Intermolecular cross-polarization studies of the miscibility

May 11, 1989 - (26) Douglass, D. C.; McBrierty, V. J. Macromolecules 1978, 11,. 766. (27) Ward ... Enhancement of PS/PMMA Blends through Ionic Interac...
0 downloads 0 Views 632KB Size
412

Macromolecules 1990,23, 412-416

(18) Noland, J. S.; Hsu, N. N.-C.; Saxon, R.; Schmitt, J. M. Ado. Chem. Ser. 1971, 99, 15. (19) Nishi, T.; Wang, T. T. Macromolecules 1975,8,909. (20) Bernstein. R. E.: Cruz. C. A,: Paul. D. R.: Barlow. J. W. Macromolecules 1977, 10, 681. (21) Wendorff, J. H. J. Polym. Sci., Polym. Lett. Ed. 1980, 18,439. (22) Roerdink, E.; Challa, G. Polymer 1978, 19, 173. (23) LBonard, C.: Halarv, J. L.: Monnerie. L. Polymer 1985.26.1507. (24) LBonard, C.; H a k y , J. L.; Monnerie, L. Macromolecules 1988,22, 1265. (25) Hahn, B. R.; Herrmann-Schonherr, 0.;Wendorff, J. H. Polymer 1987,28, 201. (26) Douglass, D. C.; McBrierty, V. J. Macromolecules 1978, 11, 766

(27) Ward, T. C.; Lin, T. S. In Polymer Blends and Composites in Multiphase Systems; han, C. D., Ed.; Advances in Chemistry 206; American Chemical Society: Washington, DC, 1984, p 59. (28) Ward, T. C.; Lin, T. S. Polym. Prepr. 1983, 24, 136. (29) TBkBly, P.; Laupretre, F.; Monnerie, L. Polymer 1985,26,1081. (30) Grinsted, R. A.; Koenig, J. L. Polym. Prepr. 1988, 29(1), 15. (31) Stejskal, E. 0.;Schaefer, J. J . Magn. Reson. 1975, 18, 560. (32) Kendrick, R. D.; Yannoni, C. S. J.Magn. Reson. 1987, 75,506. (33) The Radio Amateur's Handbook; Myers, R., Ed.; The American Radio Relay League: Newington, CT, 1974.

(34) Mehring, M. Principles of High Resolution NMR in Solids. In NMR-Basic Principles and Progress, 2nd ed.; Springer-Verlag: New York, 1983; Vol. 12, p 282. (35) Demco, D. E.; Tegenfeldt, J.; Waugh, J. S. Phys. Reu. B 1975, 11, 4133. (36) Slichter, C. P. Principles of Magnetic Resonance. In Springer Series in Solid-State Sciences, 2nd ed.; Springer: New York, 1980, Vol. 1. (37) Maricq, M. M.; Waugh, J. S. J . Chem. Phys. 1979, 70, 3300. (38) Staverman, A. J. In Integration ofFundamenta1Polymer Science and Technology; Kleintjens, L. A,; Lemstra, P. J., Eds.; Elsevier: London, 1986, p 19. (39) CHEMX, developed and distributed by Chemical Design Ltd., Oxford. The van der Waals volume of a repeating unit of PVF, and PMMA was calculated by using CHEMX. Values found were 40.4 and 77.3 A, respectively. (40) DiPaola-Baranvi. G.: Fletcher. S. J.: Deer&.P. Macromolecules 1982, 15, "885. (41) LBonard, C.: Halarv, J. L.: Monnerie, L. Macromolecules 1988,21, 2988. (42) Alemany, L. B.; Grant, D. M.; Pugmire, R. J.; Alger, T. D.; Zilm, K. W. J . Am. Chem. SOC. 1983, 105, 2142. I

Y

i

Registry No. PMMA, 9011-14-7; PVF,, 24937-79-9.

Intermolecular Cross-Polarization Studies of the Miscibility Enhancement of PS/PMMA Blends through Ionic Interactions Xinsheng Zhang,t Almeria Natansohn,$ and Adi Eisenberg**t Departments of Chemistry, McGill University, Montreal, Quebec, Canada H3A 2K6, and Queen's University, Kingston, Ontario, Canada K7L 3N6. Received December 27, 1988; Revised Manuscript Received May 11, 1989

ABSTRACT: The CPfMAS 13C NMR technique is employed in this study to probe the bulk structures of deuteriated PSfprotonated PMMA blends containing ionically interacting groups. Deuteriated PS does not show a 13C NMR signal in CPfMAS experiments since the magnetization of 13C is primarily polarized by protons. However, if protons of the PMMA chains can be found within a few angstroms of the deuteriated PS, then the 13C NMR signals of P S can be observed, with the intensity of P S signals depending upon the proximity of deuteriated PS to the PMMA. The present results show that the PSfPMMA pair is immiscible. However, when P S is lightly sulfonated (3.3 mol % of -SO,H) and PMMA is copolymerized with 2.3 mol % 4-vinylpyridine (4VP), the miscibility of the blend is enhanced, due to proton transfer from the -SO,H to the 4VP with the formation of ionically interacting sites on the deuteriated PS and the PMMA. By the introduction of about 9.5 mol % of interacting groups (-SO,H and 4VP), the blend shows much greater enhancement in miscibility. When the -SO,H on the deuteriated P S is neutralized with N(CH,),OH and the 4VP is quaternized with CH,I, the blends exhibit similar or even better miscibility compared with the proton-transfer blends. This is attributed to the direct ion-ion interactions in the blends. Blend recovery methods affect the chain proximity in the blend.

Introduction In recent years, polymer blends have been the s u b j e c t of extensive investigation^.'-^ In m a n y instances, the properties of the blends are superior to those of the individual components. S i n c e most polymer p a i r s are not miscible, one of the i m p o r t a n t f e a t u r e s of polymer research is the investigation of miscibility enhancement techn i q u e s since control of miscibility allows one to control the final properties. M a n y miscibility enhancement strategies h a v e been explored in the past. These include copolymerization, e i t h e r i n the f o r m of r a n d o m copolymers or preferably i n the f o r m of blocks used as emulsifiers: utilization of

* To whom correspondence should be addressed. McGill University.

* Queen's University.

chain^,^.^ formation of donor-acceptor complexes,' and, in addition, dipole-dopole? ion-dipole: and ion-ion interactions." Miscibility enhancement b y ionic interactions has been the s u b j e c t of extensive s t u d i e s i n t h i s laboratory. For example, the immiscible polymer p a i r poly(ethy1 acrylate) (PEA)/polystyrene ( P S ) c a n be made miscible b y the incorporations of ca. 5 m o l % 4-vinylpyridine i n t o the PEA and a c o m p a r a b l e amount of sulfonic acid in the PS." In the process of mixing, proton transfer occurs f r o m the sulfonic acid to the pyridine, which results in the formation of opposite charges on the different c h a i n s and leads t o s t r o n g coulombic interactions which hold the c h a i n s together. A wide r a n g e of other s y s t e m s has b e e n treated i n a s i m i l a r m a n n e r , including the p a i r poly(tetrafluoroethylene)/poly(ethyl acrylate)." Iondipole interactions are another way for improving miscihydrogen bonding between the dissimilar

0 1990 American Chemical Society

Macromolecules, Vol. 23, No. 2, 1990

sample no.

I I1

I11 IV V VI a

blends PS/PMMA PSSSAIPMMAIVP PSSSAlPMMA4VP PSSSN/PMMAQVPQ PSSSN/PMMA4VPQ PSSSNIPMMAIVPQ

Miscibility Enhancement Studies of PS/PMMA Blends 413 Table I Blend Preparation Methods content of blending recovery SSAa/4VPb ratio 010 3.312.3 9.519.6

3.312.3 9.519.6 9.519.6

50150 50150 50150 50150 50150 50150

methods A A A A A

B

RI' 0

0.48

1.00 0.44 1.31 1.72

Styrenesulfonicacid. 4-Vinylpyridine. Relative intensity.

bility of polymer systems, illustrated by the case of poly(ethylene oxide) and poly(styrene-co-lithium methacrylate) blendsg Many techniques are available for the study of miscibility in polymers. Light scattering, for example, can probe the domain sizes of the order of the wavelength of light (ca. 1000-10 000 A). Dynamic mechanical measurements are sensitive to the dimensions of ca. 100 A, but they require a Tgdifference of at least 30 OC between the individual components. Other methods include FTIR, UV, fluorescence spectroscopy, dielectric measurements, and optical and electron microscopy, among many others. Recently, high-resolution solid-state NMR spectroscopy has become available and has been utilized to explore the microstructures of polymer blends on a molecular level. A variety of techniques have been developed in this field in recent years. Relaxation time measurements,12 spin diffusion determination^,'"'^ signal attenuation in fluorine-containing systems,15and different delay and decoupling methods16 are a few examples. In the present work, intermolecular cross-polarization technique will be used to study the phase structure of deuteriopolystyrene (PS)/poly( methyl methacrylate) (PMMA) blends containing ionic groups. Generally, in CP/MAS 13C NMR measurements, the deuteriated polymer chains will not show NMR resonance lines since the polarization of carbon-13 magnetization originates primarily from the proton reservoir. However, if the deuteriated component forms an intimate mixture with a protonated component and the distance between the deuteriated chains and the protonated chains is within a few angstroms, then the deuteriated component may get polarized by the nearby protonated chains so that a partial or full spectrum of t h e deuteriated component can be detected. Since the cross-polarization only occurs if the interacting atoms are within a very short range, this method can give a good estimate of chain proximity. The applicability of this technique in polymer blends has been studied recently with a well-known miscible polymer pair PS/ PVME and an immiscible polymer pair PS/PMMA.",l8 The results show that the technique is an effective tool in characterizing the miscibility of polymer blends as well as interface interdiffusions. Although it is known that the blend of PS/PMMA is immi~cible,'~ a recent solution NMR study revealed that when PMMA was copolymerized with a small amount of 4-vinylpyridine and PS was lightly sulfonated, the mixture of poly(methy1 methacrylate-co-4-vinylpyridine) (PMMA4VP) and poly(styrene-co-styrenesulfonic acid) (PSSSA) in DMSO resulted in a close proximity of the chains of the two components.20 The driving force for miscibility enhancement in this polymer pair is the formation of the pyridinium sulfonate ion pair by proton transfer from the PSSSA t o the PMMA4VP. Obviously, it is of great interest to study such blends in the solid state, since in solutions the effect of solvent on the miscibility can be crucial. Furthermore, in most cases,

polymers, as well as their blends and composites, are used in solid form. An understanding of the bulk structures of polymer systems gives a better base for property design. Due to the small difference in the T i s of the two blending components, this system cannot be effectively studied with dynamic mechanical methods. The present work, therefore, uses the CP/MAS 13C NMR technique t o study the miscibility enhancement of the blends of PMMA and PS with different contents of interacting groups in various forms.

Experimental Section Materials. Deuteriated polystyrene with a molecular weight of approximately 180 O00 was made by anionic polymerization (deuteriatedstyrene: Cambridge Isotope Laboratory; d > 98%). The polymer was purified by precipitation, using benzene and methanol as the solvent and the nonsolvent. Sulfonation was conducted in 1,2-dichloroethane(American Chemicals; reagent) at 50 "C using a procedure similar to that described elsewhere.21 The polymer was recovered by steam stripping,washed with deionized water, dried, dissolved in benzene/methanol(90/ 10, v/v), and precipitated in methanol. The final polymer was vacuum dried at 50 "C until constant weight was obtained. The degree of sulfonation was determined by dissolving an adequate amount of PSSSA in benzene/methanol(90/10)and titrating the solution with either standardized NaOH/methanol solution or N(CH,),OH/methanol solution. Neutralization of PSSSA was carried out by dropping the appropriate amount of a N(CH,),OH/methanol solution to PSSSA in benzene/ methanol with stirring. The composition of benzene/ methanol mixture was varied so that a clear PSSSA solution was obtained. The neutralized PSSSA (PSSSN) was freezedried followed by vacuum drying at 60 "C to constant weight. NMR measurements of PSSSN showed that the degree of sulfonation was in good agreement with the titration data. Poly(methy1methacrylate-co-4-vinylpyridine) was prepared by free radical polymerization as described elsewhere.22 The conversion was kept at about 30% so that good homogeneity of the unit distribution in the polymer chains can be obtained. 4VP contents were determined by titration with a perchloric acid/acetic acid solution. Quatemization was performed by adding excess methyl iodide (Aldrich; 99.5%, fractionallydistilled before use) to a PMMA4VP solution in benzene/ethanol (90/ 10) at reflux temperature for 2 h. The resultant polymer (PMMAIVPQ) was first freeze-dried and then vacuum dried. Blending. About 0.1 g of an accurately weighed sample was dissolved in benzene/methanol (90/10)mixture to yield a clear solution with a concentration of 1%(w/v). This solution was then added dropwise to a similar solution of the other component with vigorous stirring at room temperature, followed by continued stirring for about 10-20 min. Since the solutions were very dilute, this procedure should yield an equilibrium mixture in solution. For both blends of PSSSA/PMMA4VP and PSSSN/ PMMAIVPQ with higher concentrations of interacting groups (above 3 mol %), a gel was formed as soon as the first drop of the other solution was added, showing that a very rapid interaction is involved. The blended polymers were recovered in two ways: A. The mixtures were freeze-dried and then vacuum dried at 60 "C to constant weight. B. Only the gel part, which precipitated in blending, was taken out of the solution and then pressed between Teflon films

414

Macromolecules, Vol. 23, No. 2, 1990

Zhang et al.

1

~

2 0 l

l

l

~

~

l

l

Il l l l 1

I I / I ; I I I I

I l l 1

I

1 11 1 1 ~ 1 1 1 1

2 0

I I I I ~ I I I II I I I

5b

1 0

I O

PPH

r

-0

Figure 2. CP/MAS 13C NMR spectra of the blends. a-c cor-

respond to samples 1-111, respectively.

9,: ' :do' I

'

'id;

I

'id;

I I

lib'

r-m

Figure 3. Addition results of 20% PS spectrum and 80% PMMA spectrum with spinning sideband suppression.

of PSSSA/PMMA4VP containing 3.3 mol % SSA and 2.3 mol % 4VP, however, a recognizable peak at 128 ppm, representing resonances of aromatic carbons in PS, is seen in the CP/MAS 13C NMR spectrum (Figure 2b). This implies that at least some of the heterochains must be close to each other at the molecular level (within 10 A). Since the peak is weak, the two components do not appear to be well mixed. With 9.5 mol % interacting groups, the blend of PSSSA/ PMMA4VP shows a much more intense peak a t 128 ppm (Figure 2c), when compared with the 3 mol % blend. The relative intensities (RI) of the peaks at 128 ppm in the blends to those of the carbonyl peaks (178 ppm) in PMMA are listed in the last column of Table I. The data indicate that an enhanced chain proximity, and thus enhanced miscibility, is a direct consequence of the higher ion content. However, the efficiency of intermolecular crosspolarization is still not significant under the experimental conditions. In the normalized mode and on the same vertical scale for the most intense peak of each spectrum, the addition of about 20% of the pure PS spectrum to 80% of the PMMA spectrum with comparable sample weight gives a spectrum resembling that of the PSSSA/PMMA4VP blend with 9.5 mol 9'0 ions (Figure 3). This, however, does not imply that the blend is not completely miscible, since the experimental conditions were chosen so as to optimize the whole spectrum, not just the aromatic ring resonances. Longer contact times might be needed for the maximum intermolecular crosspolarization signals. The difference spectrum of the blend minus that of PMMA4VP shows that only the aromatic carbons of PSSSA are significantly polarized (Figure 4).

Miscibility Enhancement Studies of PS/PMMA Blends 415

Macromolecules, Vol. 23, No. 2, 1990

Figure 4. Difference spectrum of PSSSA/PMMA4VP with 9.5% ions minus that of PMMA4VP with spinning sideband suppression.

rTT

'30'

d

301

'Idol I ' \do' ' I '5b I ' I PI PW ' Figure 5. CP/MAS 13C NMR spectra of PSSSN/PMMA4VPQ blends with different ion concentrations (a and b) and different recovery methods (b and c). 2d0

I

Scheme I

*CH2CH * I

Q

CHZCH

~lhh,

1

-

@ wv C H 2 6 b

wv C H 2 6 b

This means that the aromatic rings are closer to the PMMA chains or parts of them than the main chain of PSSSA. The bulky phenyl rings provide an effective spacer between the polystyrene backbone and the protons of the PMMA. The blend of neutralized PSSSA and quaternized PMMA4VP (PSSSN/PMMA4VPQ, sample IV) containing exactly the same concentration of functional groups as sample I1 gives a similar result as that obtained from sample I1 (Figure 5a), indicating that, a t the lower ionic group concentration, both ionomer/ionomer and protontransfer blends show a weak miscibility enhancement effect. The miscibility enhancement in the PSSSN/PMMA4VPQ blend may result either from ion pair/ion pair association or from direct ionic interaction by the elimination of microions (Scheme I). The similar degree of miscibility enhancement for the blend PSSSNIPMMAIVPQ compared with the blend PSSSA/PMMA4VP implies the existence of comparable interactions in these two sys-

tems. For the blend of PSSSA/PMMA4VP, it had been demonstrated that strong ionic interactions due to proton transfer from PSSSA to PMMA4VP were involved.20 Thus, it is reasonable to assume that, in the PSSSN/PMMA4VPQ blends, ionic interaction is predominant rather than ion pair/ion pair association. This idea is supported by the following observations: when the blend of PSSSN/PMMA4VPQ was prepared in DMSO at room temperature, the polymers precipitated from the solution as a gel. The supernatant DMSO solution shows a strong signal of +N(CH3I4by NMR while the polymer signals are a t a noise level. This shows that the microions are eliminated from the polymer chains and remain in solution. If the same experiment is performed in a benzene/methanol(W/lO) mixture, the polymers also precipitate. The salt [+N(CH,),I-] is only slightly soluble in that solvent. However, when the gel is removed and the supernatant liquid is shaken with water, the aqueous solution does show a strong +N(CH3), signal. This suggests that upon blending the +N(CH,)J, perhaps in the form of microcrystals, is at least partly separated from the polymer matrix. Then the macroion pairs are formed, which leads to the miscibility enhancement a t a strength comparable to that seen in the proton-transfer blends. The ionomer/ionomer blend PSSSN/PMMA4VPQ containing 9.5 mol '% interacting groups shows an even stronger aromatic ring resonance than the 3 mol '% system (Figure 5b and Table I). This indicates that, in the ionomer/ionomer blends, heterochain proximity can also be improved with increasing ionic concentration, just as in the proton-transfer blends. If the blend is compared with proton-transfer blend containing the same concentration of interacting groups, it can be seen from Table I that an even closer chain proximity is found in ionomer/ ionomer blend. This further miscibility enhancement is the result of the purely ionic interactions between the two polymer chains, uncomplicated by the presence of hydrogen and the possibility of directional hydrogen bonding. All of the above blends are recovered by a freeze-drying method. When the gel part, which involved over 95 wt 9% of total polymers, was taken out from the mixture of the two polymer solutions and then directly dried in a vacuum oven (sample V, recovery method B), a further increase in aromatic carbon resonances was observed, possibly due to a still more efficient packing of the polymer chains.

Conclusions The study on the efficiencies of intermolecular crosspolarization demonstrates that the miscibility enhancement, characterized by a heterochain distance of within 10 A, can be achieved by introducing ionic interactions between the two polymer chains. The ionic interaction in ionomer/ionomer blends is obtained by the elimination of microions from the polymer chains. With increasing interacting group concentrations, heterochain proximity is improved in ionomer/ionomer blends, as well as in proton-transfer systems. The methods of blend isolation also have observable impact on the heterochain proximity, possibly due to the packing effect. Acknowledgment. We acknowledge the assistance of Alain Desjardins in preparing the deuteriated PS. Acknowledgment is also made to the donors of the Petroleum Research Fund, administered by the American Chemical Society, for partial support of this research. This work was also supported by the Natural Science and Engineering Research Council of Canada.

Macromolecules 1990,23, 416-422

416

(13) Caravatti, P.; Neuenschwander, P.; Ernst, R. R. Macromole-

References and Notes Polymer Blends;Paul, D. R., Newman, S.,Eds.; Academic Press: New York, 1978. Olabisi. 0.: Robeson. L. M.: Shaw. M. T. Polvmer-Polymer Miscibility: Academic Press:' New York, 1978. " Goh, S. M.; Paul, D. R.; Barlow, Y. W. J . A p p l . Polym. Sci. 1982, 27(3), 1091. Fayt, R.; Jerome, R.; Teyssie, P. J . Polym. Sci., Polym. Lett. 1981, 19, 79. Djadoun, S.; Goldberg, R. N.; Morawetz, H. Macromolecules 1977, 10, 1015. Pearce, E, M.;Kwei, T. K.; Mi% B. y. J . Macromol. SCi.9 Chem. 1984, A21, 1181. Pugh, C.; Percec, V. Macromolecules 1986, 19, 65. Prud'homme, R. E. Polym. Eng. Sci. 1982, 22, 90. Hara, M.; Eisenberg, A. Macromolecules 1984, 17, 1335. Smith, P.; Eisenberg, A. J . Polym. SCi., PolSm. Lett. Ed. 1983, 21, 223. Murali, R.; Eisenberg, A. J . Polym. Sci., Part B: Polym. Phys. 1988, 26, 1385. Douglas, D. C.; McBrierty, V. J. Macromolecules 1978, 11, 766.

cules 1986, 19, 1889.

(14) Henrichs, M. P.; Tribone, J.; Massa, D. J.; Hewitt, J. M. Mac-

romolecules 1988, 21, 1282. (15) Ward. T. C.: Lin. T. S.: ACS S v m n Ser. 1984. No. 206. 59. (16) Schaefer, J.;Sefc'ik, M.'D.; SteGkil, E. 0.;Mckay, R. A: Macromolecules 1981, 14, 188. (17) Parmer, J. F.; Dickinson, L. C.; Chien, J. C. W.; Porter, R. S. Macromolecules 1987, 20, 2308. (18) Gobbi, G. C.; Silvestri, R.; Russell, T. P.; Lyerla, J. R.; Fleming, W. W.; Nishi, T. J . Polym. Sci., Part C: Polym. Lett. 1987, 25, 61. (19) Krause, S. In Polymer Blends; Paul, D. R., Newman, S.Eds.; Academic Press: New York, 1978; Vol. 1, p 7 5 . (20) Natansohn, A.; Eisenberg, A. Macromolecules 1987, 20, 323. (21) Makowski, H. S.; Lundberg, R. D.; Singhal, G. H. US. Patent

3,870,841, 1975. ( 2 2 ) Duchesne, D. Ph.D. Thesis, McGill University, 1985.

Registry No. (PMMA)(4VP) (copolymer), 26100-41-4; (PMMA)(4VP).CH31(copolymer), 110923-53-0; N(CH,),OH, 7559-2.

Hydrostatic Pressure Dependence of Molecular Motions in Polycarbonates J. H. Walton, Martin J. Lizak, and Mark S. Conradi Department of Physics, Washington University, S t . Louis, Missouri 63130

Terry Gullion and Jacob Schaefer' Department of Chemistry, Washington University, St. Louis, Missouri 63130. Received September 15, 1988; Revised Manuscript Received June 26, 1989

ABSTRACT: T h e temperature dependence of the proton NMR line width of polycarbonate and of the phenoxy resin formed from bisphenol A and epichlorohydrin have been measured as a function of hydrostatic pressure. These measurements lead to the conclusion that for both polymers, ring motions are suppressed by the denser chain packing resulting from hydrostatic pressure. The magnitude of the NMR pressure dependence is comparable to the pressure variation of the y mechanical loss peak in polycarbonate. T h e 'H NMR results, together with those from a variety of cross-polarization magic-angle spinning 13C NMR experiments performed a t room temperature and atmospheric pressure, are interpreted in terms of a bundle model of chain packing in the glassy matrix. From the observed activation volumes, activation energies, and main-chain reorientation rates, the bundles are inferred to involve the correlated motions of just a few chains.

Introduction Polycarbonate (PC) forms a glassy polymer that is remarkable for its high-impact resistance and ductility over a wide temperature range. Molecular motions occurring below T have long been believed to be at least partly responsible for PC's favorable mechanical properties.' Indeed, a substantial mechanical loss peak ("y") observed in PC indicates the presence of 1-Hz motions (which are coupled to bulk and shear modes) 250 "C below T,. Nuclear magnetic resonance (NMR) has been used to assemble a picture of the motions present in polycarbonate. Deuterium NMR line shapes,' 13C chemical shift anisotropy pattern^,^ and 13C-lH dipolar spectra4 have yielded the most specific information. The most obvious motions in the NMR spectra are 180" flips of the phenylene groups about their C, axes and methyl rotations about the C, axes. Because these motions carry the molecule back into itself, they cannot be directly responsible for the mechanical loss and favorable mechanical properties of PC. However, the rate of phenylene 180' flips does appear on the same temperature0024-9297/ 9012223-04 16$02.50/0

frequency relaxation line with the y mechanical and dielectric loss peaks.5 Closer examination of the 13C-lH dipolar spectra of phenylene and methyl carbons indicates that other motions are also present a t room temperature? these include approximately 30" oscillations of the phenylene groups about the C, axes and 15" mainchain reorientations ("wiggles"), It has been proposed7 that the main-chain motions create sufficient volume to enable, or gate, the 180" ring flips. Thus, the ring flips are an indirect measure of the mechanically active mainchain motions. In this paper, we establish a link between the NMR measurements and the mechanically active motions. The mechanically active motions (specifically, the bulk modes) necessarily produce volume fluctuations that can be probed by changing the conjugate variable, p r e s s ~ r e . ~Thus, '~ we have measured the temperature and pressure dependence up to 1800 bars of the proton T , in PC and in the phenoxy resin of bisphenol A and epichlorohydrin (PK). Because proton NMR measurements often are unable to specify the exact nature of motions present, our interpretation of motion is based on the high-pressure proton 8 1990 American Chemical Society