Subscriber access provided by Iowa State University | Library
Biofuels and Biobased Materials
Preparation and characterization of cellulose grafted with epoxidized soybean oil aerogels for oil absorbing materials Xu Xu, Fuhao Dong, Xinxin Yang, He Liu, Lizhen Guo, Yuehan Qian, Aiting Wang, Shifa Wang, and Jinyue Luo J. Agric. Food Chem., Just Accepted Manuscript • DOI: 10.1021/acs.jafc.8b05161 • Publication Date (Web): 02 Jan 2019 Downloaded from http://pubs.acs.org on January 3, 2019
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 25
Journal of Agricultural and Food Chemistry
1
Preparation and characterization of cellulose grafted with
2
epoxidized soybean oil aerogels for oil absorbing materials
3
Xu Xu*a,b, Fuhao Donga, Xinxin Yang c, He Liu*c, Lizhen Guoa, Yuehan Qiana,
4
Aiting Wangc, Shifa Wanga,b, Jinyue Luoa,b
5
a. College of Chemical Engineering, Nanjing Forestry University Nanjing, Jiangsu
6
Provincial Key Lab for the Chemistry and Utilization of Agro-forest Biomass, Nanjing
7
210037, Jiangsu Province, China.
8
b. Jiangsu Co-Innovation Centre of Efficient Processing and Utilization of Forest
9
Resources, Nanjing 210037, Jiangsu Province, China.
10
c. Institute of Chemical Industry of Forestry Products, Chinese Academy of Forestry,
11
Nanjing 210042, Jiangsu Province, China
12
Contact information: College of Chemical Engineering, Nanjing Forestry University
13
Jiangsu Nanjing 210037, Jiangsu Province, China;
14
*Corresponding author:
[email protected] and
[email protected] 15 16
Abstract: The absorbent materials synthesized from bio-sources with low cost and high
17
selectivity for oils and organic solvents have attracted increasing attention in the field
18
of oil spillage and discharge of organic chemicals. We developed a convenient surface-
19
grafting method to prepare efficient and recyclable bio-based aerogels from epoxidized
20
soybean oil (ESO)-modified cellulose at room temperature. The porous network-like
21
structure of the cellulose aerogel was still fully retained after undergoing hydrophobic 1
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
22
modification with ESO. Moreover, the modified aerogels possessed excellent
23
hydrophobicity with a water-contact angle of 132.6°. Moreover, the absorbent ability
24
of the hydrophobic cellulose aerogels was systematically assessed. The results showed
25
that modified aerogels could retain more than 90% absorption capacity even after 30
26
absorption−desorption cycles, indicating that the ESO-grafted cellulose aerogels have
27
practical applications in the oil-water separation from industrial wastewater and oil-
28
leakage removal.
29
Keywords: Cellulose aerogels, Epoxidized soybean oil, Oil-absorbing materials, Oil-
30
water separation, Oil/water selectivity
31 32
1. Introduction
33
The ocean is one of Earth's most valuable natural resources, but the ocean pollution
34
due to oil spillage accidents and discharge of organic chemicals has become more and
35
more severe to global environment.1-3 Therefore, scientists focus on developing
36
efficient methods for collection and removal of oil spills and organic chemicals from
37
the ocean. Generally, oil-absorbing materials are commonly used to handle oil leakages
38
due to its fast and efficient absorption in water.4-10
39
The oil-absorbing materials usually include inorganic products, synthetic resins,
40
and natural polymers.11, 12 The inorganic oil-absorbing materials, such as clay, activated
41
carbon, and silica, etc. appear as powders or small particles, making the transportation
42
and recycling costs high.2, 3, 8, 13 Synthetic oil-absorbing resins, including acrylic and 2
ACS Paragon Plus Environment
Page 2 of 25
Page 3 of 25
Journal of Agricultural and Food Chemistry
43
olefinic resins, are one of the most efficient oil-absorbing materials widely used in the
44
treatment of oil spills. However, the resin may not be degradable or easy to be
45
biodegraded, which results in some environmental problems. Furthermore, some
46
natural polymers, like cellulose, straw, wood chips, and other natural plant fiber-based
47
products, play an essential role in this field because of its recyclability, low cost, and
48
biodegradability.4, 6, 7, 14-18
49
Among bio-based absorbents, hydrophobic aerogels have been used as oil
50
absorbents due to their low density, high porosity, and large specific surface area.7, 19-
51
21
52
renewability, biodegradability, and porosity.17, 18, 22-24 However, the hydroxyl groups in
53
the cellulose aerogels lead to several issues, including poor oil/water selectivity and
54
loss of mechanical properties after prolonged exposure to water. On the other hand, the
55
hydroxyl groups have good reactivity, which can lead to surface modification of
56
cellulose aerogels. Indeed, cellulose aerogels can overcome the inherent hydrophilicity
57
of aerogel skeleton to obtain hydrophobicity and oleophilicity; in other words, it means
58
they can exhibit excellent oil/water selectivity. Therefore, natural cellulose aerogels are
59
promising candidates as oil sorbents after undergoing surface hydrophobization to
60
improve their oil selectivity.25-28 Among the methods to improve the cellulose-aerogel
61
surface hydrophobicity, the absorption of surfactants or polymers and covalent
62
modification of the surfaces are widely used. However, most of the modified cellulose
63
aerogels by surfactants have excess surfactant that has to be removed and are unstable
Cellulose aerogels exhibit good advantages, such as abundant sources, natural
3
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
64
in different media.11,
65
urethanization, amidation, and silylation.16,
66
modifications are carried out at high temperature, in toxic organic solvents and by non-
67
renewable resources, which might cause significant environmental and ecological
68
impacts. Consequently, increasing effort has been dedicated to attaching natural
69
polymer chains via grafting to prepare hydrophobic and oleophilic porous cellulose
70
based on aerogels with excellent oil-water selective absorption ability.32-36
29
Covalent modifications mostly consist of esterification, 23, 30, 31
However, most of these
71
We report on an efficient method for the formation of modified cellulose based on
72
materials with enhanced hydrophobic properties, which were grafted with polymeric
73
epoxidized soybean oil (ESO) as a renewable environmentally friendly and low-cost
74
raw material.37 Based on this previous work, cellulose grafted with ESO aerogels were
75
prepared and used as oil-absorbing materials. The effects of ESO on the structure,
76
thermal stability, and surface morphology of the ESO modified cellulose aerogels were
77
studied as well. The oil selectivity, oil absorption capacity, and repeated absorption
78
performance of the oil-absorbing material were evaluated in the water-oil mixture
79
system as well.
80
2. Experimental section
81
2.1. Materials.
82
Cellulose pulp from hardwood was provided by the Hubei Chemical Fiber Group
83
Ltd. ESO, sodium hydroxide (NaOH), 1,4-butanediol diglycidyl ether (BDE), and urea
84
were purchased from Aladdin Reagent Corporation. Crude oil was obtained from China 4
ACS Paragon Plus Environment
Page 4 of 25
Page 5 of 25
Journal of Agricultural and Food Chemistry
85
Petroleum & Chemical Corporation, Jinan Petroleum Branch. Engine oil, silicone oil,
86
paraffin liquid, cyclohexane (≥98%), and n-hexane (≥99%) were purchased from
87
Macklin Chemical Reagents Co., Ltd. (Shanghai, China). Dimethyl sulfoxide (DMSO,
88
≥99%), toluene (≥99.5%), isopropyl alcohol (≥99%), and dichloromethane (CH2Cl2,
89
≥99.5%) were bought from Sinopharm Chemical Reagent Co., Ltd (Shanghai, China).
90
All chemicals and solvents were used as received without further purification.
91
Deionized water was used in all experiments.
92
2.2. Preparation of cellulose aerogels.
93
Cellulose pulp was dried to remove moisture by vacuum and precooled to -10 °C
94
before use. The aqueous solution containing NaOH/urea/H2O at 7:12:81 by weight was
95
used as the solvent. 4.0 g of cellulose pulp was added to 96.0 g NaOH/urea/H2O
96
solution and mixed at -12 °C under stirring for 30 min; thus, a transparent and viscous
97
cellulose solution was obtained. BDE was added to the solution, and the mixture was
98
kept at room temperature for 1 h to form the cellulose hydrogels. Here, the molar ratio
99
between anhydroglucose unit (AGU, M = 162) of cellulose and BDE was 1:3. The
100
hydrogels were separated via centrifugation and purified with water until the pH was 7.
101
Next, the purified hydrogels were diluted to 1.5% by adding deionized water. Finally,
102
the diluted hydrogels were freeze-dried in a lyophilizer for 48 h to obtain the porous
103
cellulose aerogels.
104
2.3. Preparation of cellulose grafted with ESO aerogels.
5
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
Page 6 of 25
105
0.1 g of cellulose aerogels and 15 g of n-hexane solvent were charged into a three-
106
necked flask with magnetically stirrer and reflux. 10 μL SnCl4 was added as a catalyst.
107
1, 2, 4, 6, and 8 g of ESO (5, 10, 20, 30, and 40 wt% of n-hexane, respectively) were
108
dissolved in 20 g n-hexane, respectively. The ESO solution was dropped into a three-
109
necked flask with a constant-pressure dropping funnel. The hydrophobically modified
110
cellulose material was prepared at room temperature for 30 min reaction and, then, was
111
washed three times with n-hexane to remove the unreacted ESO and ESO self-
112
aggregated products. The cellulose grafted with ESO aerogels was obtained after
113
drying. Cellulose aerogel without ESO modification is defined as Cell/BDE and ESO
114
in 5, 10, 20, 30, and 40 wt% of n-hexane are defined as 5Cell/BDE,
115
20Cell/BDE, 30Cell/BDE,
116
2.4. Characterization.
117
2.4.1. Fourier-transform infrared (FT-IR) spectroscopy. The chemical composition
118
of cellulose samples was analyzed via FT-IR spectroscopy (Nicolet iS 10 spectrometer).
119
The spectra were recorded ranging from 4000-600 cm−1 at a resolution of 4 cm−1 and
120
averaged over 16 scans per sample.
121
2.4.2. X-ray diffraction (XRD). The X-ray diffraction patterns were measured via an
122
X-ray diffractometer (D8 FOCUS, Bruker, Germany) with a Cu-Kα anode. The analysis
123
was recorded at a scanning speed of 0.01° s-1 in the range of 2θ = 10-50°.
124
2.4.3. Thermodynamic analysis. The thermal stability was assessed with a TGA-
125
60AH thermogravimetric analyzer (Shimadzu, Japan) in the range from 25 to 800 °C at
10Cell/BDE,
and 40Cell/BDE, respectively.
6
ACS Paragon Plus Environment
Page 7 of 25
Journal of Agricultural and Food Chemistry
126
a constant heating rate of 10 °C/min under a nitrogen atmosphere. Differential scanning
127
calorimetry (DSC) was conducted via DSC-60A (Shimadzu, Japan) under a nitrogen
128
atmosphere.
129
2.4.4. Scanning electron microscopy (SEM). The surface morphology of the samples
130
was analyzed via scanning electron microscopy (FE-SEM, JSM-7600F, JEOL, Japan).
131
The samples were attached to the sample holders with conductive double-sided carbon
132
tape and sputter-coated with a platinum layer to avoid charging during the tests.
133
2.4.5. Contact angle measurements. The contact angles of the water droplets were
134
measured at room temperature via a goniometer (Attension® Theta Lite,
135
BolinScientific, Sweden). A double-sided piece of adhesive tape was placed on a glass
136
coverslip, on top of which the cellulose specimen was placed. Then, 5 μL of deionized
137
water were placed on the surface for measurement of the contact angle. Three
138
measurements were taken at different points for each sample from which the average
139
contact angle values were determined.
140
2.4.6. Absorbent ability. The absorption capacity of cellulose grafted with ESO
141
aerogels was measured by immersing samples in 200 mL solvent. The saturated
142
aerogels were weighed after absorbing the surface solvent with filter paper. The
143
absorbent ability (g/g) of cellulose aerogels was measured and calculated as:
144
Absorbent ability = (m1 - m0)/m0 × 100%
145
here, m1 is the weight of the solvent-saturated cellulose aerogel, whereas m0 is the
146
weight of the dried-cellulose aerogel, respectively.
(1)
7
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
147
3. Results and discussion
148
3.1. Structural characterization of cellulose grafted with ESO aerogels.
149
Figure 1 shows the FT-IR spectrum of cellulose grafted with ESO aerogels before
150
and after undergoing the hydrophobic modification. The band ranging from 3350 to
151
3500 cm-1 in the spectra of cellulose aerogel can be associated to the stretching vibration
152
of O–H. The peaks at 2860 cm-1 and 2935 cm-1 correspond to the symmetric and
153
asymmetric stretching vibrations of methylene, respectively. It can be seen from Figure
154
1a that there is no absorption peak of ester carbonyl group before hydrophobicity
155
modification. With the increase of ESO content during the modification process, the
156
absorption peak of ester carbonyl group at 1742 cm-1 in cellulose grafted with ESO
157
aerogels is enhanced. The results indicate that the cellulose aerogel has been modified
158
by ESO successfully. However, the increase of the absorption intensity of ester
159
carbonyl in
160
increased to 40 wt%, which is consistent with fact that the hydrophobicity of the
161
40Cellu/BDE-modified aerogel was similar to that of the 30Cellu/BDE-modified aerogel.
40Cellu/BDE
was no longer obvious when the mass fraction of ESO
162 8
ACS Paragon Plus Environment
Page 8 of 25
Page 9 of 25
163
Journal of Agricultural and Food Chemistry
Figure 1. FT-IR spectra of cellulose grafted with ESO aerogels.
164
XRD was used to investigate the effect of the surface modification on the cellulose-
165
aerogel crystal structure. Figure 2 shows the XRD pattern of cellulose grafted with ESO
166
aerogels with different ESO content. There is a significant diffraction absorption peak
167
near 20.9° before and after hydrophobic modification by ESO that can be associated to
168
the amorphous cellulose.7 It indicates that cellulose grafted with ESO aerogels exhibits
169
an amorphous structure, which is not affected by the amount of ESO used in the
170
modification process.
171 172 173
Figure 2. X-ray diffraction patterns of cellulose grafted with ESO aerogels. 3.2. Thermal stability of cellulose grafted with ESO aerogels.
174
Thermogravimetric analysis (TG) and Differential thermal analysis (DTG) curves
175
of cellulose aerogel and cellulose grafted with ESO aerogels are shown in Figure 3. As
176
shown in the Figure 3A, the weight loss of the cellulose aerogel Cellu/BDE within 100
177
°C is more than that of cellulose grafted with ESO aerogels because of the volatilization
178
of water, which indicates that the pure cellulose aerogel without modification has a
179
hydrophilic property and high water-absorption ability, while samples from 9
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
180
5Cellu/BDE
181
The temperature of the maximum thermal-decomposition rate of Cellu/BDE is 345 °C;
182
however, that of cellulose grafted with ESO is slightly lower but still higher than 271
183
°C, which still shows excellent thermal stability. When the mass fraction of ESO
184
reaches 40 wt%, the final residual rate is the highest in all samples due to the carbon
185
residue produced by the decomposition of the grafted ESO on the surface of aerogels.
186
In addition, two maximum thermal decomposition peaks of 40Cellu/BDE appear in the
187
DTG curve (Figure 3B), which are ascribed to the maximum thermal decomposition of
188
the ESO grafted on the aerogel surface and that of the cellulose skeleton, respectively.
to 40Cellu/BDE after modification by ESO exhibits high hydrophobicity.
189 190
Figure 3. TG and DTG curves of cellulose grafted with ESO aerogels.
191
The thermal behavior of the cellulose aerogels before and after hydrophobic
192
modification can be evaluated via DSC as well. Figure 4 shows the thermal behavior of
193
the unmodified-cellulose aerogel Cellu/BDE (Figure 4a) and the cellulose grafted with
194
ESO aerogels with ESO content of 10 wt% and 20 wt%, respectively (Figure 4b and
195
4c). As a result of the low concentration of ESO grafted on the aerogel surface, no glass-
196
transition temperature Tg appears in the test temperature range from -50 to 50 °C, when 10
ACS Paragon Plus Environment
Page 10 of 25
Page 11 of 25
Journal of Agricultural and Food Chemistry
197
the mass fraction of ESO is less than 10 wt%. In Figure 4c, it can be found that Tg of
198
20Cellu/BDE
199
glass-transition temperature of 20Cellu/BDE is that ESO has reacted with the hydroxyl
200
groups on the cellulose aerogel surface and then form polymeric ESO. This reaction
201
has affected the chemical composition and surface free energy of the cellulose grafted
202
with ESO aerogels, which increases the mobility of the molecular chains and enhances
203
the plasticity of the material.
is -9.43 °C when EOS content is 20 wt%. The reason for the significant
204 205 206
Figure 4. DSC curves of the cellulose samples. 3.3. Morphological analysis of the cellulose grafted with ESO aerogels.
207
The SEM images of the three-dimensional network structure of cellulose aerogels
208
consisting of continuous and homogeneous porous are shown in Figure 5 at the micro
209
level. After the hydrophobic modification with ESO, the porous web-like structure is
210
still fully retained. However, with the increase of ESO content, more protrusions and
211
uneven wrinkles appear on the aerogel surface. This phenomenon is attributed to
212
polymerized particles formed by ESO grafted with cellulose by the ring-opening
213
reaction on the aerogel surface. When the mass fraction of ESO is increased to 40 wt%, 11
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
214
the porosity of 40Cellu/BDE is reduced as more pores are covered by film-like polymers
215
due to ESO-grafted cellulose inside the pores.
216 217 218
Figure 5. SEM images of the cellulose samples. 3.4. Wettability of the cellulose grafted with ESO aerogels.
219
Oil/water selectivity plays a vital role in oil-absorbing materials. The cellulose
220
aerogels without hydrophobic modification have a large number of hydroxyl groups
221
lacking good oil/water selectivity; therefore, they cannot be used as oil absorbents for
222
the oil-water mixture. As presented in Figure 6, both the macromorphologies of
223
cellulose before and after hydrophobic modification are white and regular cuboid,
224
indicating that the process with ESO has not affected the shape of the cellulose, which
225
is consistent with the SEM results. But the density of the cellulose aerogel was 26.7
226
mg·cm-3 and that of the 30Cellu/BDE aerogel was 72.8 mg·cm-3. The increase of density
227
also indicates that cellulose was successfully grafted with ESO. As shown in Figure 6a1 12
ACS Paragon Plus Environment
Page 12 of 25
Page 13 of 25
Journal of Agricultural and Food Chemistry
228
and a2, 5 μL of water (stained with CuSO4 in blue colour) were dropped on the
229
Cellu/BDE aerogel surface; then, its surface becomes rapidly wet and with a contact
230
angle of 0°. Moreover, the Cellu/BDE aerogel still displays good absorption ability of
231
pump oil (stained with Sudan red in red colour) as well, which means that the
232
unmodified cellulose aerogels do not have the advantage of oil/water selectivity. In
233
contrast, the same water droplet exhibits a nearly spherical shape on the surface of
234
30Cellu/BDE
235
hydrophobicity of the cellulose grafted with ESO aerogel. In addition, the pump-oil
236
droplet was absorbed by the
237
cellulose aerosol grafted with ESO has both lipophilic and hydrophobic properties.
with a contact angle of 132.6° (Figure 6b1 and b2), indicating good
30Cellu/BDE
aerogel immediately, suggesting that the
238 239
Figure 6. Contact angle of Cellu/BDE and 30Cellu/BDE. (a1) Image of the contact angle
240
with water in Cellu/BDE; (a2) Photo of the water and oil droplets on the surface of 13
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
241
Cellu/BDE; (b1) Image of the contact angle with water in 30Cellu/BDE; (b2) Photo of
242
the water and oil droplets on the surface of 30Cellu/BDE. The water and pump oil were
243
pained with CuSO4 and Sudan red, respectively.
244
3.5. Deformation recovery of the cellulose grafted with ESO aerogels.
245
The deformation recovery of
30Cellu/BDE
aerogels was further tested by
246
performing several cycles of squeezing and re-absorption (Figure 7). The 30Cellu/BDE
247
aerogel was immersed in red-colored pump oil (stained with Sudan red) (Figure 7a-d);
248
it reached its maximum absorption capacity after 16 s. Then, it was squeezed out with
249
an external force until no more water was removed, as shown in Figure 7e-f. The
250
30Cellu/BDE
251
reached its maximum absorption capacity after 11 s (Figure 7g-h), indicating that the
252
aerogel can be reused when the squeezed cylinder could swell to its original shape.
253
Figure 7i shows the height recovery of 30Cellu/BDE as a function of the recycle number.
254
The height of 30Cellu/BDE sample can still reach 90% of the original height after 30
255
cycles of repeated compression-recovery, which confirms its good elasticity and
256
deformation recovery. Compared with some other brittle carbon-absorbent materials,
257
the
258
undergoing the hydrophobic modification.
aerogel was re-immersed in red-colored pump oil; in this second cycle it
30Cellu/BDE
aerogels display improved flexibility and re-use performance after
14
ACS Paragon Plus Environment
Page 14 of 25
Page 15 of 25
Journal of Agricultural and Food Chemistry
259 260
Figure 7. High efficiency in pump oil recovery and absorbent reusability of
261
30Cellu/BDE.
262
30Cellu/BDE
263
a function of squeezing–re-absorption cycles.
264
3.6. Absorbent ability evaluation of the cellulose grafted with ESO aerogels.
(a-d) Absorption of
30Cellu/BDE
in pump oil; (e-h) Re- absorption of
in pump oil after squeezing; (i) The absorbent abilities of 30Cellu/BDE as
265
As shown in Figure 8, pump oil and dichloromethane were dropped on the surface
266
and bottom of the water, respectively. The cellulose grafted with ESO aerogels can
267
selectively absorb the pump oil and dichloromethane from water as well as the oil-filled
268
cellulose grafted with ESO aerogels can be separated from water expediently (Figure
269
8). Figure 8 shows different states of the unmodified cellulose aerogel Cellu/BDE and
270
the cellulose oil-absorbing material
271
Cellu/BDE is placed in pump oil-water system (top row in Figure 8), it absorbs both
272
part of pump oil (red color) and part of water (blue color) due to hydroxyl groups in the
273
molecular chain of the cellulose aerogels, which exhibit hydrophilic and lipophilic
274
properties. Cellu/BDE moves down to the aqueous layer after 15 min and then sinks
275
into the bottom of the water layer after 30 min, which confirms that the unmodified
30Cellu/BDE
in the oil-water system. When
15
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
276
cellulose aerogel can absorb oil, but its selectivity to water is higher than that of oil.
277
When the modified-cellulose aerogel 30Cellu/BDE is placed in pump oil/water system
278
(middle row in Figure 8), it keeps floating on the blue-colored water layer surface after
279
selectively absorbing red-colored pump oil, which shows its lipophilic and hydrophobic
280
performance because of the hydrophobization with ESO. This modified aerogel absorbs
281
not only the oil with lower density than water but also the oil with higher density than
282
water, such as dichloromethane (as shown in the bottom row in Figure 8). When
283
30Cellu/BDE
284
colored dichloromethane, while the volume of the water remains unchanged. This
285
observation demonstrates that cellulose aerogel modified by ESO exhibits good
286
oil/water selectivity.
has been placed into the bottom of the beaker, it absorbs all of the red-
287
16
ACS Paragon Plus Environment
Page 16 of 25
Page 17 of 25
Journal of Agricultural and Food Chemistry
288
Figure 8. Removal of a red-colored pump oil spill from water with the slices of (top
289
row) Cellu/BDE and (middle row) 30Cellu/BDE; (bottom row) removal of
290
dichloromethane from the bottom of water with the slice of 30Cellu/BDE.
291
The absorption performance of
30Cellu/BDE
towards different oils and organic
292
solvents was further investigated (Figure 9A). We found that the samples reach
293
absorption equilibrium within 16 s in oils or organic solvents. As shown in Figure 9A,
294
30Cellu/BDE
295
absorbent abilities of
296
liquid, silicone oil, DMSO, cyclohexane, toluene, isopropyl alcohol, and
297
dichloromethane are 37, 30, 28, 32, 34, 43, 9, 27, 13, and 48 g/g, respectively.
has different absorption capacity for oils or organic solvents. The 30Cellu/BDE
towards crude oil, engine oil, pump oil, paraffin
298
To test the reusability, the cellulose grafted with ESO aerogels absorbed crude oil,
299
DMSO, and CH2Cl2, respectively until reaching absorption equilibrium, as described
300
in the Experimental Section. Then, the oil and the solvents were removed thoroughly
301
as one cycle. The cellulose grafted with ESO aerogels were used to absorb oil again, as
302
shown in Figure 9B. After 30 cycles, the absorption capacity of 30Cellu/BDE towards
303
crude oil, DMSO, and CH2Cl2 decreased from 37, 43, and 48 g/g to 33, 39, and 43 g/g,
304
respectively, whereas the absorption capacity remains higher than 90%.
17
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
305 306
Figure 9. The absorbent ability of
307
30Cellu/BDE
308
absorbent ability of 30Cellu/BDE of crude oil, DMSO, and CH2Cl2.
30Cellu/BDE.
(A) The absorbent ability of
towards a series of oils and organic solvents; (B) The recycle of the
309
Cellulose-based oil-absorbing material grafted with ESO was successfully
310
fabricated via freeze-drying without undergoing any shape and microstructure change.
311
The grafting reaction occurs on the hydroxyl groups attached to the surface of cellulose
312
with ESO. It results in the modification of the cellulose-aerogel surface characteristics
313
from being hydrophilic to hydrophobic. The so-prepared aerogels have multiple
314
advantages in terms of straightforward fabrication process with mild reaction
315
conditions, shape recoverability, and excellent selective absorption of oils and organic
316
solvents. When the mass fraction of ESO is 30 wt%, the water contact angle of modified
317
cellulose aerogels is 132.6°, whereas the absorption ability towards crude oil, DMSO,
318
and CH2Cl2 reaches 37, 43, and 48 g/g, respectively. The absorbed aerogels can retain
319
more than 90 % of the initial absorption capacity and high hydrophobicity even after
320
30 separation cycles. These newly developed cellulose-based oil-absorbing materials 18
ACS Paragon Plus Environment
Page 18 of 25
Page 19 of 25
Journal of Agricultural and Food Chemistry
321
are promising candidates for absorption applications in industrial wastewater,
322
environmental remediation, and oil spill containment.
323
Acknowledgments
324
This work was supported by the Fundamental Research Funds of CAF
325
(CAFYBB2017QB007),
326
(2017YFD0601004), Jiangsu Provincial Department of Education (JPDE), Top-notch
327
Academic Programs Project of Jiangsu Higher Education Institutions (ATPP) and the
328
priority Academic Program Development of Jiangsu Higher Education Institutions
329
(PAPD).
330
References
331 332 333 334
the
National
Key
R&D
Program
of
China
(1) Chen, D.; Zhu, H.; Yang, S.; Li, N.; Xu, Q.; Li, H.; He, J.; Lu, J. Micronanocomposites in environmental management. Adv. Mater. 2016, 28, 10443-10458. (2) Liu, H.; Geng, B.; Chen, Y.; Wang, H. Review on the aerogel-type oil sorbents derived from nanocellulose. ACS Sustainable Chem. Eng. 2016, 5, 49-66.
335
(3)Xiong, Y.; Wang, C.; Wang, H.; Yao, Q.; Fan, B.; Chen, Y.; Sun, Q.; Jin, C.; Xu,
336
X. A 3D titanate aerogel with cellulose as the adsorption-aggregator for highly efficient
337
water quality purification. J. Mater. Chem. A 2017, 5, 5813-5819.
338
(4) Chen, X.; Weibel, J. A.; Garimella, S. V. Continuous oil-water separation using
339
polydimethylsiloxane-functionalized melamine sponge. Ind. Eng. Chem. Res. 2016, 55,
340
3596-3602.
19
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
341
(5) Feng, J.; Nguyen, S. T.; Fan, Z.; Duong, H. M. Advanced fabrication and oil
342
absorption properties of super-hydrophobic recycled cellulose aerogels. Chem. Eng. J.
343
2015, 270, 168-175.
344
(6) Nguyen, S. T.; Feng, J.; Le, N. T.; Le, A. T. T.; Hoang, N.; Tan, V. B. C.; Duong,
345
H. M. Cellulose aerogel from paper waste for crude oil spill cleaning. Ind. Eng. Chem.
346
Res. 2013, 52, 18386-18391.
347
(7) Meng, G.; Peng, H.; Wu, J.; Wang, Y.; Wang, H.; Liu, Z.; Guo, X. Fabrication of
348
superhydrophobic cellulose/chitosan composite aerogel for oil/water separation. Fibers
349
Polym. 2017, 18, 706-712.
350
(8) Yu, L.; Zhou, X.; Jiang, W. Low-cost and superhydrophobic magnetic foam as an
351
absorbent for oil and organic solvent removal. Ind. Eng. Chem. Res. 2016, 55, 9498-
352
9506.
353 354
(9) Yang, Y.; Yi, H.; Wang, C. Oil absorbents based on melamine/lignin by a dip adsorbing method. ACS Sustainable Chem. Eng. 2015, 3, 3012-3018.
355
(10) Pham, V. H.; Dickerson, J. H. Superhydrophobic silanized melamine sponges as
356
high efficiency oil absorbent materials. ACS Appl. Mater. Interfaces 2014, 6, 14181-
357
14188.
358
(11) Shimizu, M.; Saito, T.; Isogai, A. Bulky quaternary alkylammonium counterions
359
enhance the nanodispersibility of 2,2,6,6-tetramethylpiperidine-1-oxyl-oxidized
360
cellulose in diverse solvents. Biomacromolecules 2014, 15, 1904-1909.
20
ACS Paragon Plus Environment
Page 20 of 25
Page 21 of 25
Journal of Agricultural and Food Chemistry
361
(12) Lei, Z.; Zhang, G.; Deng, Y.; Wang, C. Thermoresponsive melamine sponges
362
with switchable wettability by interface-initiated atom transfer radical polymerization
363
for oil/water separation. ACS Appl. Mater. Interfaces 2017, 9, 8967-8974.
364
(13) Cheng, W.; Liu, G.; Wang, X.; Han, L. Adsorption removal of glycidyl esters
365
from palm oil and oil model solution by using acid-washed oil palm wood-based
366
activated carbon: kinetic and mechanism study. J. Agric. Food Chem. 2017, 65, 9753-
367
9762.
368
(14) Li, D.; Zhu, F. Z.; Li, J. Y.; Na, P.; Wang, N. Preparation and characterization of
369
cellulose fibers from corn straw as natural oil sorbents. Ind. Eng. Chem. Res. 2013, 52,
370
516-524.
371
(15) Wang, B.; Karthikeyan, R.; Lu, X. Y.; Xuan, J.; Leung, M. K. H. Hollow carbon
372
fibers derived from natural cotton as effective sorbents for oil spill cleanup. Ind. Eng.
373
Chem. Res. 2013, 52, 18251-18261.
374
(16) Fumagalli, M.; Sanchez, F.; Boisseau, S. M.; Heux, L. Gas-phase esterification
375
of cellulose nanocrystal aerogels for colloidal dispersion in apolar solvents. Soft Matter
376
2013, 9, 11309-11317.
377
(17) Liao, H.; Zhang, H.; Hong, H.; Li, Z.; Qin, G.; Zhu, H.; Lin, Y. Novel cellulose
378
aerogel coated on polypropylene separators as gel polymer electrolyte with high ionic
379
conductivity for lithium-ion batteries. J. Membr. Sci. 2016, 514, 332-339.
380 381
(18) Zhuo, X.; Liu, C.; Pan, R.; Dong, X.; Li, Y. Nanocellulose mechanically isolated from amorpha fruticosa linn. ACS Sustainable Chem. Eng. 2017, 5, 4414-4420. 21
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
382
(19) Yu, M.; Li, J.; Wang, L. Preparation and characterization of magnetic carbon
383
aerogel from pyrolysis of sodium carboxymethyl cellulose aerogel crosslinked by iron
384
trichloride. J. Porous Mater. 2016, 23, 997-1003.
385
(20) Rege, A.; Schestakow, M.; Karadagli, I.; Ratke, L.; Itskov, M. Micro-mechanical
386
modelling of cellulose aerogels from molten salt hydrates. Soft Matter 2016, 12, 7079-
387
7088.
388
(21) Jiang, J.; Zhang, Q.; Zhan, X.; Chen, F. Renewable, biomass-derived,
389
honeycomblike aerogel as a robust oil absorbent with two-way reusability. ACS
390
Sustainable Chem. Eng. 2017, 5, 10307-10316.
391
(22) Liao, Q.; Su, X.; Zhu, W.; Hua, W.; Qian, Z.; Liu, L.; Yao, J. Flexible and durable
392
cellulose aerogels for highly effective oil/water separation. RSC Adv. 2016, 6, 63773-
393
63781.
394 395
(23) Jiang, F.; Hsieh, Y. L. Cellulose nanocrystal isolation from tomato peels and assembled nanofibers. Carbohydr. Polym. 2015, 122, 60-68.
396
(24) Zhang, H.; Li, Y.; Xu, Y.; Lu, Z.; Chen, L.; Huang, L.; Fan, M. Versatile
397
fabrication of a superhydrophobic and ultralight cellulose-based aerogel for oil spillage
398
clean-up. Phys. Chem. Chem. Phys. 2016, 18, 28297-28306.
399
(25) Sai, H.; Fu, R.; Xing, L.; Xiang, J.; Li, Z.; Li, F.; Zhang, T. Surface modification
400
of bacterial cellulose aerogels' web-like skeleton for oil/water separation. ACS Appl.
401
Mater. Interfaces 2015, 7, 7373-7281.
22
ACS Paragon Plus Environment
Page 22 of 25
Page 23 of 25
Journal of Agricultural and Food Chemistry
402
(26) Nemoto, J.; Saito, T.; Isogai, A. Simple freeze-drying procedure for producing
403
nanocellulose aerogel-containing, high-performance air filters. ACS Appl. Mater.
404
Interfaces 2015, 7, 19809-19815.
405 406
(27) Mulyadi, A.; Zhang, Z.; Deng, Y. Fluorine-free oil absorbents made from cellulose nanofibril aerogels. ACS Appl. Mater. Interfaces 2016, 8, 2732-2740.
407
(28) Jiang, F.; Hsieh, Y. L. Dual wet and dry resilient cellulose II fibrous aerogel for
408
hydrocarbon–water separation and energy storage applications. ACS Omega 2018, 3,
409
3530-3539.
410
(29) Hu, Z.; Berry, R. M.; Pelton, R.; Cranston, E. D. One-pot water-based
411
hydrophobic surface modification of cellulose nanocrystals using plant polyphenols.
412
ACS Sustainable Chem. Eng. 2017, 5, 5018-5026.
413
(30) Dash, R.; Elder, T.; Ragauskas, A. J. Grafting of model primary amine
414
compounds to cellulose nanowhiskers through periodate oxidation. Cellulose 2012, 19,
415
2069-2079.
416
(31) Taipina; Oliveira, M. D.; Ferrarezi, F.; Maria, M.; Yoshida, P.; Valeria, I.;
417
Goncalves; Carmo, M. D. Surface modification of cotton nanocrystals with a silane
418
agent. Cellulose 2013, 20, 217-226.
419
(32) Alatalo, S. M.; Pileidis, F.; Makila, E.; Sevilla, M.; Repo, E.; Salonen, J.;
420
Sillanpaa, M.; Titirici, M. M. Versatile cellulose-based carbon aerogel for the removal
421
of both cationic and anionic metal contaminants from water. ACS Appl. Mater.
422
Interfaces 2015, 7, 25875-25883. 23
ACS Paragon Plus Environment
Journal of Agricultural and Food Chemistry
423
(33) Feng, J.; Le, D.; Nguyen, S. T.; Tan Chin Nien, V.; Jewell, D.; Duong, H. M.
424
Silica cellulose hybrid aerogels for thermal and acoustic insulation applications.
425
Colloids Surf., A 2016, 506, 298-305.
426
(34) Yang, H.; Sheikhi, A.; Tg, V. D. V. Reusable green aerogels from crosslinked
427
hairy nanocrystalline cellulose and modified chitosan for dye removal. Langmuir 2016,
428
32, 11771-11779.
429
(35) Jiang, F.; Hsieh, Y. L. Cellulose nanofibril aerogels: synergistic improvement of
430
hydrophobicity, strength, and thermal stability via cross-linking with diisocyanate.
431
ACS Appl. Mater. Interfaces 2017, 9, 2825-2834.
432 433
(36) Jiang, F.; Hsieh, Y. L. Amphiphilic superabsorbent cellulose nanofibril aerogels. J. Mater. Chem. A, 2014, 2, 6337-6342.
434
(37) Huang, X.; Wang, A.; Xu, X.; Liu, H.; Shang, S. Enhancement of hydrophobic
435
properties of cellulose fibers via grafting with polymeric epoxidized soybean oil. ACS
436
Sustainable Chem. Eng. 2016, 5, 1619-1627.
437 438 439 440 441 442
24
ACS Paragon Plus Environment
Page 24 of 25
Page 25 of 25
443
Journal of Agricultural and Food Chemistry
TOC Graphic
444
25
ACS Paragon Plus Environment