Cellulose hydrolysis using oxidized carbon catalyst in a plug flow slurry process Abhijit Shrotri, Hirokazu Kobayashi, Hiroyuki Kaiki, Mizuho Yabushita, and Atsushi Fukuoka Ind. Eng. Chem. Res., Just Accepted Manuscript • DOI: 10.1021/acs.iecr.7b03918 • Publication Date (Web): 21 Nov 2017 Downloaded from http://pubs.acs.org on November 23, 2017
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Industrial & Engineering Chemistry Research is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1
Cellulose hydrolysis using oxidized carbon catalyst
2
in a plug flow slurry process
3
Abhijit Shrotri, Hirokazu Kobayashi, Hiroyuki Kaiki, Mizuho Yabushita and Atsushi Fukuoka*
4
Institute for Catalysis, Hokkaido University, Kita 21 Nishi 10, Kita-Ku, Sapporo, Hokkaido 001-
5
0021, Japan. E-mail:
[email protected].
6
KEYWORDS: Cellulose, Carbon Catalyst, Air-oxidation, Hydrolysis, Slurry process,
7
8
ABSTRACT: Catalytic conversion of cellulose to glucose at industrial scale is a sustainable way
9
to produce fuels and chemicals. Here, we report hydrolysis of cellulose to glucose using an
10
inexpensive carbon catalyst in a continuous slurry process. Carbon catalyst prepared by air-
11
oxidation showed the highest activity for cellulose hydrolysis owing to the large number of
12
weakly acidic functional groups. Air-oxidized carbon catalyst hydrolyzed cellulose in a plug
13
flow slurry reactor after mix-milling to produce soluble β-1,4-glucans. Further hydrolysis of β-
14
1,4-glucans to glucose was achieved using a fixed bed reactor containing Amberlyst-70 catalyst
15
in series with the slurry reactor to obtain glucose in 59% yield. Another approach was to use
16
dilute H3PO4 for hydrolysis of β-1,4-glucans to glucose with 70% yield resulting in space time
17
yield of 456 kg m-3 h-1 of glucose. Simple design, short residence time and high space time yield
18
will enable scale up of this process using existing chemical technology.
ACS Paragon Plus Environment
1
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2
Page 2 of 29
1. Introduction Lignocellulosic biomass, abundantly available as agricultural waste and energy crop, is a
3
carbon-based renewable feedstock for the synthesis of liquid fuels and chemicals.1–4 Large-scale
4
processing of lignocellulose is necessary to replace the enormous global demand of fossil fuel
5
derived chemicals.5 Design of a feasible and cost effective catalytic process for lignocellulose
6
conversion is challenging due to its recalcitrant structure and disparate composition.6,7
7
Hydrolysis of cellulose, the largest and the most recalcitrant component of lignocellulose, is the
8
first step for synthesis of many value added chemicals (Figure 1).8 Commercial application of
9
catalytic cellulose hydrolysis is currently prohibited by many factors including efficient synthesis
10
of an active catalyst and lack of a scalable continuous hydrolysis process.
11 12
Figure 1. Glucose produced by hydrolysis of cellulose is the gateway for synthesis of valuable
13
chemicals and precursors in biomass based industries.
14
Carbon catalysts containing acidic functional groups have the potential for cellulose hydrolysis
15
at large scale. The polyaromatic surface of carbon materials strongly adsorbs cellulosic
16
molecules through CH−π and hydrophobic interactions.9 The adsorbed molecules are then
17
hydrolyzed by acidic functional groups present on the carbon surface.10–12 Sulfonic acid groups
18
introduced by sulfuric acid treatment can hydrolyze β-1,4-glycosidic bonds.10,11 However,
ACS Paragon Plus Environment
2
Page 3 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1
stability of sulfonic acid groups under hydrothermal conditions is not very high and the active
2
sites are lost at temperature required to achieve high rate of reaction.13 Moreover, synthesis of
3
catalyst containing sulfonic acid groups generates large amount of acid waste that must be
4
treated before disposal. Alternatively, carbon catalysts decorated with weakly acidic carboxyl
5
and hydroxyl groups are hydrothermally stable and show high activity for cellulose
6
hydrolysis.12,14 Weakly acidic carboxyl and hydroxyl groups can be introduced by oxidation of
7
carbon materials. Oxidizing agents such as HNO3 and H2O2 are commonly used for the oxidation
8
of carbon materials.15 However, disposal of spent oxidizing agents causes an economic and
9
environmental burden on the process. Air-oxidation is a promising method for synthesis of
10
weakly acidic carbon catalyst because it utilizes atmospheric oxygen as oxidant.16 Nevertheless,
11
processes for carbon catalyzed cellulose hydrolysis are limited to lab scale demonstrations that
12
cannot be scaled up for commercialization.
13
Development of a continuous hydrolysis process using carbon catalyst is necessary to achieve
14
the processing capacity required to replace the demand of fossil derived fuels and chemicals. The
15
nature of cellulose, an insoluble polymer, makes the development of a continuous process rather
16
difficult. Pilot and industrial scale continuous hydrolysis of cellulose was previously tried using
17
homogenous acid catalysts.17 A plug flow process with H2SO4 catalyst (0.5–2.0 %) could process
18
concentrated lignocellulose to yield glucose with 52% yield.18 However, economic viability of
19
these processes was difficult due to the cost of acid separation and neutralization. Heterogeneous
20
carbon catalysts for cellulose hydrolysis claim to have overcome these issues by easy separation
21
of catalyst.10,11,19,20 Choice of the reactor is crucial for continuous hydrolysis of cellulose using
22
carbon catalyst. Initial hydrolysis occurs at the solid-solid interface between cellulose and
23
catalyst particles until the β-1,4-glucans formed are small enough to dissolve in water (Figure
ACS Paragon Plus Environment
3
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 29
1
2).21 Subsequent hydrolysis occurs on the solid-liquid interface by adsorption of dissolved β-1,4-
2
glucans on the catalyst surface. Vigorous mechanical mixing is important to promote the
3
interaction between solid catalyst and cellulose particles in the first step. Therefore, lab-scale
4
batch reactors equipped with mechanical stirrers are used for catalyst design and screening.
5
Scaling up a batch reactor to continuous stirred tank reactor (CSTR) has its limitations due to the
6
energy required for stirring and difficulty in designing large pressurized CSTRs. A plug flow
7
slurry reactor is ideally suited for large-scale conversion of cellulose. However, lack of stirring
8
mechanism in a plug flow reactor limits the catalyst and cellulose interaction.
9 10
Figure. 2. Schematic showing steps of cellulose hydrolysis using carbon catalyst. Initial
11
hydrolysis occurs at the solid-solid interface followed with reaction at solid-liquid interface when
12
the β-1,4-glucans dissolve in water. After reaction, the dissolved products and the catalyst is
13
easily separated.
14
The preferential adsorption of cellulose on carbon catalyst offers a solution to facilitate the use
15
of a plug flow continuous process for cellulose hydrolysis. Longer chains of β-1,4-glucans
16
present in cellulose are favorably adsorbed on carbon as the adsorption equilibrium constant
17
increases with the degree of polymerization.22 The strong interaction of β-1,4-glucans with
18
catalyst surface can eliminate the requirement for vigorous mechanical stirring to promote inter-
ACS Paragon Plus Environment
4
Page 5 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1
particle contact. Therefore, a simple plug flow slurry reactor can be used after the adsorption of
2
cellulose on carbon surface. However, the insolubility of cellulose in conventional solvents
3
prevents the adsorption of cellulose on the carbon catalyst. Alternatively, cellulose can also be
4
adsorbed on carbon by ball-milling them together in a pre-treatment step called mix-milling.12,23
5
Ball-milling alters the crystalline structure of cellulose and makes a solid mixture of cellulose
6
and carbon.
7
In this study, we report the synthesis of carbon catalysts using different oxidizing methods and
8
compare their activity for cellulose hydrolysis. We also demonstrate a process for hydrolysis of
9
cellulose and lignocellulose to soluble β-1,4-glucans and monomeric sugars, glucose and xylose,
10
in a continuous plug flow reactor using air-oxidized carbon catalyst.
11
2. Experimental Section
12
2.1 Oxidized Carbon Catalyst Synthesis
13
Dried activated carbon named BA (Hokuetsu BA, Ajinomoto Fine-Techno) was used for
14
preparation of all oxidized carbon catalysts. Air-oxidation was done by spreading 4 g of BA with
15
a thickness of 3-5 mm on a Pyrex dish (ø130) and calcining under air in an electric furnace
16
(Denken-Highdental, KDF S90) with the following program: 25 to 425 °C at 5 °C min-1 and 425
17
°C for 10 h. This sample was named BA-Air. Nitric acid oxidation was done by slowly adding
18
80 mL of ice cold 68% HNO3 aq. to 4 g of BA and stirring it at room temperature in the absence
19
of light for 24 h. The recovered solid was washed with hot and cold water until the pH of filtrate
20
was above 5. After drying under vacuum this sample was named BA-HNO3. Hydrogen peroxide
21
oxidation was done by adding 30 mL of cold 30% H2O2 aq. solution to 3 g of BA and stirring it
22
for 48 h at room temperature. The solid was recovered by filtration and then washed with 0.1 M
ACS Paragon Plus Environment
5
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
oxalic acid followed by repeated washing with water. After drying under vacuum this sample
2
was named BA-H2O2. Alkali oxidation was done by mixing 0.6 g of BA with 1.8 g of KOH in a
3
mortar. The sample was spread on a stainless steel film and then heated under N2 flow (20 mL
4
min-1) at 700 °C for 1 h in a tube furnace. The recovered solid was first washed with water then
5
with 50 mL of 1 M HCl solution and then again repeatedly with water. The washed solid was
6
dried under vacuum and named BA-KOH.
7
2.2 Catalyst characterization
8
Surface oxygenated functional groups were characterized by titration method reported by
9
Boehm.24 For the titration, oxidized carbon (200 mg) was stirred in 20 mL of 0.05 M solutions of
10
NaOH and NaHCO3 for 24 h. Subsequently, the solutions were filtered and 10 mL of 0.05 M
11
HCl solution was added to 5 mL of filtrates. The resulting solutions were titrated with 0.05 M
12
NaOH using methyl orange as an indicator to determine the presence of oxygenated functional
13
groups. Consumption of NaHCO3 and NaOH was attributed to carboxyl groups and total acidic
14
functional groups, respectively. Temperature programmed desorption (TPD) of oxygenated
15
functional groups was measured in a MicrotracBel instrument by heating the catalyst under He
16
flow (30 mL min-1) up to 1000 °C at 10 °C min-1 and detecting the evolution of gases using a
17
mass spectrometer. Surface area was calculated by applying BET approximation to the N2
18
adsorption isotherm of catalysts measured at -196 °C using a Belsorp mini analyzer. Raman
19
spectra were collected using a Renishaw inVia Reflex spectroscope with a 532 nm laser.
20
2.3 Cellulose hydrolysis in batch reactor
21
Batch reactions were performed in a MMJ-100 batch reactor procured from OM Lab-tech.
22
Page 6 of 29
Microcrystalline cellulose (10 g, Merck column chromatography grade) was ball milled for 96 h
ACS Paragon Plus Environment
6
Page 7 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1
at 60 rpm prior to the reaction with 1 kg of ø10 zirconia balls in a ceramic pot using an ANZ-51S
2
rotator. For each hydrolysis reaction 324 mg of ball milled cellulose and 50 mg of catalyst were
3
added to the reactor with 40 mL of water. The reactor was heated under stirring to 230 °C and
4
then the temperature was immediately reduced back to room temperature using an air blower.
5
The solid was separated by centrifugation, dried and weighed to determine cellulose conversion
6
and the liquid was analyzed to determine the product yield.
7
2.4 Mix-milling
8
Microcrystalline cellulose (Avicel PH-101) or Eucalyptus (5 g) and BA-Air (0.77 g) were
9
milled together in an Al2O3 pot (250 mL) with alumina balls (ø5, 200 g) using a Fritsch P-6
10
planetary ball mill. Milling condition was 500 rpm for 2 h with a 10-min interval after every 10
11
min of milling.
12
2.5 Hydrolysis in flow reactor
13
The hydrolysis reaction was performed by mixing 1.87 g of mix-milled substrate in 200 mL
14
solvent (water or 4.5 mM H3PO4) and feeding it to the pneumatic pump reservoir (Figure 3). The
15
flow reaction system was pressurized to 3.0–3.5 MPa using N2 gas flow of 35 mL min-1 through
16
a bypass gas line. After the system pressure and reactor temperature were stable, the N2 gas flow
17
was diverted inside the pneumatic pump to start the slurry flow. The oil bath temperature for the
18
slurry reactor was maintained at 220 °C for mix-milled cellulose hydrolysis and 240 °C for mix-
19
milled Eucalyptus hydrolysis. The fixed bed reactor was filled with 4 g of as received
20
Amberlyst-70. The catalyst bed temperature was maintained at 140 °C. The fixed bed reactor
21
was bypassed using three-way valves when not in operation. Samples were collected from the
22
outlet of back pressure regulator at regular interval and analyzed.
ACS Paragon Plus Environment
7
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 29
1 2
Figure 3. Cellulose hydrolysis process with plug flow slurry reactor and fixed bed reactor for
3
continuous hydrolysis to β-1,4-glucans and monomers.
4
2.6 Product analysis
5
Liquid products obtained from batch and flow reactor were analyzed by high-performance
6
liquid chromatography (Shimadzu; refractive index and ultraviolet detectors) with a SUGAR
7
SH1011 (Shodex; ø8×300 mm; eluent: water 0.5 mL min-1; 50 °C) column. Composition of
8
Eucalyptus was determined by NREL/TP-510-42618 method on dry basis.25 Yields of glucose
9
and xylose from Eucalyptus were based on the glucan and xylan content determined by the
10
NREL method.25
11
3. Results and Discussion
12
3.1 Carbon oxidation and characterization
13
Activated carbon is the cheapest source of high surface area carbon material suitable for
14
catalysis. Therefore, we used a biomass derived activated carbon named BA for the synthesis of
15
oxygenated carbon catalysts. This carbon was oxidized using air, HNO3, H2O2 and KOH (Table
16
1). After air oxidation 52% wt. of catalyst was lost in the form of CO and CO2 due to the partial
ACS Paragon Plus Environment
8
Page 9 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1
combustion of BA. The surface area of BA-Air was 870 m2 g-1, a slight reduction from 1230 m2
2
g-1 of BA. After nitric acid oxidation, 11% carbon was lost and the surface area decreased to
3
1080 m2 g-1. Weight loss after H2O2 oxidation was only 1% as it is the weakest of all oxidizing
4
agents we used. The surface area of BA-H2O2 was 1020 m2 g-1. Treatment of BA with KOH
5
resulted in weight loss of 42 % and the surface area increased to 2040 m2 g-1. Alkali treatment
6
creates micropores in the carbon materials that increases the surface area of catalyst.26
7
Table 1. Characterization and cellulose hydrolysis activity of oxidized carbon catalysts.a
Entry
Catalyst
BET Weight surface lossb Area (%) (m2 g-1)
Total acidity
Carboxyl group density
Cellulose conversion
Glucose yield
(mmol g1 ) (mmol g-1)
(%)
(%)
1
BA
-
1230
0.3
0.1
48
15
2
BA-Air
52
870
2.6
1.0
68
35
3
BA-HNO3
11
1080
1.1
0.5
59
27
4
BA-H2O2
1
1020
0.6
0.2
55
22
5
BA-KOH
42
2040
1.9
0.8
60
23
6
Blank
-
-
-
-
33
2.1
a
Hydrolysis reaction condition: ball-milled cellulose (324 mg), carbon catalyst (50 mg) and water (40 mL) were added to high-pressure reactor and heated to 230 °C and then rapidly cooled. b
Weight loss of carbon during oxidation.
8
Oxidation of BA introduced varying amount of acidic functional groups on carbon surface.
9
The number of acidic functional groups were determined by titration of solid with NaOH and
10
NaHCO3. NaOH reacts with all acidic functional groups and it represents the total acidity of the
11
catalyst. NaHCO3 is a weak base and it reacts with carboxylic acids and sulfonic acids. As the
12
presence of sulfonic groups is unlikely in our catalysts, the consumption of NaHCO3 was
ACS Paragon Plus Environment
9
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 29
1
attributed to the presence of carboxylic acids. Among weak acid sites, carboxylic acid is the most
2
active functional group for hydrolysis of β-1,4 glycosidic bond.27 Unoxidized BA contained 0.30
3
mmol g-1 of acidic functional groups with 0.10 mmol g-1 of carboxyl groups. Among all the
4
oxidation methods, air oxidation was the most effective for introduction of acidic functional
5
groups (Table 1). BA-Air had 2.6 mmol g-1 of acidic functional groups with 1.0 mmol g-1 of
6
carboxyl groups. Alkali treatment introduced 1.9 mmol g-1 of acidic functional groups with 0.8
7
mmol g-1 of carboxyl groups. Both HNO3 and H2O2 were less effective for introducing acidic
8
functional groups. Consequently, the degree of oxidation was related to weight loss as the
9
severity of oxidation increased.
10
3.2 Cellulose hydrolysis in batch reactor
11
Activity of carbon catalysts were tested for cellulose hydrolysis in a batch reactor (Table 1). In
12
the absence of carbon catalyst, cellulose conversion was 33% with a glucose yield of only 2.1% .
13
Unoxidized BA catalyst increased the conversion to 48% and the glucose yield increased to 15%.
14
The activity of BA was attributed to the presence of small number of acidic functional groups
15
and the favorable interactions between cellulose and carbon surface. Cellulose conversion in the
16
presence of BA-Air was 68% with glucose yield of 35% (Table 1 Entry 2). The activity of other
17
catalysts for cellulose conversion was lower than BA-Air. Cellulose conversion was proportional
18
to the total acidity of carbon catalyst. Glucose yield in the presence of BA-KOH was lower than
19
BA-HNO3 despite having a higher conversion and more number of oxygenated functional
20
groups. Strong adsorption of products in the micropores of BA-KOH was attributed to the lower
21
glucose yield. Therefore, simple air-oxidation was the most effective way for introducing large
22
number of oxygenated functional groups that show high activity for cellulose hydrolysis.
ACS Paragon Plus Environment
10
Page 11 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1
3.3 Characterization of BA-Air
2
BA-Air was characterized in more detail to identify the structural and chemical changes during
3
air-oxidation. Temperature programmed desorption (TPD) of carbon catalyst under inert
4
atmosphere releases CO and CO2. The evolution of CO and CO2 is used to determine the
5
concentration of functional groups. TPD of BA released 0.17 mmol g-1 of CO2 that increased to
6
1.2 mmol g-1 after air oxidation (Figure 4A). The amount of CO2 evolved from BA-Air agreed
7
with the number of carboxyl groups determined by titration. CO evolved from BA and BA-Air
8
during TPD was 0.41 mmol g-1 and 5.3 mmol g-1 (Figure 4B). The evolution of CO from BA-Air
9
was twice that of the total acidic functional groups determined titration. This result indicates that
10
the non-acidic functional groups such as carbonyl and ether groups were also present in BA-Air.
11
However, these functional groups are not expected to be active for acid catalyzed hydrolysis of
12
cellulose. The porous structure was not remarkably changed after air oxidation apart from the
13
reduction in surface area (Figure 4C). Raman spectra of BA and BA-Air did not show an
14
increase in the degree of graphitization due to air-oxidation (Figure 4D). Therefore, the effect of
15
air oxidation on BA was primarily introduction of oxygenated functional groups that catalyzed
16
the hydrolysis of cellulose to glucose.
ACS Paragon Plus Environment
11
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 29
1 2
Figure 4. Characterization of BA and BA-Air catalysts. (A) and (B): CO2 and CO evolution
3
during TPD under He flow. (C) N2 adsorption isotherm (D) Raman spectra measure using 532
4
nm laser.
5
3.4 Hydrolysis in flow reactor
6
BA-Air was chosen as the preferred catalyst for cellulose hydrolysis in a lab-scale continuous
7
plug flow slurry reactor. The plug flow slurry reactor is crucial for high throughput reactions. At
8
lab scale, the process design is difficult due to the lack of slurry pumping systems at high
9
pressure. The design of flow reactor system is shown in Figure 3, which consisted of the
10
following elements:
11
1. Pneumatic feeder: The slurry pump was built in-house by modifying a high-pressure
12
batch reactor. Slurry was continuously stirred before being fed into the reactor by
13
overhead N2 gas pressure. The slurry flow rate was controlled by N2 gas flow rate.
14 15
2. Slurry reactor: Stainless steel (SS) 316 tube of OD 1/16 inch (1.58 mm) and ID 1.0 mm was coiled and dipped in a stirred oil bath.
ACS Paragon Plus Environment
12
Page 13 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2 3 4 5 6 7
Industrial & Engineering Chemistry Research
3. Solid separator: The solid catalyst and unreacted residue was separated from the product solution by gravity settling and removed through the drain valve. 4. Fixed bed reactor: SS 316 tube of OD 3/8 inch (9.52 mm) filled with Amberlyst-70 catalyst. 5. Product removal: The clear product solution was passed through an inline filter before exiting through a backpressure regulator. Slurry pump design was challenging due to frequent clogging in piston type pumps. The slurry
8
particles settle within tubes and compact under compression to block the lines. Therefore, we
9
devised a pneumatic pump to continuously stir the slurry and feed it into the reactor. A
10
continuous tube without any fittings was used from the feed inlet until the solid separator to
11
avoid clogging due to the build-up of particles on obstructions. The inner diameter of tube was
12
small (1 mm) to achieve high linear velocity. Under the reaction condition, the flow was laminar
13
(Reynolds number = 1020) and turbulent mixing did not occur.
14
Unlike batch reactor the catalyst and cellulose contact cannot be initiated by mechanical
15
stirring in a plug flow reactor. Therefore, prior adsorption of cellulose on the carbon surface is
16
necessary. Cellulose was adsorbed on carbon surface under solvent free condition by ball milling
17
them together in a planetary ball mill. Adsorption by mix-milling does not degrade the structure
18
of cellulose. Only small amount of soluble products were detected (3.7%) when the mix-milled
19
substrate was dispersed in water, suggesting the polymeric cellulose structure was preserved. The
20
large cellulose molecules are insoluble in water and remain adsorbed on carbon surface under
21
aqueous condition. In contrast, when strong acid catalysts are used during ball milling significant
22
depolymerization occurs and soluble products are obtained.28–30 When the mix-milled substrate is
ACS Paragon Plus Environment
13
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 29
1
subjected to hydrothermal conditions the β-1,4-glycosidic bonds linking cellulose monomers are
2
rapidly cleaved by neighboring weakly acidic functional groups.
3
Cellulose hydrolysis in our process occurs in two steps. Initially, cellulose undergoes
4
hydrolysis to soluble β-1,4-glucans over carbon catalyst. At first, we tested the performance of
5
slurry reactor for hydrolysis of cellulose to β-1,4-glucans. Time on stream of mix-milled
6
cellulose hydrolysis in the slurry reactor with the fixed bed reactor bypassed is shown in Figure
7
5A. The slurry concentration during this experiment was 9.3 g L-1 and the slurry reactor
8
temperature was 220 °C. The residence time of reactants within the slurry reactor was 90 s. The
9
process approached steady state within short time and was stable for the course of the reaction.
10
β-1,4-Glucans were the primary products (57%, DP = 2−6, See supporting information (SI) for
11
characterization of β-1,4-glucans) followed by glucose (25%). By-product yield was 9%, which
12
included fructose, mannose, levoglucosan and 5-hydroxymethylfurfural. β-1,4-Glucan is a high
13
value product with potential application in livestock farming to enhance the growth rate of
14
animals and as an alternative to antibiotics for controlling pathogenic gut bacteria.31,32 β-1,4-
15
Glucans are also used in food industry to enhance the taste, texture and physiological effect of
16
human food products.33
ACS Paragon Plus Environment
14
Page 15 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1 2
Figure 5. Yield of products for cellulose hydrolysis over the course of reaction in the slurry
3
reactor with fixed bed reactor bypassed. Residence time within the reactor was 90 s (A) and 155
4
s (B). Reaction condition: substrate mix milled cellulose, slurry concentration 9.3 g L-1, slurry
5
reactor temperature 220 °C, pressure 3.2 MPa.
6
Conversion of β-1,4-glucans to glucose is required to produce chemical platforms. Further
7
hydrolysis of β-1,4-glucan did not occur by simply increasing the residence time of reactants in
8
the slurry reactor to 155 s. Under this condition the yield of by-products increased to 14% with
9
only a small improvement in the glucose yield (30%) (Figure 5B). Therefore, at high
10
temperatures the weakly acidic carbon catalyst alone is not suitable for synthesis of glucose due
11
to the slow hydrolysis rate and increase in by-product formation.
12
We studied homogeneous and heterogeneous catalysts for hydrolysis of β-1,4-glucans to
13
glucose to evaluate their process feasibility. Heterogeneous approach used a fixed bed reactor
14
with Amberlyst-70 sulfonic acid resin catalyst. When the oligomer feed obtained from slurry
ACS Paragon Plus Environment
15
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 29
1
reactor was directly fed to the fixed bed reactor (4 g Amberlyst-70, catalyst bed temperature 140
2
°C) the glucose yield increased to 59 % and β-1,4-glucan yield was 7.7 % (Table 2 entry 2). In
3
the homogenous approach, we used diluted H3PO4 solution (4.5 mM, pH 2.5) as a solvent instead
4
of pure water. Under this condition the β-1,4-glucans rapidly underwent hydrolysis in the slurry
5
reactor itself to form glucose in high yield (67%) (Table 2 entry 3). Use of H3PO4, a weak acid,
6
is in contrast with acid hydrolysis processes that utilize HCl and H2SO4, which are corrosive and
7
not compatible with downstream processes. Furthermore, neutralization of H3PO4 produces
8
phosphate salts that are useful as fertilizer for biomass production.
9
Table 2: Steady state yield of products in the continuous flow process using cellulose and Ecalyptus as substrate.a
10
Yield of products (%) Entry Substrate
Solvent
β-1,4Glucans
Glucose Xylose
C6 isomers Levoglucosan 5-HMF Furfural
STYb (kg m3 h-1)
1
Cellulose
H2O
57
25
-
3.8
2.7
2.3
-
82
2
Cellulosec
H2O
7.7
59
-
3.2
4.2
2.5
-
-
3
Cellulose
dil. H3PO4
1.8
67
-
3.8
5.0
2.6
-
219
4
Cellulosed
dil. H3PO4
9.6
70
-
4.5
4.5
1.0
-
456
5
Cellulosee
dil. H3PO4
6.5
36
-
2.6
2.4
0.5
5
Eucalyptusf
H2O
53
20
46
-
1.2
2.6
9.5
32
6
Eucalyptusc,f
H2O
3.0
46
40
-
5.0
1.0
20
-
7
Eucalyptusf dil. H3PO4
5.1
71
73
-
9.9
4.1
17
116
a
-1
472
-1
Slurry concentration 9.3 g L , slurry flow rate 1 mL min , reactor temperature 220 °C for cellulose feed and 240 °C for
Eucalyptus feed, pressure 3.2 – 3.4 MPa. bSpace time yield of glucose production in slurry reactor. cFixed bed reactor was used for conversion of β-1,4-glucans to glucose using Amberlyst-70 catalyst with catalyst bed temperature of 140 °C. dSlurry concentration 18.7 g L-1. eSlurry concentration 37.4 g L-1. fYield of C6 products was based on glucan content in Eucalyptus and yield of xylose and furfural was based on xylan content.
11
ACS Paragon Plus Environment
16
Page 17 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1
We tested the performance of slurry reactor to handle higher slurry concentration to achieve
2
practical applicability (Table 2 entry 4 and 5). Using the dilute H3PO4 as solvent, we obtained
3
similar glucose yield of 70% when slurry concentration was doubled to 18.7 g L-1 (SI Figure S4
4
A). Further increasing the slurry concentration to 37.4 g L-1 did not cause any clogging in the
5
reactor. However, the glucose yield under the same reaction condition (220 °C, 90 s residence
6
time) reduced to 36% (SI Figure S4 B). The decrease in yield is expected as it is known that the
7
rate of cellulose hydrolysis is slower at higher cellulose concentration.34 Furthermore, the β-1,4-
8
glucans are poorly soluble in water and their limited dissolution may also reduce the product
9
yield.
10
Space time yield (STY) for slurry reactor, defined here as yield of glucose (kg) obtained from
11
a reactor of volume 1 m3 in 1 h, was 219 kg m-3 h-1 using H3PO4 solvent and slurry concentration
12
of 9.3 g L-1. In comparison, the STY for the same reaction utilizing carbon catalyst and dilute
13
HCl solvent in a batch reactor would be 8 kg m-3 h-1.16 Therefore, the flow reactor shows 27
14
times higher rate of glucose synthesis for the same reactor volume and slurry concentration per
15
unit time. STY increased to 456 kg m-3 h-1 when the slurry concentration was 18.7 g L-1. The
16
high STY obtained in our process will reduce the operation energy requirement and cost of the
17
process at an industrial scale.
18
The slurry flow reactor can also process lignocellulosic biomass such as Eucalyptus,
19
containing 42.2% glucan and 13.9% xylan by weight as analyzed by NREL TP-510-42618
20
method. (See SI Table S1 for detailed composition). Hydrolysis of mix milled Eucalyptus in
21
water without the fixed bed reactor provided 53% yield of β-1,4-glucans and 20% glucose (9.3 g
22
L-1 slurry, 240 °C) (Table 2 entry 5). Xylan present as hemicellulose was also hydrolyzed to
23
xylose with 46% yield. With the fixed bed reactor in line, the glucose yield increased to 46% and
ACS Paragon Plus Environment
17
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 29
1
β-1,4-glucans yield was 3.0%. Using dilute H3PO4 as solvent, and without the fixed bed reactor,
2
the β-1,4-glucans were hydrolyzed to yield 71% glucose and 73% xylose. Lignin present in
3
Eucalyptus adsorbs on the surface of carbon and partially inhibits the catalytic activity. The
4
activity can be recovered by air-oxidation of lignin containing carbon residue after the reaction.14
5
Many factors influence the scale up capability of this process for large-scale. Clogging of
6
reactor is a major issue for continuous operation. Turbulent flow is a straightforward approach to
7
prevent clogging due to stratification of biomass slurry.35 Our process worked under laminar
8
flow rate due to the absence of any obstruction in the slurry flow path, thereby reducing the
9
energy requirement to achieve turbulent flow. Build-up of humin compound, complex polymers
10
formed by degradation of glucose, is another reason for clogging after prolonged use. The humin
11
formation in our process was limited by the short residence time of products. Use of the fixed
12
bed reactor also reduces humin formation by using lower temperature for hydrolysis of β-1,4-
13
glucans. The carbon catalyst recovered during the reaction can be recycled as it is or after re-
14
oxidation to remove residual lignin from biomass.14 The carbon catalyst did not show any
15
decline in activity after reuse experiments in the batch reactor at 230 °C (Figure S5). The
16
stability of Amberlyst-70 catalyst was studied separately using cellobiose as a model oligomer
17
feed. Cellobiose conversion was 98% in the fixed bed reactor and glucose yield was 90% (8.1 g
18
L-1 cellobiose feed, 1 mL min-1, bed temperature 140 °C). The Amberlyst-70 catalyst did not
19
show any decline in activity after 30 h of continuous operation (Figure S6).
20
4. Conclusions
21
We report the synthesis of an inexpensive carbon catalyst by air-oxidation of activated carbon
22
and its application for cellulose and lignocellulose hydrolysis in a plug flow slurry reactor. BA-
ACS Paragon Plus Environment
18
Page 19 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1
Air showed higher total acidity and abundance of carboxyl groups in comparison to catalysts
2
prepared by other oxidation methods. Consequently, BA-Air was the most active catalyst for
3
cellulose hydrolysis in a batch reactor. Application of BA-Air in a plug flow slurry reactor
4
required adsorption of cellulose on carbon by mix-milling. β-1,4-Glucans, high value products
5
used as food additives, were primary product after hydrolysis of mix-milled cellulose and
6
lignocellulose in the plug flow reactor. Monomeric sugars, glucose and xylose, were easily
7
obtained in high yield by using a fixed bed reactor in series or by using a dilute acid solution as
8
solvent to catalyze the sequential hydrolysis within the slurry reactor itself. Space time yield of
9
glucose was as high as 456 kg m-3 h-1 in our process. Mix-milling used in our process is an
10
energy intensive method and development of an alternative pre-treatment for adsorption of
11
cellulose on carbon catalyst is the next challenge.
12
Supporting Information. Characterization of β-1,4 glucans using NMR spectroscopy and LC-
13
MS, time on stream data for reactions in flow reactor, catalyst reusability test and composition of
14
Eucalyptus.
15
Corresponding Author
16
*
[email protected] 17
ACKNOWLEDGMENT
18
This work was supported by funding received from Japan Science and Technology Agency (JST)
19
through the Advanced Low Carbon Technology Research and Development Program (ALCA).
20
REFERENCES
21
(1)
22
Chheda, J. N.; Huber, G. W.; Dumesic, J. A. Liquid-Phase Catalytic Processing of Biomass-Derived Oxygenated Hydrocarbons to Fuels and Chemicals. Angew. Chemie Int.
ACS Paragon Plus Environment
19
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Page 20 of 29
Ed. 2007, 46 (38), 7164.
2
(2)
Rubin, E. M. Genomics of Cellulosic Biofuels. Nature 2008, 454 (7206), 841.
3
(3)
Tuck, C. O.; Pérez, E.; Horváth, I. T.; Sheldon, R. A.; Poliakoff, M. Valorization of
4 5
Biomass: Deriving More Value from Waste. Science 2012, 337 (6095), 695. (4)
Luterbacher, J. S.; Rand, J. M.; Alonso, D. M.; Han, J.; Youngquist, J. T.; Maravelias, C.
6
T.; Pfleger, B. F.; Dumesic, J. A. Nonenzymatic Sugar Production from Biomass Using
7
Biomass-Derived γ-Valerolactone. Science 2014, 343 (6168), 277.
8
(5)
IEA. Oil Information 2016; OECD Publishing, 2016.
9
(6)
Sanderson, K. Lignocellulose: A Chewy Problem. Nature 2011, 474 (7352), S12.
10
(7)
Gallezot, P. Conversion of Biomass to Selected Chemical Products. Chem. Soc. Rev.
11 12
2012, 41 (4), 1538. (8)
13 14
Rinaldi, R.; Schüth, F. Acid Hydrolysis of Cellulose as the Entry Point into Biorefinery Schemes. ChemSusChem 2009, 2 (12), 1096.
(9)
Chung, P.-W.; Charmot, A.; Gazit, O. M.; Katz, A. Glucan Adsorption on Mesoporous
15
Carbon Nanoparticles: Effect of Chain Length and Internal Surface. Langmuir 2012, 28
16
(43), 15222.
17
(10)
Suganuma, S.; Nakajima, K.; Kitano, M.; Yamaguchi, D.; Kato, H.; Hayashi, S.; Hara, M.
18
Hydrolysis of Cellulose by Amorphous Carbon Bearing SO3H, COOH, and OH Groups.
19
J. Am. Chem. Soc. 2008, 130 (38), 12787.
20
(11)
21 22 23
Onda, A.; Ochi, T.; Yanagisawa, K. Selective Hydrolysis of Cellulose into Glucose over Solid Acid Catalysts. Green Chem. 2008, 10 (10), 1033.
(12)
Kobayashi, H.; Yabushita, M.; Komanoya, T.; Hara, K.; Fujita, I.; Fukuoka, A. HighYielding One-Pot Synthesis of Glucose from Cellulose Using Simple Activated Carbons
ACS Paragon Plus Environment
20
Page 21 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
1 2
and Trace Hydrochloric Acid. ACS Catal. 2013, 3 (4), 581. (13)
Van Pelt, A. H.; Simakova, O. A.; Schimming, S. M.; Ewbank, J. L.; Foo, G. S.; Pidko, E.
3
A.; Hensen, E. J. M.; Sievers, C. Stability of Functionalized Activated Carbon in Hot
4
Liquid Water. Carbon 2014, 77, 143.
5
(14)
Kobayashi, H.; Kaiki, H.; Shrotri, A.; Techikawara, K.; Fukuoka, A. Hydrolysis of Woody
6
Biomass by a Biomass-Derived Reusable Heterogeneous Catalyst. Chem. Sci. 2016, 7 (1),
7
692.
8
(15)
9 10
Surface Chemistry of Activated Carbons. Carbon 1999, 37 (9), 1379. (16)
11 12
(17)
(18)
(19)
Pang, J.; Wang, A.; Zheng, M.; Zhang, T. Hydrolysis of Cellulose into Glucose over Carbons Sulfonated at Elevated Temperatures. Chem. Commun. 2010, 46 (37), 6935.
(20)
19 20
Thompson, D. R.; Grethlein, H. E. Design and Evaluation of a Plug Flow Reactor for Acid Hydrolysis of Cellulose. Ind. Eng. Chem. Prod. Res. Dev. 1979, 18 (3), 166.
17 18
Kobayashi, H.; Fukuoka, A. Synthesis and Utilisation of Sugar Compounds Derived from Lignocellulosic Biomass. Green Chem. 2013, 15 (7), 1740.
15 16
Shrotri, A.; Kobayashi, H.; Fukuoka, A. Air Oxidation of Activated Carbon to Synthesize a Biomimetic Catalyst for Hydrolysis of Cellulose. ChemSusChem 2016, 9 (11), 1299.
13 14
Figueiredo, J. L.; Pereira, M. F. R.; Freitas, M. M. A.; Órfão, J. J. M. Modification of the
Huang, Y.-B.; Fu, Y. Hydrolysis of Cellulose to Glucose by Solid Acid Catalysts. Green Chem. 2013, 15 (5), 1095.
(21)
To, A. T.; Chung, P.-W.; Katz, A. Weak-Acid Sites Catalyze the Hydrolysis of Crystalline
21
Cellulose to Glucose in Water: Importance of Post-Synthetic Functionalization of the
22
Carbon Surface. Angew. Chemie Int. Ed. 2015, 54 (38), 11050.
23
(22)
Yabushita, M.; Kobayashi, H.; Hasegawa, J.; Hara, K.; Fukuoka, A. Entropically Favored
ACS Paragon Plus Environment
21
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 29
1
Adsorption of Cellulosic Molecules onto Carbon Materials through Hydrophobic
2
Functionalities. ChemSusChem 2014, 7 (5), 1443.
3
(23)
Yabushita, M.; Kobayashi, H.; Hara, K.; Fukuoka, A. Quantitative Evaluation of Ball-
4
Milling Effects on the Hydrolysis of Cellulose Catalysed by Activated Carbon. Catal. Sci.
5
Technol. 2014, 4 (8), 2312.
6
(24)
7 8
Carbon 2002, 40 (2), 145. (25)
9
2011. (26)
12 13
Sluiter, A.; Hames, B.; Ruiz, R.; Scarlata, C.; Sluiter, J.; Templeton, D.; Crocker, D. Determination of Structural Carbohydrates and Lignin in Biomass, NREL/TP-510-42618;
10 11
Boehm, H. P. Surface Oxides on Carbon and Their Analysis: A Critical Assessment.
Evans, M. J. B.; Halliop, E.; MacDonald, J. A. F. The Production of Chemically-Activated Carbon. Carbon 1999, 37 (2), 269.
(27)
Kobayashi, H.; Yabushita, M.; Hasegawa, J.; Fukuoka, A. Synergy of Vicinal Oxygenated
14
Groups of Catalysts for Hydrolysis of Cellulosic Molecules. J. Phys. Chem. C 2015, 119
15
(36), 20993.
16
(28)
Hick, S. M.; Griebel, C.; Restrepo, D. T.; Truitt, J. H.; Buker, E. J.; Bylda, C.; Blair, R. G.
17
Mechanocatalysis for Biomass-Derived Chemicals and Fuels. Green Chem. 2010, 12 (3),
18
468.
19
(29)
20 21
Meine, N.; Rinaldi, R.; Schüth, F. Solvent-Free Catalytic Depolymerization of Cellulose to Water-Soluble Oligosaccharides. ChemSusChem 2012, 5 (8), 1449.
(30)
Shrotri, A.; Lambert, L. K.; Tanksale, A.; Beltramini, J. Mechanical Depolymerisation of
22
Acidulated Cellulose: Understanding the Solubility of High Molecular Weight Oligomers.
23
Green Chem. 2013, 15 (10), 2761.
ACS Paragon Plus Environment
22
Page 23 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Industrial & Engineering Chemistry Research
(31)
Otsuka, M.; Ishida, A.; Nakayama, Y.; Saito, M.; Yamazaki, M.; Murakami, H.;
2
Nakamura, Y.; Matsumoto, M.; Mamoto, K.; Takada, R. Dietary Supplementation with
3
Cellooligosaccharide Improves Growth Performance in Weanling Pigs. Anim. Sci. J. 2004,
4
75 (3), 225.
5
(32)
Hasunuma, T.; Kawashima, K.; Nakayama, H.; Murakami, T.; Kanagawa, H.; Ishii, T.;
6
Akiyama, K.; Yasuda, K.; Terada, F.; Kushibiki, S. Effect of Cellooligosaccharide or
7
Synbiotic Feeding on Growth Performance, Fecal Condition and Hormone Concentrations
8
in Holstein Calves. Anim. Sci. J. 2011, 82 (4), 543.
9
(33)
10 11
Mussatto, S. I.; Mancilha, I. M. Non-Digestible Oligosaccharides: A Review. Carbohydr. Polym. 2007, 68 (3), 587.
(34)
Yamaguchi, D.; Kitano, M.; Suganuma, S.; Nakajima, K.; Kato, H.; Hara, M. Hydrolysis
12
of Cellulose by a Solid Acid Catalyst under Optimal Reaction Conditions. J. Phys. Chem.
13
C 2009, 113 (8), 3181.
14 15
(35)
Franzidis, J.-P.; Porteous, A.; Anderson, J. The Acid Hydrolysis of Cellulose in Refuse in a Continuous Reactor. Conserv. Recycl. 1982, 5 (4), 215.
16
ACS Paragon Plus Environment
23
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 1 42x14mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 24 of 29
Page 25 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Figure 2 41x20mm (600 x 600 DPI)
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 3 161x56mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 26 of 29
Page 27 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
Figure 4 65x51mm (300 x 300 DPI)
ACS Paragon Plus Environment
Industrial & Engineering Chemistry Research
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 5 82x114mm (300 x 300 DPI)
ACS Paragon Plus Environment
Page 28 of 29
Page 29 of 29
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Industrial & Engineering Chemistry Research
TOC 39x19mm (300 x 300 DPI)
ACS Paragon Plus Environment