Medium chain-length polyhydroxyalkanoate copolymer modified by bacterial cellulose for medical devices Denis Mihaela Panaitescu, Irina Lupescu, Adriana Nicoleta Frone, Ioana Chiulan, Cristian Andi Nicolae, Vlad Tofan, Amalia Stefaniu, Raluca Somoghi, and Roxana Trusca Biomacromolecules, Just Accepted Manuscript • DOI: 10.1021/acs.biomac.7b00855 • Publication Date (Web): 11 Sep 2017 Downloaded from http://pubs.acs.org on September 15, 2017
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
Biomacromolecules is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
Medium Chain-Length Polyhydroxyalkanoate
2
Copolymer Modified by Bacterial Cellulose for
3
Medical Devices
4
Denis Mihaela Panaitescu1*, Irina Lupescu2, Adriana Nicoleta Frone1, Ioana Chiulan1, Cristian
5
Andi Nicolae1, Vlad Tofan3, Amalia Stefaniu2, Raluca Somoghi1, Roxana Trusca4
6
1
7
Independentei, 060021, Bucharest, Romania
8
2
9
Romania
Polymer Department, National Institute for R&D in Chemistry and Petrochemistry, 202 Splaiul
National Institute for Chemical Pharmaceutical R&D, 112 Calea Vitan, 031299, Bucharest,
10
3
11
Independentei, 050096, Bucharest, Romania
12
4
13
Bucharest, 1-7 Gh. Polizu Street, 011061 Bucharest, Romania
14
KEYWORDS: poly(3-hydroxyoctanoate), thermal stability, aging, mechanical properties, tubing,
15
cytocompatibility
16
ABSTRACT
17
Medium chain-length PHAs (mPHAs) are flexible elastomeric biopolymers with valuable
18
properties for biomedical applications like artificial arteries and other medical implants.
Cantacuzino National Institute of R&D for Microbiology and Immunology, 103 Splaiul
Science and Engineering of Oxide Materials and Nanomaterials, University Politehnica of
1 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 2 of 38
1
However, an environmentally friendly and high productivity process together with the tuning of
2
the mechanical and biological properties of mPHAs are mandatory for this purpose. Here, for the
3
first time, a melt processing technique was applied for the preparation of bionanocomposites
4
starting from poly(3-hydroxyoctanoate) (PHO) and bacterial cellulose nanofibers (BC). The
5
incorporation of only 3 wt% BC in PHO improved its thermal stability with 25°C and reinforced
6
it, increasing the Young’s modulus with 76% and the tensile strength with 44%. The percolation
7
threshold calculated with the aspect ratio of the fibers after melt processing was very low and
8
close to 3 wt%. We showed that this bionanocomposite is able to preserve the ductile behavior
9
during storage, no important aging being noted between 3 h and one month after compression-
10
molding. Moreover, this study is the first to investigate the melt processability of PHO
11
nanocomposite for tube extrusion. In addition, biocompatibility study showed no pro-
12
inflammatory immune response and better cell adhesion for PHO/BC nanocomposite with 3 wt%
13
BC and demonstrated the high feasibility of this bionanocomposite for in vivo application of
14
tissue-engineered blood vessels.
15
INTRODUCTION
16
Polyhydroxyalkanoates (PHAs) have been extensively studied over the past years due to their
17
promising applications.1-4 Short-chain length PHAs (sPHAs) such as poly(3-hydroxybutyrate)
18
(PHB)
19
commercialized and tested for biomedical and packaging applications.2,4 However, sPHAs are
20
extremely brittle and show poor melt processing behavior.4 Unlike sPHAs, elastomeric medium
21
chain-length PHAs (mPHAs) are very promising for biomedical purposes due to their unique
22
properties.2,5
and
poly(3-hydroxybutyrate-co-3-hydroxyvalerate)
(PHBV)
have
been
already
2 ACS Paragon Plus Environment
Page 3 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
Poly(3-hydroxyoctanoate) (PHO) and its copolymers are from the most studied
2
mPHAs.5,6 Cytocompatibility tests demonstrated the attachment, differentiation, and maturation
3
of human keratinocytes cells on PHO (homopolymer) film obtained by solvent casting.6
4
However, some biomedical applications require a specific range of mechanical and biological
5
properties. For this purpose, PHO was modified by crosslinking or graft copolymerization or by
6
the addition of other biopolymers and micro/nanofillers.7-11 PHO grafted with vinylimidazole
7
showed higher hydrophilicity, biocompatibility and antimicrobial activity than the starting
8
polymer.7 The nanocomposite from PHO copolymer (7.6 mol% of 3-hydroxyhexanoate (3HH))
9
and 2.5 wt% organoclay showed a nanoindentation modulus five times higher than that of the
10
pure matrix.9 PHO - diethylene glycol hybrid copolymer showed improved hydrophilicity and
11
self-assembling ability forming microporous arrays.11
12
PHB/PHO blends with adjustable biodegradability were studied for biodegradable stents.5
13
These stents may be more advantageous than metal stents because they do not have to be
14
removed after fulfilling their function to support the injured artery. The mPHAs are flexible
15
elastomeric biopolymers with low crystallinity and glass transition temperature, moderate tensile
16
strength and high elongation to break, which recommend them for heart valves and
17
cardiovascular implants, skin and nerve tissue engineering.12,13 From aliphatic biopolyesters,
18
only poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), which is available in larger quantities,
19
has been studied for these purposes.5,13 Hence, PHAs are more hydrophobic than most of natural
20
biopolymers, such as collagen14 and the use of hydrophilic agents is necessary to overcome this
21
drawback and to enhance the biological properties of PHAs. It has been reported that both the
22
hydrophilicity and mechanical properties of PHAs were improved by the addition of small
23
amount of nanocellulose.15
3 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 38
1
PHO/nanocellulose composites have been scarcely studied.10,12 In the pioneering work of
2
Dubief et al. starch microcrystals from yellow pea and cellulose whiskers from tunicin were
3
tested in a PHO latex to increase its hydrophilicity and mechanical properties.10 Higher storage
4
modulus values were obtained in the case of PHO reinforced with high aspect ratio cellulose
5
whiskers from a percolation threshold as low as 1.5 wt %.10 On the other hand, Basnett et al.
6
were the first who addressed this issue in the perspective of medical applications.12 They
7
obtained bacterial cellulose microcrystals by the weak acid hydrolysis of bacterial cellulose and
8
modified their surface by acetylation. Composite films from PHO homopolymer and acetylated
9
microcrystals in high amount (5, 15, and 25%), prepared by solvent casting using chloroform,
10
showed enhanced in vitro degradability and increased cell growth and proliferation. However,
11
some deterioration of the elastic properties was observed due to the high concentration of
12
acetylated bacterial cellulose microcrystals in the films.12
13
Great advantage could be brought to PHO by the nanodimension of the cellulosic filler,
14
in agreement with the results obtained with cellulose whiskers from tunicates.10 Thus, the
15
amount of bacterial cellulose modifier in PHO can be greatly decreased to a few percent by
16
working with bacterial cellulose nanofibers instead of microfillers and the elastomeric properties
17
of the matrix may be, thus, maintained. Moreover, for successful scale-up of these PHO
18
nanocomposites to an industrially meaningful scale, free-solvent methods should be used. In the
19
present work, we applied for the first time a melt processing technique for the preparation of
20
PHO composites with bacterial cellulose nanofibers. Compared to the common method
21
consisting in the solvent casting using chloroform, melt processing is environmentally friendly,
22
cost effective and ensures high productivity, being a major step toward the fabrication of medical
23
devices like stents.
4 ACS Paragon Plus Environment
Page 5 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
The main aim of this study was to obtain PHO/bacterial cellulose nanocomposites with
2
enhanced mechanical properties and thermal stability, suitable for melting processing to obtain
3
medical devices. For this purpose, bacterial cellulose nanofibers in dry form, that will be denoted
4
from now on with BC for simplicity, were used in low amount (1.5 wt% and 3 wt%) in a PHO
5
copolymer to obtain nanocomposites by melt processing. BC were obtained by the mechanical
6
disintegration of bacterial cellulose pellicles; the size of BC and their dispersion in PHO were
7
assessed by transmission electron microscopy (TEM), scanning electron microscopy (SEM) and
8
by atomic force microscopy (AFM); calorimetric study was conducted to observe the effect of
9
the nanofiller on the crystallization of PHO and the mechanical properties were determined for
10
different aging times. Biocompatibility study was performed by assessing the pro-inflammatory
11
immune response triggered by PHO/BC nanocomposite in an in vitro macrophage cell line
12
model and by in vitro cytotoxicity tests through the analysis of L929 murine fibroblasts’
13
behavior on the surface of neat PHO and PHO/BC nanocomposites. By this study we propose a
14
green approach to obtain bionanocomposites for in vivo applications and we demonstrate that
15
PHO nanomaterials are able to preserve their ductile behavior during storage, a step forward
16
relative to PHB and other sPHAs. Moreover, this study is the first to investigate the melt
17
processability of PHO/BC nanocomposites for tube extrusion as an important step for the
18
manufacture of artificial arteries and other medical implants.
19
EXPERIMENTAL PART
20
Materials
21
The wild-type Gram-negative bacteria Pseudomonas putida ICCF 391, from the Collection of
22
Microorganisms of Industrial Interest of National Institute for Chemical-Pharmaceutical
23
Research & Development (Bucharest, Romania) was used in this study. The strains have an 5 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 38
1
optimum growth temperature range from 30°C to 34°C and were maintained in Cantacuzino
2
Agar tubes at 4°C and used for all culture experiments. Bacterial cellulose pellicles were
3
produced in static culture by the bacterial strain Gluconacetobacter Xylinus DSM 2004
4
purchased from Leibniz Institute DSMZ (German Collection of Microorganisms and Cell
5
Cultures) in the conditions mentioned in our previous work.16 All chemicals (of analytical grade)
6
were supplied by Sigma-Aldrich and used as received.
7
Biosynthesis of PHO copolymer
8
PHO
9
7.5:87.9:3.3) was produced by Pseudomonas putida using sodium octanoate as carbon source.
copolymer
(poly(3-hydroxyhexanoate-co-3-hydroxyoctanoate-co-3-hydroxydecanoate)
10
Further details about the biosynthesis of PHO are given in the Supporting Information.
11
Preparation of bacterial cellulose nanofibers in dry form
12
BC were obtained from fresh bacterial cellulose pellicles using a mechanical defibrillation
13
process as described before16 with the differences: the gel-like sample collected from the blender
14
was diluted to about 1% with distilled water and passed through a vertical colloid mill at about
15
2000 min-1 for 180 min. From time to time, cold water was added to prevent the raising of the
16
temperature above 40 ºC. The suspension containing BC was 5-fold concentrated in a rotavapor
17
(Heidolph Instruments, Germany) at 40 °C and then freeze dried (FreeZone 2.5 L - Labconco
18
USA) resulting powdered BC.
19
Preparation of PHO/BC nanocomposites. PHO pellicles prepared in the conditions mentioned
20
in the Supporting Information were introduced in the mixing chamber of a Brabender LabStation
21
(Germany) heated to 45 ºC and melted. The calculated amount of BC powder was slowly poured
22
into the melted polymer and, then, they were mixed for another 3 min at 40 min-1. The mixtures 6 ACS Paragon Plus Environment
Page 7 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
were shaped in foils on a laboratory two-roll mill (Polymix 110L, Germany) and compression
2
molded in an electrically heated press (P200E Dr. Collin, Germany) at 46-48°C, 120 s preheating
3
(5 bar), 30 s under pressure (50 bar) and cooling for another 120 s (5 bar) in a cooling cassette.
4
Sheets (0.8-1 mm in thickness) of nanocomposites with 1.5 and 3 wt% BC (PHO-1.5BC and
5
PHO-3BC) were thus obtained. A neat PHO reference was prepared in the same conditions.
6
Before characterization, PHO and nanocomposite plates were kept for 30 days at room
7
temperature.
8
Characterization techniques
9
Cryo-TEM analysis. The size and morphology of BC were investigated by TEM using a
10
Tecnai™ G2 F20 TWIN Cryo-TEM instrument (FEI, Hillsboro, USA) at 200 kV accelerating
11
voltage. The nanofibers were observed directly without any staining to improve contrast. A small
12
droplet of diluted BC suspension in water was poured on a holey carbon grid and left to dry in
13
vacuum at 25 °C. PHO-3BC nanocomposite sample was cut with a Leica EM FC7 cryo
14
ultramicrotome at a temperature of -30 °C which is close to its Tg value. Slices of 100 nm were
15
obtained at a cutting speed of 40 mm/s which were then carefully placed on holey carbon copper
16
grids. Temperature and cutting speed were optimized for this sample. The dispersion of BC in
17
the polymer matrix was then investigated using the Cryo-TEM instrument at an accelerating
18
voltage of 200 kV in bright field mode. Images were analyzed with Digital Micrograph software
19
(Gatan, USA) to obtain the width distribution of bacterial cellulose nanofibers.
20
Thermal characterization. Thermo-gravimetric analysis (TGA) was carried out on a TA-Q5000
21
V3.13 (TA Instruments Inc., USA) with nitrogen as the purge gas at a flow rate of 40 mL/min.
22
The thermograms were acquired between 25 °C and 700 °C at a heating rate of 10 °C/min. The
23
error on temperature determination was ±0.5 °C. Differential scanning calorimetry (DSC) was 7 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 38
1
performed with a DSC Q2000 from TA Instruments under a helium flow (100 mL/min). Samples
2
weighing around 7 mg were cooled to -10 ºC, heated to 80 ºC, held at that temperature for 3 min
3
to delete the thermal history, then cooled to -80 ºC, kept isothermal for 2 min and heated again to
4
80 oC at a constant heating/cooling rate of 10 oC/min. The melting temperature (Tm) was taken as
5
the peak temperature of the melting endotherm. Two parallel samples were tested for the
6
reference and for each PHO nanocomposite.
7
Mechanical properties. Tensile properties of PHO/BC nanocomposites were measured at room
8
temperature with a crosshead speed of 10 mm/min, using an Instron 3382 Universal Testing
9
Machine equipped with a cell load of 1 kN. Five specimens, 5A type according to ISO 527, were
10
tested for each sample and analyzed using the Bluehill 2 Software.
11
Attenuated Total Reflectance Fourier Transform Infrared (ATR-FTIR) spectroscopy. ATR-FTIR
12
spectra were recorded on a FTIR spectrometer TENSOR 37 from Bruker (USA). Data were
13
collected at room temperature from 4000 to 400 cm-1 with 16 scans.
14
AFM investigation. AFM was employed to study the surface properties of PHO before and after
15
BC addition. A MultiMode 8 from Bruker (USA) working in Peak Force (PF) Quantitative
16
Nanomechanical Mapping (QNM) mode was used for this purpose. Silicon probe from Bruker
17
with the following characteristics, stated by the specification - nominal tip radius of 8 nm,
18
cantilever length of 225 µm and resonant frequency of 75 kHz - was used for the measurements.
19
The tests were performed at room temperature, with a scan rate of 0.5 – 0.7 Hz. The images
20
(256x256 pixels per line) were analyzed with NanoScope 1.20 software.
21
SEM analysis. Surface morphology was assessed by scanning electron microscopy. A Quanta
22
Inspect F50 scanning electron microscope (FEI, Hillsboro, USA), equipped with a field emission
8 ACS Paragon Plus Environment
Page 9 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
gun, with a resolution of 1.2 nm and working at an accelerating voltage of 30 kV was used for
2
this purpose. The PHO and nanocomposite films were sputter-coated with gold before analysis.
3
Cell line culture and differentiation into macrophage-like cells. Human monocytic cell line THP-
4
1, purchased from Health Protection Agency Culture Collections, was cultured at 37 oC in a
5
humidified atmosphere and 5% CO2 in a RPMI-1640 medium (Sigma-Aldrich Corporation,
6
USA). This was supplemented with 10% fetal bovine serum (Biochrom AG, Germany), 1 mM L-
7
glutamine, 100 U/ml penicillin, 100 µg/ml streptomycin (Lonza, Belgium) and 5 mM 2-
8
mercaptoethanol (complete culture medium). THP-1 cells were seeded at 2x105cells/mL, 200
9
µL/well in a 96 -well flat bottom culture plate. They were treated with 30 ng/mL phorbol-12-
10
myristate-13 acetate for 72h, resulting in macrophage-like cells.
11
Evaluation of pro-inflammatory effect. Roughly equal amounts of each nanocomposite material
12
were sterilized by overnight incubation in 70% ethanol solution followed by washing steps with
13
sterile Phosphate Buffer Saline (PBS) to completely remove ethanol. Samples were incubated at
14
37 oC in PBS for 20 days to allow elution of their constituents. PBS alone, incubated in a similar
15
manner was used as a control. Following incubation, supernatants (elution samples) were
16
collected and tested for endotoxin activity with LAL QCL-1000 kit (Lonza, Belgium).
17
Differentiated macrophage-like cells were incubated in the presence of elution samples (diluted
18
1/10 in complete culture medium) for 24h. Cells incubated with lipopolysaccharide (LPS 100
19
ng/mL) or without stimuli were used as positive and negative controls. Supernatants were
20
collected and stored at -80 oC until use. The influence of elution samples on differentiated
21
macrophages was evaluated by measuring Tumor Necrosis Factor-α (TNF-α) and Interleukin-6
22
(IL-6) concentrations in culture supernatants using ELISA (DuoSet kits from R&D Systems Inc.,
23
USA). 9 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 38
1
Evalutation of cytocompatibility. Cytotoxic effect of neat PHO, PHO-1.5BC and PHO-3BC on
2
L929 cell line was evaluated using round disc-shaped samples, 10 mm in diameter. The samples
3
were sterilized by incubation in 70% ethanol solution for 30 minutes and another 30 minutes in
4
30% ethanol solution; washes with sterile Phosphate Buffer Saline (PBS) were performed to
5
discard residual ethanol. Afterwards, the samples were equilibrated in DMEM medium (Sigma-
6
Aldrich Co, USA) supplemented with 10% fetal bovine serum (Biochrom AG, Germany), 1 mM
7
L-glutamine, 100 U/ml penicillin, 100 µg/ml streptomycin (Lonza, Belgium). L929 murine
8
fibroblast cells were cultured at 37ºC in a humidified atmosphere and 5% CO2 in complete
9
DMEM culture medium. At passage 9, the cells were trypsinized and seeded on previously
10
sterilized disc-shaped samples (neat PHO and nanocomposites) in ultra-low attachment flat-
11
bottom 24 well plates (Greiner Bio-One, Austria) at a cell density of 20,000 cells/cm2. The
12
medium was refreshed every two days. The disc-shaped samples were analyzed after 3 and 7
13
days using fluorescence microscopy as described elsewhere.15 Images were acquired using a
14
Eclipse TE2000 inverted fluorescence microscope (Nikon, Austria) and processed with Huygens
15
software (SVI, Hilversum, Netherlands). Cellular morphology and cell density were assessed by
16
using CellProfiler software; eight different images per well were analyzed. To observe the
17
adhesion of L929 cells on the surface of the films, the cells were fixed with 4%
18
paraformaldehyde and permeabilized with Triton X-100 before staining. Nuclei were stained
19
with SYBR ® -Green I (Lonza, Belgium) and actin filaments with Texas-Red ® -X Phalloidin.
20
RESULTS AND DISCUSSION
21
TEM analysis
22
TEM images of BC are shown in Figure 1. The pellicles were completely disintegrated in sparse
23
network nanostructures (Figure 1a) and individual nanofibers (Figure 1b). The length of the 10 ACS Paragon Plus Environment
Page 11 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
nanofibers was larger than 5 µm and the width from a couple of nm to 100 nm. Therefore, the
2
nanofibers have a high aspect ratio (AR), of more than 50. The detailed image from Figure 1
3
shows a single crystalline microfibril of about 20 nm in width at the top right of the image and
4
several protofibrils of about 4 nm. These protofibrils are the most elementary blocks in the
5
formation of the bacterial cellulose network.17 Therefore, the morphology of BC nanofibers was
6
preserved after the mechanical treatment, which succeeded in the release of the nanofibers from
7
the bacterial pellicle.
8 9
Figure 1. TEM images of BC as sparse network small piece (a) and individual nanofibers (b).
10 11
Thermal stability
12
The degradation of PHO is a single step process, similar to that observed in PHB (Figure 2a)
13
with a maximum degradation temperature (Td) of 250 °C (Figure 2b). This Td value is close to
14
that obtained for a PHO copolymer with 2 mol% 3HH,18 but lower than that obtained for a
15
mPHA containing both saturated and unsaturated monomers (around 280 °C).19 It is worth
16
mention that TGA experiments were made on melt processed samples, which were exposed to
11 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 38
1
mechanical stress, temperature, oxygen and humidity influences; the original films showed a
2
higher Td, of 277 ºC.
3
The addition of BC greatly increased the thermal stability of PHO, regardless the amount
4
of nanofibers; the Td value was around 275 °C for nanocomposites, with 25°C higher than that of
5
PHO matrix and even better compared to that of a commercial PHB (fine powder, Biomer,
6
Germany) (Figure 2).
7
The influence of BC nanofillers on the thermal stability of mPHAs was not studied so far;
8
the previous works were focused on sPHAs composites with cellulose nanofillers and have
9
reported different results.20,21 For example, nanofibrillated cellulose obtained from TEMPO
10
oxidized cellulose by mechanical defibrillation decreased the thermal stability of PHBV20 and
11
cellulose nanocrystals (CNC) obtained by acid hydrolysis increased the thermal stability of
12
PHBV.21 In this last case it was hypothesized that, in the early stages of PHBV decomposition,
13
the formation of a six-membered ring ester was blocked due to the hydrogen bonds between
14
CNC and PHBV, which hindered the degradation by chain scissions. A shift of Td to higher
15
temperatures for PHBV with low amount of bacterial cellulose nanowhiskers (1 wt%) but a
16
decrease of the thermal stability for higher loading (3 wt%) was also reported.22 Moreover, Sin et
17
al have shown that the mechanism of mPHAs decomposition is different from that of sPHAs,19
18
which is associated with the ester cleavage by β-elimination reaction.23 It was hypothesized that
19
the aliphatic side chain composed of more than three carbons in mPHAs could hinder the
20
formation of a stable six-membered ring ester intermediate.19 They proposed a random chain
21
scission reaction determined by the hydrolytic chain cleavage initiated at the ester bond at 160 -
22
180 ºC, followed by a secondary process, the dehydration of hydroxyl-esters above 195 ºC,
23
producing terminally unsaturated oligomers.19
12 ACS Paragon Plus Environment
Page 13 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
2 3
Figure 2. TGA (a) and DTG (b) diagrams for PHO and nanocomposites with PHB as a
4
reference; inset – DTG curves (second degradation step) have been offset for clarity.
5 6
The hydrolytic chain cleavage mechanism was considered as a possible mechanism in the
7
case of PHO/BC nanocomposites. However, BC are highly hydrophilic and even after drying
8
they contain a certain amount of bound water as reported before;24 their weight loss at 150 ºC 13 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 38
1
determined by TGA in the same conditions with the nanocomposites was 2.0% (Figure 2a) and
2
that of PHO and nanocomposites was less than 0.2%. Therefore, the higher thermal stability of
3
nanocomposites compared to that of the matrix can’t be explained by the influence of BC in
4
reducing the hydrolytic degradation. Indeed, BC should favor the hydrolytic degradation of
5
PHO, providing the necessary water for the chain cleavage. On the other hand, BC have better
6
thermal stability and much higher crystallinity than PHO. Their Td value (334 ºC) is 80 ºC higher
7
than that of PHO and a degree of crystallinity of 84% was reported for BC nanofibers16 while the
8
crystallinity of PHO do not, generally, exceed 30%.25 Therefore, BC may slow down the
9
absorption of water serving as a barrier and delaying the hydrolytic degradation. Likewise, the
10
interactions between BC and PHO by hydrogen bonding could also delay the degradation, as for
11
sPHAs.21 Therefore, the increase of BC concentration could have antagonistic effects on the
12
thermal stability of PHO, which may explain the small influence of BC concentration on the
13
thermal degradation of nanocomposites.
14
Unlike PHO, the thermal degradation of PHO-BC nanocomposites was a two step
15
process (Figure 2), with the main degradation caused by the chain scission of PHO and the
16
second due to BC degradation. The intensity of this second process depended on the amount of
17
BC, being less intense for the nanocomposite with 1.5 wt% BC. Interestingly, the Td value
18
corresponding to the degradation of BC in nanocomposites (346-348 ºC) was higher than that of
19
pure BC (334 ºC), before the melt compounding with PHO (Figure 2 - inset). A decrease of the
20
thermal stability of cellulose after melt processing would be expected because of the effects of
21
shear stress and temperature and not an increase. The increase of BC stability in nanocomposites
22
may result from the hydrogen bonds between the nanofibers and PHO matrix21 or from the
23
different thermal conductivity in pure BC and nanocomposites.26
14 ACS Paragon Plus Environment
Page 15 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1 2
DSC analysis
3
The thermal characteristics of PHO copolymer and the influence of BC on its glass
4
transition (Tg) and crystallinity were assessed by DSC (Figures S1 and S2). A very small
5
endothermic peak just above the glass transition temperature was detected in the thermograms of
6
PHO and composites (Figure S1). This event, characterized by a small enthalpy relaxation of
7
only 0.5 J/g, is commonly connected to the enthalpy recovered during the heating of an aged
8
sample.27 Since Tg was determined from the second melting, after a heating cycle which erased
9
the thermal history caused by the melt processing and ambient storage for 30 days, it can be
10
supposed that the physical aging was promoted in the previous cooling cycle, when the
11
temperature of the samples was lowered below Tg.
12
No change in the glass transition temperature was induced by the addition of BC; Tg
13
values between -37 and -38 °C were obtained for all the samples, likewise the temperature of the
14
relaxation peak was similar (about -34 °C). Therefore, the addition of BC did not influence the
15
mobility of PHO chains probably because the weight fraction of BC nanofibers was small and
16
their effect on the segmental dynamics of PHO was, thus, negligible. Moreover, previous works
17
on nanocomposites filled with cellulose whiskers reported no change of Tg value with the
18
increase of whiskers amount, regardless of the nature of the polymer matrix.28
19
Interestingly, a melting endotherm was obtained only in the first melting cycle for PHO
20
and nanocomposites; no crystallization was observed in the cooling step and no melting event in
21
the second melting cycle (Figure S2). This is a consequence of the very slow crystallization of
22
mPHAs, much slower than the cooling rate.29-31 The storage of the samples for 30 days in
23
ambient conditions, between the melting temperature and the glass transition of PHO, allowed
15 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 38
1
the crystallization before DSC analysis but the recrystallization could not take place during the
2
short time of the cooling cycle.
3
For a deeper insight into the crystallization process of PHO in PHO/BC nanocomposites,
4
the samples were annealed before DSC characterization in the following conditions, denoted as
5
“a”: PHO and nanocomposites were heated in an oven up to 80 °C with about 5 °C/min, kept
6
isothermally for 5 minutes, then stored in a fridge for 48 h at a temperature of 5 °C; thereafter
7
they were characterized by DSC in the same conditions as for the first test. The temperature of 5
8
°C was chosen because it was demonstrated that the crystallization rate of PHO reaches a
9
maximum at 0-5 °C.25 After annealing in “a” conditions, a melting endotherm was obtained for
10
all the samples only in the first heating cycle (Figure 3) but no crystallization appeared at
11
cooling, similar to the first test. Indeed, the annealing conditions “a” allowed the crystallization
12
of PHO but the short time of the cooling cycle was not enough for recrystallization.
13
14 15
Figure 3. DSC diagrams for un-annealed PHO (a), PHO-1.5BC (b), PHO-3BC (c) and annealed
16
samples (PHOa, PHO-1.5BCa and PHO-3BCa).
17 18
The DSC diagrams for un-annealed and annealed (“a”) samples are shown in Fig. 3 for
19
comparison. A melting peak around 53 ºC with a shoulder at lower temperature was obtained for
16 ACS Paragon Plus Environment
Page 17 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
PHO and nanocomposites in the first test. No variation of the melting point was caused by the
2
addition of BC up to 3 wt%. However, the shoulder was smaller and the main endotherm
3
narrower for the composite with 3 wt% BC compared to the pure matrix, which means increased
4
population of more perfect crystals due to BC addition. This may result from the nucleating
5
effect of BC, as previously reported for other PHAs modified by cellulose nanofibers.20-22
6
However, the degree of crystallinity remained almost unchanged as illustrated by the melting
7
enthalpy normalized by the proportion of PHO in the composite: 25.6 J/g for PHO, 25.4 J/g for
8
PHO-1.5BC and 26.2 J/g for PHO-3BC. The influence of BC on the degree of crystallinity of
9
PHO was verified by FTIR. The absorbance at 1165 cm-1, which is crystallinity-sensitive in
10
PHO,32 showed no change in intensity or position in nanocomposites compared to pure PHO;
11
therefore no variation in crystallinity was obtained from FTIR spectra, which is consistent with
12
the DSC results.
13
After annealing in conditions “a”, a lower melting temperature of 48 ºC and a lower
14
melting enthalpy of 20 J/g were obtained for all the samples, indicating smaller less perfect
15
crystals and lower crystallinity. Indeed, previous DSC study showed that about 7 weeks at 20 ºC
16
or 3 weeks at 5 ºC are required to reach the maximum level of crystallinity in PHO.25 As
17
expected, the annealing conditions “a”, in fact two days at 5 ºC, led to a lower degree of
18
crystallinity compared to the storage at room temperature for 30 days; this shows the influence of
19
the storage conditions on the properties of PHO. It has been reported that sPHAs undergo
20
physical ageing and secondary crystallization during storage, with dramatic effect on the
21
mechanical properties.33 Therefore, the mechanical properties of nanocomposites were
22
determined for different storage conditions.
23
17 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Page 18 of 38
Mechanical properties
2
The stress-strain curves of PHO and nanocomposites, determined after one month from
3
the compression-molding of the sheets, are shown in Figure 4a. A strong increase in both tensile
4
strength and modulus with the increase of BC concentration was noted although no chemical
5
modification of the filler or matrix was done: 3 wt % BC increased the Young’s modulus (YM)
6
with 76% and the tensile strength (TS) with 44%. A weaker increase of YM and TS was
7
observed for PHB or PHBV reinforced with similar amount of cellulose nanofillers.20,26 An
8
increase of the YM by 22% and almost no variation of TS were reported for PHBV
9
nanocomposite with 2.5 wt% nanofibrilated cellulose.20 Likewise, similar increase in YM (77%)
10
and TS (36%) were noted for a higher amount of cellulose nanowhiskers (5 wt%) in PHBV.26
11
The mechanical properties of PHO-3BC (YM of 25 MPa, TS greater than 12 MPa and
12
elongation at break (S) of 65%) promotes this nanocomposite as a suitable material for tissue
13
engineering; its properties fall in the characteristic limits for skin: 15-150 MPa for YM, 5-30
14
MPa for TS and 35-115 % for S, depending on the type of the tissue.34
15
The significant increase of TS in PHO-3BC is, probably, determined by the good
16
interfacial bonding between the carbonyl groups of PHO and the hydroxyl groups of cellulose
17
nanofibers.10,26 This was also suggested by the TGA results. The increase of YM in
18
nanocomposites compared to the matrix may be related to: (i) the restriction of the polymer chain
19
mobility; (ii) the increased crystallinity of the polymer or (iii) the high rigidity of the nanofibers
20
and their good dispersion in the polymer matrix.
18 ACS Paragon Plus Environment
Page 19 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1 2
Figure 4. Stress-strain curves of PHO and nanocomposites (a); Young’s modulus (YM), tensile
3
strength – (TS) and strain at break (S) in function of the aging time (b).
4 5
DSC analysis showed no change in Tg value of PHO after BC addition, and hence chain
6
mobility was not restricted by the small amount of nanofibers. On the other hand, the increase in
7
polymer crystallinity and crystal perfection after nanofillers addition enhances the stiffness and is
8
considered the main cause of a higher YM in nanocomposites.5,29 However, no significant
9
increase of PHO crystallinity was noticed by DSC analysis after BC addition but more perfect
10
crystals in the case of PHO-3BC nanocomposite, which may contribute to some increase in YM.
11
Therefore, the high rigidity of BC nanofibers and their good dispersion in PHO must have
12
contributed to the improvement of YM; it should be kept in mind that the YM of cellulose
13
nanowhiskers was reported to be 143 GPa35, so more than 5000 times higher than that of PHO
14
matrix.
15
Besides polymer-fiber interactions which contribute to a good stress transfer from the
16
matrix to the nanofibers, the high aspect ratio of BC, illustrated by the TEM image (Figure 1), is
17
another factor that should be considered. A percolation model is commonly used to explain the 19 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 38
1
good reinforcing effect of cellulose nanofillers in polymers.10 The formation of a network is
2
possible from a low percolation threshold (P) for high aspect ratio nanofibers. In our system, a P
3
value as low as 1.4 vol% (1.8 wt%. considering the densities of BC and PHO as 1.5 and 1.2
4
g/cm3, respectively) was estimated on the bases of the aspect ratio (AR) of BC before processing:
5
P = 0.7/AR,22 with AR = 50. Therefore, the formation of a continuous network can be assumed
6
in PHO-3BC nanocomposite.
7
AFM – PF QNM technique was used to get more insight into the dispersion of BC in
8
PHO-3BC nanocomposite and the reinforcement mechanism (Figure 5). Long, thin nanofibers
9
(30-40 nm in width and less than 15 nm in height) were observed on the surface of the
10
nanocomposite (Figure 5b), at least some of them being in contact with each others. The larger
11
width of cellulose nanofibers compared to their height in AFM images could be an influence of
12
the tip widening effect.36
13 14
Figure 5. AFM topographic, peak force error and deformation images on the surface of PHO (a)
15
and PHO-3BC (b). 20 ACS Paragon Plus Environment
Page 21 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
The length of nanofibers could not be determined in these images and, therefore, lower
2
magnification AFM scans were taken (Figure 6a and b). Many long nanofibers of more than 5
3
µm in length and 30 - 60 nm in width, besides a few short nanofibers, evenly spread on the
4
surface of PHO-3BC were observed. It should be noted that at a larger scan area the nanofibers
5
were not detected anymore. Interestingly, TEM image of the same magnification of cryo-
6
microtomed layer from the bulk material (Figure 6c) particularly showed well dispersed short
7
fibers; nanofibers of 60 - 80 nm in width and no more than 1 µm in length were observed by
8
TEM. This difference between the surface and bulk nanofibers is intriguing. The shear forces
9
during melt processing may influence both the fibers’ length and their dispersion in PHO, by
10
decreasing the length and improving the dispersion. However, the same size characteristics
11
should be obtained in bulk and on the surface. Moreover, scanning transmission electron
12
microscopy (STEM) image (Figure 6d) showed a thin, long and slightly curved nanofiber in
13
PHO-3BC nanocomposite; indeed, “zigzag” fibers (see Figure 6d – detail) were often observed
14
in TEM images. Hence, it can be hypothesized that the “zigzag” fibers may be cut during the
15
release of the slices, resulting fragments. Having in mind that the cryo-microtomed layer of
16
nanocomposite has a thickness of about 100 nm, which is close to the width of BC nanofibers, it
17
can be assumed that the cutting process may unfold the bundles of BC nanofibrils leading to
18
broaden fibers and may remove parts of the fibers leading to a “dash-dot” like structure in the
19
TEM image. SEM images (Figure 6e-g) confirm the high proportion of long nanofibers and their
20
good dispersion in PHO-3BC; a real network of BC nanofibers is obvious in these images. The
21
nanofibers’ width, determined after a systematic analysis of TEM, AFM and SEM images, was
22
usually between 40 to 110 nm (see histograms in Figure 6h), consistent with previously reported
23
data for BC nanofibers in the initial pellicle.16,17
21 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 38
1 22 ACS Paragon Plus Environment
Page 23 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
Figure 6. Lower magnification AFM images of PHO-3BC nanocomposite - height (a) and peak
2
force error (b); Cryo-TEM image of PHO-3BC nanocomposite (c); STEM image of bacterial
3
cellulose nanofibril in PHO-3BC nanocomposite; curved nanofiber (detail) (d); SEM images of
4
PHO-3BC nanocomposite – different magnifications (e-g); histogram showing the width
5
distribution of BC nanofibers in PHO-3BC nanocomposite from TEM (154 counts), AFM (45
6
counts) and SEM (40 counts) analyses (h)
7 8
The mean width value was 79±22 nm when determined from TEM images analysis,
9
52±23 nm from AFM data and 56±29 nm from SEM analysis. The difference between the mean
10
values may come from the difficulty to “see” the entire fiber which is embedded in the polymer
11
in the case of surface analyses but also from the disruption of fibers as discussed above, in the
12
case of TEM analysis. In conclusion, the melt processing did not induce large changes in the
13
length and width of BC nanofibers in the composite; only a higher proportion of short fibers was
14
observed. Therefore, it can be assumed that the aspect ratio of nanofibers was only slightly
15
decreased and considering the bent and coiled nanofibers (see Fig. 6) as well as nanofiber
16
clusters, it may be supposed that 3 wt% BC is close to the limit from which the percolation is
17
occurring.
18
DSC analysis showed that the aging process influenced the degree of crystallinity of PHO
19
samples, which could affect the mechanical behavior. Therefore, the mechanical properties of
20
PHO-3BC nanocomposite and PHO matrix were determined at different intervals after
21
compression-molding: 3 h, 3days, one week and one month. During these times, the samples
22
were kept at room temperature and 50% relative humidity. The intervals were chosen based on
23
previously reported data regarding the crystallization of PHO.29 Thus, XRD study on a PHO 23 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 24 of 38
1
copolymer containing 5.7% 3HH showed that the first XRD peaks were observed after about 50
2
min for the sample isothermally crystallized at 21 °C and the maximum crystallization rate was
3
noted between 50 and 200 min (about 3 h). Likewise, in a long-term crystallization study by
4
means of DSC, the melting enthalpy showed only a slight growth between 2 to 4 weeks.29
5
The tensile test results (YM in MPa, TS in MPa and S in %) are given in Figure 4b;
6
higher values of tensile strength and modulus were obtained for the nanocomposite compared to
7
the pure matrix regardless the aging time. YM of PHO matrix slightly decreased after 3 days of
8
storage and finally recovered the initial value (measured after 3 h) (Figure 4b); similar variation
9
was noted for TS. Interestingly, only a slight decrease of S with about 10% was observed in the
10
case of PHO over one month of storage, the value of the elongation at break (77%) indicating a
11
ductile behavior. Indeed, PHO sample did not show significant aging during storage and it was
12
able to preserve the ductile behavior within the tested period. Similar conclusion was drawn by
13
Larrañaga et al on a PHO copolymer tested between 2 and 4 weeks of storage at 21 °C;
14
unfortunately, no initial measurement of the mechanical properties was done to observe the
15
variation of the properties between the first day and the 28th.29 Contrarily, a dramatic decrease of
16
the elongation at break (more than 75%) was reported for PHB after 2 weeks of ambient storage,
17
indicating a remarkable embrittlement.37 Similar results were obtained for a PHB copolymer
18
containing different amount, between 2.5 and 8.1 mol%, of 3HH.38 However, the copolymer with
19
3HH fraction higher than 10 mol% showed no significant changes in the mechanical properties
20
after 30 days room-temperature aging.39 The increased brittleness of PHAs was mainly explained
21
by the secondary crystallization and the constraints on the amorphous regions. Considering the
22
inherent low crystallinity of PHO,25 much lower than that of PHB and the higher crystallization
23
rate observed in the first 200 min (about 3 h) of storage close to the room temperature,29 the
24 ACS Paragon Plus Environment
Page 25 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
amorphous region can keep a high mobility regardless the storage time and the influence of the
2
small amount of tiny crystals formed during the storage is insignificant.
3
Several differences were noticed in the variation of the mechanical properties of PHO-
4
3BC with the aging time: almost no variation of the tensile strength but an increase with almost
5
15% of YM and a decrease with about 20% of S over one month of storage. Indeed, BC
6
nanofibers may put supplementary constraint on the amorphous region between crystallites, thus
7
increasing the rigidity. However, the elongation at break of PHO-3BC over one month of
8
storage, 65%, shows a ductile behavior.
9
The surface of PHO-3BC nanocomposite and PHO matrix was investigated by AFM
10
(Figure S3) to observe the crystalline structure, if any, after 3 h of storage. A lamellar structure
11
was visible on the surface of the nanocomposite but less clear on the surface of the matrix,
12
probably because of the nucleating effect of BC; this is consistent with DSC results. Indeed,
13
AFM investigation shows that some crystalline formations have already grown on the surface of
14
PHO samples after 3h of storage and confirms the previous observations for PHO-3HH
15
copolymer.29 The long spacing summing the thickness of crystalline and amorphous layers was
16
estimated to be 44 nm, which is a larger value than the previous estimate for PHB (below 14
17
nm40). This was expected because the crystallization of PHO was not completed and, unlike
18
PHB, the crystallinity in PHO is small. The tip widening effect could also influence the results.36
19
However, no comparison with previous results is possible since this is the first trial to estimate
20
the periodicity in mPHAS. No significant difference in AFM images after one week of storage
21
was noted for both samples, which support the observation that the aging process and
22
recrystallization are not important in the case of PHO matrix and PHO-3BC nanocomposite.
23
25 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Page 26 of 38
Melt processing of PHO/3BC nanocomposite for tube extrusion
2
A simulation of the melt processing of PHO-3BC nanocomposite was undertaken using a
3
homemade extrusion plastometer (Figure 7a) with a tube-shaped die shown as detail in Figure
4
7a. The tube-shaped die had an inner diameter of 3.5 mm, and an outer diameter of 5.5 mm. The
5
cylinder temperature was set to 50 °C. The nanocomposite was filled in the cylinder and kept at
6
the set temperature for about 4 min; then, a weight of 10 kg was applied on the piston and a
7
molded article having a tube-like shape was extruded through the die (Figure 7b). The tube was
8
highly flexible as can be seen in Figure 7c and recovered its form after bending (Figures 7d and
9
e).
10 11
Figure 7. Melt extrusion plastometer used in the tests (a) with the die shown in the detailed
12
image; the tube is flexible and recovered its form after bending (b-e).
13 14
Cell adhesion and cell proliferation studies were performed on PHO homopolymer6 but
15
no information on the pro-inflammatory immune response was found in the literature. Therefore,
16
an evaluation of pro-inflammatory effect was done on PHO and nanocomposites.
17 18
Evaluation of pro-inflammatory effect
19
Macrophages are known to engulf foreign material and to potentially elicit an immune signaling
20
cascade by means of secreted cytokines, chemokines and other immune effectors. TNF-α and IL26 ACS Paragon Plus Environment
Page 27 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
6 are potent pro-inflammatory effectors whose secretion by the macrophages can be triggered by
2
various danger signals, therefore evaluation of inflammatory susceptibility is of utmost
3
importance for biomedical applications.
4
Evaluation of the potential adverse immunological effects of PHO and PHO-3BC was
5
performed in an indirect manner: the eluted constituents of polyhydroxyalkanoate composite
6
were incubated with THP-1 derived macrophages. A PHB sample was tested in similar
7
conditions and served as a polymer reference. Prior to ELISA, all elutions were tested for
8
endotoxin activity to avoid inaccurate results due to bacterial contamination or residual LPS
9
from biosynthesis. All tested samples showed endotoxin activity under the 0.005 EU/mL
10
threshold. After incubation, TNF-α and IL-6 proteins were measured in culture supernatants. IL-
11
6 presence was undetectable in all the samples, except for the LPS treated sample. Likewise,
12
TNF-α concentration was very low (Figure 8), similar to PBS control or cell culture medium
13
control, which is less than 0.3 pg/mL.
14
15 16
Figure 8. TNF-α level in supernatants of THP-1 derived macrophage cells stimulated with
17
elution samples from polyhydroxyalkanoates (undetectable for PHO sample) 27 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 28 of 38
1 2
These results show that PHB, PHO and PHO-3BC nanocomposite will not release
3
components that can drive an acute pro-inflammatory response when used in-vivo, qualifying
4
them as feasible candidates for tissue engineering and biomedical devices.
5 6
Evaluation of cytotoxicity effect
7
The images acquired on the third day (Figure 9) showed the adhesion of L929 cells and
8
their characteristic spindle-shaped morphology for all the three samples, neat PHO, PHO-1.5BC
9
and PHO-3BC nanocomposites. In the seventh day, cells extensively proliferated and completely
10
cover the entire available surface of each tested samples (data not shown). These results prove
11
the ability of neat PHO and PHO nanocomposites to allow cell adherence and to promote cell
12
proliferation.
13
Images acquired on the third day were further analyzed with CellProfiler to yield
14
information about cell density and morphological features. Regarding cell density, the results
15
show small differences between samples, with a higher value for the nanocomposite with 1,5%
16
BC (Figure S4, Supporting Information). The evaluation of cell area revealed a higher tendency
17
of L929 cells to spread over the nanocomposite with 3 wt% BC (Figure S5). The result can be
18
explained by the presence of the more hydrophilic bacterial cellulose on the surface of PHO-
19
3BC, which may greatly promote cell anchoring and adhesion. This hypothesis is also sustained
20
by the form factor analysis (Figure S6). Although there are no statistical significant differences,
21
one may observe a lower form factor value for PHO-3BC sample, indicating a tendency to a
22
more elongated morphology corresponding to a heavily anchored fibroblast, as opposed to a
23
rounder one, characteristic to loosely adhered cells.
24 28 ACS Paragon Plus Environment
Page 29 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1 2
Figure 9. Inverted fluorescence microscope images of L929 cells acquired in the third day on the
3
surface of neat PHO and nanocomposites 29 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 30 of 38
1 2
In conclusion, neither of the tested materials can be deemed cytotoxic. On the contrary,
3
both PHO and PHO/BC nanocomposites are highly biocompatible and favor cell attachment.
4
PHO-3BC, with a more hydrophilic surface due to the higher content of BC showed greater
5
compatibility with L929 cells allowing them to spread over larger areas and to adopt a more
6
natural morphology.
7
CONCLUSIONS
8
A melt processing technique was used for the first time to obtain nanocomposites from a
9
PHO copolymer and bacterial cellulose nanofibers with high aspect ratio. The addition of BC
10
had a benefic effect on the thermal stability of PHO which was increased with 25°C; this is very
11
important for the further melt processing of medical devices. A hydrolytic chain cleavage
12
mechanism was considered to explain the thermal behavior of the nanocomposites. No change of
13
chain mobility and glass transition was observed after BC addition in PHO; likewise, the melting
14
temperature was not influenced but the changes in the shape of the melting endotherm indicated
15
increased population of more perfect crystals in PHO-3BC nanocomposite. The slow
16
crystallization of pure PHO and PHO/BC nanocomposites was evidenced by the lack of
17
crystallization during the cooling cycle, regardless of the storage or annealing conditions. The
18
aging phenomena in PHO and nanocomposites were studied by testing the mechanical properties
19
at different intervals, between 3 h and one month after compression-molding. Crucially, PHO
20
and PHO-3BC nanocomposite were able to preserve their ductile behavior during storage and did
21
not show significant aging, totally opposite to PHB and other sPHAs which show secondary
22
crystallization and increased brittleness during storage. Higher values of tensile strength and
23
modulus were obtained for the nanocomposite compared to the pure matrix regardless the aging 30 ACS Paragon Plus Environment
Page 31 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
time. Only 3 wt % BC was enough to reinforce PHO, increasing the YM with 76% and TS with
2
44%. With a Young’s modulus of 25 MPa, a tensile strength of 12 MPa and an elongation at
3
break of 65%, PHO-3BC nanocomposite is a suitable material for tissue engineering. This
4
nanocomposite was successfully melt processed by tube extrusion and this is an important step
5
for the manufacture of artificial arteries and other medical implants. Biocompatibility study
6
showed no pro-inflammatory immune response of PHO and nanocomposites and no cytotoxic
7
effect on L929 cell line. PHO-3BC showed a greater compatibility and is considered a feasible
8
candidate for in vivo application of tissue-engineered blood vessels.
9
Supporting Information
10
Details on the biosynthesis of PHO copolymer; glass transition temperature from DSC
11
thermograms (second melting) (Figure S1); DSC thermograms (first melting, cooling, second
12
melting) of PHO and nanocomposites (Figure S2); AFM images after 3h of storage (Figure S3).
13
L929 cell density, cell area and factor form (Figures S4-S6).
14
Notes
15
The authors declare no competing financial interest.
16
AUTHOR INFORMATION
17
Corresponding Author
18
* E-mail:
[email protected] (DMP)
19
Acknowledgement
31 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
The financial support from the Romanian Ministry of Education-UEFISCDI, grant 122/2017
2
(PNIII PED-2016-0287 - CELLAB-SLP) and grant 158/2012 (POLYBAC) is greatly
3
acknowledged.
Page 32 of 38
4 5
References
6
(1) Hiroe, A.; Ishii, N.; Ishii, D.; Kabe, T.; Abe, H.; Iwata, T.; Tsuge, T. Uniformity of Monomer
7
Composition and Material Properties of Medium-Chain-Length Polyhydroxyalkanoates
8
Biosynthesized from Pure and Crude Fatty Acids. ACS Sustainable Chem. Eng. 2016, 4, 6905–
9
6911.
10
(2) Panaitescu, D. M.; Frone, A. N.; Chiulan, I. Nanostructured Biocomposites from Aliphatic
11
Polyesters and Bacterial Cellulose. Ind. Crops Prod. 2016, 93, 251-266.
12
(3) Barrett, J. S. F.; Abdala, A. A.; Srienc, F. Poly(hydroxyalkanoate) Elastomers and Their
13
Graphene Nanocomposites. Macromolecules 2014, 47, 3926–3941.
14
(4) Panaitescu, D. M.; Nicolae, C. A.; Frone, A. N.; Chiulan, I.; Stanescu, P. O.; Draghici, C.;
15
Iorga, M.; Mihailescu, M. Plasticized Poly(3-Hydroxybutyrate) with Improved Melt Processing
16
wnd Balanced Properties. J. Appl. Polym. Sci. 2017, 134, 44810.
17
(5) Basnett, P.; Ching, K. Y.; Stolz, M.; Knowles, J. C.; Boccaccini, A. R.; Smith, C.; Locke, I.
18
C.; Keshavarz, T.; Roy, I. Novel Poly(3-hydroxyoctanoate)/Poly(3-hydroxybutyrate) Blends for
19
Medical Applications. React. Funct. Polym. 2013, 73, 1340–1348.
20
(6) Rai, R.; Boccaccini, A. R.; Knowles, J. C.; Mordon, N.; Salih, V.; Locke, I. C.; Moshrefi-
21
Torbati, M.; Keshavarz, T.; Roy, I. The Homopolymer Poly(3-hydroxyoctanoate) as a Matrix
22
Material for Soft Tissue Engineering. J. Appl. Polym. Sci. 2011, 122, 3606–3617.
32 ACS Paragon Plus Environment
Page 33 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
(7) Chung, M. G.; Kim, H. W.; Kim, B. R.; Kim, Y. B.; Rhee, Y. H. Biocompatibility and
2
Antimicrobial Activity of Poly(3-hydroxyoctanoate) Grafted with Vinylimidazole. Int. J. Biol.
3
Macromol. 2012, 50, 310– 316.
4
(8) Dufresne, A.; Vincendon, M. Poly(3-hydroxybutyrate) and Poly(3-hydroxyoctanoate)
5
Blends: Morphology and Mechanical Behavior. Macromolecules 2000, 33, 2998-3008.
6
(9) Chardron, S.; Bruzaud, S.; Lignot, B.; Elain, A.; Sire, O. Characterization of
7
Bionanocomposites Based on Medium Chain Length Polyhydroxyalkanoates Synthesized by
8
Pseudomonas Oleovorans. Polym. Test. 2010, 29, 966–971.
9
(10) Dubief, D.; Samain, E.; Dufresne, A. Polysaccharide Microcrystals Reinforced Amorphous
10
Poly(β-hydroxyoctanoate) Nanocomposite Materials. Macromolecules 1999, 32, 5765-5771.
11
(11) Foster, L. J. R.; Sanguanchaipaiwong, V.; Gabelish, C. L.; Hook, J.; Stenzel, M. A Natural-
12
Synthetic Hybrid Copolymer of Polyhydroxyoctanoate-diethylene glycol: Biosynthesis and
13
Properties. Polymer 2005, 46, 6587–6594.
14
(12) Basnett, P.; Knowles, J. C.; Pishbin, F.; Smith, C.; Keshavarz, T.; Boccaccini, A. R.; Roy, I.
15
Novel Biodegradable and Biocompatible Poly(3-hydroxyoctanoate)/Bacterial Cellulose
16
Composites. Adv. Eng. Mater. 2012, 14, B330-B343.
17
(13) Rai, R.; Yunos, D. M.; Boccaccini, A. R.; Knowles, J. C.; Barker, I. A.; Howdle, S. M.;
18
Tredwell, G. D.; Keshavarz, T.; Roy, I. Poly-3-hydroxyoctanoate P(3HO), a Medium Chain
19
Length Polyhydroxyalkanoate Homopolymer from Pseudomonas Mendocina.
20
Biomacromolecules 2011, 12, 2126–2136.
21
(14) Goonoo, N.; Khanbabaee, B.; Steuber, M.; Bhaw-Luximon, A.; Jonas, U.; Pietsch, U.;
22
Jhurry, D.; Schönherr, H. κ-Carrageenan Enhances the Biomineralization and Osteogenic
33 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 34 of 38
1
Differentiation of Electrospun Polyhydroxybutyrate and Polyhydroxybutyrate Valerate Fibers.
2
Biomacromolecules 2017, 18, 1563-1573.
3
(15) Chiulan, I.; Panaitescu, D. M.; Frone, A. N.; Teodorescu, M.; Nicolae, C. A.; Căşărică, A.;
4
Tofan, V.; Sălăgeanu, A. Biocompatible Polyhydroxyalkanoates/Bacterial Cellulose Composites:
5
Preparation, Characterization, and in vitro Evaluation. J. Biomed. Mater. Res., Part A 2016, 104,
6
2576-2584.
7
(16) Panaitescu, D. M.; Frone, A. N.; Chiulan, I.; Casarica, A.; Nicolae, C. A.; Ghiurea, M.;
8
Trusca, R.; Damian, C. M. Structural and Morphological Characterization of Bacterial Cellulose
9
Nano-Reinforcements Prepared by Mechanical Route. Mater. Des. 2016, 110, 790–801.
10
(17) Brown, R.M. Jr. In Cellulose: Structural and Functional Aspects; Kennedy, J.F., Phillips
11
G.O., Williams P.A., Eds.; Ellis Horwood Ltd., England, 1989; p. 145.
12
(18) Wang, H.; Zhou, X.; Liu, Q.; Chen, G. Biosynthesis of Polyhydroxyalkanoate
13
Homopolymers by Pseudomonas Putida. Appl. Microbiol. Biotechnol. 2011, 89, 1497–1507.
14
(19) M. C. Sin, S. N. Gan, M. S. M. Annuar, I. K. P. Tan, Thermodegradation of Medium-Chain-
15
Length Poly(3-hydroxyalkanoates) Produced by Pseudomonas Putida from Oleic Acid. Polym.
16
Degrad. Stab. 2010, 95, 2334-234.
17
(20) Srithep, Y.; Ellingham, T.; Peng, J.; Sabo, R.; Clemons, C.; Turng, L.-S.; Pilla, S. Melt
18
Compounding of Poly (3-hydroxybutyrate-co-3-hydroxyvalerate)/Nanofibrillated Cellulose
19
Nanocomposites. Polym. Degrad. Stab. 2013, 98, 1439-1449.
20
(21) Yu, H-Y.; Qin, Z.-Y.; Liu, Y.-N.; Chen, L.; Liu, N.; Zhou, Z. Simultaneous Improvement of
21
Mechanical Properties and Thermal Stability of Bacterial Polyester by Cellulose Nanocrystals,
22
Carbohydr. Polym. 2012, 89, 971– 978.
34 ACS Paragon Plus Environment
Page 35 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
(22) Martínez-Sanz, M.; Villano, M.; Oliveira, C.; Albuquerque, M. G.; Majone, M.; Reis, M.;
2
Lopez-Rubio, A.; Lagaron, J. M. Characterization of Polyhydroxyalkanoates Synthesized from
3
Microbial Mixed Cultures and of Their Nanobiocomposites with Bacterial Cellulose
4
Nanowhiskers. New Biotechnol. 2014, 31, 364–376.
5
(23) Gonzalez, A.; Irusta, L.; Fernandez-Berridi, M. J.; Iriarte, M.; Iruin, J. J. Application of
6
Pyrolysis/Gas Chromatography/Fourier Transform Infrared Spectroscopy and TGA Techniques
7
in the Study of Thermal Degradation of Poly (3-hydroxybutyrate). Polym. Degrad. Stab. 2005,
8
87, 347-354.
9
(24) Brown, E. E.; Laborie, M.-P. G. Bioengineering Bacterial Cellulose/Poly(ethylene oxide)
10
Nanocomposites. Biomacromolecules 2007, 8, 3074-3081.
11
(25) Gagnon, K. D.; Lenz, R. W.; Farris, R. J.; Fuller, R. C. Crystallization Behavior and its
12
Influence on the Mechanical Properties of a Thermoplastic Elastomer Produced by Pseudomonas
13
Oleovorans. Macromolecules 1992, 25, 3723-3728.
14
(26) Ten, E.; Turtle, J.; Bahr, D.; Jiang, L.; Wolcott, M. Thermal and Mechanical Properties of
15
Poly(3-hydroxybutyrate-co-3-hydroxyvalerate)/Cellulose Nanowhiskers Composites. Polymer
16
2010, 51, 2652-2660.
17
(27) Frone, A. N.; Panaitescu, D. M.; Chiulan, I.; Nicolae, C. A.; Vuluga, Z.; Vitelaru, C.;
18
Damian, C. M. The Effect of Cellulose Nanofibers on the Crystallinity and Nanostructure of
19
Poly(lactic acid) Composites. J. Mater. Sci. 2016, 51, 9771-979.
20
(28) Bras, J.; Hassan, M. L.; Bruzesse, C.; Hassan, E. A.; El-Wakil, N. A.; Dufresne, A.
21
Mechanical, Barrier, and Biodegradability Properties of bagasse Cellulose Whiskers Reinforced
22
Natural Rubber Nanocomposites. Ind. Crops Prod. 2010, 32, 627–633.
35 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 36 of 38
1
(29) Larrañaga, A.; Pompanon, F.; Gruffat, N.; Palomares, T.; Alonso-Varona, A.; Larrañaga
2
Varga, A.; Fernandez-Yague, M.A.; Biggs, M. J. P.; Sarasua, J. R. Effects of Isothermal
3
Crystallization on the Mechanical Properties of a Elastomeric Medium Chain Length
4
Polyhydroxyalkanoate. Eur. Polym. J. 2016, 85, 401–410.
5
(30) Nerkar, M.; Ramsay, J. A.; Ramsay, B. A.; Vasileiou, A. A.; Kontopoulou, M.
6
Improvements in the Melt and Solid-State Properties of Poly(lactic acid), Poly-3-
7
hydroxyoctanoate and Their Blends through Reactive Modification. Polymer 2015, 64, 51-61.
8
(31) Marchessault, R. H.; Monasterios, C. J.; Morin, F. G.; Sundararajan, P. R. Chiral Poly(beta-
9
hydroxyalkanoates): an Adaptable Helix Influenced by the Alkane Side-Chain. Int. J. Biol.
10
Macromol. 1990, 12, 158-165.
11
(32) Randriamahefa, S.; Renard, E.; Guerin, P.; Langlois, V. Fourier Transform Infrared
12
Spectroscopy for Screening and Quantifying Production of PHAs by Pseudomonas Grown on
13
Sodium Octanoate. Biomacromolecules 2003, 1092-1097.
14
(33) Srubar III, W. V.; Wright, Z. C.; Tsui, A.; Michel, A. T.; Billington, S. L.; Frank, C. W.
15
Characterizing the Effects of Ambient Aging on the Mechanical and Physical Properties of two
16
Commercially Available Bacterial Thermoplastics. Polym. Degrad. Stab. 2012, 97, 1922-1929.
17
(34) Li, W-J.; Laurencin, C. T.; Caterson, E. J.; Tuan, R. S.; Ko, F. K. Electrospun nanofibrous
18
structure: A novel scaffold for tissue engineering, J. Biomed. Mater. Res. 2002, 60, 613–621.
19
(35) Sturcova, A.; Davies, G. R.; Eichhorn S. J. Elastic modulus and stress-transfer properties of
20
tunicate cellulose whiskers. Biomacromolecules 2005, 1055-1061.
21
(36) Zhong, J.; Liu, X.; Wei, D.; Yan, J.; Wanga, P.; Sun, G.; He, D. Effect of incubation
22
temperature on the self-assembly of regenerated silk fibroin: A study using AFM. Int. J. Biol.
23
Macromol. 2015, 76, 195–202.
36 ACS Paragon Plus Environment
Page 37 of 38
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Biomacromolecules
1
(37) de Koning, G. J. M.; Lemstra, P. J. Crystallization phenomena in bacterial poly[(R)-3-
2
hydroxybutyrate]: 2. Embrittlement and rejuvenation. Polymer 1993, 34, 4089-4094.
3
(38) Asrar, J.; Valentin, H. E.; Berger, P. A.; Tran, M.; Padgette, S. R.; Garbow, J. R.
4
Biosynthesis and properties of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) polymers.
5
Biomacromolecules 2002, 3, 1006-1012.
6
(39) Alata, H.; Aoyama, T.; Inoue, Y. Effect of aging on the mechanical properties of poly(3-
7
hydroxybutyrate-co-3-hydroxyhexanoate). Macromolecules, 2007, 40, 4546–4551.
8
(40) de Koning, G. J. M.; Scheeren, A. H. C.; Lemstra, P. J. Crystallization phenomena in
9
bacterial poly[(R)-3-hydroxybutyrate]: 3. Toughening via texture changes. Polymer 1994, 35,
10
4598-4605.
37 ACS Paragon Plus Environment
Biomacromolecules
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Table of Contents Graphic 83x35mm (300 x 300 DPI)