Subscriber access provided by UNIV OF CALIFORNIA SAN DIEGO LIBRARIES
Article
Fluorescent multifunctional polysaccharides for sustainable supramolecular functionalization of fibers in water Olga Grigoray, Holger Wondraczek, Annett Pfeifer, Pedro Fardim, and Thomas Heinze ACS Sustainable Chem. Eng., Just Accepted Manuscript • Publication Date (Web): 26 Dec 2016 Downloaded from http://pubs.acs.org on December 26, 2016
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
ACS Sustainable Chemistry & Engineering is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
To ACS Sustainable Chemistry and Engineering
2
Fluorescent multifunctional polysaccharides for
3
sustainable supramolecular functionalization of
4
fibers in water
5
Olga Grigoray,1 Holger Wondraczek,2 Annett Pfeifer,2Pedro Fardim,1,3,* Thomas Heinze1,2,*
6
1
7
20500, Åbo, Finland
8
2
9
Macromolecular Chemistry, Friedrich Schiller University of Jena, Humboldtstraße 10, 07743
Laboratory of Fiber and Cellulose Technology, Åbo Akademi University, Porthansgatan 3, FI-
Center of Excellence for Polysaccharide Research, Institute of Organic Chemistry and
10
Jena, Germany
11
3
12
2424, 3001 Leuven, Belgum
13
KEYWORDS: multifunctional cellulose derivatives, naphthalimide group, polyelectrolyte,
14
eucalyptus Kraft fibers, fluorescent fibers, authenticity indicator
Department of Chemical Engineering (CIT), University of Leuven, Celestijnenlaan 200f - box
15
ACS Paragon Plus Environment
1
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 2 of 37
16
ABSTRACT
17
The paper describes the synthesis of multifunctional cellulose derivatives (MCD) containing a
18
fluorescent- and a cationic moiety and their application in the functionalization of pulp fibers.
19
The cellulose derivatives, namely N-(3-propanoic acid)- and N-(4-butanoic acid)-1,8-
20
naphthalimide esters of cellulose, differed in the degree of substitution (DS) and by the aliphatic
21
chain connecting naphthalimide photoactive groups to the polymer backbone. The derivatives
22
were decorated with a cationic moiety, namely (3-carboxypropyl)trimethylammonium chloride.
23
The fluorescent pulp fibers were prepared by direct self-assembly of the water soluble
24
fluorescent MCDs on the fibers in water at room temperature. The results indicated that the
25
adsorption was mainly driven by an ion exchange mechanism. UV-vis- and fluorescence
26
spectroscopic studies showed that the adsorption yield of the fluorescent MCDs depended on the
27
length of the aliphatic chain of the photoactive groups. Because of the adsorption, the modified
28
pulp fibers gained fluorescence in the visible part of the spectrum. Under black light
29
illumination, the modified fibers fluoresced, which made them visually distinguishable from the
30
reference fibers. Thus, the fluorescent pulp fibers prepared in a simple way can be potentially
31
used as an authenticity indicator in packaging materials.
32
INTRODUCTION
33
Supramolecular functionalization of pulp fibers by adsorption of bio-based polymers is a method
34
that allows the introduction of novel properties to the fibers without impairing their bulk
35
properties. This type of functionalization is characterized by the formation of supramolecular
36
assemblies which are created by association of biopolymers with pulp fiber constituents through
37
non-covalent intermolecular interactions, such as hydrogen bonding, electrostatic or hydrophobic
ACS Paragon Plus Environment
2
Page 3 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
38
interactions.1 The adsorption of the polymers can be carried out at mild conditions in water,
39
which simplifies the integration of this stage in the industrial processes, and preserves the
40
structure of the fiber. Supramolecular functionalization of pulp fibers can be done using specially
41
designed multifunctional cellulose derivatives (MCDs). Such cellulose derivatives are decorated
42
with specific functional groups that endow new functionality to the fibers and ionic functional
43
groups that impart solubility to the derivatives in water and facilitate interaction with the
44
fibers.2,3 Depending on the target applications, different functional groups can be introduced into
45
the structure of MCDs. For instance, Grigoray et al.4,5 used coumarin-type cellulose
46
polyelectrolytes to prepare light-responsive pulp fibers/fibrous materials whose mechanical
47
properties could be controlled by light. Vega et al.6 prepared functional fibers by adsorption of
48
cellulose polyelectrolytes containing amino groups for efficient immobilization of enzymes.
49
Thus, supramolecular functionalization of fibers gives an opportunity to improve the
50
performance of the existing fibrous materials and to create novel bio-based materials, which, in
51
turn, helps to valorise pulp fibers and broadens their application. In this study, supramolecular
52
functionalization was applied to prepare fluorescent pulp fibers for application as authenticity
53
indicators.
54
Nowadays, counterfeiting causes serious problems for modern society, and large quantities of
55
various fake products among pharmaceuticals, perfumes, clothes, videos, and software exist on
56
the market.7 Industries manufacturing genuine commodities suffer huge profit losses and struggle
57
to compete in the market with cheap, fake products. In addition, consumers pay excessive price
58
for poor quality products that can also put their health and safety in danger.
59
One of the approaches which manufacturers utilize to protect their goods from forgery is secure
60
packaging. Such packaging is identifiable and contains specific features that are difficult to copy.
ACS Paragon Plus Environment
3
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 37
61
Commonly, both overt (visible) and covert (invisible) features are applied to insure security of
62
the packaging. Overt features are instantly recognized by visual perception, and they include
63
holograms, color-shift inks, barcoding, and tamper-resistant tape. In contrast, covert features are
64
impossible to notice without special equipment and conditions. Presence and location of such
65
features in the package is highly confidential. Covert features include invisible printing (UV
66
inks), UV fluorescing fibers, and micro-text printing.7–10
67
Designing secure packaging requires consideration of its life cycle. To decrease negative impact
68
on the environment, utilization of sustainable materials is a necessary measure. This brings
69
paper-based packaging into wide use. Wood derived fibers (pulp fibers) being a main component
70
in paper-based packaging could also serve as its security elements, for example in a form of
71
fluorescent fibers. Such security fibers are invisible under daylight, which means that they are
72
indistinguishable from other fibers. Under UV light exposure, the security fibers fluoresce, what
73
makes them clearly visible.7,9,11
74
To our knowledge, only few approaches have been proposed aiming at modification of wood
75
derived pulp fibers for subsequent application as fluorescent security fibers. In one of the
76
approaches it was proposed to treat pulp fibers with fluorescent whitening agents (FWAs)7 and in
77
another one FWAs were loaded into the lumen of the fibers.11 In both cases, the modification
78
steps were applied prior to mixing with neat fibers and formation of fibrous materials. However,
79
FWAs used in such approaches suffer one significant disadvantage of low affinity to pulp fibers,
80
which in turn requires addition of different fixing agents or salts.
81
Thus, the objective of the current study was to produce fluorescent security pulp fibers via
82
simple supramolecular modification in aqueous solution using specially-designed bio-based
ACS Paragon Plus Environment
4
Page 5 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
83
surface modifying agents. In the scope of the study, novel types of fluorescent MCDs (FMCDs)
84
containing both cationic (3-carboxypropyl)trimethylammonium chloride ester and N-(3-
85
propanoic acid)-1,8-naphthalimide or N-(4-butanoic acid)-1,8-naphthalimide moieties were
86
synthesized, characterized and used to functionalize eucalyptus Kraft pulp fibers. Interaction of
87
the synthesized derivatives with pulp fibers, the effect of modification on the optical properties
88
of the fibers as well as their potential application are covered in this study.
89
EXPERIMENTAL SECTION
90
Materials
91
Microcrystalline cellulose (Avicel® PH 101, Fluka, Neu-Ulm, Germany) used as starting
92
material for the derivatives had a degree of polymerization (DP) of 135 calculated from the
93
intrinsic viscosity (ISO 5351). Drying of the cellulose and LiCl (Sigma-Aldrich, Deisenhofen,
94
Germany) was done at 105 °C for 6 h in a vacuum over KOH before the usage. N-(3-propanoic
95
acid)-1,8-naphthalimide and N-(4-butanoic acid)-1,8-naphthalimide were synthesized according
96
to Reger et al.12 Other chemicals and solvents were purchased from Sigma-Aldrich
97
(Deisenhofen, Germany) and used without further treatment. Eucalyptus unrefined bleached
98
Kraft pulp was obtained from Metsä Fiber (a former Botnia, Kaskö, Finland). Sodium
99
bicarbonate and sodium chloride were purchased from J.T. Baker and Merck and used as
100
received.
101
Methods
102
Synthesis of N-(3-propanoic acid)-1,8-naphthalimide esters of cellulose 2a-d, typical example
103
(same procedure for N-(4-butanoic acid)-1,8-naphthalimide esters of cellulose 3a-d)
ACS Paragon Plus Environment
5
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 37
104
Cellulose (10 g, 61 mmol of AGU) was dissolved in N,N-dimethylacetamide (DMA)/LiCl
105
(300 mL/18 g) according to Wondraczek et al.2 A solution of N-(3-propanoic acid)-1,8-
106
naphthalimide (4.15 g, 15.25 mmol) and N,N-carbonyldiimidazole (CDI; 2.5 g, 15.25 mmol) was
107
prepared using DMA (130 mL) as a solvent. The solution was kept at 70 °C until the gas
108
formation ceased, and then it was added to the cellulose solution. The mixture was left to react at
109
70 °C for 20 h under stirring. The product of the reaction was precipitated in 2500 mL of 2-
110
propanol, filtered, washed twice with 700 mL of 2-propanol and once with 700 mL of water. A
111
pale yellow solid (9.8 g, 90%) was obtained by drying the product at 40 °C under a vacuum.
112
Elemental analysis (EA), [%] C: 46.78, H: 6.59, N: 1.19.
113
13
114
(C6s), 73.47 (C2), 75.28 (C3, C5), 80.51 (C4), 102.95 (C1), 120.06 (C16), 122.41 (C11), 127.63
115
(C15), 131.18 (C13, C14), 134.95 (C12), 136.75 (C10), 170,84 (C7).
116
Perpropionylation
117
A perpropionylation reaction of the cellulose esters was carried out in order to determine the DS
118
of the esters by means of 1H NMR spectroscopy.2 The success of the reaction was proven by the
119
absence of OH stretching in the FTIR spectra (Nicolet AVATAR 370 DTGS spectrometer, KBr
120
technique) and by the presence of signals of propionate moieties in 1H NMR spectra of the
121
derivatives.
122
Synthesis of mixed N-(3-propanoic acid)-1,8-naphthalimide-(3-
123
carboxypropyl)trimethylammonium chloride esters of cellulose 4a-d, typical example (same
124
procedure for corresponding N-(4-butanoic acid)-1,8-naphthalimide derivatives 5a-d)
C NMR (100 MHz, DMSO-d6/LiCl): δ [ppm] = 21.88 (C9), 35.00 (C8), 60.37 (C6), 65.12
ACS Paragon Plus Environment
6
Page 7 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
125
The N-(3-propanoic acid)-1,8-naphthalimide ester of cellulose (4 g, 20 mmol) was dissolved in
126
DMA/LiCl as described for cellulose. A solution of (3-carboxypropyl)trimethylammonium
127
chloride (1.84 g, 10 mmol) and CDI (1.62 g, 10 mmol) was prepared by dissolution in DMA
128
(50 mL). The solution was kept at 70 °C until the gas formation ceased, and then it was added to
129
the dissolved cellulose ester. The reaction was carried out at 70 °C for 20 h under stirring. The
130
product of the reaction was precipitated in 800 mL of acetone, filtered, washed thrice with
131
300 mL of acetone and twice with 250 mL of ethanol. For purification, the product was dissolved
132
in water, and dialysis against water was performed using a cellulose membrane (Spectra/Porr;
133
MWCO = 3500 g/mol). A pale yellow solid (2.85 g) was obtained after lyophilization.
134
EA, [%] C: 46.66, H: 6.38, N: 2.39, Cl: 3.39.
135
13
136
(C8), 53.04 (C21), 60.96 (C6s), 63,95 (C6), 65.31 (C20), 72.74 (C2), 73.70 (C3), 75.31 (C5),
137
80.45 (C4), 100.01 (C1s), 103,20 (C1), 116.75 (C16), 122.58 (C11), 127.65 (C15), 131.86 (C13),
138
134.82 (C14), 137.81 (C12), 163.86 (C10), 171.08 (C7), 172.03 (C17).
139
Characterization
140
Characterization of the derivatives was done as described elsewhere.2 Briefly, 13C NMR was
141
used to prove formation of covalent bond between the AGUs and the introduced functional
142
groups. DS of photoactive groups (DSPhoto) was determined by 1H NMR. NMR spectra were
143
recorded using a Bruker Avance 400 MHz spectrometer. Signals in the spectra were assigned
144
using two dimensional measurements (HSQC-DEPT, TOCSY) and by comparison with the
145
spectra of the carboxylic acids used for esterification (spectra not shown). DSPhoto was calculated
C NMR (100 MHz, DMSO-d6/LiCl): δ [ppm] = 18.48 (C19), 30.73 (C9), 32.73 (C18), 36.17
ACS Paragon Plus Environment
7
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 37
146
from the spectral integrals of the naphthalimide moiety protons (7.5–9 ppm, Figure 1) and the
147
methyl group protons of the propionate moiety (1.0 ppm, Figure 1) according to Equation 1:
3 6
!"
#
$
(1)
148
149 150
Figure 1. 1H NMR spectrum of perpropionylated N-(3-propanoic acid)-1,8-naphthalimide ester
151
of cellulose (2a, DSPhoto 0.07)
152 153
In addition to the NMR, DSPhoto and DS of cationic groups (DSCat) were obtained using UV-vis
154
spectroscopy and elemental analysis.2 Elemental analysis was carried out with a CHNS 932
155
Analyzer (Leco) and chloride content was obtained with a procedure described elsewhere.13
156
Naphthalimide substituents of FMCDs had a characteristic light absorption at λmax=334 nm
157
recorded by a UV-vis spectrophotometer. Their molar concentration (% , mol/L) was
158
calculated from calibration curves built with N-(3-propanoic acid)-1,8-naphthalimide and N-(4-
159
butanoic acid)-1,8-naphthalimide used as standards for corresponding cellulose esters.
160
Subsequently, the mass fraction of nitrogen originated from the photoactive substituents of the
161
derivatives (&' ) was calculated from the ratio of nitrogen mass concentration in the
ACS Paragon Plus Environment
8
Page 9 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
162
photoactive moieties ((' , g/L) to the total mass concentration of the derivatives (()* ,
163
g/L) used for UV-vis spectroscopic measurements: &'
% ∗ ,' ()*
(2)
164
The mass fraction of nitrogen of the cationic substituents (&' -) ) was obtained by subtracting
165
&' from the total amount of nitrogen in the derivative (&' )* ) obtained by elemental
166
analysis. The molar concentration of the cationic moieties (%-) , mol/L) was calculated as: %-)
167
()* ∗ &' -) ,'
The molar concentration of the RUs was obtained using the following formula: ()* ∗ &./0 ,./0
(4)
()* − ( − (-) ()*
(5)
%./0 168
Where &./0 was calculated as: &./0
()* − % ∗ , − , − %-) ∗ ,-) − , ,./0 DSPhoto and DSCat of the esters were found as: %./0
169
(3)
-)
2 2./0 2-) 2./0
(6)
(7) (8)
170 171
Kinetic studies of adsorption
172
An amount of wet pulp (dry content around 30 %) corresponding to 200 mg of dry pulp was
173
soaked in 10-5 M NaHCO3 solution for 30 min under agitation. The derivatives were dissolved in
ACS Paragon Plus Environment
9
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 37
174
10-5 M NaHCO3 solution to obtain stock solutions with a concentration of 0.5 g/L. A certain
175
volume of the derivative solution was added to the pulp suspension, so the dosage of the
176
derivatives was 2 % (w/w) based on dry weight of fibers, and the final pulp consistency was
177
0.6 % (based on total weight of the suspension). The adsorption was carried out at 25 ± 2 °C and
178
270 rpm agitation speed using a multipoint agitation plate. The adsorption time was varied from
179
10 min to 17 hours (overnight). After adsorption time elapsed, the suspensions were centrifuged
180
at 3500 rpm for 5 min, and the supernatants were analyzed with a Shimadzu 2600 UV-vis
181
spectrophotometer. The amounts of the remaining derivatives in the supernatants were found by
182
using a calibration curve for the corresponding derivative and an absorbance maximum in the
183
vicinity of 343 nm for all derivatives. Subsequently, the adsorbed amounts were calculated by
184
subtracting the amount of the derivatives remained in the solution from the added amounts. The
185
adsorption studies were done in duplicate.
186
Adsorption studies at different electrolyte concentrations
187
Sodium chloride solutions of 10-2, 10-3, 10-4 and 10-5 M were used to dissolve the derivatives and
188
to adjust consistency of the pulp suspension. NaCl was chosen as an electrolyte due to its low
189
effect on pH at all studied concentrations. The pHs of NaCl solutions at the applied
190
concentrations were 6.2±0.1. The reaction time of adsorption was 17 hours. Other parameters of
191
the experiment and the analysis of the supernatants were similar to ones in the kinetic studies.
192
Adsorption isotherms
193
Time for the adsorption at equilibrium (17 hours) was chosen based on the kinetic studies.
194
Dosages of the derivatives varied from 0.1 % to 5 % (w/w, based on dry pulp). Other conditions
195
were the same as for the kinetic studies. The supernatants obtained after centrifuging the
ACS Paragon Plus Environment
10
Page 11 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
196
suspension were analyzed by a Perkin-Elmer LS50B spectrofluorometer. Before the analysis, the
197
supernatants as well as the stock solutions were diluted by 10-5 M NaHCO3 solution. Thus, the
198
concentrations of the samples were adjusted to be in the linear range of the response of emission
199
intensities to the concentrations of the derivative solutions. The samples were excited at their
200
absorbance maxima and emission spectra were collected. The emission maxima were found in
201
the vicinity of 394 nm. The determination of the adsorbed amounts was done as described for the
202
kinetic studies.
203
Excitation spectra of the solutions
204
The excitation spectra were recorded with the Perkin-Elmer LS50B spectrofluorometer used for
205
fluorescence measurements. The polymer was diluted to 0.8 mg/L concentration with 10-5 M
206
NaHCO3, and excitation spectra were monitored at the emission wavelengths of 390 nm and
207
496 nm, which corresponded to maxima in the emission spectra. The solutions were diluted to
208
limit the possible effect of concentration on the excimer formation. On the other hand, the
209
concentration was kept high enough to avoid effects of artifacts in the spectra, e.g. stray light.
210
Preparation of sheets from pulp fibers
211
To evaluate optical properties, hand-sheets were formed from the reference and modified fibers
212
according to SCAN-CM 11:95. After the adsorption, the pulp suspensions were diluted 20-fold
213
by10-5 M NaHCO3 solution and transferred directly to the sheet former. The formed sheets were
214
dried overnight in a conditioned room at 50 % relative humidity and 23 °C.
215
Optical properties of the fibers
ACS Paragon Plus Environment
11
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 37
216
A Shimadzu 2600 spectrophotometer equipped with an integrated sphere ISR-2600 Plus was
217
used to collect UV-vis spectra of diffuse reflection from the fibers. Emission spectra were
218
obtained using a Perkin-Elmer LS50B spectrofluorometer. The fibers were excited at a
219
wavelength of the UV absorbance maximum of the derivatives. Fluorescence values over a full
220
visible spectrum were calculated as a difference between two whiteness values measured with
221
and without UV component in the incident light (SCAN-G 5:03) using an Elrepho
222
spectrophotometer. The fluorescence data include the values from parallel samples. Visualization
223
of the fluorescent fibers was performed using an Olympus BX60 fluorescence microscope
224
coupled with a Nikon DS-Fi2 camera. The microscope was equipped with an excitation filter
225
(330-385 nm), a dichroic mirror (400 nm) and a barrier emission filter (420 nm). To simulate an
226
incorporation of the modified fibers in the fiber material (packaging), the templates were cut
227
from the sheets made of the modified fibers and placed on the top of the sheets made of the
228
reference fibers. A UV-black light bulb (15W, absorption band 320-415 nm) was used as a
229
source of a black (UVA) light to illuminate the samples.
230 231
RESULTS AND DISCUSSION
232
In order to get photoactive cellulose derivatives, esterification of the biopolymer was carried out.
233
As demonstrated recently, a very efficient acylation method of cellulose is the application of
234
carboxylic acids activated with CDI that allows the synthesis of MCDs decorated with
235
photoactive and cationic substituents.2
236
Esterification of cellulose with photoactive- and cationic carboxylic acids
ACS Paragon Plus Environment
12
Page 13 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
237
In the current study, novel FMCDs were synthesized in a two-step procedure (Figure 2). The
238
esterification of cellulose with N-(3-propanoic acid)-1,8-naphthalimide and N-(4-butanoic acid)-
239
1,8-naphthalimide dyes was done by the reaction of cellulose dissolved in N,N-
240
dimethylacetamide/LiCl with imidazolides of the photoactive carboxylic acids obtained in a
241
separate reaction.
242 243
Figure 2. Synthesis scheme of N-(3-propanoic acid)-1,8-naphthalimide- respectively N-(4-
244
butanoic acid)-1,8-naphthalimide esters of cellulose and the corresponding mixed naphthalimide
245
(3-carboxypropyl)trimethylammonium chloride esters of cellulose via in situ activation of N-(3-
246
propanoic acid)-1,8-naphthalimide, N-(4-butanoic acid)-1,8-naphthalimide, and (3-
247
carboxypropyl)trimethylammonium chloride (4) with N,N-carbonyldiimidazole (CDI) in N,N-
248
dimethylacetamide/LiCl (DMA/LiCl)
249
ACS Paragon Plus Environment
13
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 37
250
DSPhoto of the esters could be controlled to a certain extent by the molar ratio of AGU to
251
carboxylic acid imidazolide (Table 1). At comparable molar ratio, the DSPhoto of N-(3-propanoic
252
acid)-1,8-naphthalimide esters (2a-d) was slightly lower compared to the products containing N-
253
(4-butanoic acid)-1,8-naphthalimide esters (3a-d) that can be attributed to sterical reasons, i.e.
254
the different chain length of the linker separating the bulky naphthalimide moieties from the
255
polymer backbone. At molar ratios of AGU to carboxylic imidazolide of 1:0.75 and 1:1, it was
256
noticed that the DSPhoto reached its maximum for both naphthalimide carboxylic acid derivatives
257
(samples 2c,d and 3c,d, Table 1). Thus, the maximum DSPhoto of N-(3-propanoic acid)-1,8-
258
naphthalimide esters was about 0.20 and in the case of N-(4-butanoic acid)-1,8-naphthalimide
259
esters it was about 0.32. These DSPhoto were well sufficient to get photoactive polymers.
260 261
Table 1. Results of the synthesis of N-(3-propanoic acid)-1,8-naphthalimide- and N-(4-butanoic
262
acid)-1,8-naphthalimide esters of cellulose by activation of the carboxylic acids with N,N-
263
carbonyldiimidazole (CDI) carried out in N,N-dimethylacetamide/LiCl Molar ratio Carboxylic acid
N-(3-propanoic acid)-1,8naphthalimide
N-(4-butanoic acid)-1,8naphthalimide
AGUa CDI
carboxylic acid
Sample No. DSNMRb DSUVc
1
0.25
0.25
2a
0.07
0.07
1
0.50
0.50
2b
0.14
0.13
1
0.75
0.75
2c
0.20
0.20
1
1.00
1.00
2d
0.20
0.22
1
0.25
0.25
3a
0.11
0.12
1
0.50
0.50
3b
0.18
0.20
1
0.75
0.75
3c
0.30
0.32
1
1.00
1.00
3d
0.32
0.32
264
a
265
determined by means of UV-vis spectroscopy in DMA/LiCl.
Anhydroglucose unit; bDegree of substitution (DS) determined by means of 1H NMR spectroscopy after perpropionylation; bDS
ACS Paragon Plus Environment
14
Page 15 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
266 267
To introduce cationic moieties, the photoactive cellulose derivatives (2 and 3) were allowed to
268
react with imidazolide of (3-carboxypropyl)trimethylammonium chloride (Figure 2 and Table 2).
269
At a molar ratio of modified AGU to carboxylic acid imidazolide of 1:0.5, the obtained DSCat
270
was 0.3, and it was independent of the DSPhoto of the starting polymer. In addition, no
271
transesterification occurred, thus, DSPhoto remained almost constant during the esterification.
272 273
Table 2. Results of the synthesis of mixed naphthalimide-(3-carboxypropyl)trimethylammonium
274
chloride esters of cellulose by activation of (3-carboxypropyl)trimethylammonium chloride with
275
N,N-carbonyldiimidazole (CDI) carried out in N,N-dimethylacetamide/LiCl (molar ratio of
276
modified repeating unit/CDI/(3-carboxypropyl)trimethylammonium chloride = 1.00/0.50/0.50) Product
Starting sample No.a
Solubility DSPhotob DSCatb
No.
H2O
DMSO
2a
0.07
0.31
4a
+
+
2b
0.09
0.34
4b
+
+
2c
0.18
0.35
4c
-
+
2d
0.21
0.31
4d
-
+
3a
0.11
0.32
5a
+
+
3b
0.22
0.33
5b
+
+
3c
0.32
0.30
5c
-
+
3d
0.31
0.34
5d
-
+
277 278 279
a
280
13
281
as cationic substituents. In the spectra, it can be noticed that the peaks for positions C1-C5 of the
See Table 1; analysis.
b
Degree of substitution (DS) determined by means of a combination of UV-vis spectroscopy and elemental
C NMR spectra proved the covalent linkages formed between AGU and naphthalimide- as well
ACS Paragon Plus Environment
15
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 37
282
AGU were almost unaffected while the signal of the primary C atom (C6) peak was shifted to
283
lower field (C6s) by esterification (Figure 3).
284
At a certain ratio, the introduced cationic substituents facilitated solubility of the cellulose
285
derivatives in water (Table 2). However, the obtained derivatives became water insoluble above
286
certain DSPhoto, which was about 0.2 for 2 and 0.3 for 3.
287 288
A
B
C
289
Figure 3. 13C NMR spectra of: A) cellulose dissolved in DMSO-d6/tetrabutylammonium fluoride
290
(TBAF), B) N-(4-butanoic acid)-1,8-naphthalimide ester of cellulose (degree of substitution of
291
photoactive moiety, DSPhoto 0.11) in DMSO-d6, C) N-(4-butanoic acid)-1,8-naphthalimide-(3-
ACS Paragon Plus Environment
16
Page 17 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
292
carboxypropyl)trimethylammonium chloride ester of cellulose (DSPhoto 0.11, DSCat 0.32) in
293
DMSO-d6.
294 295
Supramolecular functionalization of pulp fibers
296
Synthesized FMCDs were used for modification of eucalyptus unrefined bleached Kraft pulp
297
fibers to introduce photoactive properties to the fibers. The fiber functionalization was performed
298
in a water-based system in one single step by addition of FMCD solutions to pulp fiber
299
suspensions. The adsorption was conducted at mild conditions, i.e. at room temperature under
300
agitation. During adsorption, cationic polyelectrolytes interact quickly with negatively-charged
301
fibers through an ion exchange mechanism driven by the entropy gain from release of counter-
302
ions.14 However, the type of polymer backbone as well as its side groups have strong influence
303
on the interaction with the fibers. Hence, the adsorption of synthesized derivatives was studied in
304
more detail.
305
Among the synthesized FMCDs (Table 2), only water soluble derivatives were chosen as
306
modifying agents. In the case of cationic cellulose esters containing butanoic naphthalimide
307
moiety, there were two types of the water soluble derivatives, they were designated as 5a
308
(DSPhoto = 0.11; DSCat = 0.32) and 5b (DSPhoto = 0.22; DSCat = 0.33). These derivatives were used
309
to study the effect of the DSPhoto on the adsorption onto pulp fibers and the optical properties of
310
the resulting modified fibers. In addition, adsorption of cationic cellulose ester containing
311
propanoic naphthalimide moiety (4a, DSPhoto = 0.07 and DSCat = 0.31) was studied in order to
312
investigate how the length of the aliphatic chain connecting the photoactive moieties to the
ACS Paragon Plus Environment
17
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 37
313
cellulose backbone affects the fiber modification, and the results were compared to those
314
obtained for the 5a derivative.
315
Adsorption kinetics
316
Kinetic studies were performed in order to investigate the rate of the adsorption process and,
317
also, to find time required to achieve the equilibrium of the adsorption reaction. For that purpose,
318
adsorption isotherms were obtained by addition of the derivative solution at 2 % (w/w) dosage to
319
the fibers and measuring residual concentration versus reaction time. The results of the kinetic
320
studies are summarized in Figure 4.
321 322
Figure 4. Kinetic studies of the adsorption of FMCDs onto pulp fibers: N-(3-propanoic acid)-
323
1,8-naphthalimide-(3-carboxypropyl)trimethylammonium chloride ester of cellulose (4a, DSPhoto
324
0.07, DSCat 0.31) and N-(4-butanoic acid)-1,8-naphthalimide-(3-
325
carboxypropyl)trimethylammonium chloride esters of cellulose (5a, DSPhoto 0.11, DSCat 0.32; 5b,
326
DSPhoto 0.22, DSCat 0.33 )
327
ACS Paragon Plus Environment
18
Page 19 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
328
The adsorption isotherms showed the same trend for all three derivatives and no differences in
329
the results were observed between the derivatives. In the beginning, adsorption was fast, and the
330
concentration of the derivatives in the solutions decreased steeply during the first 10 minutes. At
331
that point, the amounts of adsorbed 4a, 5a and 5b were 75, 70 and 62 % (w/w) based on the total
332
adsorbed amount. For the rest of the reaction time the adsorption was much slower. The rate of
333
the adsorption of the derivatives during specific time intervals calculated as a difference of the
334
adsorbed amounts to the time interval (∆ads/∆time) was 3.3–4 %/min during first 10 min, and it
335
drastically decreased for the following time interval, 10–60 min (∆ads10-60/∆time10-60
336
< 0.2 %/min). During next 120 min the adsorption rate (∆ads60-180/∆time60-180) was ≤ 0.04 %/min
337
and continued to decrease thereafter approaching the equilibrium. Therefore, it is not necessary
338
to conduct adsorption for a long period of time, and 10–60 min can be sufficient for the
339
modification of pulp fibers. The high initial adsorption rate was attributed to fast ion exchange
340
reactions between the accessible negatively charged groups of the fibers and the cationic
341
moieties of the derivatives.4 Subsequent decrease of the adsorption rate could be explained by
342
several factors. First, the fibers are porous material consisting of fibrils. Therefore, the applied
343
derivatives could penetrate into the inner layers of the fiber wall, and sufficient amount of time
344
was required for the macromolecules to diffuse into the fiber wall and to reach adsorption sites.15
345
Second, steric and electrostatic repulsion could take place between the layers of adsorbed
346
polymer chains and the polymer macromolecules approaching these layers.14 Generally, these
347
types of repulsion retard adsorption of polyelectrolytes on the external fiber surfaces as well as
348
they slow down the diffusion of the polymers into the fiber wall and thus adsorption onto the
349
internal surfaces. 14
350
Effect of electrolyte concentration
ACS Paragon Plus Environment
19
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 37
351
The type of interactions contributing to the adsorption of FMCDs onto the fibers was studied
352
using various electrolyte concentrations in the suspensions during the reactions. The time and the
353
concentration of the polymers were kept constant for all experiments.
354
The results of the adsorption as a function of salt concentration are shown in Figure 5. Increasing
355
electrolyte concentration led to a gradual increase in the adsorbed amounts for all three
356
derivatives. The ions of the added salt screened the charge of both the derivatives and the fibers,
357
which, in turn, caused a decrease in the electrostatic attraction between the cationic
358
polyelectrolytes and the cellulosic fibers.16 Thus, the enhanced adsorption at higher electrolyte
359
concentration could be explained by non-ionic interactions such as hydrophobic interactions.14
360
This type of interaction could occur between hydrophobic sites of cellulose chains of the fibers
361
and of the polymers.4 Such sites are C-H groups located on the axial position of the
362
glucopyranose ring.17 In addition, photoactive groups of the polymers, which are also
363
hydrophobic, could contribute to these interactions with the fibers.4 This is in agreement with the
364
studies published earlier4 where cationic cellulose derivatives without and with coumarin
365
photoactive moieties adsorbed irreversibly onto model surfaces bearing hydrophobic methyl
366
groups.
367
Another type of non-ionic interaction, i.e. hydrogen bonding, presumably played a minor role
368
during adsorption of FMCDs. This hypothesis is based on the same study,4 where it was shown
369
that no adsorption of the derivatives took place on the model surfaces with hydroxyl groups.
370
Apart from ionization, ionic strength has also an effect on the conformation of the
371
polyelectrolytes in the solution.18 At higher electrolyte concentrations, the conformation changes
372
from expanded to more compact due to decrease of the segment repulsions. As a result, the
ACS Paragon Plus Environment
20
Page 21 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
373
adsorbed polymers occupy less area on the fibers and more free surfaces are available for the
374
adsorption.18 This could also have a positive impact on the adsorption along with non-ionic
375
interactions.
376 377
Figure 5. Effect of electrolyte concentration on the adsorption of FMCDs onto pulp fibers: N-(3-
378
propanoic acid)-1,8-naphthalimide-(3-carboxypropyl)trimethylammonium chloride ester of
379
cellulose (4a, DSPhoto 0.07, DSCat 0.31) and N-(4-butanoic acid)-1,8-naphthalimide-(3-
380
carboxypropyl)trimethylammonium chloride esters of cellulose (5a, DSPhoto 0.11, DSCat 0.32; 5b,
381
DSPhoto 0.22, DSCat 0.33 )
382 383
Independent of the ionic strength, the derivatives were strongly attached to the fibers. After re-
384
dispersion of the modified fibers in the buffers, the amount of derivatives detected in the solution
385
corresponded to less than 5 % (w/w) of the adsorbed amount. These amounts were attributed to
386
the polymers entrapped with the solutions that were not removed during the filtration of the
387
fibers after modification.
388
Equilibrium adsorption isotherms
ACS Paragon Plus Environment
21
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 37
389
The adsorption isotherms gave important information about the adsorption mechanism and an
390
effective dosage of the derivatives for the fiber modification. The adsorption was performed
391
during 17 hours to reach the reaction equilibrium, and at 10-5 M concentration of the buffer
392
solution to promote ionic interactions. The adsorption isotherms (Figure 6A) were obtained by
393
applying different dosages of the polymers to the fibers and measuring the amount of the
394
derivatives in solution before and after the reaction.
395
The adsorption isotherms of 5a and 5b derivatives reached a saturation plateau. The differences
396
in the adsorbed amounts for the derivatives were insignificant. Thus, the DSPhoto did not have any
397
impact on the adsorption of the derivatives and therefore, it can be concluded that the adsorption
398
was predominantly governed by the ion exchange mechanism. On the other hand, 4a derivative
399
adsorbed to a greater extent, especially, at higher applied dosages. In addition, the adsorption
400
isotherm of 4a derivative did not reach a clear saturation plateau. Such results could be explained
401
by differences in the structure of the photoactive moieties. 4a derivative had a shorter length of
402
alkyl chain connecting photoactive group with the cellulose backbone than the other derivatives,
403
and because of this, 4a macromolecules could take more favorable conformation for the
404
adsorption.
ACS Paragon Plus Environment
22
Page 23 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
405 406
Figure 6. Adsorption isotherms of FMCDs onto pulp fibers: N-(3-propanoic acid)-1,8-
407
naphthalimide-(3-carboxypropyl)trimethylammonium chloride ester of cellulose (4a, DSPhoto
408
0.07, DSCat 0.31) and N-(4-butanoic acid)-1,8-naphthalimide-(3-
409
carboxypropyl)trimethylammonium chloride esters of cellulose (5a, DSPhoto 0.11, DSCat 0.32; 5b,
410
DSPhoto 0.22, DSCat 0.33 )
411 412
As it was already mentioned, the FMCDs interacted with the fibers mainly through an ion-
413
exchange mechanism. Analysis of the reference fibers by a methylene blue sorption method19
ACS Paragon Plus Environment
23
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 24 of 37
414
showed that the amount of the anionic groups in the fibers was equal to 89 µmol/g.4 However,
415
the amount of cationic charge adsorbed together with the derivatives was much lower than this
416
value. At the largest adsorbed amount of the derivatives, it corresponded to 14 µmol/g of cationic
417
groups for 5a and 5b, and 24 µmol/g for 4a. This means that the derivatives did not neutralize all
418
charged groups of the fibers. One possible explanation is that the adsorbed polymers sterically
419
blocked available charged groups of the fibers for the interactions with the derivatives in the
420
solution.4 Another explanation could be limited accessibility of the fiber walls.20
421
Figure 6B shows that for all the derivatives the adsorption was more favorable at lower
422
concentrations of the polymer in the solution or polymer dosage meaning that at lower applied
423
dosages a higher portion of the added amount was adsorbed.
424
Optical properties of FMCDs treated fibers
425
Interaction of the material with UV and visible light governs its visual appearance. Hence, the
426
ability of the fibers to absorb, emit and reflect the incident light determines the potential
427
application of the fibrous materials.
428
Light absorption
429
Light absorption by the modified and reference fibers was measured in the range of 200-700 nm
430
using a UV-vis spectrometer. Reference pulp fibers exhibited two absorbance peaks at 230 and
431
275 nm, originating from residual hexenuronic acid and lignin (Figure 7A).21 The spectra of 4a,
432
5a and 5b modified fibers looked similar to each other and had strong absorption at 340 nm
433
characteristic of naphthalimides.22 The light absorbance became higher as the amount of the
ACS Paragon Plus Environment
24
Page 25 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
434
absorbed derivatives increased. Thus, the UV spectra qualitatively proved that the modification
435
reaction was successful and the fibers were endowed with new light absorption properties.
436 437
Figure 7. Optical properties of fibers treated with FMCDs at different dosages: absorption
438
spectra (A) and fluorescence spectra (B). Optical properties of solutions of FMCDs: emission
439
spectra (C) and excitation spectra (D). N-(3-propanoic acid)-1,8-naphthalimide-(3-
440
carboxypropyl)trimethylammonium chloride ester of cellulose (4a, DSPhoto 0.07, DSCat 0.31) and
441
N-(4-butanoic acid)-1,8-naphthalimide-(3-carboxypropyl)trimethylammonium chloride esters of
442
cellulose (5a, DSPhoto 0.11, DSCat 0.32; 5b, DSPhoto 0.22, DSCat 0.33 )
443 444
ACS Paragon Plus Environment
25
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 26 of 37
445
Fluorescent properties of the fibres
446
Fluorescent properties of the fibers were studied using a spectrofluorometer, and the emission
447
spectra were collected by irradiating the fibers with the light having the wavelength of the UV
448
absorbance maximum (Figure 7B). All fibers modified by FMCDs had an emission band with a
449
maximum at 393-398 nm which is typical of naphthalimides.22 However, the 5b treated fibers
450
had a second broad emission band located at longer wavelengths and overlapping with the first
451
one. This band could be attributed to the emission of photons by excimers.22 Generally, excimers
452
are dimeric structures formed by association of fluorophores located at sufficiently close
453
distance.23 To confirm the formation of the excimers the fluorescent properties of FMCDs
454
solutions were additionally studied. The emission spectrum of 4a solution showed one strong
455
band at 395 nm that originated from naphthalimide. However, in the case of 5a and 5b, the
456
spectra showed two separate emission bands, even at very low concentrations (below 5 mg/L).
457
The first band had maximum in the vicinity of 395 nm corresponding to monomer emission, and
458
the second maximum was at 482 nm for 5a and at 495 nm for 5b corresponding to excimer
459
emission (Figure 7C). The ratio of the excimer band maximum to that of monomer was 0.3 for
460
5a (concentration range of 0.8-10 mg/L) and 0.8-0.9 for 5b (concentration range of 0.4-5 mg/L).
461
The range of concentrations for 5a solutions was two times higher than for 5b in order to reach
462
similar concentration of photoactive groups in the solutions. The increase of the emission
463
originated from the excimer with increase of DSPhoto at the same concentration of photoactive
464
moieties in the solutions could be explained by intramolecular interactions of the fluorophores
465
attached to the same polymer chain. This explained the second strong emission band of the fibers
466
modified with 5b in the blue-green spectral range (Figure 7B).
ACS Paragon Plus Environment
26
Page 27 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
467
There are two types of excimers.23 Dynamic excimer is formed by association of monomer in an
468
electronic excited state with monomers in a ground state.23 Static excimers are formed by the
469
interaction of monomers in a ground state.23 To distinguish the type of excimer, the excitation
470
spectra were recorded for 5b solution and these are shown in Figure 7D. As can be seen, the
471
excitation spectrum collected at monomer emission maximum could not be superimposed with
472
the one collected at excimer emission maximum. From these spectra it was calculated that the
473
peak to valley ratio of the characteristic band in the monomer excitation spectrum was higher
474
than that in the excimer excitation spectrum. Another way to compare the excitation spectra is to
475
plot the intensity of normalized excitation spectra for excimer against of that for monomer.24
476
There was no linear correlation between the intensity of scans. These differences in the
477
excitation spectra are characteristic features for the so-called static excimers which formed by
478
the excitation of fluorophores interacting in the ground state.23
479
Visual appearance of the modified fibres
480
Figure 8 shows microscopic images of the modified fibers under white and UV light
481
illumination. In later case, the fibers were excited at 330-385 nm, and the image was obtained by
482
collecting emitted light at λ > 420 nm. As can be seen in Figure 8A, the modified fibers
483
fluoresced (glowed) under UV light exposure. By comparing the fluorescent image with one
484
obtained under white light (Figure 8B, bright field image), the same microstructural elements
485
(pits) and fiber morphology were observed indicating that the fibers were completely covered
486
with the polymer. It is important to mention that during imaging of untreated reference fibers
487
under the same conditions no clear fluorescence image could be obtained. Thus, the fibers
488
modified by the derivatives were clearly distinguishable from the reference fibers.
ACS Paragon Plus Environment
27
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 28 of 37
489
490 491 492
Figure 8.Visualization of fluorescent pulp fibers by epi-fluorescence microscope under exposure
493
of UV light (A) and white light (B). The fibers were modified with 5b and the dosage was 2 %
494
(w/w). N-(4-butanoic acid)-1,8-naphthalimide-(3-carboxypropyl)trimethylammonium chloride
495
ester of cellulose (5b, DSPhoto 0.22, DSCat 0.33).
496 497
An Elrepho spectrophotometer equipped with D65 illuminant was used to quantify the
498
fluorescence over the visible light wavelength range. The obtained values were used to compare
499
the fibers modified with different FMCDs. As shown in Figure 9, no significant differences in
500
the fluorescence were found between three types of the modified fibers. In particular, 5a and 5b
501
being adsorbed on the fibers to the same extent exhibited similar fluorescence despite the double
ACS Paragon Plus Environment
28
Page 29 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
502
difference in the DSPhoto. Thus, all modified fibers have potential to be used as authenticity
503
indicators.
504 505
Figure 9. Fluorescence intensity of the reference and the fibers modified by FMCDs over the full
506
visual spectrum. N-(3-propanoic acid)-1,8-naphthalimide-(3-carboxypropyl)trimethylammonium
507
chloride ester of cellulose (4a, DSPhoto 0.07, DSCat 0.31) and N-(4-butanoic acid)-1,8-
508
naphthalimide-(3-carboxypropyl)trimethylammonium chloride ester of cellulose (5a, DSPhoto
509
0.11, DSCat 0.32; 5b, DSPhoto 0.22, DSCat 0.33 )
510 511
Figure 10 shows the image of hand-sheets made of reference and modified fibers under black
512
light which is commonly used to reveal counterfeiting. UV light caused glowing of the modified
513
fibers. The glowing effect was stronger at higher amounts of the adsorbed polymers. Visually,
514
the difference in the optical performance between the modified fibers under black light was in
515
the following order: 4a > 5a > 5b. This difference was explained by the formation of excimers in
516
the cases of 5a and 5b that gave additional emission band in the range of 440 nm-500 nm (blue-
517
green region). On other hand, the sheets made of reference and modified fibers looked similar
518
under daylight. Hence, prepared modified fibers could serve as invisible security fibers that
ACS Paragon Plus Environment
29
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 30 of 37
519
become visible when being exposed to UV light. One of the possible applications of such fibers
520
is in smart packaging. They can serve as authenticity indicator for packaging as well as for the
521
products. 0%
0.1%
0.5%
1%
3%
5%
4a
5a
5b 522 523
Figure 10. The picture of fiber hand-sheets under black light illumination. The quadrates and the
524
background made of FMCDs treated and reference fibers, respectively. N-(3-propanoic acid)-
525
1,8-naphthalimide-(3-carboxypropyl)trimethylammonium chloride ester of cellulose (4a, DSPhoto
526
0.07, DSCat 0.31) and N-(4-butanoic acid)-1,8-naphthalimide-(3-
527
carboxypropyl)trimethylammonium chloride esters of cellulose (5a, DSPhoto 0.11, DSCat 0.32; 5b,
528
DSPhoto 0.22, DSCat 0.33 )
529
CONCLUSION
530
In summary, the FMCDs containing both fluorescent and cationic functional moieties were
531
successfully synthesized, characterized and used as surface modifying agents for pulp fibers. The
532
FMCDs possessed high affinity to pulp fibers, and they adsorbed irreversibly onto the fibers
533
mainly via charge-directed self-assembly. DSPhoto of FMCDs did not have effect on the
534
adsorption of the derivatives. On the other hand, the adsorption was dependent on the length of
535
the aliphatic chain connecting the naphthalimide moiety to cellulose backbone, thus the
ACS Paragon Plus Environment
30
Page 31 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
536
derivatives with propanoic naphthalimide moiety exhibited better adsorption compared to the
537
derivatives with butanoic naphthalimide moiety.
538
As a result of the modification, the fibers became fluorescent and they emitted visible light under
539
UV light exposure. Prepared in such way modified pulp fibers can be potentially applied as
540
security features in objects made of fibrous materials, e.g. in packaging to validate its
541
authenticity. Even though all of the tested derivatives can be used for the preparation of
542
fluorescent pulp fibers, the derivative with the butanoic naphthalimide moiety and DSPhoto of
543
0.22 was superior to others as a modifying agent. The developed in this study concept is not
544
limited only to naphthalimide moieties, and as a future work FMCDs with other type of
545
fluorescent groups, having e.g. fluorescence in specific region, can be synthesized and tested as
546
surface modifying agents.
547 548
ACS Paragon Plus Environment
31
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
549
AUTHOR INFORMATION
550
*Corresponding Author:
551
Pedro Fardim (E-mail:
[email protected])
552
Thomas Heinze (E-mail:
[email protected])
Page 32 of 37
553 554 555
ACS Paragon Plus Environment
32
Page 33 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
556
ACKNOWLEDGMENT
557
Finnish Funding Agency for Technology and Innovation (Tekes) and Tekniikan edistämissäätiö
558
(TES) foundation are acknowledged for the financial support of the work. Leonore Bretschneider
559
is kindly acknowledged for her help with the synthesis of the derivatives.
560
ACS Paragon Plus Environment
33
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
561
REFERENCES
562
(1)
563 564
Page 34 of 37
Ariga, K.; Kunitake, T. Overview-What is Supramolecular Chemistry? In Supramolecular Chemistry – Fundamentals and Applications; Springer Berlin Heidelberg, 2006; pp 1–6.
(2)
Wondraczek, H.; Pfeifer, A.; Heinze, T. Water Soluble Photoactive Cellulose Derivatives:
565
Synthesis and Characterization of Mixed 2-[(4-methyl-2-oxo-2H-chromen-7-yl)oxy]acetic
566
acid–(3-carboxypropyl)trimethylammonium Chloride Esters of Cellulose. Cellulose 2012,
567
19 (4), 1327–1335.
568
(3)
Vega, B.; Wondraczek, H.; Bretschneider, L.; Näreoja, T.; Fardim, P.; Heinze, T.
569
Preparation of Reactive Fibre Interfaces Using Multifunctional Cellulose Derivatives.
570
Carbohydr. Polym. 2015, 132, 261–273.
571
(4)
Grigoray, O.; Wondraczek, H.; Heikkilä, E.; Fardim, P.; Heinze, T. Photoresponsive
572
Cellulose Fibers by Surface Modification with Multifunctional Cellulose Derivatives.
573
Carbohydr. Polym. 2014, 111, 280–287.
574
(5)
Grigoray, O.; Wondraczek, H.; Daus, S.; Kühnöl, K.; Latifi, S. K.; Saketi, P.; Fardim, P.;
575
Kallio, P.; Heinze, T. Photocontrol of Mechanical Properties of Pulp Fibers and Fiber-to-
576
Fiber Bonds via Self-Assembled Polysaccharide Derivatives. Macromol. Mater. Eng.
577
2015, 300 (3), 277–282.
578
(6)
Vega, B.; Fazeli, E.; Näreoja, T.; Trygg, J.; Hänninen, P.; Heinze, T.; Fardim, P.
579
Advanced Cellulose Fibers for Efficient Immobilization of Enzymes. Biomacromolecules
580
2016.
581
(7)
582 583
Kurrle, F. L.; Parks, C. J. Process of Manufacturing Authenticatable Paper Products. U.S.Patent 6,054,021, 2000.
(8)
Shah, R. Y.; Prajapati, P. N.; Agrawal, Y. K. Anticounterfeit Packaging Technologies. J.
ACS Paragon Plus Environment
34
Page 35 of 37
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
584 585
Adv. Pharm. Technol. Res. 2010, 1 (4), 368–373. (9)
586 587
Pharmaceutical Packaging Technology. J. Pharm. Bioallied Sci. 2013, 5 (2), 98–110. (10)
588 589
Cozzella, L.; Simonetti, C.; Spagnolo, G. S. Drug Packaging Security by Means of WhiteLight Speckle. Opt. Lasers Eng. 2012, 50 (10), 1359–1371.
(11)
590 591
Zadbuke, N.; Shahi, S.; Gulecha, B.; Padalkar, A.; Thube, M. Recent Trends and Future of
Foster, J. J.; Mulcaahy, L. T. Process for Making and Detecting Anti-Counterfeit Paper. U.S. Patent 6,045,656, 2000.
(12)
Highly Organized Structures and Unusual Magnetic Properties of Paddlewheel Copper(II)
592
Carboxylate Dimers Containing the π-π Stacking, 1.8-Naphthalimide Synthon. Inorg.
593
Chem. 2009, 48 (18), 8911–8924.
594
(13)
595 596
organischen Verbindungen. Microchim. Acta 1956, 44 (4), 869–876. (14)
597 598
Schöniger, W. Die mikroanalytische Schnellbestimmung von Halogenen und Schwefel in
Wågberg, L. Polyelectrolyte Adsorption onto Cellulose Fibres - A Review. Nord. Pulp. Pap. Res. J. 2000, 15 (5), 586–597.
(15)
Horvath, A. T.; Horvath, A. E.; Lindstro, T.; Wågberg, L. Adsorption of Low Charge
599
Density Polyelectrolytes to an Oppositely Charged Porous Substrate. Langmuir 2008, 24
600
(13), 6585–6594.
601
(16)
602 603
Lindström, T.; Wågberg, L. Effects of pH and Electrolyte Concentration on the Adsorption of Cationic Polyacrylamides on Cellulose. Tappi 1983, 66 (6), 83–85.
(17)
Medronho, B.; Romano, A.; Grac, M. Rationalizing Cellulose ( in ) Solubility : Reviewing
604
Basic Physicochemical Aspects and Role of Hydrophobic Interactions. Cellulose 2012,
605
19, 581–587.
606
(18)
Hedborg, F.; Lindstrom, T. Adsorption of Cationic Starch on Bleached Softwood
ACS Paragon Plus Environment
35
ACS Sustainable Chemistry & Engineering
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
607 608
Page 36 of 37
Cellulosic Fibres. Nord. Pulp. Pap. Res. J. 1993, 8 (2), 258–263. (19)
Fardim, P.; Moreno, T.; Holmbom, B. Anionic Groups on Cellulosic Fiber Surfaces
609
Investigated by XPS , FTIR-ATR , and Different Sorption Methods. J. Colloid Interface
610
Sci. 2005, 290, 383–391.
611
(20)
612 613
Langmuir 2001, 17 (4), 1096–1103. (21)
614 615
Wågberg, L.; Hägglund, R. Kinetics of Polyelectrolyte Adsorption on Cellulosic Fibers.
Liitiä, T.; Tamminen, T. How tO Evaluate the Kraft Pulp Brightness Stability ? In 3rd International Colloquim on Eucalyptus Pulp; Belo Horizonte, Brazil, 2007.
(22)
Ferreira, R.; Baleizão, C.; Muñoz-Molina, J. M.; Berberan-Santos, M. N.; Pischel, U.
616
Photophysical Study of Bis(Naphthalimide)-Amine Conjugates: Toward Molecular
617
Design of Excimer Emission Switching. J. Phys. Chem. A 2011, 115 (6), 1092–1099.
618
(23)
619 620
Winnik, F. M. Photophysics of Preassociated Pyrenes in Aqueous Polymer Solutions and in Other Organized Media. Chem. Rev. 1993, 93 (2), 587–614.
(24)
Zagrobelny, J.; Betts, T. A.; Bright, F. V. Steady-State and Time Resolved Fluorescence
621
Investigations of Pyrene Excimer Formation in Supercritical CO2. J. Am. Chem. Soc.
622
1992, 114 (16), 5249.
623 624 625
ACS Paragon Plus Environment
36
Page 37 of 37
626
TABLE OF CONTENTS GRAPHIC
Cellulosic fibers
Fluorescent biopolymer
+
UV light, fiber glowing C E L L
U
L
O
S
E 800
I, [a.u.]
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
600
Fiber fluorescence Modified
400 200
Reference
0 350 400 450 500 550 600
nm
Secure packaging under UV light
627 628
SYNOPSIS:
629
Preparation of sustainable bio-based authenticity indicators via simple supramolecular
630
functionalization of pulp fibers in water using novel fluorescent multifunctional cellulose
631
derivatives
632
ACS Paragon Plus Environment
37