Subscriber access provided by University of Groningen
Article
Lightweight, Mesoporous, and Highly Absorptive AllNanofiber Aerogel for Efficient Solar Steam Generation Feng Jiang, He Liu, Yiju Li, Yudi Kuang, Xu Xu, Chaoji Chen, Hao Huang, Chao Jia, Xinpeng Zhao, Emily Hitz, Yubing Zhou, Ronggui Yang, Lifeng Cui, and Liangbing Hu ACS Appl. Mater. Interfaces, Just Accepted Manuscript • DOI: 10.1021/acsami.7b15125 • Publication Date (Web): 28 Nov 2017 Downloaded from http://pubs.acs.org on November 29, 2017
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
ACS Applied Materials & Interfaces is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
Lightweight, Mesoporous, and Highly
2
Absorptive All-Nanofiber Aerogel for Efficient
3
Solar Steam Generation
4
Feng Jiang1,2†, He Liu2†, Yiju Li2, Yudi Kuang2, Xu Xu2, Chaoji Chen2, Hao Huang3, Chao Jia2,
5
Xinpeng Zhao4, Emily Hitz2, Yubing Zhou2, Ronggui Yang4, Lifeng Cui1*, Liangbing Hu2*
6
*Lifeng Cui: Email:
[email protected] 7
*Liangbing Hu: Email:
[email protected] 8
1. School of Environment and Civil Engineering, Dongguan University of Technology,
9
Guangdong 523808, China
10
2. Department of Materials Science and Engineering, University of Maryland, College Park,
11
Maryland, 20742
12
3. Department of Mechanical Engineering, University of Maryland, College Park, Maryland,
13
20742
14
4. Department of Mechanical Engineering, University of Colorado, Boulder, Colorado, 80309
15
Keywords: Cellulose nanofibrils, carbon nanotube, aerogel, solar steam generation, water
16
treatment
17 18
1 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 2 of 24
1
ABSTRACT
2
Global fresh water shortage has driven enormous endeavors in seawater desalination and
3
wastewater purification; among these, solar steam generation is effective in extracting fresh
4
water by efficient utilization of naturally abundant solar energy. For solar steam generation,
5
primary focus is to design new material with biodegradability, sustainability, low cost and
6
high solar steam generation efficiency. Here, we designed a bilayer aerogel structure
7
employing naturally abundant cellulose nanofibrils (CNFs) as basic building blocks to fulfill
8
sustainability and biodegradability, and carbon nanotube (CNT) layer for efficient solar
9
utilization with over 97.5% of light absorbance from 300-1200 nm wavelength. The
10
ultralow density (0.0096 g/cm3) of the aerogel ensures minimal material required, reducing
11
the production cost while at the same time satisfying water transport and thermal
12
insulation requirement due to the highly porous structure (99.4% porosity). Owing to its
13
rationally designed structure and thermal regulation performance, the bilayer CNF-CNT
14
aerogel exhibits high solar energy conversion efficiency of 76.3% and 1.11 kg m-2 h-1 at 1 kW
15
m-2 (1-Sun) solar irradiation, comparable or even higher than most of the reported solar
16
steam generation devices. Therefore, the all-nanofiber aerogel presents a new route for
17
designing biodegradable, sustainable, and scalable solar steam generation device with
18
superb performance.
19 20 21 22 23 24
2 ACS Paragon Plus Environment
Page 3 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
INTRODUCTION
2
Solar energy, as a clean and inexhaustible energy source, if harvested efficiently, could
3
potentially relieve human beings from the global energy crisis and environment
4
deterioration caused by our reliance on fossil fuels. In fact, the hourly solar irradiation on
5
earth generates more than enough energy to sustain human consumption for a year.1
6
Aiming at efficient utilization, persistent endeavors have been devoted toward harvesting
7
and converting solar energy into varied forms of energy, including electrical energy via
8
solar photovoltaics2 and concentrated solar-thermoelectrics,3, 4 chemical energy via
9
photocatalysis5 and photoelectrolysis,6 as well as thermal energy via the most recent
10
developed solar steam process.7-16 Among these solar energy utilization approaches, light-
11
to-heat conversion by a heat localizing layer with excellent visible and near infrared light
12
absorbing capacity has been demonstrated to be extremely efficient, showing solar thermal
13
conversion efficiency as high as 90%.7, 17 This solar-driven steam generation process,
14
without relying on additional energy input, could be effectively applied in water purification
15
and desalination, to address global water shortage crisis.
16
Although water evaporation is a phenomenon occurring naturally within the ecosystem, it
17
is a sluggish process due to the low efficiency in heating bulk water body. Therefore, for
18
efficient solar steam generation, several design criteria must be met, including efficient
19
broad-band light absorption with thermal management to confine the absorbed light in a
20
local area, and excellent water absorbing properties to transport water upwards to the
21
heating zone.18 Most current strategies in solar steam generation generally rely on either
22
expensive metallic nanoparticles for plasmonic heating,7, 17, 19-21 or complicated fabrication
23
processes to design porous structures required for water transport, such as chemical vapor
24
deposition growth of porous graphene,22 and nanoporous anodic aluminum oxide.7, 17
25
Aerogel, due to its extraordinary properties such as super absorbency, ultralow density and
3 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 24
1
ultrahigh porosity, has attracted numerous research interests in water treatment
2
applications such as oil/water separation.23, 24 Recently, a graphene oxide based aerogel that
3
incorporated multi-walled carbon nanotubes for broadband solar absorption and sodium
4
alginate for water absorption was developed, demonstrating 83% efficiency in solar steam
5
generation, which confirms the benefits of a porous network structure in solar steam
6
generation.25
7
As a natural nanomaterial, cellulose nanofibril (CNF) has attracted abundant research
8
interest due to their nanoscale dimensions, excellent mechanical properties, sustainability
9
and biodegradability.26-31 Recently, cellulose has been widely used as green material for
10
solar energy conversion and storage application, including as photoanodes and polymer
11
electrodes for dye-sensitized solar cell,32-34 as light management layer for thin film solar
12
cell,35, 36 as well as binder and current collector in next-generation lithium-ion battery.37
13
CNF can be facilely assembled into a 3D porous aerogel structure with excellent structural
14
integrity and resilience, which has been extensively investigated in areas including
15
wastewater treatment, thermal insulation, and electrochemical energy storage.23, 38-42
16
However, application of this super solar-absorbing and thermal insulating CNF aerogel in
17
solar steam generation has not been reported, which drives us to explore its potential in
18
this emerging area.
19
RESULTS AND DISCUSSION
20
Herein, we report a bilayer-structured aerogel comprising of two types of nanofibers (i.e.,
21
CNF and carbon nanotube (CNT)) seamlessly integrated with each other to form a
22
compressible and efficient solar steam generator, as shown in Figure 1a. This bilayer
23
aerogel contains a bulk CNF skeleton with anisotropic vertically elongated macrochannels
24
of 200-300 μm wide, which function as conduits to pump water upwards owing to the
25
extremely hydrophilic nature of CNF and the capillary forces exerted by these
4 ACS Paragon Plus Environment
Page 5 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
macrochannels. The CNF aerogel also works as thermal insulation due to its high porosity,43
2
effectively reducing the parasitic thermal loss to the bulk water. The light absorbance of
3
CNT closely resembles the blackbody behavior, with extremely high absorptivity of 0.98-
4
0.99 over 250-1200 nm wavelength,44, 45 which allows it to function as an effective solar
5
absorption material in varied energy and environmental applications.46-49 To improve both
6
interfacial bonding between CNT and CNF and the structural integrity of the bilayer aerogel,
7
CNT containing 3-6% carboxylic was used as the heat absorption layer,50 which can strongly
8
interact with the (2,2,6,6-tetramethylpiperidin-1-yl)oxyl (TEMPO) oxidized CNF through
9
hydrogen bonding. With this rationally designed bilayer structure, the bilayer aerogel
10
demonstrated broadband solar absorption efficiency at the CNT layer for efficient light-to-
11
heat conversion. The highly porous CNF aerogel structure and the confined thin CNT coating
12
are effective in local heat management, guaranteeing minimum heat loss to the bulk water
13
body or surrounding environment. As water evaporates from the top CNT layer, continuous
14
water flow supply is well maintained due to the highly absorptive nature of CNFs and the
15
all-nanofiber structure to ensure inter-pores connectivity for sustained water transport.
16
Besides these advantages, the bilayer CNF-CNT aerogel is also ultra-lightweight with low
17
materials packing density, as demonstrated by a piece of aerogel standing on top of a
18
dandelion, without bending or deforming the seed hair (Figure 1b), which can ensure its
19
portability and reduce the production cost. In essence, this bilayer aerogel design satisfies
20
all the critical design criteria required for high efficiency solar steam generation, including
21
high porosity of CNF aerogel for reducing heat loss, macrochannel structures for water
22
absorption and transport, all nanofibers design to promote water and vapor escape, CNT
23
coating for solar energy concentration, and seamless binding between the carboxylic groups
24
of CNF and CNT to ensure structural integrity.
5 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 24
1 2
Figure 1. (a) Graphical illustration of all-nanofiber CNF-CNT aerogel used for solar steam
3
generation. The solar steam generation device is composed of a bilayer structure of bulk
4
CNF aerogel with a thin CNT coating layer. (b) Photograph of bilayer CNF-CNT aerogel
5
standing on top of a dandelion, demonstrating lightweight performance.
6
To fabricate the bilayer aerogel structure, TEMPO oxidized CNF, with width of
7
approximately 3-5 nm and length of several hundred nm to 1 μm (Figure S1, Supporting
8
Information), was facilely assembled into 3D porous aerogel structure by freezing-induced
9
ice crystal templating (-20 °C) and subsequent freeze-drying (Figure 2a). Freezing CNF
10
aqueous suspension leads to the growth of ice crystals that segregate CNF to wrap around
11
the formed ice crystals, which act as porogens after sublimation, leaving a honeycomb like
12
structure with hexagonal pores at a scale of 200-300 μm wide at the cross-section of aerogel
13
(Figure 2b and S2, Supporting Information). The pores are elongated in the longitudinal
14
direction, suggesting preferentially vertical growth of the ice crystals along the longitudinal
15
direction, which can benefit the upward water transport (Figure 2c). To introduce the light
6 ACS Paragon Plus Environment
Page 7 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
absorbance layer, CNT dispersed in isopropanol at 2.5 mg/mL was deposited on the top of
2
the CNF aerogel under vacuum, which is applied to infiltrate the CNT inside the macropores,
3
covering the white CNF surface with a black CNT layer (Figure 2 d).
4 5
Figure 2. (a) Schematic illustration of the fabrication of CNF-CNT bilayer aerogel via ice-
6
templating, freeze-drying, and CNT coating; SEM images of CNF (b, c) and CNF-CNT (e, f, g)
7
aerogel: (b, e) top-view showing the large pores; (c, f) longitudinal view showing the
8
elongated channels structures; (d) photograph of the bilayer aerogel showing white CNF
9
aerogel with a black CNT coating layer; (g) high magnification SEM image showing fibrous
10 11
CNT network structure on top of the bilayer aerogel. The morphology of the as-fabricated CNF-CNT bilayer aerogel was closely examined by
12
SEM, which helps to reveal the bilayer structure as well as highlight the top CNT coating
13
layer. The top surface remained porous after CNT coating, but apparently smaller in pore
7 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 24
1
sizes and less in quantities as compared to the original CNF aerogel, suggesting some pores
2
were covered by CNTs (Figure 2e and S3, Supporting Information). Closer inspection of the
3
coated CNT layers showed randomly oriented CNTs overlaid with each other, forming
4
numerous nanopores that benefit water and vapor penetration (Figure 2g). The longitudinal
5
direction of the aerogel showed elongated macropores similar to the CNF aerogel, which is
6
expected since the CNT coating was only applied to the top surface (Figure 2f). The gradual
7
transition of the CNT coating inside the aerogel is disclosed by the high magnification SEM
8
images, showing isolated CNT deposited on the surface of pore walls at a half mm below the
9
top surface (Figure S4, Supporting Information) and essentially clean pore wall surfaces
10
without any signs of CNTs at the bottom of the aerogel (Figure S5, Supporting Information).
11
Individual CNFs are hardly discerned on the pore walls, due to the close associations
12
between these CNFs through inter-fibrils hydrogen bonding. However, numerous
13
mesopores of several tens of nm wide are present on the surface of the pore walls, which
14
can facilitate water transport between adjacent pores, critical for sustained water supply
15
during the solar steam generation.
16
Material characteristics including the density and porosity are two important factors that
17
potentially affect the portability and water transport of solar steam generation (Figure 3a).
18
Owing to the nanoscale dimensions and the prevalent polar groups at the surface, CNFs tend
19
to assemble into aerogel at extremely low concentration of 0.1 wt%, rendering ultralow
20
density.23 The density of CNF aerogel used in this study is 0.0078 g/cm3, which slightly
21
increased to 0.0098 g/cm3 after CNT coating, but is still extremely low to offer easy
22
portability. The areal density of CNT coating on the aerogel was estimated to be as low as
23
0.0015 g/cm2, resulting in cost effective solar steam generation device from reduced CNT
24
packing density. The porosity of the CNT-CNF bilayer aerogel is as high as 99.4%, which,
25
combined with the low density, offers the feasibility of this device to be floating at the air-
8 ACS Paragon Plus Environment
Page 9 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
water interface for solar steam generation (Figure S6, Supporting Information). Fourier
2
transform infrared spectroscopy (FTIR) spectra of CNF aerogel showed typical cellulose
3
structure with a broad peak located at 3000-3500 cm-1 assigned to OH groups, as well as a
4
peak at 1605 cm-1 due to the carboxylate groups introduced by TEMPO oxidation (Figure
5
3b), proving its hydrophilic nature for water absorption and transport. These functional
6
groups are still present after CNT coating, albeit with much lower intensities due to large
7
quantity of CNTs.
8 9
Figure 3. Characteristics and mechanical stability of CNF-CNT bilayer aerogel used for solar
10
steam generation. (a) Density and porosity of the CNF and CNF-CNT bilayer aerogel, both
11
showing extremely low density less than 0.01 g/cm3 and high porosity of over 99%; (b)
12
FTIR spectra of CNF and CNF-CNT bilayer aerogel showing the presence of polar groups
13
contributing to water absorption; (c) Compressive stress-strain curves of CNF-CNT bilayer
9 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
aerogel in both dry and wet state; (d) Cyclic compressive stress-strain curves of CNF-CNT
2
bilayer aerogel in water.
3
Page 10 of 24
The mechanical robustness of the CNF-CNT bilayer aerogel was investigated by
4
compressive stress-strain test under both dry and wet states (Figure 3c). The dry aerogel
5
demonstrated three stages of compressive behaviors of initial linear response before yield
6
point at 0.15 strain, plastic deformation with slower stress increment after the yield point,
7
and the last sharp densification stage up to 0.8 strain. This large strain deformation
8
indicates that the aerogel is very flexible and does not break apart under compression,
9
which further confirms its portability together with the low density. However, the dry
10
aerogel showed almost no shape recovery from the compression state, as demonstrated by
11
the fast drop of stress to 0 after releasing the compressive force. When wetted, the aerogel
12
became significantly weaker due to the plasticization effect of water, with the stress at 0.38
13
strain and Young’s modulus being reduced to 2.7 and 4.6 kPa from 25.7 and 141 kPa for the
14
dry aerogel, respectively. However, the wet aerogel demonstrated better shape recovery as
15
revealed by the small hysteresis between the compression and release curves
16
(Figure 3d). This wet resilience could be triggered by the interaction between water and
17
CNFs that breaks the inter-fibrils hydrogen bonding. Most importantly, the wet aerogel is
18
strong enough to withstand repetitive compression-recovery for up to 100 cycles without
19
breaking apart. This robustness, especially the long-term stability of CNF-CNT bilayer
20
aerogel under water warrants its application for solar steam generation.
21
The efficiency of solar steam generation depends highly on the efficiency of the device
22
surface in absorbing solar energy; therefore, materials with high light absorbance are more
23
desirable. The absorbance of both CNF and CNF-CNT aerogels in the range of 300-1200 nm
24
was recorded and presented in Figure 4a. CNF aerogel is white with both high
25
transmittance (21.7%) and reflectance (68.6%), leading to very low light absorbance of less
10 ACS Paragon Plus Environment
Page 11 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
than 10% across the UV-Vis-near-IR region. As CNF aerogel contains large several micron
2
wide pores and smooth pore walls, the incident light can be directed into the pores, with
3
some penetrating through the pore walls while others being reflected by the smooth
4
cellulose surface, leaving very small portions of incident light being absorbed by the aerogel.
5
After CNT coating, the top aerogel surface turned into black, showing almost zero
6
transmittance and 2.5% reflectance, and therefore very high absorbance of 97.5%. As
7
revealed from the SEM images, CNT coating introduces porous network structure on CNF
8
aerogel, thus effectively blocking the reflectance and elongate the light transport path into
9
the CNT network. Therefore, both transmittance and reflectance can be minimized to
10
ensure broadband light absorbance required by efficient solar steam generation.
11 12
Figure 4. Thermal properties of the CNF-CNT bilayer aerogel that benefit the solar energy
13
concentration and thermal management for efficient solar steam generation. (a). Light
11 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 24
1
absorbance spectra within the visible and near infrared region for both CNF and CNF-CNT
2
bilayer aerogels; insets are photographs of the respective top surface (upper-right, CNF
3
aerogel; lower-left, CNF-CNT bilayer aerogel); (b). Infrared photos showing the surface
4
temperature of the CNF-CNT bilayer aerogel under 1 kW m-2 over time; the aerogel was
5
circled for clarity; (c) Surface temperature increase as a function of irradiation time under
6
solar irradiation of 1 kW m-2; (d) The equilibrium maximum surface temperature under
7
varied solar irradiation of 1-10 kW m-2.
8
The heat localizing effect was investigated by measuring the surface temperature of
9
aerogel at the air-water interfaces using an infrared (IR) camera. Surface heating of the
10
CNF-CNT bilayer aerogel was visualized using IR camera (Figure 4b), which showed that the
11
surface temperature increased gradually over time, and the absorbed solar energy is
12
confined on the surface of aerogel without dissipating to the surrounding water body (dark
13
blue area in the IR pictures). Under 1 kW m-2, the surface temperature of CNF-CNT bilayer
14
aerogel sharply increased from 20 to 29.6 °C within 300 s, and then gradually increased and
15
stabilized at 32.7 °C (Figure 4c). In contrast, the surface temperature of CNF aerogel only
16
slightly increased from 20 to 23.6 °C over the same irradiation period, indicating better heat
17
concentrating effect with this bilayer structure. The equilibrium surface temperature after
18
1800 s irradiation under varied solar energy intensity for both CNF and CNT-CNT aerogel
19
was recorded (Figure 4d). With solar irradiation of 1, 3, 5, 7 and 10 kW m-2, the equilibrium
20
surface temperature increased almost linearly from 32.7, 43.7, 57.4, 72.3 to 95.3 °C, all
21
significantly higher than the respective 23.6, 28.2, 31.1, 34.2, and 37.9 °C for that of CNF
22
aerogel, highlighting the more effective solar concentrating effects of the coated CNT layer.
23
Due to the highly porous aerogel structure, the aerogel presents low thermal conductivity of
24
0.06 W/mK, which is critical for thermal management, to reduce the thermal loss into the
25
water body by confining the heating zone on the top air-water interface layer.
12 ACS Paragon Plus Environment
Page 13 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
All previous morphological, chemical, structural and thermal characterizations suggest
2
that the CNF-CNT bilayer aerogel meets all the desired criteria for solar steam generation,
3
including solar-absorption and heat localization, as well as water absorption and transport.
4
In order to investigate the solar steam generation performance, the CNF-CNT bilayer
5
aerogel saturated in water was irradiated with a solar simulator under varied irradiation
6
intensities. No clear steam column could be observed under 1 kW m-2, possibly due to the
7
relative lower surface temperature that is insufficient to generate enough steam to form a
8
continuous escaping column (Figure 5a). A small steam column starts to appear at 3 kW m-
9
2,
and continues to expand as the gradual increase in the solar irradiation, suggesting the
10
evaporation was significantly enhanced at higher solar irradiation energy. The evaporation
11
rates under varied solar irradiation were recorded over irradiation time (Figure 5b).
12
Similar to the surface temperature increase curve, the evaporation rates under all
13
irradiation conditions increased rapidly over the first few minutes, corresponding to the
14
temperature increase at the early stage of irradiation. The evaporation rates reached a
15
nearly constant value once the temperature stabilized, indicating that equilibrium was
16
established between the evaporation and upwards water transport by the highly absorptive
17
aerogel.
18
As expected, the evaporation rate increased almost linearly with increasing solar
19
radiation energy, showing respective values of 1.11, 3.52, 5.89, 8.06, and 11.37 kg m-2 h-1
20
under 1, 3, 5, 7, and 10 kW m-2 (Figure 5c), significantly higher than the respective
21
evaporation rates of 0.71, 1.2, 1.83, 2.33, and 2.70 kg m-2 h-1 for CNF aerogel. The
22
enhancement factor between the evaporation rates of CNF-CNT bilayer aerogel and CNF
23
aerogel were determined as 1.6, 2.9, 3.2, 3.4 and 4.2 under 1, 3, 5, 7, and 10 kW m-2 (Figure
24
S7, Supporting Information). The mass change due to water evaporation under varied
25
experimental conditions (i.e., pure water with and without solar irradiation, as well as CNF
13 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 24
1
aerogel and CNF-CNT aerogel under 1 kW m-2) was recorded in Figure 5d. It shows that
2
without solar irradiation, the water evaporates very slowly at 0.05 kg m-2 h-1 into the
3
environment, which has been subtracted from all evaporate rate calculation throughout the
4
experiments. Under 1 kW m-2, water can absorb solar irradiation energy that heats the
5
entire water body, leading to an increased evaporation rate of 0.24 kg m-2 h-1 (Figure 5e).
6
With the presence of pure CNF aerogel, the water evaporation rate further increases to 0.61
7
kg m-2 h-1, possibly due to the better thermal insulation effect of CNF aerogel that could
8
reduce the parasitic thermal loss to the bulk water body. Coating of CNT solar absorption
9
layer further enhanced the solar evaporation rate to 1.11 kg m-2 h-1 by taking advantage of
10
better thermal localization and management capabilities using this bilayer structure. The
11
solar steam generation efficiency η of the bilayer CNF-CNT bilayer aerogel can be calculated
12
using the following equation:
13 14
(1) where ṁ (kg m-2 h-1) denotes the evaporation rate, hLV is the total enthalpy of the liquid–
15
vapor phase transition including the sensible heat, Copt is the optical concentration and P0
16
represents the nominal solar irradiation value of 1 kW m-2. The efficiencies of solar steam
17
generation under 1 sun irradiation are calculated as 16.4, 57.8, and 76.3% for water only,
18
with CNF and CNF-CNT aerogels, respectively (Figure 5e). The efficiency slightly increased
19
with increased solar energy from 1 to 3 kW m-2, to 81.4% and then kept constant with
20
further increasing the solar energy to up to 10 kW m-2 (Figure 5f). Although high efficiency
21
(81.4% at 3 kW m-2) and evaporation rate (11.37 kg m-2 h-1 at 10 kW m-2) can be achieved at
22
higher solar irradiation, the strong solar irradiation can be difficult to achieve in normal
23
environment. It is therefore more meaningful to compare the performance at 1 kW m-2. The
24
76.3% efficiency at 1 kW m-2 is significantly higher than most of the reported solar steam
25
generation devices, including bilayer wood (57.3%),51 plasmonic gold-deposited
14 ACS Paragon Plus Environment
Page 15 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
nanoporous template (65%),7 double-layer structured carbon foam with exfoliated graphite
2
layer (70%),52 and flame treated wood (72%).10 This indicates that the bilayer CNF-CNT
3
aerogel can serve as efficient solar steam generation device under 1 sun irradiation.
4
Stability tests showed that this CNF-CNT bilayer aerogel can function stably under 1 kW m-2
5
for up to 50 cycles, with almost constant evaporation rate ranging from 1.09-1.11 kg m-2 h-1
6
(Figure 5g).
7 8
Figure 5. Solar steam generation performance of the CNF-CNT bilayer aerogel. (a)
9
Photographs of steam generated under varied solar irradiation energy of 1, 3, 5, 7, and 10
10
kW m-2 (1-10 suns); (b) The dynamics of solar steam generation under different solar
11
irradiation; (c) The performance of solar steam generation by CNF and CNF-CNT bilayer
12
aerogels under different solar irradiation, as expressed by the equilibrium water
13
evaporation rate (E.R.); (d) Cumulative mass change due to water evaporation over time for
15 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 24
1
water in dark field and under 1 kW m-2, as well as CNF and CNF-CNT aerogel under 1 kW m-
2
2;
3
water alone and with CNF, CNF-CNT bilayer aerogels; (f) The solar steam generation
4
efficiency of CNF-CNT aerogel under varied solar irradiation; (g) Stability of solar steam
5
generation under 1 sun irradiation for 50 cycles.
(e) Comparison of equilibrium evaporation rate and solar steam generation efficiency of
6
CONCLUSIONS
7
A bilayer ultra-lightweight (density of 0.0098 g/cm3) and porous (porosity of 99.4%)
8
aerogel structure was successfully assembled from CNFs and CNTs, which has been
9
demonstrated as an efficient solar steam generation device. The aerogel was fabricated
10
through systematic design strategies that satisfies the criteria for solar steam generation,
11
including hydrophilic CNFs for water absorption, a highly porous aerogel structure for
12
water transport, an all-nanofiber network structure for water supply and vapor escape, low
13
thermal conductivity for heat localization to prevent parasitic thermal loss to the bulk water
14
body, a surface coating of black CNTs to absorb 97.5% incident light from 300-1200 nm for
15
heat concentration, and structure flexibility and good mechanical performance for long-
16
term under water durability. Owing to these structure and performance advantages, the
17
bilayer aerogel demonstrated a high solar thermal conversion efficiency of 81.4% at 3 kW
18
m-2 solar irradiation, as well as a high evaporation rate of 11.37 kg m-2 h-1 at 10 kW m-2.
19
Besides, cyclic tests suggest that the bilayer aerogel can be reused for over 50 cycles
20
without losing its steam generation performance. This high-performance bilayer solar
21
steam generation device offers a new designing strategy that utilizes nature-based material
22
as the primary building blocks, which ensures a sustainable way for the generation of fresh
23
water by means of desalination and purification.
24 25
16 ACS Paragon Plus Environment
Page 17 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1 2 3
EXPERIMENTAL SECTION
4
Synthesis of CNF-CNT bilayer aerogel
5
TEMPO ((2,2,6,6-tetramethylpiperidin-1-yl)oxyl) oxidized (5 mmol NaClO loading per g of
6
cellulose) softwood CNFs was used for the CNF aerogel assembly. A portion of 10 mL CNF
7
aqueous suspension (0.7 wt%) was frozen in a 10-mL small beaker at -20 °C for 6 h. The
8
beaker was wrapped with an insulation foam layer to ensure unidirectional freezing from
9
the bottom of the beaker. The frozen CNF suspension was immediately transferred to the
10
chamber of a freeze-drier (FreeZone 1.0 L Benchtop Freeze Dry System, Labconco, Kansas
11
City, MO) to sublimate the ice (-50 °C, 20 Pa, 48 h), resulting white porous CNF aerogel. The
12
aerogel was cut to 5 mm in thickness thick, and 2 mL of CNT in isopropanol suspension (2.5
13
mg/mL) was deposited on top of the CNF aerogel repeatedly to ensure complete coverage,
14
and then dried under vacuum.
15
Characterization
16
The morphology of both CNF and CNF-CNT aerogels were characterized by scanning
17
electron microscopy (SEM, Hitachi SU-70). The density of the aerogel (ρa) was calculated
18
based on the ratio of weight (wa) and volume (va) using the equation:
19 20 21
=
(2)
The porosity was calculated from the equation:
P= 1- × 100%
(3)
22
where ρf indicates the density of nanofibers taken as 1.6 g/cm3.
23
FTIR-ATR spectrum was carried out using a Thermo Nicolet NEXUS 670 FTIR-ATR.
24
Mechanical properties of the aerogel in air and water were determined using with fixed
17 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 24
1
strain rate of 1 mm/min using RSA III dynamic mechanical analyzer (TA instrument). For
2
testing in water, the CNF-CNT aerogel was completely immersed in deionized water during
3
the measurement. The light absorbance measurement of the aerogels was carried out on a
4
UV-Vis Spectrometer Lambda 35 from 300-1200 nm (PerkinElmer, USA.) with an integrated
5
sphere for reflected light collection.
6
Thermal conductivity measurement
7
The thermal conductivity of the CNF-CNT aerogel was measured using Netzsch laser flash
8
apparatus (LFA 457), a non-contact transient method to measure thermal diffusivity of
9
materials. During the measurement, an instantaneous laser pulse is used to heat up one side
10
of the aerogel, and the response of temperature on the other side is recorded by a detector.
11
The thermal conductivity (W/mK) of the samples can then be calculated by the following
12
equation, k = αρC
13
(4)
14
where α (mm2/s) is the measured thermal diffusivity along a particular direction, Cp (J/g
15
K) is the heat capacity, and ρ (g/cm3) is the density. The heat capacity, Cp, is measured with
16
scanning calorimetry (DSC 204 F1 Phoenix). However, the aerogel in this work is highly
17
porous, the laser may penetrate the sample directly rather than generate heat at the surface.
18
Thus, a sandwich structure was designed by covering the CNF-CNT aerogel with highly
19
conductive carbon tape on both sides to block the laser penetration. The influence of carbon
20
tape is evaluated and eliminated by measuring the sample with different thicknesses.
21
Solar steam generation
22
The solar steam generation was tested using an optical measurement system comprising
23
of a multi-functional solar simulator (Newport Oriel 69907) and optical components
24
(Newport Oriel 67005). CNF-CNT aerogel was placed in petri dishes filled with water as the
25
solar steam generation setup. The weight loss during solar steam generation (at ambient
18 ACS Paragon Plus Environment
Page 19 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
conditions) under different irradiation intensities (1-10 kW m-2) was measured using a
2
properly calibrated electronic balance (Citizen CX301, accuracy: 0.1 mg). The infrared (IR)
3
picture and surface temperature increment were recorded using an IR camera.
4
ASSOCIATED CONTENT
5
Supporting Information
6
TEM image of CNF; SEM image of the cross-section of CNF and CNF-CNT aerogel; Cross
7
section SEM image of the CNF-CNT aerogel at 0.5 mm below the top CNT coating layer and at
8
the bottom; Photograph of the CNT-CNT aerogel floating on the air-water interface; The
9
enhancement factor (E.F.) of solar steam generation by CNF-CNT bilayer aerogel as compared to
10
the pure CNF aerogel. The Supporting Information is available free of charge on the ACS
11
Publications website.
12
ACKNOWLEDGEMENTS
13
This work is supported by National Natural Science Foundation of China (Grant No.
14
51528202).
15
AUTHOR CONTRIBUTION
16
F.J. and H.L. contributed equally to this work. F.J, L.H, and L.C conceived and designed the
17
experiment. F.J, H.L, Y.L, and X.X conducted the experiments. Y.K contributed in graphitic
18
illustration. C.C and H.H contributed in mechanical testing. C. J contributed in light
19
absorbance analysis. X.Z and R.Y contributed in thermal insulation measurement. E.H
20
contributed in the writing of the paper. F.J, L.H and L.C wrote the paper. Y.Z performed TEM
21
analysis. All authors commented on the paper.
22
REFERENCES
23 24
1. 801.
25
2.
Lewis, N. S., Toward cost-effective solar energy use. Science 2007, 315 (5813), 798Gratzel, M., Photoelectrochemical cells. Nature 2001, 414 (6861), 338-344.
19 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 24
1 2
3. Tritt, T. M.; Boettner, H.; Chen, L., Thermoelectrics: Direct solar thermal energy conversion. MRS Bulletin 2008, 33 (4), 366-368.
3 4 5 6
4. Kraemer, D.; Poudel, B.; Feng, H. P.; Caylor, J. C.; Yu, B.; Yan, X.; Ma, Y.; Wang, X. W.; Wang, D. Z.; Muto, A.; McEnaney, K.; Chiesa, M.; Ren, Z. F.; Chen, G., High-performance flatpanel solar thermoelectric generators with high thermal concentration. Nature Materials 2011, 10 (7), 532-538.
7 8
5. Linic, S.; Christopher, P.; Ingram, D. B., Plasmonic-metal nanostructures for efficient conversion of solar to chemical energy. Nature Materials 2011, 10 (12), 911-921.
9 10
6. Walter, M. G.; Warren, E. L.; McKone, J. R.; Boettcher, S. W.; Mi, Q. X.; Santori, E. A.; Lewis, N. S., solar water splitting cells. Chemical Reviews 2010, 110 (11), 6446-6473.
11 12 13
7. Zhou, L.; Tan, Y. L.; Ji, D. X.; Zhu, B.; Zhang, P.; Xu, J.; Gan, Q. Q.; Yu, Z. F.; Zhu, J., Selfassembly of highly efficient, broadband plasmonic absorbers for solar steam generation. Science Advances 2016, 2 (4), e1501227.
14 15 16
8. Li, Y.; Gao, T.; Yang, Z.; Chen, C.; Luo, W.; Song, J.; Hitz, E.; Jia, C.; Zhou, Y.; Liu, B.; Hu, L., 3D-printed, all-in-one evaporator for high-efficiency solar steam generation under 1 sun illumination. Advanced Materials 2017, 29, 1700981.
17 18 19
9. Liu, K. K.; Jiang, Q.; Tadepallifit, S.; Raliya, R.; Biswas, P.; Naik, R. R.; Singamaneni, S., Wood graphene oxide composite for highly efficient solar steam generation and desalination. ACS Applied Materials & Interfaces 2017, 9 (8), 7675-7681.
20 21 22
10. Xue, G. B.; Liu, K.; Chen, Q.; Yang, P. H.; Li, J.; Ding, T. P.; Duan, J. J.; Qi, B.; Zhou, J., Robust and low-cost flame-treated wood for high-performance solar steam generation. ACS Applied Materials & Interfaces 2017, 9 (17), 15052-15057.
23 24
11. Xu, N.; Hu, X.; Xu, W.; Li, X.; Zhou, L.; Zhu, S.; Zhu, J., Mushrooms as efficient solar steam-generation devices. Advanced Materials 2017, 29, 1606762.
25 26
12. Zhang, P.; Li, J.; Lv, L.; Zhao, Y.; Qu, L., Vertically aligned graphene sheets membrane for highly efficient solar thermal generation of clean water. ACS Nano 2017, 11, 5087-5093.
27 28 29
13. Yang, J.; Pang, Y.; Huang, W.; Shaw, S. K.; Schiffbauer, J.; Pillers, M. A.; Mu, X.; Luo, S.; Zhang, T.; Huang, Y.; Li, G.; Ptasinska, S.; Lieberman, M.; Luo, T., Functionalized graphene enables highly efficient solar thermal steam generation. ACS Nano 2017, 11(6), 5510-5518.
30 31 32
14. Jiang, Q. S.; Tian, L. M.; Liu, K. K.; Tadepalli, S.; Raliya, R.; Biswas, P.; Naik, R. R.; Singamaneni, S., Bilayered biofoam for highly efficient solar steam generation. Advanced Materials 2016, 28 (42), 9400-9407.
33 34
15. Li, R. Y.; Zhang, L. B.; Shi, L.; Wang, P., MXene Ti3C2: An effective 2D light-to-heat conversion material. ACS Nano 2017, 11 (4), 3752-3759.
35 36 37 38
16. Liu, Z.; Song, H.; Ji, D.; Li, C.; Cheney, A.; Liu, H.; Zhang, N.; Zeng, X.; Chen, B.; Goa, J.; Li, Y.; Liu, X.; Aga, D.; Jiang, S.; Yu, Z.; Gan, Q., Extremely cost-effective and efficient solar vapor generation under nonconcentrated illumination using thermally isolated black paper. Global Challenges 2017, 1, 1600003.
20 ACS Paragon Plus Environment
Page 21 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1 2 3
17. Zhou, L.; Tan, Y. L.; Wang, J. Y.; Xu, W. C.; Yuan, Y.; Cai, W. S.; Zhu, S. N.; Zhu, J., 3D selfassembly of aluminium nanoparticles for plasmon-enhanced solar desalination. Nature Photonics 2016, 10 (6), 393-398.
4 5 6 7
18. Li, X. Q.; Xu, W. C.; Tang, M. Y.; Zhou, L.; Zhu, B.; Zhu, S. N.; Zhu, J., Graphene oxidebased efficient and scalable solar desalination under one sun with a confined 2D water path. Proceedings of the National Academy of Sciences of the United States of America 2016, 113 (49), 13953-13958.
8 9 10
19. Bae, K.; Kang, G.; Cho, S. K.; Park, W.; Kim, K.; Padilla, W. J., Flexible thin-film black gold membranes with ultrabroadband plasmonic nanofocusing for efficient solar vapour generation. Nature Communications 2015, 6, 10103.
11 12 13
20. Liu, Y. M.; Yu, S. T.; Feng, R.; Bernard, A.; Liu, Y.; Zhang, Y.; Duan, H. Z.; Shang, W.; Tao, P.; Song, C. Y.; Deng, T., A bioinspired, reusable, paper-based system for high-performance large-scale evaporation. Advanced Materials 2015, 27 (17), 2768-2774.
14 15 16 17 18
21. Neumann, O.; Feronti, C.; Neumann, A. D.; Dong, A. J.; Schell, K.; Lu, B.; Kim, E.; Quinn, M.; Thompson, S.; Grady, N.; Nordlander, P.; Oden, M.; Halas, N. J., Compact solar autoclave based on steam generation using broadband light-harvesting nanoparticles. Proceedings of the National Academy of Sciences of the United States of America 2013, 110 (29), 1167711681.
19 20 21
22. Ito, Y.; Tanabe, Y.; Han, J. H.; Fujita, T.; Tanigaki, K.; Chen, M. W., Multifunctional porous graphene for high-efficiency steam generation by heat localization. Advanced Materials 2015, 27 (29), 4302-4307.
22 23
23. Jiang, F.; Hsieh, Y. L., Amphiphilic superabsorbent cellulose nanofibril aerogels. Journal of Materials Chemistry A 2014, 2 (18), 6337-6342.
24 25
24. Sun, H.; Xu, Z.; Gao, C., Multifunctional, ultra-flyweight, synergistically assembled carbon aerogels. Advanced Materials 2013, 25 (18), 2554-2560.
26 27 28
25. Hu, X. Z.; Xu, W. C.; Zhou, L.; Tan, Y. L.; Wang, Y.; Zhu, S. N.; Zhu, J., Tailoring graphene oxide-based aerogels for efficient solar steam generation under one sun. Advanced Materials 2017, 29 (5), 1604031.
29 30 31
26. Zhu, J. Y.; Sabo, R.; Luo, X. L., Integrated production of nano-fibrillated cellulose and cellulosic biofuel (ethanol) by enzymatic fractionation of wood fibers. Green Chemistry 2011, 13 (5), 1339-1344.
32 33 34
27. Zhu, H. L.; Luo, W.; Ciesielski, P. N.; Fang, Z. Q.; Zhu, J. Y.; Henriksson, G.; Himmel, M. E.; Hu, L. B., Wood-derived materials for green electronics, biological devices, and energy applications. Chemical Reviews 2016, 116 (16), 9305-9374.
35 36
28. Habibi, Y.; Lucia, L. A.; Rojas, O. J., Cellulose nanocrystals: chemistry, self-assembly, and applications. Chemical Reviews 2010, 110 (6), 3479-3500.
37 38 39
29. Qin, Y. L.; Qiu, X. Q.; Zhu, J. Y., Understanding longitudinal wood fiber ultra-structure for producing cellulose nanofibrils using disk milling with diluted acid prehydrolysis. Scientific Reports 2016, 6, 35602.
21 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 24
1 2
30. Jiang, F.; Hsieh, Y.-L., Chemically and mechanically isolated nanocellulose and their self-assembled structures. Carbohydrate Polymers 2013, 95 (1), 32-40.
3 4 5
31. Moon, R. J.; Martini, A.; Nairn, J.; Simonsen, J.; Youngblood, J., Cellulose nanomaterials review: structure, properties and nanocomposites. Chemical Society Reviews 2011, 40 (7), 3941-3994.
6 7
32. Bella, F.; Pugliese, D.; Zolin, L.; Gerbaldi, C., Paper-based quasi-solid dye-sensitized solar cells. Electrochimica Acta 2017, 237, 87-93.
8 9 10
33. Bella, F.; Galliano, S.; Falco, M.; Viscardi, G.; Barolo, C.; Gratzel, M.; Gerbaldi, C., Approaching truly sustainable solar cells by the use of water and cellulose derivatives. Green Chemistry 2017, 19 (4), 1043-1051.
11 12 13
34. Bella, F.; Chiappone, A.; Nair, J. R.; Meligrana, G.; Gerbaldi, C., Effect of different green cellulosic matrices on the performance of polymeric dye-sensitized solar cells. 10th Esee: European Symposium on Electrochemical Engineering 2014, 41, 211-216.
14 15 16
35. Jia, C.; Li, T.; Chen, C.; Dai, J.; Kierzewski, I. M.; Song, J.; Li, Y.; Yang, C.; Wang, C.; Hu, L., Scalable, anisotropic transparent paper directly from wood for light management in solar cells. 2017, 36, 366-373.
17 18 19 20
36. Fang, Z. Q.; Zhu, H. L.; Yuan, Y. B.; Ha, D.; Zhu, S. Z.; Preston, C.; Chen, Q. X.; Li, Y. Y.; Han, X. G.; Lee, S.; Chen, G.; Li, T.; Munday, J.; Huang, J. S.; Hu, L. B., Novel nanostructured paper with ultrahigh transparency and ultrahigh haze for solar cells. Nano Letters 2014, 14 (2), 765-773.
21 22 23 24
37. Zolin, L.; Nair, J. R.; Beneventi, D.; Bella, F.; Destro, M.; Jagdale, P.; Cannavaro, I.; Tagliaferro, A.; Chaussy, D.; Geobaldo, F.; Gerbaldi, C., A simple route toward next-gen green energy storage concept by nanofibres-based self-supporting electrodes and a solid polymeric design. Carbon 2016, 107, 811-822.
25 26 27
38. Jiang, F.; Hsieh, Y.-L., Super water absorbing and shape memory nanocellulose aerogels from TEMPO-oxidized cellulose nanofibrils via cyclic freezing-thawing. Journal of Materials Chemistry A 2014, 2 (2), 350-359.
28 29 30
39. Wicklein, B.; Kocjan, A.; Salazar-Alvarez, G.; Carosio, F.; Camino, G.; Antonietti, M.; Bergstrom, L., Thermally insulating and fire-retardant lightweight anisotropic foams based on nanocellulose and graphene oxide. Nature Nanotechnology 2015, 10 (3), 277-283.
31 32 33
40. Yang, X.; Shi, K. Y.; Zhitomirsky, I.; Cranston, E. D., Cellulose nanocrystal aerogels as universal 3D lightweight substrates for supercapacitor materials. Advanced Materials 2015, 27 (40), 6104-6109.
34 35 36
41. Zhu, H.; Yang, X.; Cranston, E. D.; Zhu, S. P., Flexible and porous nanocellulose aerogels with high loadings of metal-organic-framework particles for separations applications. Advanced Materials 2016, 28 (35), 7652-7657.
37 38
42. De France, K. J.; Hoare, T.; Cranston, E. D., Reviews of hydrogels and aerogels containing nanocellulose. Chemistry of Materials 2017, 29(11), 4609-4631.
22 ACS Paragon Plus Environment
Page 23 of 24 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1 2 3
43. Sakai, K.; Kobayashi, Y.; Saito, T.; Isogai, A., Partitioned airs at microscale and nanoscale: thermal diffusivity in ultrahigh porosity solids of nanocellulose. Scientific Reports 2016, 6, 20434.
4 5 6 7
44. Mizuno, K.; Ishii, J.; Kishida, H.; Hayamizu, Y.; Yasuda, S.; Futaba, D. N.; Yumura, M.; Hata, K., A black body absorber from vertically aligned single-walled carbon nanotubes. Proceedings of the National Academy of Sciences of the United States of America 2009, 106 (15), 6044-6047.
8 9 10 11
45. Panagiotopoulos, N. T.; Diamanti, E. K.; Koutsokeras, L. E.; Baikousi, M.; Kordatos, E.; Matikas, T. E.; Gournis, D.; Patsalas, P., Nanocomposite catalysts producing durable, superblack carbon nanotube systems: applications in solar thermal harvesting. ACS Nano 2012, 6 (12), 10475-10485.
12 13 14
46. Lin, Z. Q.; Zeng, Z. P.; Gui, X. C.; Tang, Z. K.; Zou, M. C.; Cao, A. Y., Carbon nanotube sponges, aerogels, and hierarchical composites: synthesis, properties, and energy applications. Advanced Energy Materials 2016, 6 (17), 1600554.
15 16 17 18
47. Chen, Y.; Zhang, H. B.; Yang, Y. B.; Wang, M.; Cao, A. Y.; Yu, Z. Z., High-performance epoxy nanocomposites reinforced with three-dimensional carbon nanotube sponge for electromagnetic interference shielding. Advanced Functional Materials 2016, 26 (3), 447455.
19 20 21
48. Xue, Y. H.; Yang, Y. B.; Sun, H.; Li, X. Y.; Wu, S. T.; Cao, A. Y.; Duan, H. L., A switchable and compressible carbon nanotube sponge electrocapillary imbiber. Advanced Materials 2015, 27 (44), 7241-7246.
22 23 24
49. Peng, Q. Y.; Li, Y. B.; He, X. D.; Gui, X. C.; Shang, Y. Y.; Wang, C. H.; Wang, C.; Zhao, W. Q.; Du, S. Y.; Shi, E. Z.; Li, P. X.; Wu, D. H.; Cao, A. Y., Graphene nanoribbon aerogels unzipped from carbon nanotube sponges. Advanced Materials 2014, 26 (20), 3241-3247.
25 26 27
50. Zhu, J.; Shim, B. S.; Di Prima, M.; Kotov, N. A., Transparent Conductors from Carbon nanotubes LBL-assembled with polymer dopant with pi-pi electron transfer. Journal of the American Chemical Society 2011, 133 (19), 7450-7460.
28 29 30
51. Zhu, M.; Li, Y.; Chen, G.; Jiang, F.; Yang, Z.; Luo, X.; Wang, Y.; Lacey, S. D.; Dai, J.; Wang, C.; Jia, C.; Wan, J.; Yao, Y.; Gong, A.; Yang, B.; Yu, Z.; Das, S.; Hu, L., Tree-inspired design for high-efficiency water extraction. advanced materials 2017, 29, 1704107.
31 32
52. Ghasemi, H.; Ni, G.; Marconnet, A. M.; Loomis, J.; Yerci, S.; Miljkovic, N.; Chen, G., Solar steam generation by heat localization. Nature Communications 2014, 5, 4449.
33 34 35 36 37 38
23 ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Page 24 of 24
TOC Figure 2 3 4 5 6
24 ACS Paragon Plus Environment