Subscriber access provided by University of Rochester | River Campus & Miner Libraries
Article
Mechanism of Vanadium Leaching During Surface Weathering of Basic Oxygen Furnace Steel Slag Blocks: A µXANES and SEM Study Andrew James Hobson, Douglas I. Stewart, Andrew William Bray, Robert J.G. Mortimer, William Matthew Mayes, Michael Rogerson, and Ian T. Burke Environ. Sci. Technol., Just Accepted Manuscript • DOI: 10.1021/acs.est.7b00874 • Publication Date (Web): 19 Jun 2017 Downloaded from http://pubs.acs.org on June 21, 2017
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Environmental Science & Technology is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 26
Environmental Science & Technology
1
Mechanism of Vanadium Leaching During Surface Weathering of
2
Basic Oxygen Furnace Steel Slag Blocks: A µXANES and SEM Study
3 4
Andrew J. Hobson1, Douglas I. Stewart2, Andrew W. Bray1, Robert J. G. Mortimer3, William M.
5
Mayes4, Michael Rogerson4 and Ian T. Burke1*
6 7
1
School of Earth and Environment, University of Leeds, Leeds, LS2 9JT, UK.
8
2
School of Civil Engineering, University of Leeds, Leeds, LS2 9JT, UK.
9
3
School of Animal, Rural and Environmental Sciences, Nottingham Trent University, Brackenhurst Campus,
10
Southwell, Nottinghamshire NG25 0QF, UK
11
4
12
*Email for correspondence:
[email protected], phone: +44 113 3437532, fax: +44 113 3435259.
School of Environmental Sciences, University of Hull, Hull, HU6 7RX, UK.
13 14 15 16 17
Prepared for: ES&T
18
Word Count: 4507 (+ 2100 in tables and figures)
19
ACS Paragon Plus Environment
Environmental Science & Technology
20
TOC artwork
21
22 23
ACS Paragon Plus Environment
Page 2 of 26
Page 3 of 26
Environmental Science & Technology
24
Abstract
25
Basic oxygen furnace (BOF) steelmaking slag is enriched in potentially toxic V which may become
26
mobilised in high pH leachate during weathering. BOF slag was weathered under aerated and air-
27
excluded conditions for 6 months prior to SEM/EDS and µXANES analysis to determine V host phases
28
and speciation in both primary and secondary phases. Leached blocks show development of an
29
altered region in which free lime and dicalcium silicate phases were absent and Ca-Si-H was
30
precipitated (CaCO3 was also present under aerated conditions). µXANES analyses show that V was
31
released to solution as V(V) during dicalcium silicate dissolution and some V was incorporated into
32
neo-formed Ca-Si-H. Higher V concentrations were observed in leachate under aerated conditions
33
than in the air-excluded leaching experiment.
34
Ca3(VO4)2 solubility which demonstrate an inverse relationship between Ca and V concentrations.
35
Under air-excluded conditions Ca concentrations were controlled by dicalcium silicate dissolution
36
and Ca-Si-H precipitation, leading to relatively high Ca and correspondingly low V concentrations.
37
Formation of CaCO3 under aerated conditions provided a sink for aqueous Ca, allowing higher V
38
concentrations limited by kinetic dissolution rates of dicalcium silicate. Thus V release may be
39
slowed by the precipitation of secondary phases in the altered region, improving the prospects for
40
slag reuse.
Aqueous V concentrations were controlled by
41
ACS Paragon Plus Environment
Environmental Science & Technology
42
Introduction
43
Basic oxygen furnace (BOF) steelmaking is a primary method of steelmaking which accounts
44
for ~2/3 of worldwide steel production [1, 2]. In a basic oxygen converter low carbon steel is
45
produced by blowing oxygen through molten pig iron and recycled scrap steel to remove carbon.
46
BOF slag is the primary by-product of BOF steelmaking and is produced when limestone (or
47
dolomite) is added to the molten iron as a fluxing agent to draw out impurities [3]. Due to the large
48
quantities of steel slag produced worldwide (170-250 million metric ton/year [4]) reuse has become
49
increasingly important in order to comply with environmental regulations limiting disposal of wastes.
50
Currently steel slag that cannot be recycled in blast furnaces is primarily reused as aggregate in road
51
surfacing and construction due to its high stability and skid resistance [5, 6], whilst other uses
52
include neutralisation of acidity in soils or mine wastes and possibly for CO2 sequestration [7-10].
53
Depending on its precise mineralogy, some steel slag may be unsuitable for reuse, particularly in
54
engineering applications. Steel slag may be enriched in phases such as free lime (CaO) and periclase
55
(MgO) which expand on hydration, resulting in significant volume change [11]. In situations where
56
slag cannot be reused, or where supply exceeds after-use demand, slag is generally disposed to
57
landfill [12].
58
Steel slag formed during primary steelmaking (i.e. from BOF or electric arc furnace (EAF)
59
processes) typically comprises a mixture of Ca oxides, Fe oxides and silicates. The precise chemical
60
composition varies by iron source and processing, however, the bulk chemical composition is
61
relatively consistent between locations worldwide (Table 1). Typically BOF slag is dominated by Ca,
62
Fe and Si, with minor amounts of Mg, Mn and Al [3, 13, 14]. The mineralogical composition can be
63
complex but typically contains a range of calcium-containing silicate phases (e.g. Larnite, β-Ca2SiO4;
64
Merwinite Ca3Mg(SiO4)2), calcium and aluminium ferrite phases (e.g. Brownmillerite, Ca2FeAlO5,
65
Srebrodolskite, Ca2Fe2O5), free Mg and Ca oxides (e.g. Lime, CaO; Periclase, MgO) and a refractory
66
oxide solid solution of Fe-Mg-Mn-Ca- oxides (e.g. Wüstite, FeO) [3, 11, 15-17].
ACS Paragon Plus Environment
Page 4 of 26
Page 5 of 26
67 68
Environmental Science & Technology
When stored in contact with water, CaO and Ca-silicates in BOF slag readily react with to generate a high pH leachate (typically pH 10 – 12.5), e.g. via equations 1 and 2 [18, 19]:
69
CaO + H2O → Ca2+ + 2OH-
(Eqn. 1)
70
Ca2SiO3 + H2O → 2Ca2+ + H2SiO42- + 2OH-
(Eqn. 2)
71
The release of Ca2+ and H2SiO42- to solution can lead to oversaturation with respect to
72
calcium silicate hydrates (Ca-Si-H; Eqn. 3), and secondary carbonates in the presence of atmospheric
73
CO2 (Eqn. 4; [18]). Spinels (e.g. Magnetite; Eqn. 5) and hydroxide phases can also form, where di-
74
and trivalent metal ions are released[20]. 3Ca2+ + 2H2SiO42- + 2OH- → 3CaO·2SiO2·3H2O
(Eqn. 3)
76
Ca2+ + CO2 + 2OH- → CaCO3 + H2O
(Eqn. 4)
77
Fe2+ + 2Fe3+ + 4H2O → Fe3O4 + 8H+
(Eqn. 5)
75
`
78
Steel slags usually contain a variety of trace elements from the primary ore that become
79
concentrated by processing. At high pH, several potential toxic metals are solubilised and become
80
mobile in leachate including Al, Fe, and V [18-21]. In recent years V leaching has received significant
81
attention due to its relative enrichment in BOF slag (0.04-1.48 wt%; [14, 21]) and the potential
82
mobility and toxicity of V(V) species in alkaline leachates. V is present in steel slag in multiple
83
oxidation states (V(III), V(IV) and V(V) [21, 22]), however, there is uncertainty about the exact host
84
phases and the V oxidation state within those phases, making evaluation of V leaching behaviour
85
difficult [23]. This uncertainty is compounded by the use of leaching data acquired from powdered
86
specimens, which may be unrepresentative of slag aggregate weathering in civil engineering
87
applications [8, 20]. As a result regulatory bodies, such as the UK Environment Agency, are adopting
88
worst case scenario assumptions when considering V leaching from steel slags [24]. This will have an
89
adverse effect on beneficial reuse of slag, and could lead to overly stringent long-term monitoring
90
requirements for landfills.
91
Previous research has shown that under air-excluded leaching conditions up to 1.7% of the V
92
in BOF slag was released to solution [20]. This is due to the relatively high reactivity of the V hosting
93
phase, and the prediction that V(III) and V(IV) can be oxidised to V(V) during slag weathering [17, 20,
ACS Paragon Plus Environment
Environmental Science & Technology
94
22]. No data are available concerning leaching of steel slags under aerated conditions that will be
95
more favourable to V oxidation. Equally, the role of secondary phase formation in controlling V
96
release is currently unknown, although the potential for aqueous V to be incorporated into Ca-Si-H
97
has been noted [20].
98
A thorough understanding of weathering processes in BOF slag is essential to enable long-
99
term, cost effective management and use of steel slag whilst protecting both the environment and
100
human health from its potentially hazardous components. This study used scanning electron
101
microscopy (SEM) and X-ray absorption near-edge spectroscopy (XANES) to determine the
102
distribution and speciation of V within BOF steel slag, and to determine whether leachate
103
equilibrium atmosphere affects V release during slag leaching. This research provides new insights
104
into the distribution of V within both unweathered and weathered BOF slag, and investigates the
105
mechanisms underpinning enhanced V leaching and its fate in neo-formed phases.
ACS Paragon Plus Environment
Page 6 of 26
Page 7 of 26
Environmental Science & Technology
106
Methods
107
Sample collection and characterisation
108
Basic oxygen furnace (BOF) steel slag was collected in May 2013, within one week of its
109
deposition, from British Steel’s Yarborough Landfill (Scunthorpe, UK; LAT 53°35′22.24″ LONG
110
0°35′41.52″). The sample consisted of 50-500g blocks (~100kg total). Sub-samples were either cut
111
into smaller 8g blocks (20x10x10mm) using a diamond saw for use in leaching experiments, or
112
ground to