Subscriber access provided by UNIV OF MD - ALBIN KUHN LIB
Article
Catalytic hydrodeoxygenation of algae biooil over bimetallic Ni-Cu/ZrO catalysts 2
Qingjie Guo, Man Wu, Kai Wang, Liang Zhang, and Xiufeng Xu Ind. Eng. Chem. Res., Just Accepted Manuscript • DOI: 10.1021/ie5042935 • Publication Date (Web): 02 Jan 2015 Downloaded from http://pubs.acs.org on January 6, 2015
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Industrial & Engineering Chemistry Research is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1
Catalytic hydrodeoxygenation of algae bio-oil over
2
bimetallic Ni-Cu/ZrO2 catalysts
3
Qingjie Guoa,*, Man Wua, Kai Wang a, Liang Zhanga, Xiufeng Xub1
4
a Key Laboratory of Clean Chemical Processing of Shandong Province, College of Chemical Engineering,
5
Qingdao University of Science & Technology, 53 Zhengzhou Road, Qingdao 266042, PR China;
6
b Institute of Applied Catalysis, Yantai University, 32 Qingquan Road, Yantai 264005, PR China
7
*Corresponding author. Tel./fax: 86 53284022757 E-mail address:
[email protected] 1
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
8
Abstract:
9
Bio-oil from the catalytic pyrolysis of algae biomass is an attractive energy
10
source. To improve algae bio-oil properties for co-feeding applications in
11
conventional oil refineries, bimetallic Ni-Cu/ZrO2 catalysts, with various Cu/Ni ratios
12
(0.14 to 1.00 w/w) at a fixed total metal loading of 22 wt. %, were synthesized and
13
used for hydrodeoxygenation (HDO) of bio-oils via the catalytic pyrolysis of
14
Chlorella and Nannochloropsis sp. at 350 °C and a hydrogen pressure of 2 MPa in a
15
trickle-bed reactor. It was found that the Ni-Cu/ZrO2 catalysts were more attractive
16
than Ni/ZrO2 catalysts in HDO, as the addition of copper could facilitate the reduction
17
of nickel oxide. As the loading of Cu increased, the HDO efficiency of the
18
Ni-Cu/ZrO2 catalyst for crude bio-oil increased and thereafter decreased. The
19
15.71Ni6.29Cu/ZrO2 catalyst showed the highest activity, with an HDO efficiency of
20
82% for Chlorella bio-oil. Moreover, the Ni-Cu/ZrO2 catalyst was stable with low
21
sintering and little coking according to transmission electron microscopy (TEM),
22
X-ray diffraction (XRD) and thermal gravimetric analysis (TGA) analyses of the
23
catalysts before and after reaction. In addition, this catalyst exhibited the favorable
24
properties of product bio-oils. In particular, the cetane number of the upgraded bio-oil
25
from Nannochloropsis sp. reached the EN 590-09 standard (specification of diesel
26
fuel for vehicles).
27 28
Key words: Bio-oil; Algae; Catalytic hydrodeoxygenation; Bimetallic Ni-Cu/ZrO2
29
catalyst
30
2 ACS Paragon Plus Environment
Page 2 of 45
Page 3 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
31
1 Introduction
32
Biomass, or bio-energy, has been recognized as a renewable energy source that
33
can replace fossil fuels, with the added bonus that the biomass can absorb CO2 from
34
the atmosphere and reduce the greenhouse effect. Bio-oil, obtained from the pyrolysis
35
of biomass in an inert gas atmosphere, has a significant appeal for use in
36
transportation fuels, both economically and technologically.1 Algae can produce more
37
oil than other biofuel feed stocks.2 In addition, algae, as a type of photosynthetic
38
organism, even grows on waste water generated by the agricultural, food, and coal
39
gasification industries.3, 4 In this case, the development of bio-oil from algae, as a
40
biofuel, is an innovative field of research, and this technology has been widely
41
considered as an ‘algal bio-refinery’.5
42
According to Chaiwong et al.2, the main groups of aromatic hydrocarbons,
43
including heterocyclic, phenol, amine, amide, indole, alkane and nitrile, were found in
44
algae crude bio-oil. The length of the carbon chain in the crude bio-oil was in the
45
range of C7-C17, and the oil boiling point was approximately 100 °C-300 °C. As a
46
refined fuel, diesel is made up of hydrocarbons with approximately 10 to 22 carbons,
47
mainly composed of aromatic hydrocarbon, cycloparaffin hydrocarbon and alkane.
48
Thus, the chemo-physical properties of the crude bio-oil were similar to those of
49
diesel oil.6 However, the crude bio-oil normally contained a high water content and
50
high level of oxygen and could not be directly used as a transportation fuel. Due to its
51
oxygen-rich compositions, crude bio-oil had some undesirable properties for
52
application in fuels, such as a low heating value, immiscibility with hydrocarbon fuels,
53
thermal and chemical instability, high viscosity and corrosiveness.7,
54
reasons, as an alternative energy source, an upgrading process was required for crude
55
bio-oil. Catalytic hydrotreatment, commonly known as “hydrodeoxygenation” (HDO), 3 ACS Paragon Plus Environment
8
For these
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
56
was one of the most promising technologies for improving the properties of crude
57
bio-oil.9
58
In the process of HDO, the crude bio-oil reacted with hydrogen in the presence
59
of a catalyst. Hence, the development of a catalyst with a high activity and stability
60
was a significant challenge for the HDO of crude bio-oil.10, 11 In many reports, the
61
conventional hydrotreating catalysts, such as sulfided or unsulfided Co-Mo or Ni-Mo,
62
were investigated.12, 13 However, these catalysts were unstable in the hydrotreating
63
process. Therefore, some researchers focused on noble metals, such as Pt-, Pd- and
64
Ru-based catalysts, for HDO of crude bio-oil from the pyrolysis of biomass.
65
Wildschut et al.14 studied Ru-based catalysts in the HDO process of crude bio-oil
66
from the pyrolysis of lignocellulosic biomass. It was found that the Ru/C catalyst
67
reached the de-oxygenation level of 90 wt.% and was superior to the classical HDO
68
catalysts, such as sulfided Ni-Mo/Al2O3 and Co-Mo/Al2O3. In particular, the new
69
bio-oil contained less acids and water than the original crude bio-oil after the HDO
70
process. Unfortunately, the high cost of noble metal catalysts may limit their
71
application.
72
While developing a non-noble metal catalyst with high activation and stability
73
for HDO, nickel was found to be a good choice as an active component of the
74
catalyst.15, 16 In addition, the loading of Cu to an Ni-based catalyst may enhance the
75
activity of hydrogenation reactions by reducing the reduction temperature of nickel
76
species,17 preventing the formation of carbon and limiting the sintering of active
77
phases in the catalyst.18 Initial screening studies on bimetallic Ni-Cu catalysts showed
78
their potential for model compounds, such as anisole, o-cresol19-21 and crude bio-oils
79
from lignocellulosic biomass.18,22
80
The components of crude bio-oil from algae biomass were different than the 4 ACS Paragon Plus Environment
Page 4 of 45
Page 5 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
81
components of lignocellulosic bio-oil. On the one hand, the algae bio-oil included
82
carbonyls, aromatic hydrocarbons, phenols and nitrogen-containing compounds,
83
which were absent in the terrestrial bio-oil.23 On the other hand, the crude bio-oil from
84
lignocellulosic biomass had a number of compounds and contained the guaiacyl group,
85
which had a low conversion rate compared to carboxyl or carbonyl compounds and
86
caused high coke formation during HDO. These compounds were absent in the algae
87
bio-oil.23, 24 To the best of our knowledge, the upgrading process of crude bio-oil from
88
algae using a bimetallic Ni-Cu catalyst has not been investigated, and further research
89
is needed.
90
In the present study, a series of HDO experiments were carried out using
91
bimetallic Ni-Cu catalysts with different Cu/Ni (w/w) proportions in a lab-scale
92
trickle-bed reactor to develop a low-cost, highly active and stable catalyst. In the
93
HDO process of producing bio-oil from the pyrolysis of algae, the effect of Cu on the
94
activity and stability of bimetallic Ni-Cu catalysts was examined in detail. ZrO2 was
95
selected as a support for bimetallic Ni-Cu catalysts because ZrO2 possesses rich acid
96
sites on the surface and could supply many adsorption sites for oxy-compounds.25
97
Furthermore, the activity of the Ni-Cu/ZrO2 catalyst was compared with that of a
98
sulfide Ni-Mo/Al2O3 catalyst. The purpose of the present study was to upgrade the
99
quality of algae bio-oil by using bimetallic Ni-Cu catalysts. The upgraded bio-oil
100
could partially substitute for fossil carbon in liquid transportation fuels.
101
5 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
102
2 Experimental
103
2.1 Preparation of crude bio-oils from algae
104
The algaes used in this study were Chlorella and Nannochloropsis sp. in powder
105
form, which came from the first institute of oceanography, China’s State Oceanic
106
Administration. They were dried at room temperature for one week before being fed
107
into the pyrolysis reactor. The algaes were characterized by ultimate, proximate and
108
component analyses. Ultimate analysis of a biomass sample was conductedin a
109
CHNS/O analyzer (CUBE, German vario EL). The moisture content of a biomass
110
sample (dry basis) was determined by calculating the weight loss after heating in an
111
oven at 103 °C for 16 hours according to the ASTM E 871 standard, and the ash
112
content was measured using the ASTM E 1755 standard. The fixed carbon and
113
volatile matter were measured using the ASTM E 1756 and ASTM E 872 standards,
114
respectively. Relevant properties of the Chlorella and Nannochloropsis sp. are
115
compiled in Table 1.
116
Table 1. Relevant properties of the Chlorella and Nannochloropsis sp. used in this study.
117
The crude bio-oil from Chlorella was produced by the fast pyrolysis of Chlorella
118
over a mixed MCM-41 catalyst, and crude bio-oil from Nannochloropsis sp. was
119
obtained by the fast pyrolysis of Nannochloropsis sp. on a mixed CaO catalyst in a
120
tube furnace reactor. Nitrogen was fed into the reactor at a flow rate of 0.6 L/min for
121
30 min at room temperature. Then, heat in the reactor was increased at a ramping rate
122
of 20 °C/min until a temperature of 550 °C was reached and held iso-thermally for 1 6 ACS Paragon Plus Environment
Page 6 of 45
Page 7 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
123 124
hour for the pyrolysis of Chlorella and Nannochloropsis sp. in an N2 atmosphere. Via element analysis, the mass fractions of the oxygen element in the crude
125
bio-oils from Chlorella and Nannochloropsis sp. were found to be 7.19 and 5.81 wt. %
126
(dry base), respectively. As listed in Table 2, abundant aliphatic acids, amides and
127
alcohol exist in the crude bio-oil from Chlorella, while aldehyde, ketone, aliphatic
128
acids and alcohol are the primary oxygen-containing compounds in the crude bio-oil
129
from Nannochloropsis sp.
130
131
Table 2. Main organic components in crude bio-oils from Chlorella and Nannochloropsis sp.
2.2 Preparation of HDO catalysts
132
The ZrO2 used was in the form of monoclinic crystals with an average particle
133
size of 2µm. Before use, ZrO2 was calcined at 500 °C for 3 hours to remove water and
134
other impurities.
135
ZrO2-supported catalysts were synthesized by impregnating ZrO2 with an
136
aqueous solution of Ni(NO3)2·6H2O and Cu(NO3)2·3H2O or Ni(NO3)2·6H2O alone
137
under strong agitation. After ultrasonic treatment for 3 hours, the catalysts were
138
heated while stirring to form a viscous substance. Then, the samples were dried at
139
110 °C for 10 hours and calcined in air at 550 °C for 5 hours. Before the HDO
140
reaction, the catalysts were reduced by hydrogen for activation. The reduction
141
temperature was determined by the temperature programmed reduction (TPR)
142
procedure. In the case of bimetallic Ni-Cu catalysts, the total percentage of Ni and Cu
143
was 22 wt. %, with different levels of the Cu/Ni mass ratio. For the single Ni catalyst, 7 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
144
it contained 22 wt. % of nickel.
145
The Ni-Mo/Al2O3 catalyst was provided by the Qilu petrochemical catalyst plant.
146
The mass fractions of Ni and Mo, counted in terms of metal oxide, were 4 wt. % and
147
16 wt. %, respectively.
148
2.3 Catalyst characterization
149
The weight fractions of Ni and Cu metals in the catalyst samples were
150
determined by inductively coupled plasma-optical emission spectrometry (ICP-OES),
151
with microwave digestion as the sample pretreatment method. Accurately weighed
152
50-150 mg samples werecompletely dissolved in 16 mL of aqua regia using
153
microwave digestion. Then, the samples were diluted with deionized water and
154
analyzed by ICP-OES (Prodigy XP, Leeman, USA). The contents of Ni and Cu were
155
quantified with the calibration curves of standards in known concentrations.
156
Bulk phases of catalysts were characterized by XRD (Rigaku, D/Max-3C) using
157
Cu-Kα radiation (λ=1.54056 Å) operated at 40 kV and 100 mA. 2θ scanning was
158
operated in the range of 40° to 70° with a step size of 0.02°. The average crystallite
159
size of the active phase was calculated by Scherrer’s formula, shown in Equation 1:
160
.଼ଽ
݀ = ஒୡ୭ୱd
(1)
161
where d is the crystallite size (nm), B is the FWHM of the characteristic peak, θ is the
162
characteristic diffraction angle (°) and λ is the wavelength of the X-ray.
163
The reducibility of NiO-CuO/ZrO2 and NiO/ZrO2 was examined by
164
temperature-programmed reduction (TPR) via the following steps: 0.03 g
165
NiO-CuO/ZrO2 or NiO/ZrO2 with a particle size of 80-180 µm was fed into a silica 8 ACS Paragon Plus Environment
Page 8 of 45
Page 9 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
166
tube, and then, a reducing gas (5% H2-95% N2) was pumped into the tube with a flow
167
rate of 30 mL/min. The temperature was raised to 800 °C with a heating rate of
168
5 °C/min, and hydrogen consumption was detected by a thermal conductivity detector
169
(TCD).
170
Catalyst morphology was characterized by transmission electron microscopy
171
(TEM, JEOL, JEM-2100) with an accelerating voltage of 200 kV. The samples were
172
prepared via ultrasonic dispersion in ethanol. Consequently, the suspension was
173
deposited upon a “holey” carbon film supported on a copper grid.
174
The amount of coking on the used catalyst was measured by a thermogravimetric
175
analyzer (TG 209F1, Netzsch, Germany). The used catalysts were washed with
176
alcohol to remove residual oil on the surface and dried at 200 °C for 2 hours, and then,
177
a 0.05 g dried sample was heated to 700 °C, with a heating rate of 10 °C/min in
178
flowing air. The amount of coking is calculated by Equation 2: Coke (%) =
179
m1 − m2 ×100% m1
(2)
180
where coke (%) represents the amount of coking on the used catalyst, and m1 and m2
181
are the sample weights at 200 °C and 700 °C, respectively.
182
2.4 HDO experimental setup
183
As shown in Scheme 1, the experimental setup includes a trickle-bed reactor,
184
pump, temperature controller, condenser and liquid collecting system. The reactor
185
was made of 022Cr17Ni12Mo2 stainless steel with a diameter of 11.8 mm and a
186
length of 48.4 mm. 9 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
187
Four milliliters (approximately 8.0 g) HDO catalyst was placed in the reactor, and
188
the reaction temperature was increased from room temperature to 350 °C in 15 min in
189
a nitrogen atmosphere. After reaching the desired temperature, the flow gas was
190
switched from nitrogen to hydrogen, and then, the bio-oil was pumped into the reactor.
191
Subsequently, the HDO products were cooled in the condenser, and the liquid sample
192
was centrifuged to separate the aqueous phase and oil phase. The oil phase was
193
analyzed using various techniques (see Section 2.6).
194
195
Scheme 1. Schematic layout of the hydrogenation equipment.
2.5 HDO reaction conditions
196
Before the HDO reaction, catalysts with an average size of 150 µm were
197
pre-reduced using hydrogen in the reactor. The reduction temperature was 450 °C for
198
bimetallic Ni-Cu/ZrO2 precursors and 500 °C for monometallic Ni/ZrO2 precursors,
199
according to the TPR analysis for the catalysts (see Section 3.1). These catalysts were
200
reduced for 2 hours in hydrogen under a pressure of 2 MPa and at a flow rate of 80
201
mL/min. The Ni-Mo/Al2O3 catalyst, before HDO reaction, was pre-sulfided in situ at
202
500 °C for 2 hours using dimethyl disulfide with a volume flow rate of 0.2 mL/min.
203
The pre-sulfided Ni-Mo/Al2O3 catalyst was marked as S-Ni-Mo/Al2O3.
204
The crude bio-oil derived from the catalytic pyrolysis of Chlorella was selected
205
for studying the effects of the Ni/Cu mass ratio on the catalytic activity of Ni-Cu/ZrO2
206
catalysts. For the typical HDO procedure, the operation conditions were selected
207
according to previous research.16, 26 The operation pressure was 2 MPa, operation 10 ACS Paragon Plus Environment
Page 10 of 45
Page 11 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
208
temperature was 350 °C, liquid hourly space velocity (LHSV) of feeding was 3.5
209
h-1and volume ratio of H2/oil was 450 N m3/m3. Two grams silica sand, with a size of
210
150-250 µm, was mixed with the catalyst to enhance heat transfer. The upgraded
211
bio-oil was collected after accumulating for 3 hours in the HDO process, and the
212
component and element composition of the upgraded bio-oil was measured by a
213
GC-MS analyzer and elemental analyzer, respectively. It should be noted that 0.5%
214
dimethyl disulfide was added to the crude bio-oil when S-Ni-Mo/Al2O3 was used as
215
the HDO catalyst.
216
The stability of the bimetallic Ni-Cu/ZrO2 catalyst was analyzed using crude
217
bio-oil from Chlorella under the same conditions as above. In addition, the catalyst
218
was sampled after running 3, 6, 12, 18, and 24 hours, separately, and their bulk phases
219
and amount of coking were measured by XRD and TGA analyses, respectively. The
220
HDO efficiency of upgraded bio-oil under different accumulated times was evaluated
221
on the basis of elemental analysis data.
222
2.6. The analysis of HDO products
223
The heat value of bio-oil was measured by an automatic quick calorimeter
224
(WELL800, Shanghai ouri instrument equipment co., LTD). The kinematic viscosity
225
of bio-oil at 40 °C was measured by an oil kinematic viscosity analyzer (SYD-265,
226
Shanghai changji geological instrument co., LTD). The cetane number of bio-oil was
227
measured in accordance with the standard test methods described by ASTM D613.27
228
A trace moisture analyzer (Zibo zifen instrument co., LTD) was employed for mass
229
fraction analysis of water in bio-oil. In the experiments, the elemental composition of 11 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
230
bio-oil was measured by an elemental analyzer (CUBE, German vario EL).
231
The analysis of crude bio-oils and upgraded bio-oils was performed by a Trance
232
GC/Trace MS (Thermo Finnigan, American) with an HP-5MS column (60 mm×0.25
233
mm i.d.; 0.25 µm film thickness). The injection volume was 0.4 µL. An injector
234
temperature of 300 °C and a split ratio of 1:40 were used. The oven temperature was
235
raised to 100 °C and maintained for 5 min, then increased to 280 °C at a rate of
236
20 °C/min and maintained for 20 min.
237 238
The hydrodeoxygenation efficiency was calculated by Equation 3: HDO efficiency =
ω1 − ω2 ×100% ω1
(3)
239
where ω1 and ω2 are the oxygen contents (wt. %, dry basis) of the crude bio-oil and
240
upgraded bio-oil, respectively.
241
12 ACS Paragon Plus Environment
Page 12 of 45
Page 13 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
242
3 Results and discussion
243
3.1 Effect of Cu doping on the physicochemical properties of Ni-Cu/ZrO2 catalysts
244
The catalysts were prepared via wet impregnation of Ni and Cu metals on the
245
ZrO2 support. An overview of the catalyst formulation used in this study is given in
246
Table 3. The total loading of active metals (Ni and Cu, 22 wt.%) is the same, while
247
the Ni to Cu weight ratios vary considerably. For comparison, a monometallic catalyst
248
of Ni/ZrO2 was prepared and tested as well.
249
Table 3. Chemical composition of the reduced fresh catalysts determined by the ICP method.
250
The phase composition of the active component of the catalysts after reduction
251
was determined by XRD, and the results are given in Fig. 1. According to the XRD
252
data, the characteristic diffraction peaks of Ni/ZrO2 catalyst at 44.5° and 51.8°
253
demonstrated that the active phase of the Ni/ZrO2 catalyst existed in the form of metal
254
Ni.28 Compared with the Ni/ZrO2 catalyst, the diffraction peaks of
255
15.71Ni6.29Cu/ZrO2 at 44.0° and 51.3° were shifted toward smaller angles. This
256
indicated the formation of a NixCu1-x alloy (or solid solution), where X depends on the
257
initial loading.17 Therefore, the active phase of the bimetallic Ni-Cu/ZrO2 catalyst
258
existed in the form of a Ni1-xCux alloy. Meanwhile, the characteristic diffraction peaks
259
of the Ni1-xCux alloy were wider than those of metal Ni on Ni/ZrO2. This result
260
indicated that the particle size of the active phase decreased, and the growth of Ni was
261
suppressed due to the introduction of Cu. The small particle size of the active phase
262
showed that the active phase was well dispersed on the surface of the ZrO2 support.29 13 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
263 264
Fig. 1. XRD patterns of monometallic Ni/ZrO2 and bimetallic Ni-Cu/ZrO2 catalysts. a. Ni/ZrO2; b. 17.6Ni4.4Cu/ZrO2; c. 15.71Ni6.29Cu/ZrO2.
265
Both of the catalysts (Ni/ZrO2 and 15.71Ni6.29Cu/ZrO2) were analyzed, in
266
reduced form, by TEM, and the results are given in Fig. 2. Large and non-uniformly
267
dispersed metal clusters are visible in the results of the monometallic Ni/ZrO2 catalyst
268
(Fig. 2(a)). In the results of the bimetallic Ni-Cu/ZrO2 catalyst, the metal clusters are
269
small and evenly distributed on the support (Fig. 2(b)). The observations shown in the
270
TEM figures were in accordance with the XRD measurements.
271
Fig. 2. TEM images of the reduced Ni/ZrO2 (a) and 15.71Ni6.29Cu/ZrO2 (b).
272
The reduction behavior of the active phase precursor was studied to determine
273
the activation temperature before the HDO reaction. The reduction profiles of the two
274
samples are given in Fig. 3. A strong peak, centered at approximately 500 °C, was
275
observed in the Ni/ZrO2 sample, which was attributed to the reduction of NiO. For the
276
15.71Ni6.29Cu/ZrO2 catalyst, several peaks, centered at approximately 275 °C,
277
310 °C and 450 °C, were present in the TPR curve. Note that the reduction peak
278
between 230 and 300 °C was likely associated with the reduction of Cu(II) to Cu(0).30
279
Peaks above 300 °C were associated with the reduction of bimetallic NixCu1−x
280
species16 and the reduction of Ni(II) to Ni(0)18. The reduction of weakly bound NiO
281
also took place in this temperature region, as the defective structure facilitated
282
reduction at a lower temperature compared to the well-crystallized bulk NiO31.
283
For the TPR curve of the bimetallic Ni-Cu catalyst, the reduction peaks of NiO 14 ACS Paragon Plus Environment
Page 14 of 45
Page 15 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
284
shifted to a lower temperature (centered at approximately 310 °C and 450 °C)
285
compared with that of monometallic Ni/ZrO2, demonstrating that the addition of Cu to
286
the Ni-Cu/ZrO2 catalyst promoted the nickel oxide reduction.19 This was also
287
observed by Robertson et al., who attributed the more facile reduction of CuO in the
288
bimetallic Ni-Cu sample to the molar free energy of reduction being lower for this
289
oxide (-100.65 kJ/mol at 25 °C) than for NiO (-12.31 kJ/mol at 25 °C).19, 32 Therefore,
290
the positions of the hydrogen consumption peaks for the bimetallic samples were
291
shifted to a lower temperature. Moreover, as illustrated in Fig. 3, for the same weight
292
samples, the integral area of the Ni-Cu/ZrO2 curve is larger than that of Ni/ZrO2. For
293
the Ni-Cu/ZrO2, the consumption of hydrogen was 160 mL per gram catalyst
294
precursor, while for the Ni/ZrO2, the consumption of hydrogen was 52.4 mL per gram
295
catalyst precursor. It is implied that the hydrogen consumption of Ni-Cu/ZrO2 was
296
more than that of Ni/ZrO2. Therefore, the high hydrogen consumption contributed to
297
the formation of reduced active particles on the Ni-Cu/ZrO2 catalyst.
298
299
Fig. 3. TPR profiles for the Ni/ZrO2 and 15.71Ni6.29Cu/ZrO2 catalysts.
3.2 Effect of Cu doping on the HDO performance of Ni-Cu/ZrO2 catalysts
300
The HDO performance of Ni-Cu/ZrO2 catalysts with different Cu/Ni weight
301
ratios for the crude Chlorella bio-oil was investigated, as shown in Fig. 4. Fig. 4
302
illustrates that mono- and bimetallic catalysts are both active in crude bio-oil, with
303
HDO efficiencies between 31.8 % and 81.9 %. The HDO efficiency for the
304
monometallic Ni/ZrO2 catalyst was lower (31.8 %) than those for bimetallic catalysts, 15 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
305
which indicated a positive effect of Cu. For the bimetallic catalysts, the HDO
306
efficiency of crude bio-oil has a relationship with the Cu/Ni ratio. The activity of the
307
Ni-Cu/ZrO2 catalysts was first increased and then reduced with increasing Cu/Ni ratio.
308
The 15.71Ni6.29Cu/ZrO2 catalyst was the most active in this series with a maximum
309
HDO efficiency of 82 %.
310
Such changes in the HDO efficiency were caused by the changing of the
311
electronic properties in the Ni xCu1-x alloy particle. According to the electron-band
312
theory, as a Group VIII metal, nickel has free d-orbitals delocalized in the
313
conductivity band, whereas copper, as a Group 1B, has free d-electrons. Therefore, a
314
significant change in the catalytic activity of Ni-based alloys can be expected because
315
the Ni interaction with the Group 1B metal caused the filling of the d-zone19.
316
According to the modern catalytic theory, catalysts with moderate adsorption strength
317
have higher activities. Due to the fewer d-band holes in Ni1-xCux compared to that of
318
Ni, the absorption strength of active hydrogen was weakened when moderate Cu was
319
introduced. Thus, active hydrogen could easily migrate on the catalyst’s surface,
320
promoting a hydrogenation reaction.33, 34 However, with the further increase of Cu,
321
the absorption strength of active hydrogen would be too weak. In this case, little
322
active hydrogen could be supplied to the HDO reaction. As expected, the activity of
323
the catalyst decreased.35 Moreover, an analogous effect can also occur in the
324
interaction with the desired oxygenated molecules. The Cu broke the Ni ensembles on
325
the catalyst’s surface, and the potential for back-donation from d-orbitals to the
326
adsorbed oxygenated molecules was lower for the alloy than for the pure Ni, thus 16 ACS Paragon Plus Environment
Page 16 of 45
Page 17 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
327
limiting the adsorption strength of the desired oxygenated molecules, as previously
328
proposed by other researchers 36. These reasons would explain the observed changes
329
in the HDO efficiency of crude Chlorella bio-oil with the loading of Cu, as seen in
330
Fig. 4. This is especially true in the case of Cu/Ni=40 wt.%, for which the catalytic
331
activity reached its maximum point.
332
Fig. 4. Effect of Cu/Ni weight ratios of the Ni-Cu/ZrO2 catalyst on the product yield and the catalytic
333
HDO efficiency for crude Chlorella bio-oil.
334
(Reaction conditions: Pressure, 2 MPa; Temperature, 350 °C; Liquid hourly space velocity, 3.5
335
h-1, H2/Oil (volume ratio), 450 N m3/m3; Time, 3 hours)
336
This result is also supported by XRD, TEM and TPR analyses. As demonstrated
337
from XRD and TEM, the high dispersion of the active phase was obtained via the
338
introduction of moderate Cu. Therefore, the relatively high activity of the bimetallic
339
Ni-Cu catalyst compared to the monometallic Ni-based catalyst could be forecasted,
340
due to the presence of relatively small metal clusters. In addition, a high reducibility
341
of the bimetallic Ni-Cu catalyst was observed. The formation of reduced particles was
342
also high for the bimetallic Ni-Cu catalyst, as shown by TPR analysis. Eventually, an
343
increase in the HDO activity of the Ni-Cu/ZrO2 catalyst was caused.
344
3.3 The stability of bimetallic Ni-Cu catalysts
345
For the HDO reaction, one of the major challenges was catalyst stability.
346
Therefore, the stability of the catalyst was studied in a trickle-bed reactor using
347
Chlorella crude bio-oil under constant reaction conditions, with the exception of time. 17 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
348
The structure, morphology and texture of the catalysts may be affected over long time
349
periods. To obtain a better understanding of the deactivation phenomena for the
350
bimetallic Ni-Cu catalyst, the spent catalysts were analyzed by XRD, TEM and TGA,
351
and the data were compared with those for the fresh catalysts.
352
After a 24 hours reaction, the 15.71Ni6.29Cu/ZrO2 catalyst showed no major
353
changes in appearance by visual observation. The color of the catalyst was slightly
354
dark after the reaction, most likely due to carbon deposition, and the particle size of
355
the 15.71Ni6.29Cu/ZrO2 catalyst was minimally different.
356
Carbon deposition on the surface of the catalyst was measured by TGA analysis
357
using the spent catalysts in air. Fig. 5 shows the variation of catalytic HDO efficiency
358
and the amount of coking on the 15.71Ni6.29Cu/ZrO2 catalyst with different
359
operation times during the HDO process for crude bio-oil from Chlorella. The
360
experiments were carried out at different times, showing that the HDO efficiency
361
decreased with running time, whereas the coke deposition increased. Even for a
362
long-termrun of 24 hours, the HDO efficiency for crude oil was still larger than 77%;
363
meanwhile, the amount of coking on 15.71Ni6.29Cu/ZrO2was only 2%, indicating
364
that the stability of the bimetallic Ni-Cu catalyst was very high.
365
In this study, the reaction data presented in Fig. 5 show that HDO efficiency
366
decreases over a 24 hours run time but declines more slowly in the latter portion of
367
the run. This can be explained by the following reasons. On the one hand, the HDO
368
efficiency was the average during the reaction time. It can be seen that the HDO
369
efficiency per hour was high at the beginning and then declined with the increase of 18 ACS Paragon Plus Environment
Page 18 of 45
Page 19 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
370
time-on-stream in the latter period. Thus, the average of the HDO efficiency
371
decreased with increasing time. On the other hand, during the experiment, the
372
fluctuation of HDO efficiency, determined by elemental analysis, was inevitably
373
caused by experimental error. When the time increased from 18 hours to 24 hours, the
374
average of the HDO efficiency only changed from 77.5 % to 77 %. That small
375
decrease in the HDO efficiency was a normal fluctuation. Therefore, the
376
15.71Ni6.29Cu/ZrO2 catalyst is stable.
377
Coking and sulfur poisoning are two important constraints for the activity of
378
hydrotreating catalysts. The surface’s active sites can be covered by the generated
379
coke, and in addition, sulfur poisoning can result in a decline in catalyst activity. As
380
shown in Table 6, due to the insignificant amounts of sulfur in the algae bio-oil, sulfur
381
poisoning via the Ni-Cu catalyst could be ignored during the HDO process.
382
Conversely, polymerization reactions were the major reactions leading to coke on the
383
catalyst’s surface.37,
384
nitrogen-containing heterocyclic compounds in the algae bio-oil, polymerization
385
reactions rarely occurred during the HDO process using the bimetallic Ni-Cu catalyst.
386
Hence, coking on the catalyst was not considered significant during the HDO process.
387
Fig. 5. Effect of continuous operating time on the coking amount of the 15.71Ni6.29Cu/ZrO2 catalyst
38
Due to having few condensed aromatic compounds and
388
and the catalytic HDO efficiency of 15.71Ni6.29Cu/ZrO2 and S-Ni-Mo/Al2O3 for the crude
389
Chlorella bio-oil.
390
(Reaction conditions for the 15.71Ni6.29Cu/ZrO2 catalyst: Pressure, 2 MPa; Temperature, 350 °C;
391
Liquid hourly space velocity, 3.5 h-1, H2/Oil (volume ratio), 450 N m3/m3).
19 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
392
The XRD characterizations of the fresh and spent 15.71Ni6.29Cu/ZrO2 catalysts
393
are depicted in Fig. 6. The average particle size of active phase NixCu1-x was
394
calculated using Scherrer’s formula. After running 12 and 24 hours, the average size
395
of active phase NixCu1-x on the catalysts increased to 15.2 nm and 15.8 nm,
396
respectively, which were almost the same as the fresh catalyst value of 14.3 nm. The
397
stability of active phase NixCu1-x indicated that the growth and agglomeration of the
398
active phase was low, which led to the stable activity of the 15.71Ni6.29Cu/ZrO2
399
catalyst over a long operational time.
400
Fig. 6 XRD patterns of 15.71Ni6.29Cu/ZrO2 catalysts.
401
a. fresh catalyst; b. 12 hours running; c. 24 hours running.
402
The TEM images of the 15.71Ni6.29Cu/ZrO2 catalyst, before and after reaction,
403
are given in Fig. 7. It illustrates that the active metal particles of the bimetallic
404
Ni-Cu/ZrO2 catalyst were stable. Sintering during the hydrotreatment reaction was not
405
serious, which was also supported by the XRD analysis.
406
Fig. 7. TEM images of fresh (a) and spent (b) 15.71Ni6.29Cu/ZrO2catalysts.
407
The results show that the activity of the bimetallic Ni-Cu/ZrO2 catalyst was
408
stable in the bio-oil HDO process, even over long operational times. Therefore, using
409
bimetallic Ni-Cu/ZrO2 catalysts can be considered a promising method in the
410
hydrotreatment of algae bio-oil.
411
3.4 Properties of the upgraded bio-oil 20 ACS Paragon Plus Environment
Page 20 of 45
Page 21 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
412
To investigate the changes in the main components of crude and upgraded
413
bio-oils, a GC-MS analysis was carried out. The results for Chlorella bio-oil are listed
414
in Table 4, while Nannochloropsis sp. bio-oil results are listed in Table 5. Chlorella
415
was a typical algae with a protein content of 44.6 wt.%. The 15.71Ni6.29Cu/ZrO2
416
catalyst showed a good HDO performance for the crude bio-oil from the catalytic
417
pyrolysis of algae with high protein. In this study, the HDO efficiency for the crude
418
Chlorella bio-oil reached up to 82 %. The acid and amide in the bio-oil, from the
419
pyrolysis of proteins, were completely converted during the catalytic hydrotreatment
420
reaction, as seen in Table 4. For the Nannochloropsis sp. crude bio-oil, the
421
15.71Ni6.29Cu/ZrO2 catalyst also showed a high HDO performance, with an HDO
422
efficiency of 90 %. Table 5 shows that acids, aldehydes and ketones have been almost
423
completely removed in the upgrading of the crude bio-oilvia pyrolysis of
424
Nannochloropsis sp.. Hence, the bimetallic Ni-Cu/ZrO2 catalyst can be applied to the
425
upgrading process of algae bio-oils.
426
Table 4. Distribution and content of oxygenates in bio-oil from the catalytic pyrolysis of Chlorella and
427
its upgraded bio-oil (% mass).
428
Table 5. Distribution and content of oxygenates in bio-oil from the catalytic pyrolysis of
429
Nannochloropsis sp. and its upgraded bio-oil (% mass).
430
To evaluate the properties of upgraded bio-oil, low heat value, viscosity and
431
water content are quantified in Table 6, and the elemental compositions are also listed
432
in Table 6.
433
After the Chlorella crude bio-oil was hydrotreated on a 15.71Ni6.29Cu/ZrO2 21 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
434
catalyst, the hydrogen content in the bio-oil increased from 9.61 to 11.53 wt.%,
435
revealing that the hydrotreatment occurred during the upgrading process. For the
436
Nannochloropsis sp. bio-oil, the hydrogen content increased from 6.20 to 11.39 wt.%.
437
Additionally, the oxygen content decreased significantly, possibly because the water
438
affected by the dehydration reactions was removed prior to the elemental analysis of
439
the upgraded bio-oil. Meanwhile, the 15.71Ni6.29Cu/ZrO2 catalyst could similarly be
440
employed to convert the organic compounds containing N and S. Compared to the
441
crude bio-oils, the content of nitrogen and sulfur elements in the upgraded bio-oils
442
was significantly lower, as shown in Table 6.
443
When considering the bio-oils for use in co-feeding in existing oil refinery units,
444
the relevant product properties of upgraded bio-oils, such as viscosity, heat value,
445
water content and cetane number, should be determined. As shown in Table 6, the
446
properties of low heat value, kinematic viscosity at 40 °C and water content all
447
effectively improvedin both of the upgraded bio-oils, with the removal of oxygen in
448
the crude bio-oils. The low heat value, kinematic viscosity at 40 °C and cetane
449
number of the upgraded Nannochloropsis sp. bio-oil were 40 MJ/kg, 3.5 mm2/s and
450
50, respectively. In particular, the cetane number met the standard of the EN 590-09
451
specification of diesel fuel for vehicles.39 In addition, the water content in the
452
upgraded bio-oil was reduced to 1.0 %. Therefore, the properties of the upgraded
453
bio-oils were improved significantly.
454
Earlier studies40, 41 have noted that the H/C molar ratio of the bio-oil was an
455
important indicator for its suitability. The H/C ratios of the upgraded bio-oils from 22 ACS Paragon Plus Environment
Page 22 of 45
Page 23 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
456
Chlorella and Nannochloropsis sp. were 1.77 and 1.93, which were higher than the
457
values of the crude bio-oils (1.57 and 0.93). This was partly due to the hydrogen
458
uptake, and a high hydrogen uptake led to a high H/C ratio.22
459
Interestingly, as shown in Table 6, it seems that there is a relation between the
460
kinematic viscosity and H/C molar ratio of the upgraded bio-oil. In the case of high
461
H/C molar ratio, the kinematic viscosity of the bio-oil was low in both types of algae.
462
These findings may be rationalized by considering the reaction network established
463
by Venderbosch et al.42 for the hydrotreatment reaction on a Ru/C catalyst. In the
464
initial phase of the hydrotreatment process, catalytic hydrogenation and thermal,
465
non-catalytic re-polymerization occurred in a parallel pathway. Recently, Ardiyantia
466
et al.22 studied this reaction network and found that the catalytic hydrogenation
467
pathway was dominant in the HDO reactions on Ni-Cu catalysts and eventually
468
determined the ultimate product properties. The hydrogenation pathway involved the
469
hydrogenation of thermally labile components in the bio-oil, forming stable molecules
470
that were not prone to polymerization. Subsequent reactions (hydrogenations and
471
hydrocracking), on a time scale of hours, led to products with low oxygen contents
472
and high H/C ratios. High H/C ratios caused low molecular weights, which is
473
associated with the low viscosity of the bio-oil.
474
475
476
Table 6. Properties of crude and upgraded bio-oils from Chlorella and Nannochloropsis sp.
3.5 Catalytic performance comparison of Ni-Cu/ZrO2 and S-Ni-Mo/Al2O3
During the HDO process of crude bio-oil from Chlorella, the HDO performances 23 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
477
of bimetallic Ni-Cu/ZrO2 and S-Ni-Mo/Al2O3 catalysts were compared. For the
478
different running times, the Ni-Cu/ZrO2 catalyst showed a high HDO activity.
479
Specifically, when the continuous running time extended from 3 hours to 24 hours,
480
the HDO efficiency of the Ni-Cu/ZrO2 catalyst for the crude bio-oil changed from 82 %
481
to 77 %, while the HDO efficiency of the S-Ni-Mo/Al2O3 catalyst decreased from 78 %
482
to 67 %, as shown in Fig. 5, indicating that the activity of the Ni-Cu/ZrO2 catalyst was
483
not only higher but also more stable than that of the S-Ni-Mo/Al2O3 catalyst.
484
The activity and stability of the S-Ni-Mo/Al2O3 catalyst was largely affected by
485
the composition of the crude bio-oil. The S-Ni-Mo/Al2O3 catalyst was not appropriate
486
for the HDO process of algae bio-oil because of the low sulfur content in this
487
bio-oil.16, 43 Therefore, the sulfiding agent was added to the crude bio-oil to improve
488
the HDO performance.44 Meanwhile, to obtain optimal activity, the proper
489
concentration of SOX must be maintained in the reaction environment.45 However, it
490
was hard to maintain the concentration of SOX, which was controlled by many factors,
491
such as the amount of sulfur donor compounds, the content of sulfur compounds in
492
the bio-oil and the operating conditions.46 Therefore, all these reasons led to the
493
instability of the Ni-Mo/Al2O3 catalyst in the HDO process of crude bio-oil from
494
Chlorella.
495
Because the application of the bimetallic Ni-Cu/ZrO2 catalyst was not limited by
496
the sulfur content in the crude bio-oil, it showed a higher stability than that of the
497
Ni-Mo/Al2O3 catalyst. Therefore, the Ni-Cu/ZrO2 catalyst has a high activity and
498
stability for the HDO process of algae bio-oil. 24 ACS Paragon Plus Environment
Page 24 of 45
Page 25 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
499
4 Conclusions
500
The bimetallic Ni-Cu/ZrO2 catalystwas used for the hydrodeoxygenation of
501
crude bio-oils from Chlorella and Nannochloropsis sp. The addition of copper to the
502
Ni-Cu/ZrO2 catalyst decreased the reduction temperature of the active components
503
and prevented excessive carbon deposition on the surface. Thus the catalyst’s
504
deactivation rate was reduced. As the loading of Cu increased, the HDO efficiency of
505
Ni-Cu/ZrO2 catalysts for crude bio-oil increased and thereafter decreased, and a
506
maximum value of 82 % was reached using the 15.71Ni6.29Cu/ZrO2 catalyst.
507
Moreover, the HDO activity of the Ni-Cu/ZrO2 catalyst was higher than that of the
508
S-Ni-Mo/Al2O3 catalyst. After the HDO reaction using the 15.71Ni6.29Cu/ZrO2
509
catalyst, the properties of low heat value, kinematic viscosity at 40 °C and water
510
content in the upgraded bio-oils were effectively improved. In particular, the cetane
511
number of the upgraded bio-oil from Nannochloropsis sp. met the standard of EN
512
590-09. In summary, Ni-Cu/ZrO2 is a good catalyst for use in hydrotreating and
513
upgrading crude algae bio-oils.
514
25 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
515 516
Acknowledgments The authors gratefully acknowledge financial support from the special fund of
517
marine renewable
energy of China (GHME2001SW02), Qingdao application
518
foundation research project (14-2-4-5-jch) and Natural Science Foundation of China
519
(21276129).
520
26 ACS Paragon Plus Environment
Page 26 of 45
Page 27 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
521
References:
522
(1) Sadhukhan, J.; Ng, K. S. Economic and European Union Environmental Sustainability Criteria
523
Assesment of Bio-Oil-Based Biofuel Systems: Refinery Integration Cases. Ind. Eng. Chem. Res.
524
2011, 50, 6794-6808.
525 526
(2) Chaiwong, K.; Kiatsiriroat, T.; Vorayos, N.; Thararax, C. Study of Bio-oil and Bio-char Production from Algae by Slow Pyrolysis. Biomass Bioenerg. 2013, 56, 600-606.
527
(3) Reddy, H. K.; Muppaneni, T.; Sun, Y.; Li, Y.; Ponnusamy, S.; Patil, P. D.; Dailey, P.; Schaub, T.;
528
Holguin, F. O.; Dungan, B.; Cooke, P.; Lammers, P.; Voorhies, W.; Lu, X.; Deng, S.; Subcritical
529
Water Extraction of Lipids from Wet Algae for Biodiesel Production. Fuel 2014, 133, 73-81.
530
(4) Hamawand, I.; Yusaf, T.; Hamawand, S. Growing Algae using Water from Coal Seam Gas Industry
531
and Harvesting using an Innovative Technique: a Review and a Potential. Fuel 2014, 117,
532
422-430.
533 534
(5) Mu, D.; Min, M.; Krohn, B.; Mullins, K. A.; Ruan, R.; Hill, J. Life Cycle Environmental Impacts of Wastewater-Based Algal Biofuels. Environ. Sci. Technol. (Accepted) DOI: 10.1021/es5027689.
535
(6) Francis, W.; Peters, M. C. Fuels and fuel Technology. 2nd ed. Michigan: Pergamon Press; 1980.
536
(7) Graça, I.; Lopes, J. M.; Cerqueira, H. S.; Ribeiro, M. F. Bio-oils Upgrading for Second Generation
537 538 539 540 541 542
Biofuels. Ind. Eng. Chem. Res. 2013, 52, 275-287. (8) Lu, Q.; Li, W. Z.; Zhu, X. F. Overview of Fuel Properties of Biomass Fast Pyrolysis Oils. Energ. Convers. Manage. 2009, 50, 1376-1383. (9) Tang, Z.; Lu, Q.; Zhang, Y.; Zhu, X.; Guo, Q. One Step Bio-oil Upgrading through Hydrotreatment, Esterification, and Cracking. Ind. Eng. Chem. Res. 2009, 48, 6923-6929. (10)Chaudhari,
R.
V.;
Torres,
A.;
Jin,
X.;
Subramaniam,
B.
Multiphase
Catalytic
543
Hydrogenolysis/Hydrodeoxygenation Processes for Chemicals from Renewable Feed stocks:
544
Kinetics, Mechanism, and Reaction Engineering. Ind. Eng. Chem. Res. 2013, 52, 15226-15243.
545 546
(11) Shi, W.; Gao, Y.; Song, S.; Zhao, Y. One-Pot Conversion of Bio-oil to Diesel- and Jet-Fuel-Range Hydrocarbons in Supercritical Cyclohexane. Ind. Eng. Chem. Res. 2014, 53, 11557-11565.
547
(12) Srifa, A.; Faungnawakij, K.; Itthibenchapong, V.; Viriya-Empikul, N.; Charinpanitkul, T.;
548
Assabumrungrat, S. Production of Bio-hydrogenated Diesel by Catalytic Hydrotreating of Palm
549
Oil over NiMoS2/γ-Al2O3 Catalyst. Bioresource. Technol. 2014, 158, 81-90.
550 551 552 553 554 555
(13) Krár, M.; Kovács, S.; Kalló, D.; Hancsók, J. Fuel Purpose Hydrotreating of Sunflower oil on CoMo/Al2O3 catalyst. Bioresource Technol. 2010, 101, 9287-9293. (14) Wildschut, J.; Mahfud, F. H.; Venderbosch, R. H.; Heeres, H. J. Hydrotreatment of Fast Pyrolysis Oil Using Heterogeneous Noble-metal Catalysts. Ind. Eng. Chem. Res. 2009, 48, 10324-10334. (15) Duan, P.; Savage, P. E. Hydrothermal Liquefaction of a Microalga with Heterogeneous Catalysts. Ind. Eng. Chem. Res. 2011, 50, 52-61.
556
(16) Yakovlev, V. A.; Khromova, S. A.; Sherstyuk, O. V.; Dundich, V. O.; Ermakov, D. Yu.;
557
Novopashina, V. M.; Lebedev, M. Yu.; Bulavchenko, O.; Parmon, V. N. Development of New
558
Catalytic Systems for Upgraded Bio-fuels Production from Bio-crude-oil and Biodiesel. Catal.
559
Today 2009, 144, 362-366.
560
(17) De Rogatis, L.; Montini, T.; Cognigni, A.; Olivi, L.; Fornasiero, P. Methane Partial Oxidation on
27 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
561
Ni Cu-based catalysts. Catal. Today 2009, 145, 176-185.
562
(18) Ardiyanti A. R.; Khromova, S. A.; Venderbosch, R. H.; Yakovlev, V. A.; Melián-Cabrera, I. V.;
563
Heeres, H. J. Catalytic Hydrotreatment of Fast Pyrolysis Oil Using Bimetallic Ni-Cu catalysts on
564
Various Supports. Appl. Catal. A-Gen. 2012, 449, 121-130.
565
(19) Khromova, S. A.; Smirnov, A. A.; Bulavchenko, O. A.; Saraev, A. A.; Kaichev, V. V.;
566
Reshetnikov, S. I.; Yakovlev, V. A. Anisole Hydrodeoxygenation over Ni-Cu Bimetallic Catalysts:
567
The Effect of Ni/Cu Ratio on Selectivity. Appl. Catal. A-Gen. 2014, 470, 261-270.
568 569 570 571
(20) Dickinson, J. G.; Savage, P. E. Stability and activity of Pt and Ni catalysts for hydrodeoxygenation in supercritical water. J. Mol. Catal. A-Chem. 2014, 388-389, 56-65. (21) Dickinson, J. G.; Savage, P. E. Development of NiCu Catalysts for Aqueous-Phase Hydrodeoxygenation. ACS Catal. 2014, 4, 2605-2615.
572
(22) Ardiyanti, A. R.; Khromova, S. A.; Venderbosch, R. H.; Yakovlev, V. A.; Heeres, H. J. Catalytic
573
Hydrotreatment of Fast-pyrolysis Oil Using Non-sulfided Bimetallic Ni-Cu Catalysts on a δ-Al2O3
574
Support. Appl. Catal. B-Environ. 2012, 117-118, 105-117.
575
(23) Thangalazhy-Gopakumar, S.; Adhikari, S.; Chattanathan, S. A.; Gupta. R. B. Catalytic Pyrolysis
576
of Green Algae for Hydrocarbon Production Using H+ZSM-5 Catalyst. Bioresource Technol. 2012,
577
118, 150-157.
578
(24) Thangalazhy-Gopakumar, S.; Adhikari, S.; Gupta, R. B.; Fernando, S. D. Influence of Pyrolysis
579
Operating Conditions on Bio-oil Components: a Microscale Study in a Pyroprobe. Energ. Fuel.
580
2011, 25, 1191-1199.
581
(25) Zhou, G.; Liu, J. Tan, X.; Pei, Y.; Qiao, M.; Fan, K.; Zong, B. Effect of Support Acidity on
582
Liquid-Phase Hydrogenation of Benzene to Cyclohexene over Ru-B/ZrO2 Catalysts. Ind. Eng.
583
Chem. Res. 2012, 51, 12205-12213.
584 585 586 587
(26) Zhong, W.; Guo, Q.; , Wang, X.; Zhang, L. Catalytic hydroprocessing of fast pyrolysis bio-oil from Chlorella. Journal of Fuel Chemistry and Technology 2013, 41, 571-578. (27) ASTM, 2013. Standard test method for cetane number of diesel fuel oil. In: Annual Book of ASTM Standards, ASTM International, West Conshohocken, Method D 613-13.
588
(28) Youn, M. H.; Seo, J. G.; Cho, K. M.; Jung, J. C.; Kim, H.; La, K. W.; Park, D. R.; Park, S.; Lee
589
S.H.; Song, I. K. Effect of Support on Hydrogen Production by Auto-thermal Reforming of
590
Ethanol over Supported Nickel Catalysts. Korean J. Chem. Eng. 2008, 25, 236-238.
591
(29) Burton, A. W.; Ong, K.; Rea, T.; Chan, I. Y. On the Estimation of Average Crystallite Size of
592
Zeolites from the Scherrer Equation: A Critical Evaluation of its Application to Zeolites with
593
One-dimensional Pore Systems. Micropor. Mesopor. Mat. 2009, 117, 75-90.
594
(30) Bykova, M. V.; Ermakov, D. Yu.; Kaichev, V. V.; Bulavchenko, O. A.; Saraev, A. A.; Lebedev,
595
M. Yu.; Yakovlev, V. A. Ni-based Sol–gel Catalysts as Promising Systems for Crude Bio-oil
596
Upgrading: Guaiacol Hydrodeoxygenation Study. Appl. Catal. B-Environ. 2012, 113-114,
597
296-307.
598
(31) Mile, B.; Stirling, D.; Zammitt, M. A.; Lovell, A.; Webb, M. The location of nickel oxide and
599
nickel in silica-supported catalysts: Two Forms of “NiO” and the Assignment of
600
Temperature-programmed Reduction Profiles. J. Catal. 1988, 114, 217-229.
28 ACS Paragon Plus Environment
Page 28 of 45
Page 29 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
601
(32) Robertson, S. D.; McNicol, B. D.; De Baas, J. H.; Kloet, S. C.; Jenkins, J. W. Determination of
602
Reducibility
603
Temperature-programmed Reduction. J. Catal. 1975, 37, 424-431.
604 605
and
Identification
of
Alloying
in
Copper-nickel-on-silica
Catalysts
by
(33) Yao, Y., Goodman, D. W. Direct Evidence of Hydrogen Spillover from Ni to Cu on Ni-Cu Bimetallic Catalysts. J. Mol. Catal. A-Chem. 2014, 383-384, 239-242.
606
(34) Izadi, N.; Rashidi A. M.; Zeraatkar, A.; Varmazyar, H.; Rashtchi, M. Preparation of Highly Stable
607
Bimetallic Ni-Cu Catalyst for Simultaneous Production of Hydrogen and Fish-bone Carbon
608
Nanofibers: Optimization, Effect of Catalyst Preparation Methods and Deactivation. Int. J.
609
Hydrogen Energ. 2014, 39, 7765-7779.
610
(35) Anderson, J. R. Structure of Metallic Catalysts, Acad. Press, N.Y. 1975.
611
(36) Sitthisa, S.; Pham, T.; Prasomsri, T.; Sooknoi, T.; Mallinson, R. G.; Resasco, D. E.; Conversion of
612 613 614 615 616 617 618 619 620
furfural and 2-methylpentanal on Pd/SiO2 and Pd-Cu/SiO2 catalysts. J. Catal. 2011, 280, 17-27. (37) Zeuthen, P.; Bartholdy, J.; Wiwel, P.; Cooper, B. H. Formation of Coke on Hydrotreating Catalysts and its Effect on Activity. Stud. Surf. Sci. Catal. 1994, 88, 199-206. (38) Fisk, C. A.; Morgan, T.; Ji, Y.; Crocker, M.; Crofcheck, C.; Lewis, S. A. Bio-oil Upgrading over Platinum Catalysts Using in Situ Generated Hydrogen. Appl. Catal. A-Gen. 2009, 358, 150-156. (39) Committee for Standardization. Automotive Fuels-Diesel-Requirements and Test Methods. European Committee for Standardization, Brussels, Method EN 590: 2009. (40) Mortensen, P. M.; Grunwaldt, J. D.; Jensen, P. A.; Knudsen, K. G.; Jensen, A. D. A Review of Catalytic Upgrading of Bio-oil to Engine Fuels. Appl. Catal. A-Gen. 2011, 407, 1-19.
621
(41) Ashok, J.; Reddy, P. S.; Raju, G.; Subrahmanyam, M.; Venugopal, A. Catalytic Decomposition of
622
Methane to Hydrogen and Carbon Nanofibers over Ni-Cu-SiO2 Catalysts. Energ. Fuel. 2009, 23,
623
5-13.
624 625
(42) Venderbosch, R. H.; Ardiyanti, A. R.; Wildschut, J.; Oasmaa, A.; Heeres, H. J. Stabilization of Biomass-derived Pyrolysis oils. J. Chem. Technol. Biot. 2010, 85, 674-686.
626
(43) Du, Z.; Hu, B.; Ma, X.; Cheng, Y.; Liu, Y.; Lin, X.; Wan, Y.; Lei, H.; Chen, P.; Ruan, R. Catalytic
627
Pyrolysis of Microalgae and Their Three Major Components: Carbohydrates, Proteins, and Lipids.
628
Bioresource Technol. 2013, 130, 777-782.
629 630
(44) Şenol, O. Đ.; Ryymin, E. -M. Viljava, T. -R. Krause A. O. I. Reactions of Methyl Heptanoatehy Drodeoxygenation on Sulphided Catalysts. J. Mol. Catal. A-Chem. 2007, 268, 1-8.
631
(45) Blanchin, S.; Galtier, P.; Kasztelan, S.; Kressmann, S.; Penet, H.; Pérot, G. Kinetic Modeling of
632
the Effect of H2S and of NH3 on Toluene Hydrogenation in the Presence of a NiMo/Al2O3
633
Hydrotreating Catalyst. Discrimination between Homolytic and Heterolytic Models. J. Phys.
634
Chem. A. 2001, 105, 10860-10866.
635 636
(46) Jacobson, K.; Maheria, K. C.; Dalai, A. K. Bio-oil Valorization: A Review. Renew. Sust. Energ. Rev. 2013, 23, 91-106.
29 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Table captions: Table 1. Relevant properties of the Chlorella and Nannochloropsis sp. used in this study. Table 2. Main organic components in crude bio-oils from Chlorella and Nannochloropsis sp. Table 3. Chemical composition of the reduced fresh catalysts determined by the ICP method. Table 4. Distribution and content of oxygenates in bio-oil from the catalytic pyrolysis of Chlorella and its upgraded bio-oil (% mass). Table 5. Distribution and content of oxygenates in bio-oil from the catalytic pyrolysis of Nannochloropsis sp. and its upgraded bio-oil (% mass). Table 6. Properties of crude and upgraded bio-oils from Chlorella and Nannochloropsis sp.
30 ACS Paragon Plus Environment
Page 30 of 45
Page 31 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Table 1. Relevant properties of the Chlorella and Nannochloropsis sp. used in this study. Chlorella
Nannochloropsis sp.
C (wt.%)
44.93
49.07
H (wt.%)
6.42
7.59
O (wt.%)
40.67
35.63
N (wt.%)
6.41
6.29
S (wt.%)
1.57
1.42
Moisture (wt.%)
4.13
5.0
Volatile matter (wt.%)
69.45
79.69
Properties Ultimate analysis
Proximate analysis
Component analysis
Fixed carbon (wt.%)
16.22
10.24
Ash (wt.%)
10.20
5.03
Protein (wt.%)
42.70
44
Polysaccharide (wt.%)
9.42
21
Lipid (wt.%)
2.51
30
Others(wt.%)
45.37
5
31 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 32 of 45
Table 2. Main organic components in crude bio-oils from Chlorella and Nannochloropsis sp. Bio-oil from Chlorella
Formula
Bio-oil from Nannochloropsis sp. Area
Structure
Area Formula
Structure
(%)
(%)
O
C16H32O2
10.32
C20H40O
10.17
OH
C20H40O
OH
5.36
OH
C17H32O
5.11 O
O
C18H37NO
O
NH2
4.95
C3H6O
2.88
O
O
C22H43NO
3.46
N
C11H28N2O2
1.93
NH
NH2 O
O
O OH
C18H28O2
OH
C17H32O
3.05
C18H28O2
2.07
C15H28O2
HO
1.92
OH
1.71 O
C15H26O2
O O
1.04
32 ACS Paragon Plus Environment
Page 33 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Table 3. Chemical composition of the reduced fresh catalysts determined by the ICP method. Metal loading (wt. %) Catalyst Ni
Cu
22Ni/ZrO2
22.00
-
19.25Ni2.75Cu/ZrO2
19.25
2.75
18.6Ni3.4Cu/ZrO2
18.60
3.40
17.6Ni4.4Cu/ZrO2
17.60
4.40
15.71Ni6.29Cu/ZrO2
15.71
6.29
14.67Ni7.33Cu/ZrO2
14.67
7.33
13.2Ni8.8Cu/ZrO2
13.20
8.80
11Ni11Cu/ZrO2
11.00
11.00
33 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48
Page 34 of 45
Table 4. Distribution and content of oxygenates in bio-oil from the catalytic pyrolysis of Chlorella and its upgraded bio-oil (% mass). Acids
Alcohols
Amides
Distribution
Original Bio-oil
Upgraded bio-oil
Distribution
Original Bio-oil
Upgraded bio-oil
Distribution
Original Bio-oil
Upgraded bio-oil
C15H26O2
1.04
0.00
C14H30O
0.95
1.43
C18H37NO
4.95
0.76
C16H32O2
10.32
1.16
C15H32O
1.42
0.00
C22H43NO
3.46
0.41
C18H28O2
3.05
0.32
C17H32O
2.07
0.00
C20H40O
5.36
0.28
Sum
9.80
1.71
Sum
8.41
1.17
Sum
14.41
1.48
34
ACS Paragon Plus Environment
Page 35 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48
Industrial & Engineering Chemistry Research
Table 5. Distribution and content of oxygenates in bio-oil from the catalytic pyrolysis of Nannochloropsis sp. and its upgraded bio-oil (% mass). Acids
Aldehydes and Ketones
Alcohols Phenols
Amides Upgraded
Distribution
Original Bio-oil
Upgraded bio-oil
Distribution
Original Bio-oil
Upgraded bio-oil
Distribution
Original Bio-oil
Original
Upgraded
Bio-oil
bio-oil
C11H18N2O2
1.93
0.00
SUM
1.93
0.00
Distribution bio-oil
C15H28O2
1.71
0.00
C3H6O
2.88
0.00
C7H14O
0.33
0.00
C16H32O2
0.48
0.00
C10H14O
0.56
0.00
C14H30O
0.67
0.00
C18H28O2
1.92
0.00
C9H12O3
0.57
0.00
C20H40O
10.17
0.46
C15H30O
1.63
0.00
C20H42O
0.46
0.00
C17H32O
5.11
0.00
C20H38O2
0.66
0.00
C22H42O
0.33
0.00
C17H14O
0.00
0.32
C5H10O
0.00
0.46
C6H6O
0.00
0.78
C12H22O
0.00
0.30
C11H28O
0.00
0.50
SUM
11.08
0.76
SUM
12.29
2.06
SUM
4.01
0.00
35
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Table 6. Properties of crude and upgraded bio-oils from Chlorella and Nannochloropsis sp. Chlorella
Nannochloropsis sp.
Quality parameters
C (wt. %) H (wt. %)
Crude Bio-oil
Upgraded bio-oil
Crude Bio-oil
Upgraded bio-oil
73.2
78.3
80.2
83.2
9.61
①
11.5
6.20
13.4
O (wt. %)
7.19
1.30
5.81
1.63
N (wt. %)
9.25
8.73
6.20
1.42
S (wt. %)
0.721
0.142
1.59
0.356
H/C molar ratio
1.57
1.76
0.928
1.93
O/C molar ratio
0.0736
0.0125
0.0543
0.0147
Low heat value (MJ/kg)
31.5
36.0
37.2
40.0
40°C Kinematic viscosity (mm2/s)
20.5
8.1
12.5
3.5
8.0
2.2
3.8
Water content (%)
①
1.0 50.0
Cetane number
Oxgen in the water of the bio-oil was not included in the value.
36 ACS Paragon Plus Environment
Page 36 of 45
Page 37 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Figure Captions: Scheme 1. Schematic layout of the hydrogenation equipment. Fig. 1. XRD patterns of monometallic Ni/ZrO2 and bimetallic Ni-Cu/ZrO2 catalysts. a. Ni/ZrO2; b. 17.6Ni4.4Cu/ZrO2; c. 15.71Ni6.29Cu/ZrO2. Fig. 2. TEM images of the reduced Ni/ZrO2 (a) and 15.71Ni6.29Cu/ZrO2 (b). Fig. 3. TPR profiles for the Ni/ZrO2 and 15.71Ni6.29Cu/ZrO2 catalysts. Fig. 4. Effect of Cu/Ni weight ratios of the Ni-Cu/ZrO2 catalyst on the product yield and the catalytic HDO efficiency for crude Chlorella bio-oil. (Reaction conditions: Pressure, 2 MPa; Temperature, 350 °C; Liquid hourly space velocity, 3.5 h-1, H2/Oil (volume ratio), 450 N m3/m3; Time, 3 hours) Fig. 5. Effect of continuous operating time on the coking amount of the 15.71Ni6.29Cu/ZrO2 catalyst and the catalytic HDO efficiency of 15.71Ni6.29Cu/ZrO2 and S-Ni-Mo/Al2O3 for the crude Chlorella bio-oil. (Reaction conditions for the 15.71Ni6.29Cu/ZrO2 catalyst: Pressure, 2 MPa; Temperature, 350 °C; Liquid hourly space velocity, 3.5 h-1, H2/Oil (volume ratio), 450 N m3/m3). Fig. 6 XRD patterns of 15.71Ni6.29Cu/ZrO2 catalysts. a. fresh catalyst; b. 12 hours running; c. 24 hours running. Fig. 7. TEM images of fresh (a) and spent (b) 15.71Ni6.29Cu/ZrO2catalysts.
37 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Scheme 1. Schematic layout of the hydrogenation equipment.
38 ACS Paragon Plus Environment
Page 38 of 45
Page 39 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Fig. 1. XRD patterns of monometallic Ni/ZrO2 and bimetallic Ni-Cu/ZrO2 catalysts. a. Ni/ZrO2; b. 17.6Ni4.4Cu/ZrO2; c. 15.71Ni6.29Cu/ZrO2.
39 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Fig. 2. TEM images of the reduced Ni/ZrO2 (a) and 15.71Ni6.29Cu/ZrO2 (b).
40 ACS Paragon Plus Environment
Page 40 of 45
Page 41 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Fig. 3. TPR profiles for the Ni/ZrO2 and 15.71Ni6.29Cu/ZrO2 catalysts.
41 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Fig. 4. Effect of Cu/Ni weight ratios of the Ni-Cu/ZrO2 catalyst on the product yield and the catalytic HDO efficiency for crude Chlorella bio-oil. (Reaction conditions: Pressure, 2 MPa; Temperature, 350 °C; Liquid hourly space velocity, 3.5 h-1, H2/Oil (volume ratio), 450 N m3/m3; Time, 3 hours)
42 ACS Paragon Plus Environment
Page 42 of 45
Page 43 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Fig. 5. Effect of continuous operating time on the coking amount of the 15.71Ni6.29Cu/ZrO2 catalyst and the catalytic HDO efficiency of 15.71Ni6.29Cu/ZrO2 and S-Ni-Mo/Al2O3 for the crude Chlorella bio-oil. (Reaction conditions for the 15.71Ni6.29Cu/ZrO2 catalyst: Pressure, 2 MPa; Temperature, 350 °C; Liquid hourly space velocity, 3.5 h-1, H2/Oil (volume ratio), 450 N m3/m3).
43 ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Fig. 6 XRD patterns of 15.71Ni6.29Cu/ZrO2 catalysts. a. fresh catalyst; b. 12 hours running; c. 24 hours running.
44 ACS Paragon Plus Environment
Page 44 of 45
Page 45 of 45
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Fig. 7. TEM images of fresh (a) and spent (b) 15.71Ni6.29Cu/ZrO2catalysts.
45 ACS Paragon Plus Environment