Subscriber access provided by Universiteit Utrecht
Environmental Processes
High Performance Nanofiltration Membrane for Effective Removal of Perfluoroalkyl Substances at High Water Recovery Chanhee Boo, Yunkun Wang, Ines Zucker, Youngwoo Choo, Chinedum O. Osuji, and Menachem Elimelech Environ. Sci. Technol., Just Accepted Manuscript • DOI: 10.1021/acs.est.8b01040 • Publication Date (Web): 31 May 2018 Downloaded from http://pubs.acs.org on May 31, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 29
Environmental Science & Technology
1 2
High Performance Nanofiltration Membrane for Effective Removal of Perfluoroalkyl Substances at High Water Recovery
3 4 5 6 7 8 9 10 11
Chanhee Boo,† Yunkun Wang,§†* Ines Zucker,† Youngwoo Choo,†
12
Chinedum O. Osuji,† and Menachem Elimelech†*
13 14 15 16 17 18 19
§
Shandong Key Laboratory of Water Pollution Control and Resource Reuse, School of Environmental Science and Engineering, Shandong University, Jinan 250100, China
†
Department of Chemical and Environmental Engineering, Yale University, New Haven, Connecticut 06520-8286
20 21 22 23 24 25 26 27 §†*
Corresponding author: email:
[email protected]; Tel: +86 (531) 88365400
28 29
†*
Corresponding author: email:
[email protected]; Tel: +1 (203) 432-2789
1 ACS Paragon Plus Environment
Environmental Science & Technology
30
ABSTRACT
31
We demonstrate the fabrication of a loose, negatively charged nanofiltration (NF) membrane
32
with tailored selectivity for the removal of perfluoroalkyl substances with reduced scaling
33
potential. A selective polyamide layer was fabricated on top of a polyethersulfone support via
34
interfacial polymerization of trimesoyl chloride and a mixture of piperazine and bipiperidine.
35
Incorporating high molecular weight bipiperidine during the interfacial polymerization enables
36
the formation of a loose, nanoporous selective layer structure. The fabricated NF membrane
37
possessed a negative surface charge and had a pore diameter of ~1.2 nm, much larger than a
38
widely used commercial NF membrane (i.e., NF270 with pore diameter of ~0.8 nm). We
39
evaluated the performance of the fabricated NF membrane for the rejection of different salts (i.e.,
40
NaCl, CaCl2, and Na2SO4) and perfluorooctanoic acid (PFOA). The fabricated NF membrane
41
exhibited a high retention of PFOA (~90%) while allowing high passage of scale-forming
42
cations (i.e., calcium). We further performed gypsum scaling experiments to demonstrate lower
43
scaling potential of the fabricated loose porous NF membrane compared to NF membranes
44
having a dense selective layer under solution conditions simulating high water recovery. Our
45
results demonstrate that properly designed NF membranes are a critical component of a high
46
recovery NF system, which provide an efficient and sustainable solution for remediation of
47
groundwater contaminated with perfluoroalkyl substances.
48 49 50
TOC Art
51 52 53 54 2 ACS Paragon Plus Environment
Page 2 of 29
Page 3 of 29
Environmental Science & Technology
55
INTRODUCTION
56
Perfluoroalkyl substances (PFASs) are emerging contaminants that are persistent in the
57
environment, bio-accumulative, and toxic even at trace concentrations. 1-5 PFASs are used in
58
production of firefighting foams and their widespread use, particularly at airports, oil refineries,
59
and military bases, has led to severe groundwater contamination. 6-9 Because of their unique
60
physicochemical properties, such as strong carbon-fluorine bond and low vapor pressure, PFASs
61
are highly resistant to degradation by chemical or biological processes. 10-12
62
Nanofiltration (NF) is a low-pressure membrane-based separation process widely used in
63
water and wastewater treatment.13, 14 NF has the potential to provide an effective solution for the
64
removal of perfluorooctanoic acid (PFOA) — an important class of PFASs with significant
65
environmental concerns due to widespread industrial use 15 and frequent detection in drinking
66
water resources7 — from groundwater at high water recoveries.16, 17 Separation of PFOA by NF
67
is based on size (steric) exclusion and electrostatic interactions. 18 PFOA has relatively high
68
molecular weights (414 g/mol) and thus can be retained by NF membranes via size exclusion.
69
PFOA removal can be further enhanced via electrostatic repulsion by tailoring the NF membrane
70
surface and pore charge, because PFOA with a low dissociation constant (pKa of –0.1) is
71
negatively charged at the pH of natural waters.19 Several studies have investigated the removal of
72
PFOA by commercial NF membranes and reported relatively high retention rates ~90%. 20, 21
73
Minimizing waste (brine) streams by achieving high water recovery is crucial for successful
74
application of NF to treat PFOA contaminated groundwaters. Current NF systems are limited to
75
low recoveries (75-80%) mainly due to inorganic scaling because groundwaters contain high
76
levels of scale-forming inorganic species, including calcium, magnesium, and silica in the form
77
of silicic acid.22,
78
environmental impacts associated with brine management and, thus, enhance the feasibility and
79
sustainability of NF technology for groundwater remediation. 24, 25
23
There is a critical need to increase water recovery to reduce costs and
80
Nanofiltration membranes have a thin selective layer with pores at the nanometer scale. 26
81
While NF membranes poorly reject monovalent salt, they exhibit high retention rates for scale-
82
forming species such as calcium, sulfate, and silicic acid.23, 27 Such high rejection brings about a
83
significant concern for membrane scaling, especially when designing high water recovery NF
84
systems.28 Therefore, the development of novel NF membranes that provide high PFOA removal 3 ACS Paragon Plus Environment
Environmental Science & Technology
85
and reduced scaling potential is of paramount importance to make NF an efficient and
86
sustainable technology for groundwater remediation.
87
In this study, we demonstrate the fabrication of a loose, negatively charged NF membrane
88
with tailored rejection of perfluoroalkyl substances and scale-forming cations from feed
89
solutions simulating groundwater. The performance of the fabricated membrane for salt and
90
perfluorooctanoic acid removal was evaluated and compared to commercial NF membranes. The
91
selective polyamide layer of the fabricated NF membrane was extensively characterized to relate
92
membrane performance to the physicochemical properties of the selective layer. We further
93
demonstrated a low gypsum scaling potential of the fabricated NF membranes, highlighting the
94
potential application of NF membranes with tailored selectivity for high recovery NF systems to
95
treat PFAS-contaminated groundwaters.
96
MATERIALS AND METHODS
97
Materials and Chemicals. Polyethersulfone (PES) ultrafiltration membranes (LX-300K,
98
Synder FiltrationTM, Vacaville, CA) with a molecular weight cut-off of 300 kDa were used as a
99
substrate. The PES membranes were prewetted by immersing in deionized (DI) water for at least
100
24 h prior to use. Trimesoyl chloride (1,3,5-benzenetricarbonyl trichloride, TMC, 98%),
101
piperazine (PIP, 99%), 4,4′-Bipiperidyl dihydrochloride (BP, 97%), triethylamine (TEA, ≥99%),
102
and sodium hydroxide (NaOH) from Sigma-Aldrich (Sigma-Aldrich, St. Louis, MO) and hexane
103
from J.T. Baker (ACS reagent, Phillipsburg, NJ) were used for interfacial polymerization (IP) of
104
the polyamide (PA) selective layer.
105
The performance of the fabricated NF membranes was compared to a commercial NF
106
membrane, denoted NF270 by the manufacturer (FilmTec Corp., Minneapolis, MN). As
107
indicated by the manufacturer, the NF270 membrane comprises a semi-aromatic piperazine-
108
based, polyamide layer on top of a microporous polysulfone (PSf) support. The membranes were
109
received as flat sheet samples. They were gently washed with deionized (DI) water to remove
110
any preservatives and were stored in DI water at 4 °C.
111
Thin-Film Composite Nanofiltration Membrane Fabrication. TFC NF membranes
112
were fabricated by forming a polyamide (PA) selective layer on top of the PES support
113
membrane via interfacial polymerization (IP). For obtaining a dense PA layer structure, an 4 ACS Paragon Plus Environment
Page 4 of 29
Page 5 of 29
Environmental Science & Technology
114
aqueous solution of 1.0 wt % PIP was used while a mixture of 0.5 wt % PIP and 0.5 wt % BP
115
was employed to construct a loose, porous selective layer during the interfacial polymerization.
116
The NF membranes fabricated using 1.0 wt % PIP and a mixture of 0.5 wt % PIP and 0.5 wt %
117
BP are hereafter denoted as PIP and PIP + BP, respectively. To catalyze the reaction, 0.5 wt %
118
TEA and 0.15 wt % NaOH were added to both aqueous amine solutions. For IP reaction, the PES
119
support membrane (10 cm 15 cm) was tightly taped onto a clean glass plate with a water-proof
120
tape (Fisherbrand Colored Labeling Tape, Fisher Scientific, Inc., MA), with the skin layer facing
121
upward. Approximately 15 mL of aqueous amine solution was dispensed onto the surface of the
122
support membrane and allowed to contact for 90 s. The amine solution was then poured off, and
123
residual amine solution was removed from the membrane surface using an air knife. Next, the
124
monomer-saturated support membrane was immersed in 0.15 wt % TMC in hexane for 30 s,
125
resulting in the formation of a thin-film composite polyamide layer. The composite membranes
126
were then air dried for 120 s, rinsed thoroughly, and stored in DI at 4 °C.
127
Membrane Characterization. Zeta potential of membrane surface was evaluated by a
128
streaming potential analyzer utilizing an asymmetric clamping cell (EKA, Brookhaven
129
Instruments, Holtsville, NY) as described elsewhere.29 Measurements were performed with a
130
solution containing 1 mM KCl and 0.1 mM KHCO3. Electrolyte solution flows into the cell were
131
generated by pressure ranging from 0 to 300 mbar driven by a mechanical pump. The induced
132
streaming potential was measured using Ag/AgCl electrodes mounted at each end of the
133
clamping cell.
134
The carboxylic group density of the polyamide selective layer was measured using the silver
135
elution method.30 First, a 10-mM stock silver nitrate solution (ACS reagent, ≥99% from Sigma)
136
was prepared in 1 wt % nitric acid (trace-metal grade from Sigma) and further diluted to 40 M
137
and 1 M in DI water to obtain solutions for silver binding and rinsing, respectively. Then,
138
solution pH was adjusted to 7 and 10.5 using sodium hydroxide (0.1 M) and nitric acid (1 wt %).
139
Membranes were first wetted in DI water for at least 24 h prior to measurement after which
140
circular membrane samples (2.0 cm2) were punched and the fabric backings were physically
141
removed. The remaining polyamide/support (i.e., either PES or PSf) films were immersed twice,
142
each for 10 min, in 10 mL of the 40 M silver nitrate solution at pH 7 or 10.5 to bind silver one-
143
to-one with ionized carboxyl groups. After the binding step, isolated polyamide/support films 5 ACS Paragon Plus Environment
Environmental Science & Technology
144
were immersed four times, each time for 7 min, in 10 mL of 1 silver nitrate solution at the
145
same pH used during binding to rinse off unbound silver. After each step, film samples were
146
gently touched against Kim wipes to minimize solution carryover. Following the wash steps,
147
isolated polyamide/support films were immersed in 5 mL of 1 wt % nitric acid for 30 min to
148
protonate the carboxyl groups and elute the bound silver ions. After removing films, the silver
149
ion concentration in the solution was determined using ICP-MS.
150
Elemental mapping of the PA selective layer was performed by energy-dispersive X-ray
151
analysis (EDX) in a scanning transmission electron microscope (STEM). The NF membrane
152
samples were embedded in epoxy resin (SPI-PON 812, Structure Probe, Inc.), followed by
153
curing at 60 °C overnight. The samples were then cross-sectioned by ultramicrotome (Leica EM
154
UC7) with a diamond knife (Diatome Ultra 45). A thin specimen of ~100 nm thick cross-
155
sectional film was floated on the water trough of the diamond knife and then transferred onto
156
lacey carbon grids (Ted Pella). STEM-EDX analysis was conducted on TEM (FEI Tecnai Osiris)
157
with an accelerating voltage of 200 kV, equipped with a Super-X EDS detector.
158
The thickness of the selective layer was determined by imaging the isolated PA film using
159
atomic force microscopy (AFM).31-33 The NF membranes were cut into a small piece (~ 1 1
160
cm2) and the fabric backings were physically removed. The isolated polyamide/support films
161
were placed on a silicon wafer with two ends of the film being pressed by a glass slide to avoid
162
film folding and wrinkling during sample preparation. Then, a few drops of dimethylformamide
163
(DMF) were placed on the film to dissolve the PES or PSf support. After a few minutes, the PES
164
or PSf dissolved and DMF solution was carefully wiped off using Kim wipes without touching
165
the film. This procedure was repeated several times to achieve a complete dissolution of the
166
support and to have a transparent free polyamide film tightly fixed on the silicon wafer.
167
Prior to AFM imaging, multiple parallel dents were developed on the isolated PA films using
168
a metal precision glide needle (18 G 1 in, Becton Dickinson & Co., NJ) without damaging the
169
silicon wafer. A border region (10 10 m) between the PA film and the silicon wafer was
170
scanned by AFM using a Bruker Dimension FastScan AFM with a FastScan-B tip (5 nm tip
171
radius, Bruker, Billerica, MA) in tapping mode at a scan rate of 3 Hz. The obtained AFM images
172
were analyzed using the Section function of Nanoscope Analysis v1.5 (Bruker) to determine the
173
PA layer thickness. 6 ACS Paragon Plus Environment
Page 6 of 29
Page 7 of 29
Environmental Science & Technology
174
Estimation of NF Membrane Pore Size. The average pore size of the NF membrane
175
was determined based on a pore transport model that incorporates steric (size) exclusion and
176
hindered convection and diffusion from the rejection data of reference inert organic solutes. 34
177
Neutrally charged, low molecular weight organic molecules — erythritol, xylose, and dextrose
178
(≥99%, Sigma-Aldrich, St. Louis, MO) — were used as the reference organic tracers. 35 Prior to
179
NF experiments, the membrane was pre-compacted under 13.8 bar (200 psi) hydraulic pressure
180
with DI water as the feed for 4 h. After compaction, each organic solute was injected to the feed
181
to obtain a concentration of 40 mg/L (as total organic carbon, TOC) and subsequent experiments
182
were conducted at 4.1, 6.2, 8.3, and 10.3 bar with a crossflow velocity of 21.4 cm/s and a feed
183
temperature of 25.0 0.5 °C. The permeate flux was recorded after the system was run for 1 h at
184
each pressure. Permeate and feed samples were taken for TOC analysis (TOC V-CSH, Shimadzu
185
Corp., Japan) to determine the rejection of the reference organic solutes. Details on the pore size
186
estimation based on the pore transport model using the measured rejection of the reference
187
organic solutes are provided in the Supporting Information.
188
Salt and PFOA Rejection Tests. Single salt rejections were evaluated using 2, 10, and
189
20 mM of sodium chloride (NaCl), calcium chloride (CaCl 2), and sodium sulfate (Na2SO4)
190
solutions. Ion rejections were measured from NF experiments using a salt solution prepared by
191
mixing 5 mM NaCl, 5 mM CaCl2, and 5 mM Na2SO4 with a total ionic strength of 35 mM.
192
Retention of PFOA (Perfluorooctanoic acid, 96%, Sigma-Aldrich, St. Louis, MO) by NF
193
membranes was evaluated using feed solutions containing 1 mg/L of PFOA in DI water and in
194
the combined salt solutions. Feed solution pH was adjusted to 7.0 0.1 during NF experiments.
195
Prior to each experiment, the membranes were compacted for at least 4 h at 6.9 bar (100 psi)
196
using DI water until there was no variation in permeate flux. The feed solution temperature was
197
kept constant at 25.0 0.5 °C throughout the experiment. To compare rejection under the same
198
permeate flux conditions, the hydraulic pressures were set to approximately 6.9 bar (100 psi) for
199
the PIP + BP and PIP membranes and 3.1 bar (45 psi) for the NF270 membrane. Permeate and
200
feed samples were collected after the system was equilibrated for 1 h at each condition and
201
analyzed as described below. Rejection performance of NF membranes was determined by
202
comparing the species concentration in the feed (Cf) and permeate (Cp) samples (i.e., Robs = 1-
203
Cp/Cf). 7 ACS Paragon Plus Environment
Environmental Science & Technology
204
Concentrations of NaCl, CaCl2, and Na2SO4 in the feed and permeate were measured using a
205
calibrated conductivity meter (Oakton Instruments, Vernon Hills, IL). Ion chromatography (IC,
206
Dionex, Sunnyvale, CA) equipped with CS14 and AS14A IonPac separation columns was used
207
to quantify cation and anion concentrations, respectively. PFOA concentration was determined
208
using a high-performance liquid chromatograph (HPLC, Agilent 1290 Infinity Series) coupled
209
with a mass spectrometer (Agilent 6550A iFunnel Q-TOF MS). A sample volume of 1 µL was
210
injected into a C18 column (Eclipse Plus, 1.8 m, 4.6 50 mm) using a mobile phase gradient of
211
solvent comprising 40% methanol and 60% water with 20 mM ammonium acetate at a flow rate
212
of 0.5 mL min-1. Methanol rate was increased from 40% to 98% in 5 min, held for 1 min,
213
dropped back to 40%, followed by a 1-min stabilization. The Q-TOF MS was operated using an
214
electrospray ionization (ESI) interface in negative mode. Linearity was determined from 0.1 µg
215
L-1 to 100 g L-1 using calibration curves (R2 ≥ 0.99), with a limit of quantification (LOQ) of 10
216
ng L-1.
217
Scaling Experiments. The protocol for scaling experiments comprised the following steps.
218
First, a new membrane coupon was placed in the NF cross-flow unit and compacted under 13.8
219
bar (200 psi) hydraulic pressure with DI water as the feed for 4 h. Crossflow velocity and feed
220
solution temperature were maintained at 21.4 cm/s and 25.0 0.5 °C, respectively. After
221
compaction, the system was depressurized while allowing the feed flows to the membrane by
222
maintaining the crossflow velocity of 21.4 cm/s. Calcium chloride (1 M), calcium sulfate (1 M),
223
and sodium chloride (5 M) stock solutions were prepared in advance and filtered with a 0.45 m
224
cellulose acetate membrane filter (Corning, Tewksbury, MA). Stock solutions were added to the
225
feed reservoir to obtain a scaling solution comprising 15 mM CaCl 2, 10 mM Na2SO4, and 10 mM
226
NaCl, with a gypsum (CaSO4·2H2O) saturation index (SI) of 0.54. The feed solution pH was
227
adjusted to 7.0 0.1. The scaling solution was fully mixed and equilibrated for 1 h without
228
applying pressure (i.e., no permeate flux). After equilibrium, the hydraulic pressures were set to
229
about 7.2, 12.4, and 6.6 bar for the PIP + BP, PIP, and NF270 membranes, respectively, to
230
achieve an identical initial permeate flux of ~80 L m -2 h-1. The gypsum scaling experiments were
231
conducted for 20 h at a feed crossflow velocity of 15.0 cm/s and temperature of 25.0 0.5 °C in
232
a recycling mode (i.e., the permeate was recycled back to the feed solution such that the gypsum
233
saturation index was kept constant over time). 8 ACS Paragon Plus Environment
Page 8 of 29
Page 9 of 29
Environmental Science & Technology
234
RESULTS AND DISCUSSION
235
Polyamide Selective Layer Characteristics. We target the fabrication of NF membranes
236
having a selective layer with a loose, nanoporous structure and a negative surface charge to
237
facilitate passage of scale-forming cations and to enhance rejection of negatively charged PFOA
238
via Donnan (charge) exclusion. Interfacial polymerization is the state-of-the-art technique
239
allowing the synthesis of a thin, highly cross-linked selective polyamide layer. 36 Typical NF
240
membranes fabricated via interfacial polymerization of piperazine (PIP, MW of 86.1 g/mol) and
241
trimesoyl chloride exhibit fairly high salt rejection, especially for salts with divalent ions, such as
242
CaCl2, MgCl2, and Na2SO4.37, 38 To achieve our goal of fabricating NF membranes with reduced
243
cation rejection, we incorporated bipiperidine (BP) having a higher molecular weight (168.3
244
g/mol) than PIP during interfacial polymerization. Bipiperidine comprises two piperidine units
245
bound to each other by a carbon-carbon single bond, allowing chain extension and/or
246
crosslinking polymerization to form a loose polyamide structure as described in Figure S1. 39, 40
247
Specifically, we used a mixture of 0.5 wt % PIP and 0.5 wt % BP to obtain a loose, nanoporous
248
selective layer, while a dense polyamide layer was constructed employing 1.0 wt % PIP; these
249
membranes are denoted as PIP + BP and PIP, respectively.
250
To verify the structural properties of the selective layer, we evaluated the average pore size
251
of the PIP + BP membrane and compared it to the PIP and commercial NF270 membranes. The
252
real (intrinsic) retention of inert organic tracers (Rr) was obtained from the observed retention
253
(Ro) by accounting for the effect of concentration polarization using eq S3. Real retentions of the
254
organic tracers by the PIP + BP, PIP, and NF270 membranes at different permeate water fluxes
255
(i.e., transmembrane pressures) are presented in Figure S2.
256
The obtained real retentions were used to estimate the NF membrane average pore size using
257
the membrane pore transport model described earlier. The estimated pore radii are consistent for
258
the different organic reference solutes as summarized in Table S1 of Supporting Information.
259
Based on these results, we conclude that the PIP + BP membrane has an average pore radius of
260
0.61 nm, which is much larger than the radii of the PIP (0.47 nm) and NF270 (0.41 nm)
261
membranes. The larger pore size of the PIP + BP membrane compared to that of the PIP and
262
NF270 membranes demonstrates that incorporating BP during the interfacial polymerization
263
forms a polyamide network with a relatively loose, nanoporous structure. 9 ACS Paragon Plus Environment
Environmental Science & Technology
264
Rejection of charged solutes by electrostatic (Donnan) exclusion is directly related to the
265
charge characteristics of NF membranes.41 We investigated the charge properties of the PIP + BP,
266
PIP, and NF270 membranes by determining the zeta potential and carboxyl group density of the
267
polyamide selective layer. As shown in Figure 1a, all NF membranes display a negative surface
268
charge at solution pH of 7 and 10; the magnitude of the negative zeta potentials follows the order
269
of NF270 > PIP > PIP + BP membranes. The polyamide selective layer of desalination
270
membranes fabricated via interfacial polymerization of trimesoyl chloride (TMC) and amine-
271
based monomers (i.e., BP or PIP) inherently possesses an outer layer of negative fixed charges
272
resulting from hydrolysis of unreacted acyl chlorides of TMC to carboxyl groups. 42 The carboxyl
273
groups of the polyamide film have a dissociation constant (pKa value) of ~5.2.43, 44 The observed
274
negative zeta potential of the PIP + BP, PIP, and NF270 membranes at the investigated pH range
275
is attributed to the ionized surface carboxyl groups.
276
FIGURE 1
277
Streaming potential analysis allows qualitative evaluation of the membrane surface charge
278
characteristics. However, this method does not quantify the fixed charge density but rather
279
determines the zeta (electrokinetic) potential, which is determined by the combined effects of
280
charged groups on the surface as well as ions near the membrane surface. 45 In addition, zeta
281
potential does not account for functional groups buried within the polyamide polymer network or
282
inside the pores,30,
283
mechanisms of NF membranes.
45
although such information is critical to understand the separation
284
To better quantify NF membrane charge characteristics, we measured the carboxylic group
285
density of the PA layer using the recently developed silver elution method. 30 This method allows
286
for the quantification of areal carboxyl density based on the assumption that small, cationic silver
287
ions are bound one-to-one with ionized carboxyl groups that are present on the membrane
288
surface as well as those buried within the polyamide network. 44 As presented in Figure 1b, the
289
areal carboxyl group densities of the PIP + BP, PIP, and NF270 membranes measured at pH 7
290
were in the range of 0.7 – 1.7 sites/nm2, while much higher values were obtained at pH 10.5
291
ranging from 3.8 – 13.0 sites/nm2. These values are relatively small compared to those reported
292
for commercial reverse osmosis (RO) membranes,30 likely due to the thinner polyamide film of
293
NF membranes,46,
47
which has lower degree of cross-linking formed by the semi-aromatic 10 ACS Paragon Plus Environment
Page 10 of 29
Page 11 of 29
Environmental Science & Technology
294
piperazine-based monomer compared to that formed on RO membranes by the fully aromatic m-
295
phenylenediamine monomer.
296
The carboxylic group density measured at pH 7 follows the order of NF270 > PIP > PIP +
297
BP membranes, which correlates well with the results obtained from zeta potential measurements
298
(Figures 1a-b). At a solution pH 10.5, the measured carboxylic group densities were much higher
299
than those measured at pH 7 for all membranes. Additionally, the PIP membrane was found to
300
have much higher carboxylic group density than the PIP + BP and NF270 membranes at a
301
solution pH of 10.5. Such a substantial difference in carboxyl group densities at low (pH 7) and
302
high (pH 10.5) solution pH is consistent with our previous observation of a series of commercial
303
RO membranes.30 We attribute the results to the likely increase in acidity within the polyamide
304
film during the silver binding process. Considering the relatively high carboxylic group
305
concentration within the polyamide film, which is estimated to be 0.2–0.7 M, 44, 48 a substantial
306
decrease in local pH within the polyamide film is postulated; that is, the local pH within the
307
polyamide film would be much lower compared to the bulk solution pH employed during the
308
silver binding procedure. Thus, when a bulk solution pH of 10.5 was employed, the majority of
309
carboxylic groups within the polyamide film remain deprotonated/ionized (COO -), while only a
310
fraction of carboxyl groups exist in ionized form within the film at bulk solution pH of 7.0. It can
311
be concluded that the areal density measured at pH 7.0 corresponds to the carboxyl groups on the
312
membrane surface, while that measured at pH 10.5 corresponds to groups buried within the
313
polyamide network.30 The remarkably high density of carboxylic groups of the PIP membrane
314
observed at pH 10.5 (Figure 1b) based on this proposed mechanism is further discussed in the
315
following subsections.
316
We conducted STEM-EDX elemental mapping to depict the cross-section images of the PA
317
films. The polyamide selective layer is rich in nitrogen while the underlying PSf or PES support
318
layer contains sulfur but no nitrogen, providing elemental contrast in STEM-EDX analysis
319
(Figures 2a-1 to a-3). Although the STEM-EDX elemental mapping was limited to characterize
320
the distinct shape of the protruding polyamide layer nodules,49 it allowed visualization of the
321
relative polyamide layer thickness for the PIP + BP, PIP, and NF270 membranes. The PA layer
322
thickness of the NF270 membrane is likely in the range of 20–30 nm (Figure 2a-3), similar to
323
values reported from other high-resolution microscopy and surface characterization studies. 31, 50 11 ACS Paragon Plus Environment
Environmental Science & Technology
324
A relatively high and thicker signal of nitrogen was detected for the PIP membrane (Figure 2a-2),
325
indicating that the PIP membrane may have a thicker PA selective layer than the other two
326
membranes.
327
FIGURE 2
328
To achieve a more quantitative analysis of the selective layer thickness, the PA film was
329
imaged by atomic force microscopy (AFM). The isolated PA film on the silicon wafer was
330
scratched using a precision glide needle (Figure S4). A border region between the PA film and
331
the silicon wafer was scanned using AFM to determine the PA layer thickness as shown in
332
Figures 2b-1 to b-3. The average PA layer thicknesses of the PIP + BP, PIP, and NF270
333
membranes were 43 2, 61 7, and 29 4 nm, respectively. Consistent with the previous
334
STEM-EDX elemental mapping analysis, the PIP membrane had a thicker PA layer than the PIP
335
+ BP and NF270 membranes. In particular, the thickness of the PIP membrane PA layer was
336
more than two times higher than that of the NF270 membrane. The measured polyamide layer
337
thickness explains the previously observed higher carboxylic group density of the PIP membrane
338
at pH 10.5 compared to that of the other two membranes (Figure 1b). The thicker PIP membrane
339
PA layer contains more carboxylic groups buried within the polyamide network or inside the
340
pores.
341
The investigated structural and charge properties of the PIP + BP, PIP, and NF270
342
membranes are schematically visualized in Figures 2c-1 to c-3. As we intended, the PIP + BP
343
membrane had a pore diameter of ~1.2 nm, much larger than the pore diameters of the PIP
344
(~0.94 nm) and NF270 (~0.80 nm) membranes. All membranes possess negative surface and
345
pore charge, which is attributed to the carboxylic groups of the polyamide film. The thickness
346
normalized carboxyl group density, indicated as “COO-” in Figures 2c-1 to c-3, was calculated
347
by dividing the total carboxylic group density at pH 10.5 (shown in Figure 1b) by the average PA
348
layer thickness measured using AFM (shown in Figure 2b). It is assumed that the carboxyl areal
349
density shown in Figure 1b is based on a dimensionless unit square value. The thickness
350
normalized carboxylic group density is the highest for the PIP membrane (0.21 mn -1), followed
351
by the NF270 (0.19 nm-1) and PIP + BP (0.11 nm-1) membranes.
12 ACS Paragon Plus Environment
Page 12 of 29
Page 13 of 29
Environmental Science & Technology
352
In the following subsections, we relate the polyamide selective layer characteristics discussed
353
above to the salt and PFOA rejection behavior of the NF membranes. We further depict the
354
underlying rejection and scaling mechanisms of the fabricated membranes.
355
Single Salt Rejection Performance. Salt rejection behavior of the PIP + BP, PIP, and
356
NF270 membranes was evaluated with sodium chloride, calcium chloride, and sodium sulfate at
357
concentrations of 2, 10, and 20 mM (Figure 3). We employed hydraulic pressure of 6.9 bar (100
358
psi) for the PIP + BP and PIP membranes and 3.1 bar (45 psi) for the NF270 membrane during
359
the NF experiments to compare the rejection performance of all membranes that had different
360
permeabilities (Figure S3), at the same permeate water flux. As shown in Figure 3a, the rejection
361
of NaCl decreased with increasing salt concentration for all three membranes, which is typically
362
observed for negatively charged NF membranes.51, 52 For symmetric salts like NaCl, electrostatic
363
repulsion between co-ions (ions with the same charge as the membrane) and the membrane
364
governs the NF rejection mechanism.18 For this reason, NF membranes exhibit higher NaCl
365
rejection with increasing solution pH because more carboxylic groups on the PA selective layer
366
are deprotonated (COO-) at higher pH, thereby enhancing Cl- rejection by charge repulsion.53
367
Similarly, at higher salt concentration, screening of the charge on the PA selective layer reduces
368
the effectiveness of electrostatic repulsion of Cl - ions, resulting in a decrease of NaCl rejection.
369
We also observe that the PIP + BP membrane showed much lower NaCl rejections of ~50% and
370
~25% at low (2 mM) and high (20 mM) concentrations, respectively, than the PIP and NF270
371
membranes.
372
FIGURE 3
373
It is interesting to note that NaCl rejection of the PIP membrane was higher than that of the
374
NF270 membrane at all salt concentrations tested, despite the PIP membrane having a larger
375
pore size (Table S1) and less negative zeta potential than the NF270 membrane (Figure 1a). The
376
observed higher NaCl rejection of the PIP membrane can be explained by the thickness of the
377
selective polyamide layer. As described in Figures 2c-2 and c-3, the PIP membrane has a
378
polyamide layer much thicker (61 nm) than the NF270 membrane (29 nm), which induces higher
379
resistance to ion transport through the selective layer. This result highlights the fact that in
380
addition to membrane pore size and charge properties, the PA selective layer thickness plays a
13 ACS Paragon Plus Environment
Environmental Science & Technology
381
critical role in governing ion rejection/selectivity as well as water permeability (Figure S3) of NF
382
membranes.
383
Observed trends of CaCl2 rejection as a function of salt concentration were opposite to those
384
observed with NaCl, where the rejection of CaCl 2 increased at higher concentrations for all NF
385
membranes (Figure 3b). Charge-based separation of asymmetric salts, such as CaCl 2 and Na2SO4,
386
is dominated by the ions of higher valency (Ca2+ for CaCl2 and SO42- for Na2SO4) because the
387
electrostatic repulsive or attractive interactions between such ions and the membrane control the
388
rate of salt transport.18, 53 Hence, CaCl2 rejection by the negatively charged PIP + BP, PIP, and
389
NF270 membranes is mainly controlled by the rate of Ca 2+ permeation through the PA selective
390
layer. At a relatively low CaCl2 concentration (2 mM), electrostatic attraction between Ca2+ and
391
the negative membrane charge facilitates the transport of Ca 2+, resulting in a low CaCl2 rejection.
392
However, cation transport through the negatively charged membrane is reduced at higher salt
393
concentrations (20 mM in Figure 3b) due to effective charge neutralization and screening of the
394
membrane carboxyl groups, resulting in reduced electrostatic attraction and thus higher rejection
395
of CaCl2. When the effect of charge interaction diminishes at high ionic strengths, size exclusion
396
has a stronger effect on Ca2+ retention. Considering the size of the hydrated Ca2+ ion (radius of
397
~0.41 nm)54 and the estimated pore radii of the PIP (~0.47 nm) and NF270 (~0.41 nm)
398
membranes (Table S1), size exclusion of Ca2+ can be effective at high salt concentrations. In
399
contrast, the PIP + BP membrane showed a much lower CaCl 2 rejection (