Subscriber access provided by SUNY DOWNSTATE
Article
Mixed Electronic and Ionic Conductor-Coated Cathode Material for High Voltage Lithium Ion Battery Jae-Hyun Shim, Jung-Min Han, Joon-Hyung Lee, and Sanghun Lee ACS Appl. Mater. Interfaces, Just Accepted Manuscript • DOI: 10.1021/acsami.6b03113 • Publication Date (Web): 29 Apr 2016 Downloaded from http://pubs.acs.org on May 3, 2016
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a free service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are accessible to all readers and citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
ACS Applied Materials & Interfaces is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Mixed Electronic and Ionic Conductor-Coated Cathode Material for High Voltage Lithium Ion Battery
Jae-Hyun Shim,1 Jung-Min Han,1 Joon-Hyung Lee,2* Sanghun Lee3*
J.-H. Shim and J.-M. Han 1
Battery R&D Center, Samsung SDI, Suwon, Gyunggido 16677, Republic of Korea
J.-H. Lee 2
Automotive & ESS Business, Samsung SDI, Yongin, Gyunggido 17084, Republic of Korea
Sanghun Lee 3
Department of BioNano Technology, Gachon University, Seongnam, Gyunggido 13120, Republic of
Korea
Corresponding Authors E-mail:
[email protected] (J.H.L.),
[email protected] (S.L.)
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Abstract A lithium ionic conductor, Li1.3Al0.3Ti1.7(PO4)3 (LATP), is introduced as a coating material on the surface of Mg-doped LiCoO2 to improve electrochemical performances for high voltage (4.5 V) lithium ion batteries. Structure, morphology, elemental distribution, and electrical properties of the materials are thoroughly characterized by SEM, TEM, EELS, EDS, and C-AFM. The coating layer is electrically conductive with the aid of Mg ions which are used as a dopant for the active materials; therefore, this mixed electronic ionic conductor strongly enhances the electrochemical performances of initial capacity, cycling property, and rate capability. The LATP coating layer also demonstrates very promising applicability for 4.4 V prismatic full cells with graphite anode, which corresponds to the 4.5 V half cells with lithium anode. The 2900 mAh full cells show 85 % of capacity retention after 500 cycles and more than 60 % after 700 cycles.
Keywords: Lithium ion battery, Mixed electronic and ionic conductor, Lithium cobalt oxide, High voltage cell, Full cell application
ACS Paragon Plus Environment
Page 2 of 20
Page 3 of 20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1. Introduction For the well-balanced electrochemical performances of energy density, power, rate capability, and cyclability, LiCoO2 has been the most commonly used cathode material for the lithium ion battery (LIB) since the first commercialization by SONY in 1991.1 However, the recent development of high performance mobile electronics and transportations powered by electric energy, such as, electric vehicles and hybrid electric vehicles, strongly requires improving performances of the LIB.2,3 In particular, increasing the energy density is one of the priority-tasks for future advanced energy storages. With finding new materials possessing many lithium ions in a unit volume or mass, for example, lithium-rich oxides,4-6 raising cut-off voltages of currently known materials is a main strategy to obtain the high energy density. Because the layer-structured materials including LiCoO2 without any modification, in which transition metal ions are directly coordinated by oxygen, may suffer from easy structure collapse during cycling, particularly, at high voltages, the recent progress in the high voltage LIBs has been made primarily in polyanion oxides or spinel materials.7 However, because the theoretical capacities of these materials are much lower than those of the layered materials, they are not practically employed in commercial batteries and LiCoO2 is still one of the most popular cathode materials for LIB. The vulnerability of LiCoO2 at the high voltages is mainly attributed to the two factors of 1) oxygen loss caused by the side reactions with electrolytes and 2) irreversible structural transformation at higher voltages than 4.5 V (vs Li+/Li). Hence, Chen and Dahn suggested that coating with metal oxide materials under heat-treatment would remarkably improve retention property of LiCoO2 by suppressing the side-reactions when charging to 4.5 V.8 This surface modification by metal oxide coating to improve electrochemical performances of LiCoO2 was originally proposed by Cho et al.9-11 and many researchers confirmed the successful improvement with various metal oxides as coating materials.12-18 However, because the most of metal oxides, such as, MgO, ZrO2, Al2O3, ZnO, etc are the insulators for lithium ions, the coating materials may work as obstacles for ionic conduction, which is one of the main reasons for high resistivity at the interface between electrode and electrolytes.
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 20
Therefore, in order to improve the ionic conductivity of the coating layer, recently, lithium ion conductors have been introduced as alternative coating materials. For example, Lu et al. proposed that monoclinic Li2TiO3 would be a good candidate.19 They reported that Li2TiO3-coated LiMO2 (M = Ni, Co, and Mn) nanobelts exhibited very good rate capability and cycling property. In addition, based on the fact that Li4Ti5O12 does not suffer from significant volume change during lithium cycling, which is another
example
of
lithium
ion
conductor
and
known
as
“zero-strain
material”
on
lithiation/delithiation, several researchers have tested it as a coating material for the layer-structured cathode materials.20-24 Even though the above studies reported that the lithium ion conductor-coated cathode materials demonstrated considerable successes in half coin-cells, they failed to be employed in battery industry because they could not overcome serious capacity fade in full cells due to their poor electrical conductivity and/or structural instability during cycling. In fact, the most available application of the lithium ion conductors is a solid electrolyte for allsolid-state batteries. Among them, Li1+xAlxTi2-x(PO4)3 (LATP) of the NASICON structure exhibits the excellent ionic conductivity at room temperature25 and, therefore, it is one of the most promising solid electrolyte materials for all-solid-state LIBs.26-28 In a few recent studies, however, LATP was tested not as a solid electrolyte but as a minor constituent for cathode composite (LiCoO2 and LATP). Morimoto et al. prepared this composite by simple mechanical mixing and reported high capacity and good cycling property with a high cut-off potential (4.5 V) in a liquid electrolyte LIB.29 Meanwhile, Nakamura et al. obtained this material by a similar method and used it as a cathode for all-solid-state LIB.30 They showed that this material exhibited much better electrochemical performances than the LiCoO2 cathode without LATP. In this study, we use LATP (x = 0.3 in this work) as a coating material for the LiCoO2 cathode and, consequently, improve lithium ionic conductivity at the interface between the active materials and electrolytes. Moreover, as shown in our previous study,24 it is possible to increase electrical conductivity of the coating layer by diffusion of dopant ions (Mg2+ in this work) from the active materials. As a result, we obtain mixed electronic and ionic conductor-coated LiCoO2 with Mg doping.
ACS Paragon Plus Environment
Page 5 of 20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
We thoroughly characterize the coating layer by various analysis techniques including scanning electron microscopy (SEM), transmission electron microscopy (TEM) with electron energy loss spectroscopy (EELS), and conductive atomic force microscopy (C-AFM), and understand the mechanism of the excellent electrochemical performances of this material. Finally, this material is adopted for a prismatic 4.4 V full cell with a graphite anode, which is corresponding to the 4.5 V cathode vs Li+/Li, and exhibits very good capacity retention over 700 cycles. This work provides a very informative guide to the development of good cathode materials by introducing mixed electronic and ionic conductive coating layers.
2. Experimental Section Prior to the LATP coating, Mg-doped LiCoO2 (LiMg0.03Co0.97O2) was prepared by the solid state reaction as in our previous study.24 Then, the sol-gel method was employed for the LATP coating. First, 1.555 g of Ti(OBu)4 was dissolved in 19 mL of ethanol. In a separate container, 0.549 g of LiNO3 and 0.900 g of NH4H2PO4 were dissolved in 8 mL of water. After completely mixing the two solutions, 0.296 g of Al(NO3)3•9H2O was added. Then, this final solution and 50 g of the active material were mixed by the ball-milling for 1h (zirconia ball, 150 rpm). Following evaporating the solvent on a hot plate at 110 °C, the mixture was dried in a convection oven at 120 °C. Then, the obtained powder was heat-treated at 750 °C for 6 h in a furnace and naturally cooled to room temperature. This product is hereafter denoted by LATP-LCOMg. In order to demonstrate the excellence of this material, we prepared two references for comparison. The one is LATP-coated but Mg-undoped LiCoO2 (LATP-LCO), the coating procedure of which was the same as described above, the other one is Mg-doped LiCoO2 without the coating (uncoated-LCOMg). The morphology of the materials was investigated by a field emission SEM (Magellan XHR, FEI Co., Oregon, USA). The scanning TEM (STEM) measurements were performed using a Cs-corrected STEM (JEM-2100F, JEOL, Co., Tokyo, Japan) at 200 kV, which is equipped with a spherical aberration corrector (CEOS Gmbh, Heidelberg, Germany). The elemental distribution of the materials
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
was characterized by the energy dispersive spectrometer (EDS, EDAX, USA) equipped in the SEM or TEM. The EELS spectrum was obtained in the STEM mode with a total beam current of 0.2 nA for a probe size of 0.5 nm (Gatan GIF200 spectrometer). The electrical conductivity of the materials was analyzed by a C-AFM (Danish Microscope Engineering, Denmark) in the direct contact mode. Following the sample preparation by helium ion microscope (Carl Zeiss Microscopy GmbH), the measurements were performed in an ultrahigh vacuum (10-8 Torr) to avoid contamination. To evaluate the electrochemical performances, 2032-type coin-cells were fabricated. For the preparation of the cathode, the active material (LATP-LCOMg, LATP-LCO, or uncoated-LCOMg), conducting material (Super-P carbon black), and binder (polyvinyliden fluoride, PVDF) were blended (96:2:2 in weight ratio) in N-methyl-2-pyrrolidone. Then, the slurry was cast on an aluminum foil and dried at 110 °C for 10 h in a vacuum oven. The electrolyte solution was 1.15 M LiPF6 in ethylene carbonate/dimethyl carbonate/ethylmethyl carbonate mixture (3:3:4 in volume ratio). The lithium foil was used as the anode and the capacity of the manufactured cells was 1.5 mAh/cm2. The cycling capacities were measured between 3.0 and 4.5 V. In order to see if this new material has the potential for industrial use, prismatic full cells of 2900 mAh were manufactured. The cathode was composed of the active material, conducting material, and binder (97.4:1.3:1.3 in weight ratio), in which the contents of the latter two components were reduced to increase the capacity per volume of a full cell. The natural graphite (BSG-L, BTR, China) anode and the electrolyte of 0.9 M LiPF6 solution in ethylene carbonate/ethylmethyl carbonate/diethyl carbonate mixture (3:5:2 in volume ratio) were used with several minor additives (fluoroethylene carbonate, vinyl ethylene carbonate, propylsultone, and LiBF4). The electrolyte composition of the full cells was designed differently from that of the coin cells for common use in various product lines under consideration of the effects from the graphite anode. The cells were cycled between 3.0 and 4.4 V with the rate of 1 C.
3. Results and Discussion
ACS Paragon Plus Environment
Page 6 of 20
Page 7 of 20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
The morphologies and internal structures of uncoated-LCOMg and LATP-LCOMg were characterized by the SEM and TEM. The typical dimension of the synthesized particles of the both samples is ~15 µm. The LATP coating layer seems to be inhomogeneous in a relatively large scale (Figure 1b), however, it is continuous and evenly thick in a sub-µm scale as shown in Figure 1c. The selected area electron diffraction (SAED) pattern of the coating layer in Figure 1c supports that it has the NASICON hexagonal structure of Li1.3Al0.3Ti1.7(PO4)3 with parameters of a = 8.5 Å and c = 20.8 Å.31 Figure 1d shows the elemental distributions of cations from EDS analysis. The Co and Al ions are located in the regions where they are expected to be; Co in the active layer and Al in the coating layer. Meanwhile, the Mg and Ti ions are observed in both the coating layer and the LiCoO2 region. Note that Mg was used as a dopant in the LiCoO2 region and Ti was used as one of the sources for the coating layer. The diffusion of Mg ions from the active material to the coating layer was previously reported, where the coating layer containing the diffused Mg ions exhibited improvement of the electrical conductivity and, consequently, the enhanced electrochemical performances.24 We observed similar behaviors in this study, which will be shown later. The Ti ions migrated to the active material are mixed with the Co ions in the transition metal (TM) layers. For identification of the TM ions, the EELS spectra were obtained along the TM layers (yellow dotted arrows in Figure 1e). Even though only the Co ions were detected in most of the measured area (spectra B), a few TM ions were identified as the Ti ions (marked in a red dotted circle, spectra A), which indicates that the small amounts of Co ions occupied on arbitrary sites are replaced by the Ti ions. In Figure 2a and b, the cycling performance at 1 C and the C-rate property of the materials are respectively shown. The capacities were measured within a range of 3.0-4.5 V vs Li metal anode and two cycles were performed at 0.1 C for the formation before the measurements. Compared to uncoated-LCOMg (167.6 mAhg-1), LATP-LCOMg exhibits a significantly improved discharge capacity at the first cycle (185.0 mAhg-1). Even more remarkable is the enhanced cycling ability of LATPLCOMg. As shown in Figure 2a, uncoated-LCOMg demonstrates a very sharp discharge capacity fade, particularly, after 30 cycles whereas LATP-LCOMg shows an extremely improved cycling ability; its capacity after 100 cycles (176.8 mAhg-1) is higher than 95.5 % of its initial capacity. In addition, the
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
LATP coating also offers superiority in the C-rate capability of the cathode materials. As shown in Figure 2b, the positive influence of the coating on the discharge capacity becomes greater as the Crate of cycling increases; the capacity of LATP-LCOMg is 1.07 and 1.46 times higher than that of uncoated-LCOMg at 0.1 and 3.0 C, respectively. This improvement of the cell performances with the LATP coating is even more noteworthy when it is applied to the prismatic full cells, which will be shown later. Another important point which deserves attention in Figure 2a and b is that the coating effect on the electrochemical performances is fairly limited without the Mg doping. As shown earlier, the coating layer of LATP-LCOMg contains a considerable amount of Mg ions. We suppose that the migrated Mg ions improve the electrical conductivity of the coating layer and, as a result, the cells from LATP-LCOMg exhibit the much better performances than the ones from LATP-LCO. Experimental evidence supporting this assertion will be presented later. Sometimes, differential capacity (dq/dv) vs cell voltage plots provide very useful information on the phase transitions of electrode materials during lithiation or delithiation. Figure 2c and d shows the dq/dv plots of uncoated-LCOMg and LATP-LCOMg, respectively, as a function of number of cycles. In these measurements, charging and discharging were performed within a range of 3.0-4.6 V. For the both samples, several peaks indicating phase transitions are clearly recognized in the curves of the first cycle. As previously reported,32-35 the peak of “a” at 3.92 V corresponds to the transition between the two O3 phases and the “b” (4.09 V) and “c” (4.18 V) peaks are assigned to the order-disorder (hexagonal to monoclinic and monoclinic to hexagonal) transitions. In addition, the forth peak of “d” at 4.53 V is also shown, which corresponds to the transition from the O3 phase to the H1-3 phase. The most remarkable difference between the two samples is the variation of the “a” peak with continuing cycles. In the case of uncoated-LCOMg, as the charging/discharging repeats, it shifts markedly to high voltages along with significant intensity reduction; however, in the case of LATP-LCOMg, the extent of variation of the “a” peak is relatively small. This observation implies that the structural transition indicated by the “a” peak of uncoated-LCOMg significantly loses its reversibility as the cycle repeats whereas LATP-LCOMg relatively well maintains its original structure even after cycles. The behaviors of the “b” and “c” peaks, which are shown in the enlarged insets, also support this argumentation. It is
ACS Paragon Plus Environment
Page 8 of 20
Page 9 of 20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
well known that the structural degradation of LiCoO2 with cycling is driven by oxygen loss due to detrimental reactions of the active materials with electrolytes. In this point of view, it is considered that the LATP coating layer successfully works as a protection layer to reduce the side reactions. To reduce the reactions with electrolytes at the electrode surface, it is necessary to obtain low resistivity, i.e. high electrical conductivity of the materials. From the electrochemical performance results in the above, we supposed that the Mg ions from the active material would improve electrical conductivity of the LATP coating layer. To support this presumption, we investigated the electrical conductivity of LATP-LCOMg and LATP-LCO using the C-AFM, which was equipped with the SEM to find a proper area to be measured in the very small scale.36 A cross-section near the interface between the coating layer and the active material of a cleaved particle was characterized. The surface topography and the corresponding current image were simultaneously obtained by applying an electrical bias of 4 V. As shown in Figure 3a, LATP-LCOMg has a relatively uniform height throughout the entire area while its coating layer displays much higher conductivity than the active material. Meanwhile, in the case of LATP-LCO, the cross-sectional topography of which is very close to that of LATP-LCOMg, the LATP coating layer is almost electrically nonconducting (Figure 3b). This observation verifies that the diffused Mg ions from the LiCoO2 region to the LATP layer noticeably raise its conductivity and, consequently, create a synergistic positive effect on the cell performances. To examine the industrial applicability of this material, prismatic full cells (3.0-4.4 V, 2900 mAh) were manufactured. It should be noted that the cells were cycled at quite rapid charging/discharging rate of 1 C to investigate the cycling ability. In Figure 4a, the capacity retention at a certain cycle represents the ratio of the discharge capacity at the corresponding cycle to that at the first cycle. The cells with LATP-LCOMg show very stable retention characteristics (85 % after 500 cycles and more than 60 % even after 700 cycles) at room temperature. On the contrary, the references for comparison show poor performances. The cells with uncoated-LCOMg undergoes a significant capacity drop at the early cycles (up to ~100 cycles), which is caused by the side reactions allowed by the absence of the protection layer, while those with LATP-LCO show a sudden catastrophe in the capacity after ~200
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
cycles even though they demonstrate quite stable performances in the beginning of the cycling tests. To compare the deteriorated states of LATP-LCOMg and uncoated-LCOMg, the SEM images and the elemental distributions from the EDS of the cross-sectioned particles after cycling are shown in Figure 4b and c. In the EDS map of uncoated-LCOMg, a large amount of F is observed in between the particles, which is obviously a consequence of the side reactions with LiPF6 salts in the electrolyte whereas, in the map of LATP-LCOMg, the F atoms are scarcely recognized. This observation is indicative of the fact that the LATP coating layer successfully works to suppress the side reactions even in the prismatic full cells for practical application. For further investigation, the surface area of LATP-LCOMg after 700 cycles was measured by the TEM. Because the particles are not completely surrounded by the LATP layer, which means that coated and non-coated areas coexist, the effects of coating can be clearly determined in one image. In Figure 5, the SAED pattern of the area covered by the LATP layer (denoted as B) proves that the area preserves its original structure of LiCoO2 (ܴ3ത݉) after cycling. However, the pattern of the non-coated surficial area (denoted as A), which is a typical pattern of the spinel structure (݀ܨ3ത݉), indicates that the non-coated region undergoes structural transformation during cycling. The STEM images in the high resolution are also consistent with this explanation. The spinel phase is clearly shown in the image of A region whereas only the layered structure of LiCoO2 is observed in the B area.
3. Conclusions We have prepared and characterized LATP-coated LiCoO2 with Mg doping for 4.5 V high performance LIBs. From the elemental distribution analysis, it has been revealed that some amounts of Mg ions, which are intended to be used a dopant for LiCoO2, are diffused to the coating layer. As a result, the lithium ionic conductor, LATP, also obtains high electrical conductivity and creates a positive effect on the electrochemical performances of cycling property and C-rate capability. In addition, we have proved that the excellence of this material is preserved in the industrial application for the 4.4 V prismatic full cells. The cells show excellent capacity retention of 85 % after 500 cycles
ACS Paragon Plus Environment
Page 10 of 20
Page 11 of 20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
and more than 60 % after 700 cycles and the cathode material demonstrates a strong structural tolerance to the cycling degradation.
References [1] Nagaura, T.; Tozawa, K. Lithium Ion Rechargeable Battery. Prog. Batteries Sol. Cells 1990, 9, 209-214. [2] Malik, M. Y. Power Consumption Analysis of a Modern Smartphone. arXiv:1212.1896v2 [cs.PF]. [3] Thackeray, M. M.; Wolverton, C.; Isaacs, E. D. Electrical Energy Storage for TransportationApproaching the Limits of, and Going Beyond, Lithium-Ion Batteries. Energy Environ. Sci. 2012, 5, 7854-7863. [4] Lu, Z.; Beaulieu, L. Y.; Donaberger, R. A.; Thomas, C. L.; Dahn, J. R. Synthesis, Structure, and Electrochemical Behavior of Li[NixLi1/3-2x/3Mn2/3-x/3]O2. J. Electrochem. Soc. 2002, 149, A778-A791. [5] Shizuka, K.; Kobayashi, T.; Okahara, K.; Okamoto, K.; Kanzaki, S.; Kanno, R. Characterization of Li1+yNixCo1-2xMnxO2 Positive Active Materials for Lithium Ion Batteries. J. Power Sources 2005, 146, 589-593. [6] Yu, X.; Lyu, Y.; Gu, L. Wu, H.; Bak, S.-M.; Zhou, Y.; Amine, K.; Ehrlich, S. N.; Li, H.; Nam, K.W.; Yang, X.-Q. Understanding the Rate Capability of High-Energy-Density Li-Rich Layered Li1.2Ni0.15Co0.1Mn0.55O2 Cathode Materials. Adv. Energy Mater. 2014, 4, 1300950. [7] Hu, M.; Pang, X.; Zhou, Z. Recent Progress in High-Voltage Lithium Ion Batteries. J. Power Sources 2013, 237, 229-242. [8] Chen, Z.; Dahn, J. R. Methods to Obtain Excellent Capacity Retention in LiCoO2 Cycled to 4.5 V. Electrochim. Acta 2004, 49, 1079-1090. [9] Cho, J.; Kim, G. Enhancement of Thermal Stability of LiCoO2 by LiMn2O4 Coating. Electrochem. Solid-State Lett. 1999, 2, 253-255.
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
[10] Cho, J.; Kim, Y. J.; Park, Y. Novel LiCoO2 Cathode Material with Al2O3 Coating for a Li Ion Cell. Chem. Mater. 2000, 12, 3788-3791. [11] Cho, J.; Kim, Y. J.; Kim, T.-J.; Park, B. Zero-Strain Intercalation Cathode for Rechargeable LiIon Cell. Angew. Chem. Int. Ed. 2001, 40, 3367-3369. [12] Wang, Z.; Huang, X.; Chen, L. Performance Improvement of Surface-Modified LiCoO2 Cathode Materials: An Infrared Absorption and X-Ray Photoelectron Spectroscopic Investigation. J. Electrochem. Soc. 2003, 150, A199-A208. [13] Zhao, H.; Gao, L.; Qiu, W.; Zhang, X. Improvement of Electrochemical Stability of LiCoO2 Cathode by a Nano-Crystalline Coating. J. Power Sources 2004, 132, 195-200. [14] Iriyama, Y.; Kurita, H.; Yamada, I.; Abe, T.; Ogumi, Z. Effects of Surface Modification by MgO on Interfacial Reactions of Lithium Cobalt Oxide Thin Film Electrode. J. Power Sources 2004, 137, 111-116. [15] Liu, L.; Chen, L.; Huang, X.; Yang, X.-Q.; Yoon, W.-S.; Lee, H. S.; McBreen, J. Electrochemical and In Situ Synchrotron XRD Studies on Al2O3-Coated LiCoO2 Cathode Material. J. Electrochem. Soc. 2004, 151, A1344-A1351. [16] Chen, Z.; Dahn, J. R. Studies of LiCoO2 Coated with Metal Oxides. Electrochem. Solid-State Lett. 2003, 6, A221-A224. [17] Chen, Z.; Dahn, J. R. Effect of a ZrO2 Coating on the Structure and Electrochemistry of LixCoO2 When Cycled to 4.5 V. Electrochem. Solid-State Lett. 2002, 5, A213-A216. [18] Shim, J.-H.; Lee, S.; Park, S. S. Effects of MgO Coating on the Structural and Electrochemical Characteristics of LiCoO2 as Cathode Materials for Lithium Ion Battery. Chem. Mater. 2014, 26, 2537-2543. [19] Lu, J.; Peng, Q.; Wang, W.; Nan, C.; Li, L.; Li, Y. Nanoscale Coating of LiMO2 (M = Ni, Co, Mn) Nanobelts with Li+-Conductive Li2TiO3: Toward Better Rate Capabilities for Li-Ion Batteries. J. Am.
ACS Paragon Plus Environment
Page 12 of 20
Page 13 of 20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Chem. Soc. 2013, 135, 1649-1652. [20] Ohta, N.; Takada, K.; Zhang, L.; Ma, R.; Osada, M.; Sasaki, T. Enhancement of the High-Rate Capability of Solid-State Lithium Batteries by Nanoscale Interfacial Modification. Adv. Mater. 2006, 18, 2226-2229. [21] Yi, T.-F.; Shu, J.; Yue, C.-B.; Zhu, X.-D.; Zhou, A.-N.; Zhu, Y.-R.; Zhu, R.-S. Enhanced Cycling Stability of Microsized LiCoO2 Cathode by Li4Ti5O12 Coating for Lithium Ion Battery Mater. Res. Bull. 2010, 45, 456-459. [22] Yi, T.-F.; Shu, J.; Wang, Y.; Xue, J.; Meng, J.; Yue, C.-B.; Zhu, R.-S. Effect of Treated Temperature on Structure and Performance of LiCoO2 Coated by Li4Ti5O12 Surf. Coat. Tech. 2011, 205, 3885-3889. [23] Fey, G. T.-K.; Huang, C.-F.; Muralidharan, P.; Chang, E. S.-S. Improved Electrochemical Performance of LiCoO2 Surface Treated with Li4Ti5O12 J. Power Sources 2007, 174, 1147-1151. [24] Shim, J.-H.; Lee, J.; Han, S. Y.; Lee, S. Synergistic Effects of Coating and Doping for Lithium Ion Battery Cathode Materials: Synthesis and Characterization of Lithium Titanate-Coated LiCoO2 with Mg Doping. Electrochim. Acta 2015, 186, 201-208. [25] Knauth, P. Inorganic Solid Li Ion Conductors: An Overview. Solid State Ionics 2009, 180, 911916. [26] Birke, P.; Salam, F.; Döring, S.; Weppner, W. A First Approach to a Monolithic All Solid State Inorganic Lithium Battery. Solid State Ionics 1999, 118, 149-157. [27] Hoshina, K.; Dokko, K.; Kanamura, K. Investigation on Electrochemical Interface between Li4Ti5O12 and Li1+xAlxTi2-x(PO4)3 NASICON-Type Solid Electrolyte. J. Electrochem. Soc. 2005, 152, A2138-A2142. [28] Cao, C.; Li, Z.-B.; Wang, X.-L.; Zhao, X.-B.; Han, W.-Q. Recent Advances in Inorganic Solid Electrolytes for Lithium Batteries. Front. Energy Res. 2014, 2, 00025. [29] Morimoto, H.; Awano, H.; Terashima, J.; Shindo, Y.; Nakanishi, S.; Ito, N.; Ishikawa, K.;
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Tobishima, S. Preparation of Lithium Ion Conducting Solid Electrolyte of NASICON-Type Li1+xAlxTi2-x(PO4)3 (x = 3) Obtained by Using the Mechanochemical Method and Its Application as Surface Modification Materials of LiCoO2 Cathode for Lithium Cell. J. Power Sources 2013, 240, 636-643. [30] Nakamura, E.; Kondo, A.; Matsuork, M.; Kozawa, T.; Naito, M.; Koga, H.; Iba, H. Preparation of LiCoO2/ Li1.3Al0.3Ti1.7(PO4)3 Composite Cathode Granule for All-Solid-State Lithium-Ion Batteries by Simple Mechanical Method. Adv. Powder Technol. 2015, DOI: 10.1016/j.apt.2015.10.013. [31] Best, A. S.; Forsyth, M.; MacFarlane, D. R. Stoichiometric Changes in Lithium Conducting Materials Based on Li1+xAlxTi2-x(PO4)3: Impedance, X-ray and NMR Studies. Solid State Ionics 2000, 136-137, 339-344. [32] Reimers, J. N.; Dahn, J. R. Electrochemical and In Situ X-ray Diffraction Studies of Lithium Intercalation in LixCoO2. J. Electrochem. Soc. 1992, 139, 2091-2097. [33] Reimers, J. N.; Dahn, J. R.; von Sacken, U. Effects of Impurities on the Electrochemical Properties of LiCoO2. J. Electrochem. Soc. 1993, 140, 2752-2754. [34] Chen, Z.; Lu, Z.; Dahn, J. R. Staging Phase Transitions in LixCoO2. J. Electrochem. Soc. 2002, 149, A1604-A1609. [35] Sun, Y.-K.; Yoon, C. S.; Myung, S.-T.; Belharouak, I.; Amine, K. Role of AlF3 Coating on LiCoO2 Particles during Cycling to Cutoff Voltage above 4.5 V. J. Electrochem. Soc. 2009, 156, A1005-A1010. [36] Shim, J.-H.; Lee, K.-S.; Missyul, A.; Lee, J.; Linn, B.; Lee, E. C.; Lee S. Characterization of Spinel LixCo2O4-Coated LiCoO2 Prepared with Post-Thermal Treatment as a Cathode Material for Lithium Ion Batteries. Chem. Mater. 2015, 27, 3273-3279.
ACS Paragon Plus Environment
Page 14 of 20
Page 15 of 20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Figure 1. SEM images of (a) uncoated-LCOMg and (b) LATP-LCOMg. (c) Bright-field TEM image and SAED pattern of LATP coating layer. (d) STEM image and elemental distributions from EDS of LATP coating layer. (e) Enlarged STEM image and EELS spectrum of active material of Mg-doped LiCoO2.
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 2. (a) Cycling performance at 1 C and (b) rate capability of half coin-cells in the range of 3.04.5 V. Differential capacity vs voltage (dq/dv) curves of (c) uncoated-LCOMg and (d) LATP-LCOMg cells.
ACS Paragon Plus Environment
Page 16 of 20
Page 17 of 20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Figure 3. Height and current maps of (a) LATP-LCOMg and (b) LATP-LCO obtained from C-AFM.
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Figure 4. (a) Retention capacity of 2900 mAh 4.4 V prismatic full cells with graphite anode. SEM images and elemental distributions obtained from EDS of cross-sections of (b) LATP-LCOMg and (c) uncoated-LCOMg particles. For the measurements, the cells were disassembled after 700 and 400 cycles, respectively.
ACS Paragon Plus Environment
Page 18 of 20
Page 19 of 20
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
Figure 5. Bright-field TEM image in the interface of LATP-LCOMg after 700 cycles. The SAED patterns and STEM images of A and B regions are also shown.
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces
1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Table of Contents
ACS Paragon Plus Environment
Page 20 of 20