Enhanced sulfur tolerance of nickel-based anodes for oxygen-ion conducting solid-oxide fuel cells by incorporating a secondary water storing phase Feng Wang, Wei Wang, Jifa Qu, Yijun Zhong, Moses O. Tade, and Zongping Shao Environ. Sci. Technol., Just Accepted Manuscript • Publication Date (Web): 17 Sep 2014 Downloaded from http://pubs.acs.org on September 29, 2014
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Environmental Science & Technology is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 36
Environmental Science & Technology
1
Enhanced sulfur tolerance of nickel-based anodes for
2
oxygen-ion conducting solid-oxide fuel cells by
3
incorporating a secondary water storing phase
4
Feng Wang1, Wei Wang2*, Jifa Qu1, Yijun Zhong1, Mose O. Tadé2, Zongping Shao1,2*
5 6 7 8 9
1
State Key Laboratory of Materials-Oriented Chemical Engineering, College of Chemistry &
Chemical Engineering, Nanjing Tech University, No.5 Xin Mofan Road, Nanjing 210009, China 2
Department of Chemical Engineering, Curtin University, Perth, WA 6845, Australia
* Corresponding Authors
10
Telephone: +61-8-92665602. Email:
[email protected] (W. Wang)
11
Telephone: +86-25-83172242. Email:
[email protected] (Z. Shao)
12
1
ACS Paragon Plus Environment
Environmental Science & Technology
13
Page 2 of 36
TABLE OF CONTENTS
14
2
ACS Paragon Plus Environment
Page 3 of 36
15
Environmental Science & Technology
ABSTRACT
16
In this work, Ni+BaZr0.4Ce0.4Y0.2O3-δ (Ni+BZCY) anode with high water storage
17
capability is used to increase the sulfur tolerance of nickel electrocatalysts for solid oxide fuel
18
cells (SOFCs) with oxygen-ion conducting Sm0.2Ce0.8O1.9 (SDC) electrolyte. Attractive power
19
outputs are still obtained for cell with Ni+BZCY anode operating on hydrogen fuels containing
20
100-1000 ppm H2S, while for a similar cell with Ni+SDC anode it displays much reduced
21
performance by introducing only 100 ppm H2S into hydrogen. Operating on a hydrogen fuel
22
containing 100 ppm H2S at 600 oC and a fixed current density of 200 mA cm-2, a stable power
23
output of 148 mW cm-2 is well maintained for a cell with Ni+BZCY anode within a test period of
24
700 min, while it was decreased from an initial value of 137 mW cm-2 to only 81 mW cm-2 for a
25
similar cell with Ni+SDC anode after a test period of only 150 min. After the stability test, loss of
26
Ni percolating network and reaction between nickel and sulfur are appeared over Ni+SDC anode,
27
but it is not observed for Ni+BZCY anode. It highly promises the use of water-storing BZCY as
28
anode component in improving sulfur tolerance for SOFCs with oxygen-ion conducting SDC
29
electrolyte.
3
ACS Paragon Plus Environment
Environmental Science & Technology
30
Page 4 of 36
1. INTRODUCTION
31
Fuel cells are well recognized as an outstanding clean power generation technology,
32
characterized by high energy conversion efficiency, low emissions of greenhouse gas such as
33
CO2 and environmental pollutants like NOx, and size flexibility. Among various types of fuel
34
cells, solid oxide fuel cells (SOFCs) have received particular attention because of some additional
35
important advantages, such as fuel flexibility, high-quality exhaust heat and a wide range of
36
material selection for main cell components.1-3 Actually all combustible fuels, such as hydrogen,
37
hydrocarbons, carbon, alcohols, natural gas and biogas, could be direct fuels of SOFCs.4-8
38
For scientific in-lab research purpose, a fuel with simple component is often used for the
39
investigation of fuel cell performance, such as pure hydrogen, methane and hydrocarbons.
40
However, for practical applications, the fuel composition is much more complicated. As we know,
41
there are no natural resources of hydrogen, while most hydrogen is produced by reforming of
42
natural gas or coal. Since natural gas and coal contain a certain level of sulfur impurity, while the
43
state-of-the-art Ni-based cermets anodes are very sensitive to sulfur poisoning,9-14 the poisoning
44
of the anodes by sulfur in a practical fuel is thus a big concern. Actually, natural gas or biogas,
45
the most promising fuel for SOFCs, contain a high concentration of H2S (> 50 ppm),15,
46
well exceeds the upper limit (10 ppm) for stable operation of a SOFC with conventional Ni-based
47
cermet anodes.17,
48
introducing into fuel cell system. For example, hydrodesulfurization is a useful technique for
49
reducing sulfur content in high sulfur-containing fuels; however, it is difficult to reduce the sulfur
50
concentration to lower than 10 ppm.19, 20 Some sorbents such as activated carbon, zeolites are
51
useful for reducing sulfur levels to a lower extent than hydrodesulfurization and have received
52
increasing attention recently.21-24 However, there are several drawbacks associated with this
18
16
which
Thereby, fuel processing is required to reduce the sulfur content before
4
ACS Paragon Plus Environment
Page 5 of 36
Environmental Science & Technology
53
process, such as production of toxic carbonyl sulfide (COS) gas and difficulty to regenerate the
54
activated carbon and zeolites.
55
Electrode materials modification and operation conditions optimization are two most
56
important ways for improving the sulfur tolerance of Ni-based anodes. For example, surface
57
modification with some oxides such as CeO2 and doped CeO2 was found to be effective in
58
improving sulfur tolerance of Ni+YSZ anode.25-27 In those studies, CeO2 or doped CeO2 particles
59
were deposited over Ni+YSZ anode surface randomly through infiltration, which could have a
60
negative effect on the electrode porosity. In addition, Ni-Sm doped ceria (SDC) often showed
61
better sulfur tolerance than Ni+YSZ since CeO2 has been used as a high temperature desulfurizer
62
agent.28 In another study, it was found the presence of 10 vol.% water in fuel gas effectively
63
promoted the performance recoverability to a large extent of SOFCs operating on sulfur-
64
containing fuel.29 Wang and Liu further predicted the regeneration of sulfur-poisoned nickel by
65
O2 and H2O and found that sulfur adsorption on the nickel surface can only be cleaned with
66
water.30 However, since water is not a fuel, to maximize the fuel efficiency, the water content in a
67
fuel gas should be as low as possible.
68
Recently, M.L. Liu from Georgia Institute of Technology reported the superior sulfur
69
tolerance/coking resistance of proton-conductor based anodes, in which the proton-conducting
70
phase acted as the main component of anode ceramic phase, used to decorate conventional
71
Ni+YSZ anode surface or in-situ formed in the Ni+YSZ anode by the addition of BaCO3.31-33 As
72
we know, for SOFCs with oxygen-ion conducting electrolyte, the fuel oxidation will occur at the
73
anode side. If a hydrocarbon or hydrogen is applied as the fuel, water will be produced at the
74
anode side under current polarization. This water can be used for the elimination of carbon/sulfur
75
deposition over the anode. However, the water concentration varies from time to time in the 5
ACS Paragon Plus Environment
Environmental Science & Technology
Page 6 of 36
76
anode chamber of a SOFC with oxygen-ion conducting electrolyte, depending on the operation
77
conditions. A similar variation of oxygen concentration was also appeared in automobile exhaust
78
treatment. In that case, a ceria is used to act as an oxygen storage-and-release component to
79
stabilize the local oxygen partial pressure at the catalyst surface even when the air-to-fuel ratio in
80
the engine exhaust fluctuates with time.34 Similarly, a water storage material may be beneficial
81
for improving carbon/sulfur removal over the anode. M.L. Liu et al. demonstrated that nano BaO
82
modified Ni+YSZ anode showed high sulfur tolerance, and they further pointed out that the high
83
performance was closely related to the water adsorption capability of nanosized BaO.35 As
84
compared to surface water adsorption of BaO nanoparticles, proton-conducting perovskite oxides
85
have bulk water storage capability, in particular at lower temperatures.36-38 More recently,
86
Sengodan et al. have used infiltration method to modify the conventional Ni/YSZ anode by
87
BaZr0.1Ce0.7Y0.1Yb0.1O3-δ (BZCYYb) to improve the sulfur tolerance.32 However, due to limited
88
amount of proton conductor in the Ni-based anode by infiltration, the sulfur tolerance was not
89
satisfied at higher H2S contents in the fuel. Indeed, we have demonstrated recently that those
90
proton conducting phases could be used as water storage material and the whole ceramic phase to
91
significantly improve the coking resistance of nickel-based anodes for operating on ethanol
92
fuel.39
93
Similarly, a water-storing material may also be applied to facilitate the elimination of
94
sulfur adsorption over the nickel surface, thus improving the sulfur tolerance of SOFC anode.
95
Figure 1 shows the proposed mechanism for water-induced sulfur removal process on an anode
96
with water storage capability based on proton conducting oxide. Firstly, the H2 in the fuel is
97
oxidized by the O2- from the cathode on the triple phase boundary (TPB) with the generation of
98
water; in parallel, sulfur absorbs on the surface of Ni to produce surface-adsorbed sulfur (SNi*).
6
ACS Paragon Plus Environment
Page 7 of 36
Environmental Science & Technology
99
Secondary, the water incorporation or storage into the proton-conducting oxide with the
100
formation of (OH)o species is happened. Then, the incorporated (OH)o reacts with SNi* to
101
generate SO2 and H2. Finally, SO2 is removed from the Ni surface while H2 is oxidized by O2- to
102
form H2O.
103 104
Figure 1. Proposed mechanism for water-induced sulfur removal process on the Ni-based anode
105
with a water-storing phase.
106
To support our above consideration, we fabricated similar cells with Ni+BZCY anode and
107
SDC electrolyte, which were previously used for coking resistance test,39 and operated them on
108
H2S-containing fuels. The effect of H2S contents (100, 200 and 1000 ppm) in the H2 fuel gas on
109
the cell performance was systematically studied. For comparison, Ni+Sm0.2Ce0.8O1.9 (SDC) anode,
110
which has negligible water storing capability, was conducted in the same way. In addition, the
111
possible reasons for the different tolerance of these two anodes towards sulfur were proposed.
112
This study will provide some useful guidelines for the development of sulfur-resistant anodes for
113
SOFCs operating on the fuel with high H2S amount at lower temperatures.
7
ACS Paragon Plus Environment
Environmental Science & Technology
114
Page 8 of 36
2. EXPERIMENTAL SECTION
115
NiO+BZCY and NiO+SDC anodes with 60 wt.% NiO were synthesized by a solution
116
combustion method based on glycine nitrite process.39 The powders from the direct combustion
117
process were further calcined at 1000 oC for 5 h in static air to yield the primary anode powders
118
for the dry-pressing process. Ba0.5Sr0.5Co0.8Fe0.2O3- (BSCF), Sm0.5Sr0.5CoO3- (SSC) cathodes
119
and SDC electrolyte were prepared by an EDTA-citrate complexing process.35, 36 The fuel cells
120
used in this study were in a 60 wt.% NiO + 40 wt.% BZCY or SDC cermet anode-supported thin-
121
film SDC electrolyte configuration, and the bilayer cells were fabricated by a dual dry-
122
pressing/sintering process.40 The BSCF or SSC cathode slurry was sprayed on the central surface
123
of the electrolyte layer for the bi-layer cells and fired at 1000 oC in static air for 2 h to form the
124
complete cells for later performance investigation. The thicknesses of the anode, cathode and the
125
electrolyte are about 500, 15 and 20 µm, respectively. The active area of the cell is 0.48 cm-2. The
126
dimensions of the three SOFC cells are about 13 mm in diameter after calcined at 1400 oC. The
127
porosities of the SOFC cells are about 40 % after the hydrogen reduction process.
128
The phase structures of the various samples were examined by an X-ray diffractometer
129
(XRD, D8 Advance, Bruker, Germany) equipped with a Cu K radiation (λ=0.1541 nm). The
130
cross-sectional morphologies of the fuel cells were examined by a scanning electron microscope
131
(SEM, S3400) equipped with an EDX detector. The surface morphologies of the fuel cells were
132
examined by a scanning electron microscope (SEM, S4800). The water storage in the anode
133
materials were investigated by Fourier Transform Infrared spectroscopy (Thermo Nicolet iS10).
134
For this investigation, the samples were first reduced at 750 oC for 1 h and then exposed to 20
135
vol.% H2O/Ar at 150 oC for 1 h.
8
ACS Paragon Plus Environment
Page 9 of 36
Environmental Science & Technology
136
The I-V polarization curves of the fuel cells were obtained using a Keithley 2420 source
137
meter in the 4-probe mode. During the measurements, H2 or H2S-containing H2 fuels was fed into
138
the anode chamber while ambient air was used as the cathode atmosphere. The flow rate of H2 or
139
H2+H2S fuel gas was controlled at 80 mL min-1 [STP]. The cell resistance was determined using
140
electrochemical impedance spectroscopy (EIS) with a Solartron 1260 frequency response
141
analyzer in combination with a Solartron 1287 potentiostat. The frequencies used for the EIS
142
measurements ranged from 0.1 to 1000 kHz for signal amplitude of 20 mV.
143
3. RESULTS AND DISCUSSION
144
Figure S1 shows XRD patterns of Ni+SDC and Ni+BZCY anode materials after the calcination at
145
1400 oC for 5 h at a ramping rate of 5 oC min-1, before and after the hydrogen reduction process.
146
SDC and BZCY crystalline phases were detected respectively for Ni+SDC and Ni+BZCY
147
samples, before and after the hydrogen reduction. NiO was completely reduced to Ni in the
148
reduction process for these two anodes. Figure S2a&b shows the FE-SEM images of the reduced
149
Ni+SDC and Ni+BZCY anodes. It was found that the two phases in the anodes are well
150
connected and no etched interfaces of Ni and BZCY/SDC were observed.
151
In our previous work, we have demonstrated that Ni+BZCY anode catalyst had a strong
152
water storage capability, much higher than the conventional Ni-based catalysts such as Ni-
153
Ce0.8Zr0.2O2 and Ni-Al2O3.39 In this study, the water storage capabilities of the Ni+BZCY and
154
Ni+SDC anodes were also comparatively studied by FTIR with the corresponding spectra
155
presented in Figure 2. The small peaks of the two anodes before water treatment come from the
156
surface absorbed water in the preparation process for the samples. As can be seen, after the
157
treatment in water-containing atmosphere, Ni+BZCY anode displayed a much bigger water
158
desorption peak at around 3430 cm-1 in the FTIR spectra than the fresh reduced Ni+BZCY anode
9
ACS Paragon Plus Environment
Environmental Science & Technology
Page 10 of 36
159
and also the water-treated Ni+SDC anode. In addition, the difference in intensity of the water
160
desorption peaks for the Ni+SDC anodes before and after the water treatment not as large as
161
Ni+BZCY, suggesting the poor water storage capability of the Ni+SDC anode. These results
162
suggested that the current Ni+BZCY anode also had a much higher water storage capability than
163
Ni+SDC anode. As we know water vapor can facilitate the sulfur oxidation reaction, thus
164
improved sulfur tolerance is expected, which will be studied in later text.
165 166
Figure 2. Fourier Transform Infrared spectroscopy of the reduced anodes before and after the
167
water adsorption.
168
Anode-supported thin-film SDC electrolyte-based fuel cells using BSCF as a cathode were
169
fabricated and tested. The thickness of the electrolytes for different cells was fixed at around 20
170
μm by precisely controlling the amount of SDC powder in the dry pressing process. Figure S3
171
shows typical SEM images of the fuel cells with reduced Ni+BZCY and Ni+SDC anodes from
172
the cross-sectional view. The SDC electrolyte was well densified without any penetrating
173
pinholes. In this section, the various fuel cells were first tested using pure hydrogen as the fuel.
174
Typical power outputs of these two fuel cells at various temperatures are shown in Table 1. As
10
ACS Paragon Plus Environment
Page 11 of 36
Environmental Science & Technology
175
can be seen, the cell delivered peak power densities (PPDs) of 678, 1018, 1143, 1043 and 926
176
mW cm-2 at 550, 600, 650, 700 and 750 oC, respectively, which are comparable to the literature
177
results with similar cells.41, 42 The lower power outputs at 750 and 700 oC than that at 650 oC is
178
due to the increased current leakage within the SDC electrolyte. The fuel cell with Ni+BZCY
179
anode also demonstrated promising power outputs with PPDs of 499, 596, 729, 894 and 1032
180
mW cm-2 at 550, 600, 650, 700 and 750 oC, respectively. On the other hand, as shown in Figure
181
S4, high open circuit voltages (OCVs) were obtained by the fuel cell with Ni+BZCY anode at all
182
temperatures and for instance, 1.01 V at 750 oC, much higher than 0.709 V for a cell with
183
Ni+SDC anode. The improved OCVs of the cell with Ni+BZCY anode should be attributed to the
184
beneficial reaction of BZCY and SDC to form an interfacial layer between the anode and
185
electrolyte.43
186
In addition to H2 fuel, we have also tested the fuel cells on H2 fuels containing different
187
amounts of H2S (1000 ppm, 200 ppm and 100 ppm). Table 1 also lists the PPDs of the fuel cells
188
with Ni+SDC and Ni+BZCY anodes at different temperatures operating on H2+1000 ppm H2S,
189
H2+200 ppm H2S and H2+100 ppm H2S gas mixtures as the fuels. For the Ni+SDC anode, when
190
operated on H2+1000 ppm H2S as the fuel, PPDs of 64, 189, 477, 738 and 846 mW cm-2 were
191
reached at 550, 600, 650, 700 and 750 oC, respectively. A sharp decrease in cell power output
192
was observed with the decrease of temperature when operating on H2+1000 ppm H2S fuel, and
193
the PPD decreased to 738 mW cm-2 at 700 oC, which is only 70.7 % compared to the value of
194
hydrogen fuel. On the other hand, for the same H2+1000 ppm H2S fuel, Ni+BZCY anode showed
195
a better sulfur tolerance sine the PPD reached 98.1 % of the value of H2 fuel. However, at the
196
temperatures lower than 700 oC, the power outputs on H2+1000 ppm H2S fuel with Ni+BZCY
197
anode were still much lower than those of H2.
11
ACS Paragon Plus Environment
Environmental Science & Technology
Page 12 of 36
198
Table 1. PPDs of fuel cells with Ni+BZCY and Ni+SDC anodes operating on different fuels at
199
various temperatures. Anodes
Ni+BZCY
Ni+SDC
Fuels H2 1000 ppm H2S+H2 200 ppm H2S+H2 100 ppm H2S+H2 H2 1000 ppm H2S+H2 200 ppm H2S+H2 100 ppm H2S+H2
750 oC 1032 1010 1017 1019 926 846 894 904
PPDs at different temperatures (mW cm-2) 700 oC 650 oC 600 oC 550 oC 916 729 596 499 877 304 137 121 901 660 405 218 913 674 522 290 1043 1143 1018 678 738 477 189 64 905 572 293 103 1033 748 384 181
200 201
Taking PPDs of the cells with these two anodes operated on H2 as a criterion, the
202
reduction ratios of the PPDs on the H2+200 ppm H2S fuel at different temperatures are shown in
203
Figure 3. It was found that the reduction of operational temperature led to a much faster decrease
204
in PPDs, suggesting much more serious sulfur poisoning at the reduced temperatures for these
205
two anodes. This phenomenon was in good agreement with that reported in literatures since the
206
sulfur desorption on the Ni surface became faster at higher temperature.9,
207
Ni+BZCY anode displayed a much more moderate reduction ratio than Ni+SDC, for example,
208
9.4 % compared with 50 % at 650 oC, suggesting much better sulfur tolerance of Ni+BZCY due
209
to the higher water storage capability. With the further reduction of H2S concentration to 100
210
ppm, it was found that the cell performance of the Ni+SDC anodes below 700 oC was still not
211
satisfied although H2S contents was reduced from 1000 ppm to 100 ppm in the fuel. The above
212
results suggested that Ni+SDC composites were not a practical anode for SOFCs operating on
213
H2S-containing fuels at intermediate temperatures. For the fuel cell with Ni+BZCY anode, the
214
power outputs on H2+100 ppm H2S fuel were comparable to those on hydrogen at the
10
In addition,
12
ACS Paragon Plus Environment
Page 13 of 36
Environmental Science & Technology
215
temperatures from 600 to 750 oC, suggesting high sulfur tolerance of this anode for the fuel with
216
100 ppm H2S. As compared with the results of Ni+SDC anode, it was found that Ni+BZCY
217
anode displayed a much superior sulfur tolerance, which could be attributed to the enhanced
218
water storage capability of Ni+BZCY.
219 220
Figure 3. The reduction ratios of the PPDs for the cell with Ni+BZCY and Ni+SDC anodes
221
operated on the H2+200 ppm H2S fuel compared with H2 fuel at different temperatures.
222
More specifically, the I-V, I-P curves and EIS of the fuel cells with these two anodes
223
operating on various fuels at 600 oC are presented in Figure 4. It is clear that the fuel cell with
224
Ni+BZCY anode showed a slightly lower power output on H2+100ppm H2S or 200 ppm H2S
225
compared with H2 fuel, while the addition of H2S even in the amount of 100 ppm could obviously
226
decrease the electrochemical activity of Ni+SDC anode operating on H2 fuel. To obtain more
227
information to interpret the cell performance with different anodes operating on various fuels, the
228
EIS of the fuel cells was measured with the results shown in Figure 4c&d. In EIS, the high-
229
frequency offset on the real axis represents the electrolyte resistances, whereas the difference
230
between the high and low frequency intercepts on the real axis is associated with electrode
231
polarization resistances including the contributions of both anode and cathode. As shown in 13
ACS Paragon Plus Environment
Environmental Science & Technology
Page 14 of 36
232
Figure 4c, the fuel cell with Ni+SDC anode operating on H2 fuel showed the lowest electrode
233
polarization resistance and the fuel cell with H2+1000 ppm H2S fuel presented the largest value,
234
which was in good agreement with the results in Figure 4a. For the fuel cell with Ni+BZCY
235
anode, besides the H2+1000 ppm H2S fuel, the electrode polarization resistances were
236
comparable for the other three fuels (Figure 4d). It was also found that there were some
237
differences for the electrolyte resistances for the two fuel cells, especially for the cell with
238
Ni+SDC anode. The difference in electrolyte resistance could be attributed to the reconstruction
239
and diffusion of Ni and the loss of percolating Ni network.44 The sharp increase in the electrode
240
polarization and electrolyte resistances of Ni+SDC in H2S-containing fuels resulted in the
241
obvious decrease in power outputs. In addition, the cell with Ni+BZCY anode displayed similar
242
electrode polarization and electrolyte resistances for the 100 or 200 ppm H2S-containing fuels.
243
14
ACS Paragon Plus Environment
Page 15 of 36
Environmental Science & Technology
244 245
Figure 4. I-V, I-P curves and EIS for the fuel cells with Ni+SDC (a, c) and Ni+BZCY (b, d)
246
anode operating on different fuels at 600 °C.
247
To determine the effect of water storage capability of the anodes on the operational
248
stability, two similar fuel cells were first polarized under a constant current density of 200 mA
249
cm-2 for 20 h at 600 oC by operating on H2 to obtain a stable performance, and then the stability
250
tests were conducted by operating on 100 ppm H2S-containing H2 fuel with Ni+BZCY and
251
Ni+SDC anodes. To avoid the possible CO2 poisoning and phase transition of BSCF cathode,
252
which may mask the effect of H2S poisoning on the degradation of cell performance, SSC was
253
used as cathode material for the stability test instead. In the stability test, a mesh-like
254
morphological structure of silver paste was drawn with a stick directly onto the SSC cathode
255
surface to create the current collector, and then fired at 180 °C for 1 h.45 Figure 5 showed the
256
time dependence of the voltage under different current densities and temperatures. For the cell
257
with Ni+SDC anode, the voltage was not stable and the cell was failed after a continuous
258
operation for 150 minutes under a current density of 200 mA cm-2 at 600 oC. In contrast, the cell
259
operation was stable for 700 minutes under different current densities and temperatures when
260
Ni+BZCY anode was applied. This improvement in the operational stability is clearly due to the
261
improved water storage capability and then enhanced sulfur tolerance of Ni+BZCY anode.
15
ACS Paragon Plus Environment
Environmental Science & Technology
Page 16 of 36
262 263
Figure 5. Time-dependent voltages of the fuel cells with Ni+SDC and Ni+BZCY anodes
264
operating on H2+100 ppm H2S as the fuel under different current densities and temperatures.
265
The element distributions over the anode in the fuel cells after the stability test were
266
investigated by SEM-EDX at selected regions and the typical SEM images are shown in Figure
267
S5. First of all, the sulfur content of the active layer of the anode (about 10-20 µm in depth near
268
the anode-electrolyte interface) was studied with results shown in Figure S5. For the comparison
269
purpose, the sulfur amount of the SDC electrolyte was also studied. It was found that the sulfur
270
contents of the active layer of the Ni+BZCY anode and the SDC electrolyte are comparable.
271
However, the sulfur amount of the active layer of the Ni+SDC anode was more than 10 times
272
higher than that of the similar position of the Ni+BZCY anode. As shown in Figure S6, the XRD
273
results of these two anodes after the operational stability test suggested that no obvious difference
274
was observed for the Ni+BZCY anode while there were some obvious diffraction peaks assigned
275
to NiSx phases in the XRD pattern of the Ni+SDC after the stability test. It suggested that more
276
severe sulfur poisoning of Ni+SDC anode was appeared, which could be accountable for the
277
poorer operational stability. Furthermore, the anode surface of used fuel cells was also conducted 16
ACS Paragon Plus Environment
Page 17 of 36
Environmental Science & Technology
278
by SEM as shown in Figure 6. Comparison of micrographs for the anodes operated in pure H2
279
(Figure S2) and after operation on H2+H2S fuels in Figure 6 shows microstructural differences
280
expressed as etched interfaces of Ni and SDC originated from the reaction of Ni with S after the
281
operational stability test, which is in good agreement with the literature.46 On the other hand, for
282
the Ni+BZCY anode as shown in Figure 6, no obvious differences were observed as compared
283
with the SEM image in Figure S2. The EDX results of the surfaces of these two anodes were also
284
shown in Figure S7. It was found that the sulfur content on the Ni+SDC anode surface was 12
285
times higher than that of the Ni+BZCY anode, further confirming the excellent sulfur tolerance
286
of the Ni+BZCY anode.
287 288
Figure 6. SEM photos of the Ni+BZCY (a) and Ni+SDC (b) anodes after the operational stability
289
test from the surface view.
290
Hauch et al. have demonstrated a possible sulfur poisoning mechanism for nickel catalyst
291
that the sulfur poisoning could result in the loss of percolating Ni network.44 For the fuel cells
292
operating on H2, the Ni particles in the anodes are well distributed and a well percolating network
293
exists. In this study, EDX was used to study the Ni contributions in these two anodes before and
294
after sulfur poisoning, as shown in Table 2. The Ni distributions in the Ni+BZCY anodes after
17
ACS Paragon Plus Environment
Environmental Science & Technology
Page 18 of 36
295
stability tests were uniform and Ni contents were comparable to those of the fresh reduced anode
296
and for instance, the Ni amount in the used anode was 61.3±5.6 wt.% compared with the value of
297
63.6±5.4 wt.% for the fresh one. In addition, the Ni amount in the used Ni+SDC anode was
298
28.8±15.9 wt.% compared with the value of 59.8±3.4 wt.% for the fresh one. In the Ni+SDC
299
anode, a percolating Ni network was lacking in the active layer of anode, resulting a rapid
300
decrease in cell performance. In summary, the degradation of the fuel cells with Ni+SDC anode
301
should be attributed to the loss of percolating Ni network and the harmful reaction of nickel and
302
sulfur. However, for the fuel cell with Ni+BZCY anode, the high water storage capability of the
303
anode could reduce the reaction between nickel and sulfur as well as the diffusion of Ni from the
304
active layer, and then, an improved operational stability was obtained.
305 306
Table 2. EDX results of the Ni contents for the two fuel cells before and after the operational
307
stability test. Anode Ni+SDC Ni+BZCY
Conditions
Ni contents in the different regions (%) Region 1
Region 2
Region 3
Region 4
Before stability test
59.2
56.4
62.3
57.8
After stability test
44.7
21.4
12.9
20.9
Before stability test
64.1
69.0
58.2
65.3
After stability test
63.7
63.4
66.9
55.6
308 309
In conclusion, a Ni+BZCY composite with high water storage capability was synthesized
310
and demonstrated as a promising alternative anode material for SOFCs operating on H2S-
311
containing fuels. The effect of H2S content and water storage capability on the sulfur poisoning
312
behavior of the anodes for SOFCs was systematically studied. The Ni+BZCY anode was superior
18
ACS Paragon Plus Environment
Page 19 of 36
Environmental Science & Technology
313
to the state-of-the-art Ni+SDC anode in sulfur tolerance, especially for the lower temperatures
314
and higher H2S amount. A significant improvement in sulfur tolerance of the Ni+BZCY anode
315
was observed at low temperatures with the reduction of H2S amount in the fuel; however, there
316
was no increase in sulfur tolerance for Ni+SDC anode even with 100 ppm H2S in the fuel. An
317
obvious degradation was observed for the Ni+SDC anode while the power output of the fuel cell
318
with Ni+BZCY anode was well maintained. It was found that the degradation of the Ni+SDC
319
anode could be assigned to the loss of Ni percolating network and the harmful reaction between
320
nickel and sulfur of Ni and SDC ceramic phase. The high water storage capability of Ni+BZCY
321
anode could significantly reduce the above phenomenon in the stability tests. In sum, the above
322
results clearly suggest the potential applications of the Ni+BZCY composite with high water
323
storage capability for the anode materials of SOFCs operating on various sulfur-containing fuels.
324 325
ASSOCIATED CONTENT
326
Supporting Information
327
(1) XRD patterns, SEM photos, EDX profiles of Ni+BZCY and Ni+SDC anodes under different
328
test conditions, (2) I-V, I-P curves for the cells with Ni+SDC and Ni+BZCY anodes, This
329
material is available free of charge via the Internet at http://pubs.acs.org.
330
NOTES
331
The authors declare no competing financial interest.
332 333
19
ACS Paragon Plus Environment
Environmental Science & Technology
Page 20 of 36
334
ACKNOWLEDGMENT
335
This work was supported by the program of “National Science Foundation for Distinguished
336
Young Scholars of China” under contract No. 51025209 and the Doctoral Fund of Ministry of
337
Education of China (20113221110002).
338
REFERENCES
339
(1)
340
nickel-based anodes operating on methane and related fuels. Chem. Rev. 2013, 113 (10), 8104-
341
8151.
342
(2)
Wei, T.; Singh, P.; Gong, Y.; Goodenough, J.B.; Huang, Y.H.; Huang, K. Sr3-3xNa3xSi3O9-
343
1.5x
(x= 0.45) as a superior solid oxide-ion electrolyte for intermediate temperature-solid oxide
344
fuel cells. Energy Environ. Sci. 2014, 7 (5), 1680-1684.
345
(3)
346
Electric power and synthesis gas co-generation from methane with zero waste gas emission.
347
Angew. Chem. Int. Ed. 2011, 50 (8), 1792-1797.
348
(4)
349
for direct hydrocarbon-type solid oxide fuel cells. J. Am. Chem. Soc. 2011, 133 (48), 19399-
350
19407.
351
(5)
352
power output by integrating with in situ catalytic reverse boudouard reaction. Electrochem.
353
Commun. 2009, 11 (6), 1265-1268.
Wang, W.; Su, C.; Wu, Y.Z.; Ran, R.; Shao, Z.P. Progress in solid oxide fuel cells with
Shao, Z.P.; Zhang, C.M.; Wang, W.; Su, C.; Zhou, W.; Zhu, Z.H.; Park, H.J.; Kwak, C.
T.H. Shin, S. Ida, T. Ishihara, Doped CeO2-LaFeO3 composite oxide as an active anode
Wu, Y.Z.; Su, C.; Zhang, C.M.; Ran, R.; Shao, Z.P. A new carbon fuel cell with high
20
ACS Paragon Plus Environment
Page 21 of 36
Environmental Science & Technology
354
(6)
Wang, W.; Wang, F.; Ran, R.; Park, H.J.; Jung, D.W.; Kwak, C.; Shao, Z.P. Coking
355
suppression in solid oxide fuel cells operating on ethanol by applying pyridine as fuel additive. J.
356
Power Sources 2014, 265, 20-29.
357
(7)
358
solid oxide fuel cells with ruthenium anode in natural gas. J. Power Sources 2013, 243, 1-9.
359
(8)
360
biogas. Int. J. Hydrogen Energy 2010, 35 (15), 7905-7912.
361
(9)
362
Fuchino, H.; Tsujimoto, K.; Uchida, Y.; Jingo, N.; H2S poisoning of solid oxide fuel cells. J.
363
Electrochem. Soc. 2006, 153 (11), A2023-A2029.
364
(10)
365
solid oxide fuel cells. J. Electrochem. Soc. 2007, 154 (2), B201-B206.
366
(11)
367
containing fuels. J. Power Sources 2011, 196 (17), 7271-7276.
368
(12)
369
model for biogas steam reformingon Ni and catalyst deactivation due to sulfur poisoning. Appl.
370
Catal. A: Gen. 2014, 471,118-125.
371
(13)
372
catalyst during steam reforming of model biogas: An experimental investigation. Int. J. Hydrogen
373
Energy, 2014, 39 (1), 297-304.
Takagi, Y.; Kerman, K.; Ko, C.; Ramanathan, S. Operational characteristics of thin film
Shiratori, Y.; Ijichi, T.; Oshima, T.; Sasaki, K. Internal reforming SOFC running on
Sasaki, K.; Susuki, K.; Iyoshi, A.; Uchimura, M.; Imamura, N.; Kusaba, H.; Teraoka, Y.;
Zha, S.; Cheng, Z.; Liu, M.L. Sulfur poisoning and regeneration of Ni-based anodes in
Hagen, A.; Rasmussen, J.F.B.; Thydén, K. Durability of solid oxide fuel cells using sulfur
Appari, S.; Janardhanan, V.M.; Bauri, R.; Jayanti, S.; Deutschmann, O. A detailed kinetic
Appari, S.; Janardhanan, V.M.; Bauri, R.; Jayanti, S. Deactivation and regeneration of Ni
21
ACS Paragon Plus Environment
Environmental Science & Technology
Page 22 of 36
374
(14)
Ashrafi, M.; Pfeifer, C.; Pröll, T.; Hofbauer, H. Experimental study of model biogas
375
catalytic steam reforming: 2. Impact of sulfur on the deactivation and regeneration of Ni-based
376
catalysts. Energy & Fuels 2008, 22 (6), 4190-4195.
377
(15)
378
anode materials for H2S-containing CH4 fueled solid oxide fuel cells. J. Power Sources 2012, 213,
379
69-77.
380
(16)
381
methane containing fuel. Fuel Cells 2010, 10 (6), 1135-1142.
382
(17)
383
Energy 2008, 33 (21), 6316-6321.
384
(18)
385
SOFC anode: Part I. Dependence on temperature, time, and impurity concentration. Solid State
386
Ionics 2000,132 (3-4), 261-269.
387
(19)
388
desulfurization and deep dearomatization. Appl. Catal. B: Environ. 2003, 41 (1-2), 207-238.
389
(20)
390
pre-treated gas oil over nanosized MoS2, CoMo-sulfide, and commercial CoMo/Al2O3 catalysts.
391
J. Colloid Interface Sci. 2012, 372 (1), 121-129.
392
(21)
393
species from a straight run gas oil over activated carbons for its deep hydrodesulfurization. Appl.
394
Catal. B: Environ. 2004, 49 (4), 219-225.
Li, J.-H.; Fu, X.-Z.; Luo, J.-L.; Chuang, K.T.; Sanger, A.R. Application of BaTiO3 as
Rasmussen, J. F. B.; Hagen, A.; The effect of H2S on the performance of SOFCs using
Shiratori, Y.; Oshima, T.; Sasaki, K. Feasibility of direct-biogas SOFC. Int. J. Hydrogen
Matsuzaki, Y.; Yasuda I. The poisoning effect of sulfur-containing impurity gas on a
Song, C.; Ma, X. New design approaches to ultra-clean diesel fuels by deep
Farag, H.; Mochida, I. A comparative kinetic study on ultra-deep hydrodesulfurization of
Sano, Y.; Choi, K.-H.; Korai, Y.; Mochida, I. Adsorptive removal of sulfur and nitrogen
22
ACS Paragon Plus Environment
Page 23 of 36
Environmental Science & Technology
395
(22)
Cui, H.; Turn, S.Q.; Reese, M.A. Removal of sulfur compounds from utility pipelined
396
synthetic natural gas using modified activated carbons. Catal. Today 2009, 139 (4), 274-279.
397
(23)
398
Lemaire, M. Deep desulfurization: reactions, catalysts and technological challenges. Catal.
399
Today 2003, 84 (3-4), 129-138.
400
(24)
401
of diesel using ion-exchanged zeolites. Chem. Eng. Sci. 2006, 61 (8), 2599-2608.
402
(25)
403
nanocoating for sulfur tolerant ni-based anodes of solid oxide fuel cells. Electrochem. Solid-State
404
Lett. 2007, 10 (9), B135-B138.
405
(26)
406
h2s poisoning of ni/ysz anodes for solid oxide fuel cells. J. Electrochem. Soc. 2010, 157 (12),
407
B1825-B1830.
408
(27)
409
electrode by impregnation of Mo0.1Ce0.9O2+δ. J. Power Sources 2012, 204, 40-45.
410
(28)
411
oxide fuel cell application. J. Power Sources 2007, 168 (2), 289-298.
412
(29)
413
composition on H2S poisoning behavior evaluated using a disaggregation scheme. J.
414
Electrochem. Soc. 2009, 156 (12), B1383-B1388.
Breysse, M.; Djega-Mariadassou, G.; Pessayre, S.; Geantet, C.; Vrinat, M.; Pérot, G.;
Bhandari, V.M.; Ko, C.H.; Park, J.G.; Han, S.-S.; Cho, S.-H.; Kim, J.-N. Desulfurization
Kurokawa, H.; Sholklapper, T.Z.; Jacobson, C.P.; De Jonghe, L.C.; Visco, S.J. Ceria
Yun, J.W.; Yoon, S.P.; Han, J.; Park, S.; Kim, H.S.; Nam, S.W. Ceria coatings effect on
Chen, Y.; Bunch, J.; Jin, C.; Yang, C.; Chen, F.L. Performance enhancement of Ni-YSZ
Gong, M.; Liu, X.; Trembly, J.; Johnson, C. Sulfur-tolerant anode materials for solid
Li, T.S.; Miao, H.; Chen, T.; Wang, W.G.; Xu, C. Effect of simulated coal-derived gas
23
ACS Paragon Plus Environment
Environmental Science & Technology
Page 24 of 36
415
(30)
Wang, J.; Liu, M.L. Surface regeneration of sulfur-poisoned Ni surfaces under SOFC
416
operation conditions predicted by first-principles-based thermodynamic calculations. J. Power
417
Sources 2008, 176 (1), 23-30.
418
(31)
419
and coking tolerance of a mixed ion conductor for SOFCs: BaZr0.1Ce0.7Y0.2–xYbxO3–δ. Science
420
2009, 326 (5949), 126-129.
421
(32)
422
a Ni-YSZ anode through BaZr0.1Ce0.7Y0.1Yb0.1O3−δ infiltration. J. Electrochem. Soc. 2014, 161
423
(5), F668-F673.
424
(33)
425
cells: A promising power for transportation. Nano Energy 2012, 1 (3), 448-455.
426
(34)
427
storage capacity of nanocrystalline ceria and ceria-zirconia, J. Phys. Chem. B 2000, 104 (47),
428
11110-11116.
429
(35)
430
Liu, M.L. Promotion of water-mediated carbon removal by nanostructured barium oxide/nickel
431
interfaces in solid oxide fuel cells. Nat. Commun. 2011, 2, 357, DOI: 10.1038/ncomms1359.
432
(36)
433
oxide fuel cells: a critical review. Chem. Soc. Rev., 2010, 39 (11), 4355-4369.
Yang, L.; Wang, S.; Blinn, K.; Liu, M.; Liu, Z.; Cheng, Z.; Liu, M.L. Enhanced sulfur
Sengodan, S.; Liu, M.; Lim, T.; Shin, J.; Liu, M.L.; Kim, G. Enhancing sulfur tolerance of
Liu, M.; Choi, Y.; Yang, L.; Blinn, K.; Qin, W.; Liu, P.; Liu, M.L. Direct octane fuel
Mamontov, E.; Egami, T.; Brezny, R.; Koranne M.; Tyagi, S. Lattice defects and oxygen
Yang, L.; Choi, Y.; Qin, W.; Chen, H.; Blinn, K.; Liu, M.; Liu, P.; Bai, J.; Tyson, T.A.;
Fabbri, E.; Pergolesi, D.; Traversa, E. Materials challenges toward proton-conducting
24
ACS Paragon Plus Environment
Page 25 of 36
Environmental Science & Technology
434
(37)
Malavasi, L.; Fisher, C.A.J.; Islam, M.S. Oxide-ion and proton conducting electrolyte
435
materials for clean energy applications: structural and mechanistic features. Chem. Soc. Rev.,
436
2010, 39 (11), 4370-4387.
437
(38)
Kreuer, K.D. Proton-conducting oxides, Annu. Rev. Mater. Res. 2003, 33, 333-359.
438
(39)
Wang, W.; Su, C.; Ran, R.; Zhao, B.T., Shao, Z.P., Tade, M.O., Liu, S.M. Nickel-based
439
anode with water storage capability to mitigate carbon deposition for direct ethanol solid oxide
440
fuel cells. Chemsuschem 2014, 7 (6) 1719-1728.
441
(40)
442
acid treatment on the cathode performance of Ba0.5Sr0.5Co0.8Fe0.2O3−δ perovskite oxide via
443
combined EDTA-citric complexing process. J. Power Sources 2007, 174 (1), 237-245.
444
(41)
445
Ba0.5Sr0.5Co0.8Fe0.2O3−δ+Co3O4 composite electrode for IT-SOFCs with improved electrical
446
conductivity and catalytic activity. Electrochem. Commun. 2011, 13 (2), 197-199.
447
(42)
448
cell with novel BSCF cathode. J. Power Sources 2006, 161 (1), 123-128.
449
(43)
450
voltage and power output by utilizing beneficial interfacial reaction. Phys. Chem. Chem. Phys.
451
2012, 14 (35), 12173-12181.
452
(44)
453
overpotential on long-term degradation. J. Electrochem. Soc. 2014, 161 (6) F734-F743.
Zhou, W.; Ran, R.; Shao, Z.P.; Gu, H.X.; Jin, W.Q.; Xu, N.P. Significant impact of nitric
Chen, D.J.; Huang, C.; Ran, R.; Park, H.J.; Kwak, C.; Shao, Z.P. New
Liu, Q.L.; Khor, K.A.; Chan, S.H. High-performance low-temperature solid oxide fuel
Su, C.; Shao, Z.P.; Lin, Y.; Wu, Y.Z.; Wang, H.T. Solid oxide fuel cells with both high
Hauch, A.; Hagen, A.; Hjelm, J.; Ramos, T. Sulfur Poisoning of SOFC Anodes: Effect of
25
ACS Paragon Plus Environment
Environmental Science & Technology
Page 26 of 36
454
(45)
Chen, Y. B.; Wang, F.C.; Chen, D.J.; Dong, F.F.; Park, H.J.; Kwak, C.; Shao, Z.P. Role
455
of silver current collector on the operational stability of selected cobalt-containing oxide
456
electrodes for oxygen reduction reaction. J. Power Sources 2012, 210, 146-153.
457
(46)
458
dynamics of sulphur with Ni/GDC anode during SOFC operation at mid- and low-range
459
temperatures: An operando S K-edge XANES study. J. Power Sources 2013, 240, 448-457.
Nurk, G.; Huthwelker, T.; Braun, A.; Ludwig, C.; Lust, E.; Struis, R.P.W.J. Redox
460
26
ACS Paragon Plus Environment
Page 27 of 36
Environmental Science & Technology
TOC 180x100mm (150 x 150 DPI)
ACS Paragon Plus Environment
Environmental Science & Technology
Proposed mechanism for water-induced sulfur removal process on the Ni-based anode with a water-storing phase. 199x149mm (150 x 150 DPI)
ACS Paragon Plus Environment
Page 28 of 36
Page 29 of 36
Environmental Science & Technology
Fourier Transform Infrared spectroscopy of the reduced anodes before and after the water adsorption. 594x419mm (150 x 150 DPI)
ACS Paragon Plus Environment
Environmental Science & Technology
The reduction ratios of the PPDs for the cell with Ni+BZCY and Ni+SDC anodes operated on the H2+200 ppm H2S fuel compared with H2 fuel at different temperatures. 594x419mm (150 x 150 DPI)
ACS Paragon Plus Environment
Page 30 of 36
Page 31 of 36
Environmental Science & Technology
558x431mm (150 x 150 DPI)
ACS Paragon Plus Environment
Environmental Science & Technology
558x431mm (150 x 150 DPI)
ACS Paragon Plus Environment
Page 32 of 36
Page 33 of 36
Environmental Science & Technology
577x404mm (150 x 150 DPI)
ACS Paragon Plus Environment
Environmental Science & Technology
577x404mm (150 x 150 DPI)
ACS Paragon Plus Environment
Page 34 of 36
Page 35 of 36
Environmental Science & Technology
594x419mm (150 x 150 DPI)
ACS Paragon Plus Environment
Environmental Science & Technology
254x95mm (150 x 150 DPI)
ACS Paragon Plus Environment
Page 36 of 36