide application for controlling biofouling of SWRO membranes - an overview. Desalination 238, 43–52 (2009). Herzberg, M. & Elimelech, M. Biofouling of reverse osmosis membranes: Role of biofilm-enhanced osmotic pressure. J. Memb. Sci. 295, 11–20 (2007). Thewes, N. et al. Hydrophobic interaction governs unspecific adhesion of staphylococci: a single cell force spectroscopy study. Beilstein J. Nanotechnol. 5, 1501– 1512 (2014). Kang, S. & Elimelech, M. Bioinspired Single Bacterial Cell Force Spectroscopy.
30 ACS Paragon Plus Environment
Page 31 of 35
752 753 754 755 756 757 758 759 760 761 762 763 764 765 766 767 768 769 770 771 772 773 774 775 776 777 778 779 780 781 782 783 784 785 786 787 788 789 790 791 792 793 794 795 796 797 798 799 800 801
Environmental Science & Technology
61.
62.
63. 64.
65. 66. 67. 68. 69. 70. 71. 72. 73.
74.
75. 76.
77.
78.
79.
80.
Langmuir 25, 9656–9659 (2009). Tang, L., Livi, K. J. T. & Chen, K. L. Polysulfone Membranes Modified with Bioinspired Polydopamine and Silver Nanoparticles Formed in Situ To Mitigate Biofouling. Environ. Sci. Technol. Lett. 2, 59–65 (2015). McCloskey, B. D. et al. Influence of polydopamine deposition conditions on pure water flux and foulant adhesion resistance of reverse osmosis, ultrafiltration, and microfiltration membranes. Polymer (Guildf). 51, 3472–3485 (2010). Wei, Q., Zhang, F., Li, J., Li, B. & Zhao, C. Oxidant-induced dopamine polymerization for multifunctional coatings. Polym. Chem. 1, 1430 (2010). van der Leeden, M. C. Are Conformational Changes, Induced by Osmotic Pressure Variations, the Underlying Mechanism of Controlling the Adhesive Activity of Mussel Adhesive Proteins? Langmuir 21, 11373–11379 (2005). Lee, H., Scherer, N. F. & Messersmith, P. B. Single-molecule mechanics of mussel adhesion. Proc. Natl. Acad. Sci. 103, 12999–13003 (2006). Lee, H., Rho, J. & Messersmith, P. B. Facile Conjugation of Biomolecules onto Surfaces via Mussel Adhesive Protein Inspired Coatings. Adv. Mater. 21, 431–434 (2009). Dreyer, D. R., Miller, D. J., Freeman, B. D., Paul, D. R. & Bielawski, C. W. Elucidating the Structure of Poly(dopamine). Langmuir 28, 6428–6435 (2012). Ding, Y. et al. Insights into the Aggregation/Deposition and Structure of a Polydopamine Film. Langmuir 30, 12258–12269 (2014). Liebscher, J. et al. Structure of Polydopamine: A Never-Ending Story? Langmuir 29, 10539–10548 (2013). Hutter, J. L. & Bechhoefer, J. Calibration of atomic-force microscope tips. Rev. Sci. Instrum. 64, 1868–1873 (1993). Senden, T. J. Force microscopy and surface interactions. Curr. Opin. Colloid Interface Sci. 6, 95–101 (2001). Hoffman, A. S. Non-Fouling Surface Technologies. J. Biomater. Sci. Polym. Ed. 10, 1011–1014 (1999). Miller, D. J., Dreyer, D. R., Bielawski, C. W., Paul, D. R. & Freeman, B. D. Surface Modification of Water Purification Membranes. Angew. Chemie Int. Ed. 56, 4662–4711 (2017). Zangmeister, R. A., Morris, T. A. & Tarlov, M. J. Characterization of Polydopamine Thin Films Deposited at Short Times by Autoxidation of Dopamine. Langmuir 29, 8619–8628 (2013). Waite, J. H. Surface chemistry: Mussel power. Nat. Mater. 7, 8–9 (2008). Jiang, J., Zhu, L. L., Zhu, L. L., Zhu, B. & Xu, Y. Surface Characteristics of a SelfPolymerized Dopamine Coating Deposited on Hydrophobic Polymer Films. Langmuir 27, 14180–14187 (2011). Lee, N., Amy, G., Croué, J. P. & Buisson, H. Identification and understanding of fouling in low-pressure membrane (MF/UF) filtration by natural organic matter (NOM). Water Res. 38, 4511–4523 (2004). Cho, J., Amy, G., Pellegrino, J. & Yoon, Y. Characterization of clean and natural organic matter (NOM) fouled NF and UF membranes, and foulants characterization. Desalination 118, 101–108 (1998). Jermann, D., Pronk, W., Meylan, S. & Boller, M. Interplay of different NOM fouling mechanisms during ultrafiltration for drinking water production. Water Res. 41, 1713– 1722 (2007). Zularisam, A. W. W., Ismail, A. F. F. & Salim, R. Behaviours of natural organic matter in membrane filtration for surface water treatment — a review. Desalination 194, 211– 231 (2006).
31 ACS Paragon Plus Environment
Environmental Science & Technology
802 803 804 805 806 807 808 809 810 811 812 813 814 815 816 817 818 819 820 821 822 823 824 825 826 827 828 829 830 831 832 833 834 835 836 837 838 839 840 841 842 843 844 845 846 847 848 849 850 851
81.
Page 32 of 35
Meritt, K. & An, Y. H. in Handbook of Bacterial Adhesion Principles, Methods, and Applications (eds. An, Y. H. & Friedman, R. J.) 53–72 (Humana Press Inc., 2000). 82. Zhao, W., Yang, S., Huang, Q. & Cai, P. Bacterial cell surface properties: Role of loosely bound extracellular polymeric substances (LB-EPS). Colloids Surfaces B Biointerfaces 128, 600–607 (2015). 83. Zhao, W., Walker, S. L., Huang, Q. & Cai, P. Adhesion of bacterial pathogens to soil colloidal particles: Influences of cell type, natural organic matter, and solution chemistry. Water Res. 53, 35–46 (2014). 84. Li, J. & McLandsborough, L. . The effects of the surface charge and hydrophobicity of Escherichia coli on its adhesion to beef muscle. Int. J. Food Microbiol. 53, 185–193 (1999). 85. Hoek, E. M. V, Bhattacharjee, S. & Elimelech, M. Effect of Membrane Surface Roughness on Colloid−Membrane DLVO Interactions. Langmuir 19, 4836–4847 (2003). 86. Boussu, K. et al. Roughness and hydrophobicity studies of nanofiltration membranes using different modes of AFM. J. Colloid Interface Sci. 286, 632–638 (2005). 87. Benjamin, M. M. & Lawler, D. F. in Water Quality Engineering Physical/Chemical Treatment Processes 731–845 (John Wiley & Sons, Inc., 2013). 88. Mehta, A. & Zydney, A. L. Permeability and selectivity analysis for ultrafiltration membranes. J. Memb. Sci. 249, 245–249 (2005). 89. Kweon, J. H. & Lawler, D. F. Evaluating Precipitative Softening as a Pretreatment for Ultrafiltration of a Natural Water. Environ. Eng. Sci. 19, 531–544 (2002). 90. Kang, S., A, A., Mayes, A. & Elimelech, M. Protein antifouling mechanisms of PAN UF membranes incorporating PAN-g-PEO additive. J. Memb. Sci. 296, 42–50 (2007). 91. McLoughlin, S. Y., Kastantin, M., Schwartz, D. K. & Kaar, J. L. Single-molecule resolution of protein structure and interfacial dynamics on biomaterial surfaces. Proc. Natl. Acad. Sci. 110, 19396–19401 (2013). 92. Hinsa, S. M. & O’Toole, G. A. Mechanisms of Adhesion by Pseudomonas. Pseudomonas, V1 699–720 (2004). 93. Touhami, A., Jericho, M. H., Boyd, J. M. & Beveridge, T. J. Nanoscale Characterization and Determination of Adhesion Forces of Pseudomonas aeruginosa Pili by Using Atomic Force Microscopy. J. Bacteriol. 188, 370–377 (2005). 94. Docter, D. et al. The nanoparticle biomolecule corona: lessons learned - challenge accepted? Chem. Soc. Rev. 44, 6094–121 (2015). 95. Merritt, K. & An, Y. H. in Handbook of Bacterial Adhesion Principles, Methods, and Applications (eds. An, Y. H. & Friedman, R. J.) 53–72 (Humana Press Inc., 2000). 96. Meadows, P. Y., Bemis, J. E. & Walker, G. C. Single-Molecule Force Spectroscopy of Isolated and Aggregated Fibronectin Proteins on Negatively Charged Surfaces in Aqueous Liquids. Langmuir 19, 9566–9572 (2003). 97. Dexter, S. C. Influence of substratum critical surface tension on bacterial adhesion—in Situ studies. J. Colloid Interface Sci. 70, 346–354 (1979). 98. Ahn, W. Y., Kalinichev, A. G. & Clark, M. M. Effects of background cations on the fouling of polyethersulfone membranes by natural organic matter: Experimental and molecular modeling study. J. Memb. Sci. 309, 128–140 (2008). 99. Laîné, J.-M., Hagstrom, J. P., Clark, M. M. & Mallevialle, J. Effects of Ultrafiltration Membrane Composition. J. Am. Water Works Assoc. 81, 61–67 (1989). 100. Pablos, C., van Grieken, R., Marugán, J., Chowdhury, I. & Walker, S. L. Study of bacterial adhesion onto immobilized TiO2: Effect on the photocatalytic activity for disinfection applications. Catal. Today 209, 140–146 (2013). 101. Koh, L., Ahn, W. & Clark, M. Selective adsorption of natural organic foulants by
32 ACS Paragon Plus Environment
Page 33 of 35
852 853 854 855 856 857 858 859 860 861 862 863 864 865 866 867 868 869 870 871 872 873 874 875 876 877 878 879 880 881 882 883 884 885 886 887 888 889 890 891 892 893 894 895 896 897 898 899 900 901
Environmental Science & Technology
102. 103. 104. 105. 106.
107.
108.
109. 110. 111. 112. 113. 114.
115. 116. 117. 118. 119. 120.
121.
122.
polysulfone colloids: Effect on ultrafiltration fouling. J. Memb. Sci. 281, 472–479 (2006). van Loosdrecht, M. C. M., Norde, W., Lyklema, J. & Zehnder, A. J. B. Hydrophobic and electrostatic parameters in bacterial adhesion. Aquat. Sci. 52, 103–114 (1990). Müller, D. J. & Dufrêne, Y. F. Atomic force microscopy as a multifunctional molecular toolbox in nanobiotechnology. Nat. Nanotechnol. 3, 261–269 (2008). Israelachvili, J. N. Intermolecular and Surface Forces with Applications to Colloidal and Biological Systems. (Academic Press, 1985). Oberhauser, A. F., Marszalek, P. E., Erickson, H. P. & Fernandez, J. M. The molecular elasticity of the extracellular matrix protein tenascin. Nature 393, 181–185 (1998). Rief, M., Gautel, M., Oesterhelt, F., Fernandez, J. M. & Gaub, H. E. Reversible Unfolding of Individual Titin Immunoglobulin Domains by AFM. Science (80-. ). 276, 1109–1112 (1997). Stirnemann, G., Giganti, D., Fernandez, J. M. & Berne, B. J. Elasticity, structure, and relaxation of extended proteins under force. Proc. Natl. Acad. Sci. 110, 3847–3852 (2013). Abu-Lail, N. I. & Camesano, T. A. Elasticity of Pseudomonas putida KT2442 Surface Polymers Probed with Single-Molecule Force Microscopy. Langmuir 18, 4071–4081 (2002). Flory, P. J. in Statistical Mechanics of Chain Molecules (ed. Flory, P. J.) 401–403 (Hanser Publishers, 1989). Touhami, A. et al. Probing protein conformations at the oil droplet–water interface using single-molecule force spectroscopy. Soft Matter 7, 10274 (2011). Saleh, O. A. Perspective: Single polymer mechanics across the force regimes. J. Chem. Phys. 142, 194902 (2015). Walther, K. A. et al. Signatures of hydrophobic collapse in extended proteins captured with force spectroscopy. Proc. Natl. Acad. Sci. 104, 7916–7921 (2007). Dee, K. C., Puleo, D. A. & Bizios, R. An Introduction to Tissue-Biomaterial Interactions. (John Wiley & Sons, 2002). Koehler, J. A., Ulbricht, M. & Belfort, G. Intermolecular Forces between a Protein and a Hydrophilic Modified Polysulfone Film with Relevance to Filtration. Langmuir 16, 10419–10427 (2000). Poncin-Epaillard, F. et al. Surface Treatment of Polymeric Materials Controlling the Adhesion of Biomolecules. J. Funct. Biomater. 3, 528–543 (2012). Ptitsyn, O. B. Molten Globule and Protein Folding. Adv. Protein Chem. 47, 83–229 (1995). Müller, D. J., Helenius, J., Alsteens, D. & Dufrêne, Y. F. Force probing surfaces of living cells to molecular resolution. Nat. Chem. Biol. 5, 383–390 (2009). Li, H. et al. Reverse engineering of the giant muscle protein titin. Nature 418, 998–1002 (2002). Xu, L.-C. & Siedlecki, C. A. Effects of surface wettability and contact time on protein adhesion to biomaterial surfaces. Biomaterials 28, 3273–3283 (2007). Kim, J. & Somorjai, G. A. Molecular Packing of Lysozyme, Fibrinogen, and Bovine Serum Albumin on Hydrophilic and Hydrophobic Surfaces Studied by Infrared−Visible Sum Frequency Generation and Fluorescence Microscopy. J. Am. Chem. Soc. 125, 3150–3158 (2003). Oberhauser, A. F., Badilla-Fernandez, C., Carrion-Vazquez, M. & Fernandez, J. M. The Mechanical Hierarchies of Fibronectin Observed with Single-molecule AFM. J. Mol. Biol. 319, 433–447 (2002). Filloux, A., de Bentzmann, S., Aurouze, M., Lazdunski, A. & Vallet, I. Fimbrial Genes
33 ACS Paragon Plus Environment
Environmental Science & Technology
902 903 904 905 906 907 908 909 910 911 912
Page 34 of 35
in Pseudomonas Aeruginosa and Pseudomonas Putida. Pseudomonas, V1 721–748 (2004). 123. Whitechurch, C. B. Biogenesis and Function of Type IV Pili in Pseudomonas Species. Pseudomonas, V4 139–188 (2006). 124. Ye, G., Lee, J., Perreault, F. & Elimelech, M. Controlled Architecture of DualFunctional Block Copolymer Brushes on Thin-Film Composite Membranes for Integrated ‘defending’ and ‘attacking’ Strategies against Biofouling. ACS Appl. Mater. Interfaces 7, 23069–23079 (2015).
913 914 915 916 917 918 919 920 921 922 923 924 925 926 927 928 929 930 931 932 933 934 935 936 937 938 939 940 941 942 943 944 945 946 947 948
34 ACS Paragon Plus Environment
Page 35 of 35
949 950 951 952
Environmental Science & Technology
TOC Image
953
35 ACS Paragon Plus Environment