Subscriber access provided by ECU Libraries
Surfaces, Interfaces, and Applications
Spraying fabrication of durable and transparent coatings for anti-icing application: dynamic water repellency, icing delay, and ice adhesion Yizhou Shen, Yu Wu, Jie Tao, Chunling Zhu, Haifeng Chen, Zhengwei Wu, and Yuehan Xie ACS Appl. Mater. Interfaces, Just Accepted Manuscript • DOI: 10.1021/acsami.8b19225 • Publication Date (Web): 27 Dec 2018 Downloaded from http://pubs.acs.org on January 2, 2019
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1 2 3 4
Spraying fabrication of durable and transparent coatings for anti-icing application: dynamic water repellency, icing delay, and ice adhesion
5 6 7
Yizhou Shen,†,* Yu Wu,† Jie Tao,†,* Chunling Zhu,§ Haifeng Chen,‡ Zhengwei Wu,†
8
Yuehan Xie,†
9 10 11
†
12
Astronautics, Nanjing 210016, P. R. China
13
‡
14
2nd Road, Huzhou 313000, P. R. China
15
§
16
Astronautics, Nanjing 210016, P. R. China
College of Materials Science and Technology, Nanjing University of Aeronautics and
Department of Materials Chemistry, Qiuzhen School, Huzhou University, 759, East
College of Aerospace Engineering, Nanjing University of Aeronautics and
17 18 19
* Professor Jie Tao, E-mail:
[email protected]. A/Professor Yizhou Shen, E-mail:
[email protected].
20 21
KEYWORDS: coatings; spraying; water repellency; icephobicity; durability
22 1
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 2 of 36
1
ABSTRACT: Anti-icing/icephobic coatings, typically applied in the form of surface
2
functional materials, are considered to be an ideal selection to solve the icing issues
3
faced by daily life and industrial production. However, the applications of anti-icing
4
coatings are greatly limited by the two main challenges: bonding strength with
5
substrates and stability of the high anti-icing performance. Here, we designed and
6
fabricated a kind of high-performance superhydrophobic fluorinated silica (F-
7
SiO2)@polydimethylsiloxane (PDMS) coatings, and further emphasized the
8
improvement of the bonding strength with substrates and the maintenance of high anti-
9
icing performance. The resultant coatings exhibited excellent water repellency with a
10
contact angle up to 155.3° and a very short contact time (~10.2 ms) of impact droplets.
11
At low temperatures, the coming droplets still rapidly rebounded off the coating surface,
12
and the superhydrophobic coatings displayed a more than fiftyfold increase of freezing
13
time comparing with bare aluminum. The ice adhesion strength on the coatings was
14
only 26.3 kPa, which was far less than that (821.9 kPa) of bare aluminum. Furthermore,
15
the nanoporous structures constructed by anodic oxidation could tremendously enhance
16
the bonding strength of the coatings with substrate, which was evaluated through a
17
standard method (ASTM D3359). The anti-icing properties still retained high stability
18
under the conditions of 30 icing/deicing cycles, soaking and scouring of acid solution
19
(pH=5.6). This work can effectively push the anti-icing coatings towards a real-world
20
application.
21
2
ACS Paragon Plus Environment
Page 3 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
INTRODUCTION
2
Icing is a natural phenomenon, which usually occurs in many infrastructures and
3
industrial products including power lines, buildings, and aircrafts, etc, and finally gives
4
rise to severe safety issues and enormous economic losses.1,2 Up till now, a variety of
5
strategies have been applied to prevent ice formation / accretion and remove ice, such
6
as melting-ice agents,3 mechanical vibration,4 vapor heating, and electro-thermally
7
melting.5 However, these active approaches are costly, design-complex, and also
8
considered to be not environment-friendly. The continuous vibration or thermal cycle
9
certainly affects the service life of surface function materials, therefore these strategies
10
should be avoided or minimized in the future whenever possible. As an alternative,
11
passive anti-icing materials have received widespread attentions in the last decade due
12
to its “zero-energy” consumption,6-9 and it is considered to conform to the three typical
13
features: excellent superhydrophobicity to repel the coming supercooled droplets,
14
outstanding icing delay performance (or lower icing temperature), and ultralow ice
15
adhesion.10-12 As well known, freezing is an inevitable process under the condition of
16
sufficient supercooling, and the ultralow ice adhesion strength can allow the ice to be
17
readily removed with the assistance of external force or even wind-force and self-
18
gravity.13,14
19
Currently, there are two main strategies to design the anti-icing materials, i.e.,
20
microscopic rough superhydrophobic surfaces and slippery liquid-infused porous
21
surfaces (denoted as SLIPS).15-18 Based on the ultra-slippery characteristic and
3
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 36
1
chemical homogeneity, the SLIPS exhibit the extremely low wetting hysteresis and ice
2
adhesion strength.19,20 However, the SLIPS still face great challenges for practical
3
application due to the key limitation, where the infused lubricant is usually expensive
4
and prone to be damaged by mechanical abrasion or several icing/deicing cycles.21,22
5
Considering a typical ice formation and accretion process, supercooled droplets will
6
firstly wet the solid surface and rapidly freeze into ice.23 In this case, superhydrophobic
7
surfaces (contact angle (CA) > 150° and sliding angle (SA) < 10°) are naturally
8
considered to be the ideal candidates as the anti-icing materials.24 It has been widely
9
reported that the superhydrophobicity is caused by the trapped air pockets inside the
10
surface micro-nanostructures. Meanwhile, the air pockets can effectively act as a
11
thermal barrier between solid surface and supercooled water droplet to delay the
12
freezing process. Even if ice can be formed on the solid surface, the special solid-ice
13
interfacial state will result in an ultralow ice adhesion strength.25 According to the
14
previous report, Li et al. prepared the superhydrophobic Co3O4 surface by employing
15
solvothermal treatment to in-situ construct micro-nanostructures, and the resultant
16
surface exhibited excellent anti-icing property with icing-delay time of more than 1 h
17
at about -5 °C.26 Also, the superhydrophobic aluminum surface prepared by Chen et al.
18
through a combination method of anodizing in H2SO4 solution and etching in myristic
19
acid can greatly reduce the ice adhesion strength to 65 kPa.27 However, the in-situ
20
constructed micro-nanostructures on superhydrophobic surfaces are also a huge
21
challenge to resist the mechanical abrasion or the scour of freezing rain.
4
ACS Paragon Plus Environment
Page 5 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
Based on the excellent icephobicity of superhydrophobic materials, many
2
researchers have preferred to prepare the superhydrophobic coatings for the anti-icing
3
purpose, because the coatings matrix can play a supporting role in the immobilization
4
of surface microstructures, and enhances the ability to resist the mechanical abrasion or
5
damage. Ruan et al. adopted polytetrafluoroethylene (PTFE) to fabricate hierarchical
6
microstructures on polydimethylsiloxane (PDMS), and finally prepared the
7
superhydrophobic PTFE/PDMS coatings, where the high icephobicity was maintained
8
well under the conditions of mechanical abrasion.28 Furthermore, a kind of porous
9
superhydrophobic polyvinylidene difluoride (PVDF) coatings were fabricated through
10
a method of phase separation, and the as-prepared superhydrophobic coatings were
11
confirmed to possess higher icephobicity with the great ability to resist the scour of
12
supercooled water droplets for ~50 min.29 Despite a notable progress being made on
13
the superhydrophobic anti-icing coatings, studies on the durability (such as coatings
14
adhesive force with substrate, maintenance of icephobicity under multiple icing/deicing
15
cycles, and soaking and scouring of acid solution) are still insufficient, yet these are of
16
vital importance for applications.30,31
17
In this work, we firstly fluoridized the SiO2 nanoparticles, which were further
18
sprayed onto the PDMS coating matrix to obtain the superhydrophobic F-SiO2@PDMS
19
coatings. Meanwhile, the coatings bonding strength with substrate was contrastively
20
investigated with the two types (nanopores and nanopits) of nanostructures on the
21
aluminum. The icephobicity was systematically discussed and evaluated around the
22
three aspects of dynamic water repellency, icing-delay time, and ice adhesion. 5
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 36
1
Additionally, the durability of superhydrophobic F-SiO2@PDMS coatings was verified
2
under the conditions of 30 icing/deicing cycles, soaking and scouring of acid solution.
3
EXPERIMENTAL SECTION
4
Materials
5
Silica nanoparticles (20 nm, 99.0%) were supplied by Nanjing XFNANO Materials
6
Tech. Co., Ltd. Polydimethylsiloxane (PDMS) prepolymer (Sylgard 184A) and the
7
corresponding curing agent (Sylgard 184B) were obtained from Dow Corning Co., Ltd
8
(USA).32 1H,1H,2H,2H-Perfluorodecyltriethoxysilane (PFDTES, 96%) was purchased
9
from Shanghai Macklin Biochemical Co., Ltd. Anhydrous ethanol (99.7%), ammonium
10
hydroxide (25.0-28.0 wt%), and tetrahydrofuran (THF, 99.0%) were provided by
11
Sinopharm Chemical Reagent Co., Ltd. Aluminum sheets (20 mm × 20 mm × 1 mm)
12
were bought from Shenzhen Baogang Metal Co., Ltd. All chemical reagents were used
13
directly without further purification in present work. Deionized water used throughout
14
experiments was prepared in Milli-Q system in our laboratory.
15
Pretreatment of aluminum sheets
16
First, the aluminum sheets were cleaned ultrasonically with acetone and alcohol for
17
15 min in sequence, followed by drying under a stream of nitrogen. Second, two
18
common techniques were utilized to treat clean aluminum sheets and produce the
19
corresponding nanostructures. One treatment: the clean aluminum sheets were 6
ACS Paragon Plus Environment
Page 7 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
chemically etched in the solution of 1.5 M HCl for 10 min to construct the nanopits
2
structures. Another treatment: the anodic oxidation was performed in the solution of
3
120 g L-1 H3PO4 with the processing parameters of 10 V applied voltage and 20 min,
4
and the nanopores structures were grown on the surface of aluminum sheets.
5
Subsequently, the nanostructured aluminum sheets were washed with alcohol and dried
6
under nitrogen flow.
7
Fabrication of PDMS coatings matrix
8
PDMS (3 g) and curing agent (0.3 g) were dissolved in 25 mL THF under vigorous
9
stirring for 60 min. Following this, the mixed solution was coated onto the treated
10
aluminum sheets by means of airbrush at 0.4 MPa and with a distance of 10-15 cm.
11
After being cured in 80 °C oven for 2 h, the PDMS coatings matrix were finally
12
synthesized, and would be used in the following experiment procedures.
13
Preparation of superhydrophobic F-SiO2@PDMS coatings
14
Regarding the modification of SiO2 nanoparticles, PFDTES (0.6 mL) was firstly
15
mixed with ethanol (80 mL), and the solution system was kept with the constant stirring
16
for 60 min. Afterwards, 4 mL ammonium hydroxide was diluted to 20 mL with DI
17
water, and then 3 g SiO2 nanoparticles were added into the solution to form
18
homogeneous SiO2 suspension for the continuously ultrasonic-dispersion time of 10
19
min. The SiO2 suspension would be slowly transferred into the above-prepared
20
PFDTES solution followed by continuous magnetic stirring for 24 h at 40 °C. The
21
resultant precipitate was further centrifuged at 10000 rpm for 5 min, and the products 7
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 8 of 36
1
finally were washed with ethanol for twice. It was necessary to take the vacuum dried
2
treatment for obtaining the hydrophobic SiO2 nanoparticles, which were labelled as F-
3
SiO2.
4
Subsequently, 0.2 g F-SiO2 nanoparticles were ultrasonically dispersed into 25 mL
5
THF solution for 30 min. Following this, the mixed system was sprayed on the PDMS
6
coating matrix, which was pre-cured at 80 °C for 10 min (the other steps were same as
7
ones for PDMS coatings matrix). The superhydrophobic F-SiO2@PDMS coatings were
8
obtained after the further curing at 80 °C for another 2 h.
9
Characterizations and water repellent tests
10
The surface morphologies of PDMS coatings matrix and superhydrophobic F-
11
SiO2@PDMS coatings with a thin gold layer were captured by Field-Emission
12
Scanning Electron Microscope (FE-SEM, Hitachi S4800, Japan) at an acceleration
13
voltage of 5.0 kV. Energy Dispersive Spectrometer (EDS) attached to FE-SEM
14
instrument was utilized to analyze element compositions of coatings. The surface
15
groups and chemical compositions of F-SiO2 nanoparticles were directly detected by
16
Fourier Transform Infrared spectrometer (FTIR, Nexus 670, USA) and X-ray
17
photoelectron spectrometer (XPS, K-Alpha, USA), respectively. The surface 3D
18
topography and roughness were obtained from Atomic Force Microscope (AFM, NT-
19
MDT Prima, Russia) in tapping mode with a scan area of 6 μm × 6 μm. Both water
20
Contact Angle (CA) and Contact Angle Hysteresis (CAH) were measured with a
21
contact angle measured system (JC2000D2, Shanghai Zhongchen Digital Technology 8
ACS Paragon Plus Environment
Page 9 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
Apparatus Co., Ltd, China) using a 4 μL volume of DI water droplet. Water contact
2
angle (CA) could be directly obtained by the contact angle analyzer. Advancing CA
3
was recorded by the computer, when the contact area with surface changed owing to
4
expansion of droplet. If the contact area decreased via shrinking the droplet, Receding
5
CA could be recorded. CAH was the difference of Advancing CA and Receding CA.
6
Therefore, CAH can be calculated from the directly tested values. Furthermore, five
7
different locations of the sample coatings were measured for obtaining an average value.
8
Evaluations of anti-icing performance
9
Regarding the dynamic water repellency, the reference droplet (4 μL) fell from the
10
height of 5 cm under the action of gravity and impacted onto the sample surface at 1 m
11
s-1. In the process of free falling and impacting, the movement and deformation of water
12
droplet were captured by a high-speed camera (i-SPEED 713, UK) at 5000 frames per
13
second.
14
According to our previous report,33 the icing-delay test was performed in a custom-
15
built device controlled at -15 °C, which consisted of cooling system, sample chamber,
16
and monitoring system (including camera and computer). Droplets (4 μL) were dropped
17
on the coatings surface after the test specimen was placed on cooling stage for 5 min.
18
This made sure that the surface temperature was same as the temperature of cooling
19
stage. Subsequently, the freezing time and process of the reference droplet were record
20
by monitoring system.
9
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 10 of 36
1
The ice adhesion strength test was carried out with home-made system, as shown
2
in Figure S1, and the corresponding operation process was described as follows. The
3
coated substrate was placed on and faced to a cuvette (1 cm × 1 cm × 4.5 cm) with full
4
of DI water. The setup was then kept in a refrigerator at -20 °C for 12 h to form the ice
5
columns on the coatings surface. Subsequently, the sample with ice column was fixed
6
on the cold stage, and a digital force transducer (HANDPI Instruments Co., Ltd, China)
7
pushed the ice column to separate it from the coatings surface. The peak force (Fm) was
8
acquired directly from force transducer, and the ice adhesion strength (τice) could be
9
calculated by:
10
𝜏𝑖𝑐𝑒 =
𝐹𝑚 𝐴
(1)
11
Where A is the contact area between coatings surface and ice column, which was kept
12
in a constant value of 1 cm2. At least three parallel samples were measured to obtain an
13
average value.
14
RESULTS AND DISCUSSION
15
Chemical composition of F-SiO2 nanoparticles
16
Grafting low-energy groups onto the surface of SiO2 nanoparticles will benefit the
17
bonding with PDMS coatings matrix, where the firm chemical covalent bonds can be
18
formed to enhance the bonding strength. The FTIR spectra of SiO2 nanoparticles before
19
and after modifying are shown in Figure 1a. Therein, a distinct peak at 1618.6 cm-1 of
20
the both FTIR spectra indicates the existence of H2O from air.34 After modifying the 10
ACS Paragon Plus Environment
Page 11 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
SiO2 nanoparticles, these characteristic peaks at 3418.4 cm-1 (caused by -OH stretching
2
vibrations35), 947.7 cm-1 (corresponding to -OH out of plane bending36), 1111.6 cm-1
3
(belonging to Si-O-Si asymmetric stretching vibrations37), and 800.7 cm-1 (belonging
4
to Si-O-Si bending mode38) have an enhanced intensity comparing with raw SiO2
5
nanoparticles. The appeared -OH and Si-O-Si are mainly generated owing to the
6
hydrolysis of PFDTES and self-assembly of PFDTES on the surface of SiO2
7
nanoparticles, respectively. More importantly, the as-modified SiO2 nanoparticles (F-
8
SiO2) have a new chemical bond and locate around 1198.7 cm-1, which corresponds to
9
the C-F stretching vibration of -CF2- and -CF3 function groups.39 This C-F chemical
10
bond is derived from PFDTES molecules, which further demonstrates the successful
11
grafting of low-energy groups.
12 13
Figure 1. (a) FTIR spectra and (b) XPS survey spectra of SiO2 nanoparticles before
14
(blue line) and after (red line) modifying. (c-f) The XPS high-revolution spectra of F-
15
SiO2 nanoparticles for Si 2p, O 1s, C 1s, and F 1s, respectively.
11
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 36
1
Furthermore, XPS spectra were obtained to further confirm the surface chemical
2
compositions of raw SiO2 and F-SiO2 nanoparticles. As shown in Figure 1b, the
3
modification of SiO2 nanoparticles with PFDTES further increases the intensity of Si
4
2p and O 1s peaks. Also, the Si 2p high-resolution spectrum can be resolved into four
5
components assigned to Si-C (at 100.8 eV), Si-O (at 102.6 eV), Si-O-Si (at 103.4 eV),
6
and Si-OH (at 104.5 eV), respectively (see Figure 1c).40 All these Si-C components
7
originate from PFDTES, while the Si-O (at 284.8 eV), Si-O-Si (at 288.5 eV), and Si-
8
OH (at 290 eV) are the newly formed chemical covalent bonds between PFDTES and
9
SiO2 nanoparticles. Furthermore, the O 1s peaks are located at 532.1 eV, 533.7 eV and
10
540.0 eV, and mainly assigned to the oxygen of -OH, SiO2 and CO2, respectively, as
11
shown in Figure 1d. It is clear that there are four components in C 1s high-resolution
12
spectrum (see Figure 1e), which are located at 284.0 eV (C-C/C-H), 285.6 eV (C-Si),
13
292.0 eV (C-F), and 288.8 eV (C=O). The bonds of C-C/C-H, C-Si and C-F are ascribed
14
to PFDTES molecules, and C=O attributed to CO2 from air.41 Notably, it can be seen
15
that the F element only exists on the surface of the F-SiO2 nanoparticles (see Figure 1f).
16
This prominent peak is associated with the -CF2- (at 689.3 eV) and -CF3 (at 684.9 eV)
17
groups of PFDTES molecules, which have low surface energy and endow the F-SiO2
18
nanoparticles with excellent hydrophobicity.42 These analyzed results also indicate the
19
polycondensation reactions take place to form the new chemical covalent bonds
20
between PFDTES molecules and SiO2, which is in a line with FTIR analysis.
21
Non-wettability and morphologies of the superhydrophobic F-SiO2@PDMS
22
coatings 12
ACS Paragon Plus Environment
Page 13 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
The high-dispersibility F-SiO2 nanoparticles in THF solution will be sprayed onto
2
the semi-cured PDMS coatings matrix to increase the surface microscopic roughness.
3
As a response, the non-wettability is also greatly enhanced and shown in Figure 2.
4
Comparing with the intrinsic hydrophilicity of bare aluminum substrate, the non-
5
wettability of smooth PDMS coatings is enhanced and reaches the category of
6
hydrophobicity with CA increasing from 79.4° to 113.9° (see Figure 2a and b), because
7
the PDMS materials have lower surface free energy. With addition of F-SiO2
8
nanoparticles, the excellent superhydrophobicity is obtained on the surface of the F-
9
SiO2@PDMS, and the CA reaches 155.3° and the CAH reduces to 2° (see Figure 2c).
10
This mainly attributes to the microscopic rough structures caused by the F-SiO2
11
nanoparticles, as shown in Figure 2d and e. The as-formed microstructures evenly
12
distribute on the surface of PDMS coatings matrix, and the spacing distance between
13
the adjoining micropits is approximately 50 μm. Meanwhile, it can be found that the
14
PDMS coatings matrix has a strong supporting action on the microstructures, and there
15
are many nanoscale pores inside the microstructures (see inset in Figure 2e). Also, the
16
3D topography in Figure 3a exhibits lots of microscopic protuberances and cavities. It
17
can be calculated from 2D image that the root-mean-square roughness (RMS) is about
18
229.5 nm (see Figure 3c), showing the great size effect of microstructures on
19
superhydrophobicity. Besides, the EDS analyzed results (see Figure S2) further confirm
20
that the surface of F-SiO2@PDMS coatings has been successfully treated with low
21
surface free energy by grafting fluorine-containing groups original from PFDTES.43
22
Finally, the synergistic action of microscopic rough structures and low surface free 13
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 36
1
energy can induce to entrap numerous air pockets underneath water droplets, and make
2
the coatings water-repellent.
3 4
Figure 2. The photographs of 8 μL water droplets on (a) aluminum sheet, (b) PDMS
5
coatings, and (c) superhydrophobic F-SiO2@PDMS coatings. Insets are 4 μL droplets
6
for measuring CA and CAH. (d) SEM images of PDMS coatings and (e)
7
superhydrophobic F-SiO2@PDMS coatings, and inset is the high-resolution image.
14
ACS Paragon Plus Environment
Page 15 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1 2
Figure 3. (a) AFM 3D surface topography, (b) corresponding 2D image, and (c) section
3
roughness profile extracted from 2D image of the superhydrophobic F-SiO2@PDMS
4
coatings.
5
The water droplet almost suspends on the surface of superhydrophobic F-
6
SiO2@PDMS coatings. This phenomenon has been well elucidated by the Cassie-
7
Baxter wetting model, indicating that the microscopic rough structures further reduce
8
the apparent surface free energy to repel water. In this case, the apparent contact
9
interface is actually composed of solid/liquid and liquid/gas. Since the CA of a water
10 11
droplet on air is considered as 180°, the apparent CA (θ*) can be expressed as:
cos * f cos f 1
(2)
12
Where f and θ are the area fraction and Young CA of the solid, respectively. The
13
microscopic rough structures produced by F-SiO2 nanoparticles have a high aspect ratio, 15
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 36
1
which results in a large amount of air pockets being trapped. Reducing the solid contact
2
area fraction f (i.e., capturing more air pockets) is beneficial to the improvement of the
3
water repellency. When the F-SiO2 nanoparticles with suitable quantity is added into
4
the PDMS coatings matrix, the resultant microstructures can almost perfectly hold up
5
the water droplet, causing the ideal superhydrophobicity with the CA up to 155.3° and
6
the CAH of only 2°.
7
Enhancement of adhesion strength with substrates
8
The adhesion of superhydrophobic F-SiO2@PDMS coatings to substrate materials
9
was measured according to the standard method of ASTM D3359 and divided into
10
different grades from best adhesion to worst adhesion (denoted as 5B, 4B, 3B, 2B, 1B,
11
and 0B).44 As a reference, the fact that nearly 50% of the coating is removed by test
12
tape is considered to be classified as 3B. In order to enhance the adhesion strength of
13
the coatings, we performed anodic oxidation and chemical etching on the aluminum
14
substrate to produce the microscopic rough structures. It can be observed that there is a
15
layer of nanoporous (treated by anodic oxidation) and nano-ravine (treated by chemical
16
etching) structures evenly distributing on the aluminum substrate, respectively, as
17
shown in right column of Figure 4. Even though the produced nano-ravine structures
18
increase the roughness to a certain extent, the adhesion of the as-prepared
19
superhydrophobic coatings has no obvious enhancement with a major removal from the
20
chemically-etched substrate. According to the experimental results, the adhesion
21
strength only belongs to 2B grade. While there is no removal of the superhydrophobic 16
ACS Paragon Plus Environment
Page 17 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
F-SiO2@PDMS coatings on the anodized aluminum after tape peeling off, indicating
2
that the superhydrophobic coatings have a better adhesion which is rated as 5B. This is
3
also evident from SEM images that the anodic oxidation greatly increases the
4
microscopic roughness of the aluminum substrate, and a large number of nanopores
5
appear on the surface. These nanoporous structures play an anchoring role between the
6
superhydrophobic F-SiO2@PDMS coatings and substrate. Consequently, anodic
7
oxidation on the aluminum substrate is needed to enhance the adhesion strength of the
8
as-prepared superhydrophobic F-SiO2@PDMS coatings.
9 10
Figure 4. Cross-cut tape adhesion test for superhydrophobic F-SiO2@PDMS coatings
11
on the aluminum substrate with different treating types. T1: untreated aluminum
12
substrate; T2: anodic oxidation; T3: chemically etching. Left column is the actual
13
experimental images, and middle column is the schematic drawing of the test results
14
(red parts stand for the coatings not removed from the substrate). Right column is the
15
corresponding microscopic morphology.
17
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1
Page 18 of 36
Dynamic water repellency
2
Dynamic water repellency is considered to be first element to anti-icing materials,
3
because it reflects the capacity of repelling the coming supercooled droplets. Dynamic
4
water repellency is mainly evaluated by the contact time and contact process of impact
5
droplets on the sample surface. Here, two important dimensionless parameters are the
6
Weber number (We) and the Reynolds number (Re), which are defined as follows:
7
𝑊𝑒 =
8
𝑅𝑒 =
𝜌𝐷0𝑉2
(3)
σ
𝜌𝐷0𝑉
(4)
𝜇
9
where ρ is the liquid density (1 g cm-3), σ is the liquid-gas interfacial tension (72 mN
10
m-1), V is the impact speed, μ is the liquid viscosity (1.0×10-3 Pa s), and D0 denotes the
11
initial diameter of droplet.45 The droplet with a radius of 1 mm impacts onto the surface
12
at a speed of 1 m s-1, therefore it is calculated that We is approximately 27.8, and Re is
13
around 2234.9 in this work. As shown in Figure 5a and Video S1, it takes a certain
14
amount of time (3.6 ms and 2.8 ms, respectively) for the impact droplet to spread to the
15
maximum deformation on the bare aluminum and PDMS coatings. Comparing with that
16
on bare aluminum, the spreading droplet on PDMS coatings has a higher retracting
17
degree owing to the relatively low surface energy of PDMS coatings.46 However, the
18
impact droplet fails to rebound off the surface of PDMS coatings. With the gradual
19
decrease of temperature, the impact droplet is more difficult to rebound off the PDMS
20
coatings, as shown in Figure 6. In contrast, for the superhydrophobic F-SiO2@PDMS
21
coatings, the impact droplet spreads rapidly (only 2.4 ms) and completely rebounds off
22
with a retracting time of 7.8 ms. Therefore, the entire contact time of the impact droplet 18
ACS Paragon Plus Environment
Page 19 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
is 10.2 ms from the contact to the detachment. Even at lower temperatures of -5 °C and
2
-10 °C (Figure 6), the impact droplet can also rebound off the surface of
3
superhydrophobic F-SiO2@PDMS coatings, which strongly demonstrated the superior
4
dynamic water repellency at low temperature.
5 6
Figure 5. (a) Time-lapse photographs of 4 μL water droplets impacting on bare
7
aluminum (S1), PDMS coatings (S2) and superhydrophobic F-SiO2@PDMS coatings
8
(S3) at room temperature. (b) The dimensionless parameter of spreading factor (D*=
9
D/D0, where D0 is the original diameter of droplet, and D is the diameter of droplet in
10 11
contact area with the surface) versus time after the droplet touched the surface. Furthermore, the spreading factor (D*) variation of the water droplets on the 19
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 36
1
sample surfaces was also calculated and shown in Figure 5b.47 For comparison, the
2
impact droplet on superhydrophobic F-SiO2@PDMS coatings goes through three stages
3
(spread, retract, and rebound), while it cannot rebound off two other surfaces (i.e., bare
4
substrate and PDMS coatings). Also, the droplet mobility parameter (ξ) is determined
5
by the ratio of D*min and D*max.
6
𝐷 ∗ 𝑚𝑖𝑛
𝜉 = 𝐷∗
(5)
𝑚𝑎𝑥
7
where D*max denotes the maximum droplet spreading diameter, and D*min is minimum
8
diameter of contact area after retracting.10 It can be obtained that the value of ξ on the
9
bare aluminum is approximately equal to one, yet the PDMS coatings present a lower
10
value of ξ=0.48, demonstrating the PDMS coatings causing higher droplet mobility.
11
However, the superhydrophobic F-SiO2@PDMS coatings can rapidly rebound off the
12
surface, and the value of ξ can be considered to be zero. Therefore, the
13
superhydrophobic F-SiO2@PDMS coatings exhibit greater dynamic water repellency,
14
which also declares the huge anti-icing potential.
15 16
Figure 6. Time-lapse photographs of 4 μL water droplets impacting on (S2) PDMS 20
ACS Paragon Plus Environment
Page 21 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
coatings and (S3) superhydrophobic F-SiO2@PDMS coatings at -5 °C and -10 °C.
2
Icing delay performance
3
To evaluate the anti-icing behavior, the icing process of water droplets on different
4
surfaces was record. As shown in Figure 7a, water droplet is turbid as soon as it touches
5
the bare aluminum, indicating the occurrence of ice nucleation. The droplet completely
6
freezes with a tip appearing on the droplet top after a short time of 4.8 s. The reason for
7
icing in a few seconds is its high thermal conductivity of 237 W m-1 K-1 without any
8
barriers to water droplet. In contrast, the PDMS coatings exhibit a freezing delay time
9
of more than 80 s with a long precooling time (~68.5 s). This phenomenon can be
10
mainly contributed to relatively low thermal conductivity of PDMS coatings (0.16 W
11
m-1 K-1). Therefore, the heat transfer process between substrate and water droplet is
12
greatly slowed down. Notably, the superhydrophobic F-SiO2@PDMS coatings show
13
longer freezing delay time of 276.2 s, compared with PDMS coatings (81.9 s) and bare
14
aluminum (4.8 s). On the whole, there are two reasons for these results. First, the
15
superhydrophobic F-SiO2@PDMS coatings have an apparent low-surface-energy
16
which greatly reduces the contact area between water droplet and substrate surface.
17
More importantly, the superhydrophobic coatings reach the Cassie-Baxter wetting state
18
and could entrap a large amount of air pockets underneath water droplet with ultralow
19
thermal conductivity of 0.024 W m-1 K-1.48 Actually, the interface wetting regime
20
(solid-liquid and solid-ice interfaces) is complex and depended on many factors, such
21
as size, morphology, temperature, etc. The presented work demonstrated that the 21
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 22 of 36
1
structure-designed superhydrophobic coatings can display a higher extend of icing
2
delay performance than some reported research results.49,50 As a consequence, the
3
superhydrophobic F-SiO2@PDMS coatings can greatly delay the icing process of water
4
droplet. Besides, it is worth noting that icing delay time primarily depends on
5
precooling process, as shown in Figure 7b. The above-mentioned results verify that the
6
superhydrophobic F-SiO2@PDMS coatings show great potential on delaying ice
7
formation.
8 9
Figure 7. (a) Sequential images of water droplets on (S1) bare aluminum, (S2) PDMS
10
coatings, and (S3) superhydrophobic F-SiO2@PDMS coatings. (b) Required time for
11
water droplets precooling, icing growing, and freezing on three sample surfaces.
12
Ice adhesion strength
13
Ice adhesion strength is another important parameter to characterize the icephobicity.
14
As shown in Figure 8a, the ice adhesion strength of PDMS coatings is much lower than
15
that of bare aluminum. This can be explained by that interfacial slippage provided by
16
the miscible chains has a great effect on ice adhesion strength.12 In particular, the
17
superhydrophobic F-SiO2@PDMS coatings with ice adhesion strength of 26.3 kPa have
18
a 96.8% reduction over bare aluminum. The ultralow ice adhesion strength is mainly 22
ACS Paragon Plus Environment
Page 23 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
caused by the existent air pockets, which have a significant reduction in contact area
2
between ice and solid surface. Additionally, the air pockets in the concaves are
3
squeezed by surrounding ice and generate strain force to the ice, which also reduces the
4
ice adhesion strength to a certain extent.51
5 6
Figure 8. (a) Ice adhesion strength of different sample surfaces. (b) The change of the
7
ice adhesion strength on the superhydrophobic F-SiO2@PDMS coatings with the
8
number of icing/deicing cycles. (c) Effect of HCl solution immersion time on the ice
9
adhesion strength of the superhydrophobic F-SiO2@PDMS coatings. (d) Variation in
10
ice adhesion strength with different volumes of HCl solution impacting.
11
It is necessary to investigate the stability of icephobicity. The repeated
12
icing/deicing experiments were conducted in ice adhesion test system. Data presented
13
in Figure 8b show that the ice adhesion has no obviously increasing trend over 30
14
icing/deicing cycles. This is due to that the immobilization of PDMS is effective to 23
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 24 of 36
1
improve robustness of superhydrophobic F-SiO2@PDMS coatings. We also performed
2
artificial rain erosion and scour through home-made devices. As shown in Figure 8c,
3
the coatings sustain at a relative low value of ice adhesion strength after immersing in
4
HCl solution for 48 h, implying that stable air pockets on the surface enable the high
5
corrosion resistance in HCl solution. It can be also found that superhydrophobic F-
6
SiO2@PDMS coatings still remain low ice adhesion strength after impinging by water
7
jet (7 mm diameter) at ~1 m s-1 (see Figure 8d). The excellent wash-out resistance of
8
coatings is related to the pinning and supporting action of PDMS, which guarantees the
9
F-SiO2 nanoparticles firmly cover on the surface. All the above experimental results
10
strongly prove that superhydrophobic F-SiO2@PDMS coatings have favorable
11
chemical stability and mechanical durability for extending their service life.
12
Anti-condensation property
13
Finally, the anti-condensation property was also evaluated, and the condensation
14
experiments were conducted on a horizontal cooling stage at 2 °C with the relative
15
humidity is 80%. As shown in Figure 9a-b, condensed droplets cover immediately the
16
aluminum and PDMS coatings and grow in size gradually. Comparing with that on
17
aluminum, the condensed droplets on PDMS coatings have a lower growth rate and
18
form the more regular spheres due to low surface energy. It is interesting to note that
19
condensed droplets do not fully cover superhydrophobic F-SiO2@PDMS coatings, and
20
they are sphere shape with different size after 30 min. The reason for this phenomenon
21
is that the adjacent metastable droplets coalesce and lots of fresh areas are exposed for 24
ACS Paragon Plus Environment
Page 25 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
reforming smaller droplets. Furthermore, it is obvious that the small condensed droplets
2
continue to combine into lager droplet without any external force and slide readily (see
3
Figure 9d), which is caused by the decreased surface energy during the coalescence
4
process. This coalescencing and sliding behaviors contribute to the anti-condensation
5
and self-cleaning of the superhydrophobic F-SiO2@PDMS coatings at low
6
temperatures.
7 8
Figure 9. Time-lapse photographs of condensed droplets on different surfaces,
9
including (a) bare aluminum, (b) PDMS coatings and (c) superhydrophobic F-
10
SiO2@PDMS coatings. (d) Dynamic optical micrographs of condensed droplets
11
showing the coalescence and slide behaviors on superhydrophobic F-SiO2@PDMS
12
coatings.
13
CONCLUSION
25
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 26 of 36
1
In summary, the superhydrophobic F-SiO2@PDMS coatings were successfully
2
fabricated by a facile spraying method, and the bonding strength to substrate materials
3
is greatly enhanced through anodizing pretreating of aluminum. In superhydrophobic
4
F-SiO2@PDMS coatings, high-viscous PDMS is introduced to bond and support F-
5
SiO2 nanoparticles. Due to the excellent superhydrophobicity, the coatings showed an
6
ultralow contact time (10.2 ms) of impact droplets at ambient temperature and could
7
compel water droplets to rebound off even at -10 °C. The superhydrophobic F-
8
SiO2@PDMS coatings displayed a more than fiftyfold increase of freezing time
9
comparing with bare aluminum. The ice adhesion strength on the coatings was only
10
26.3 kPa, which was far less than that (821.9 kPa) of bare aluminum. Finally, the anti-
11
icing properties still retained high stability under the conditions of 30 icing/deicing
12
cycles, soaking and scouring of acid solution (pH=5.6). This work is considered to be
13
effectively to push the anti-icing coatings towards a real-world application.
14
○s Supporting Information
15
Schematic diagram of ice adhesion test system; Element detection by EDS for PDMS
16
coatings and superhydrophobic F-SiO2@PDMS coatings. (PDF)
17
Video of the moving process of impact droplets on aluminum, PDMS coatings and
18
superhydrophobic F-SiO2@PDMS coatings. (AVI)
19
26
ACS Paragon Plus Environment
Page 27 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
AUTHOR INFORMATION
2
Corresponding Author
3
* Professor Jie Tao, Tel/Fax: +86-25-5211 2911. E-mail:
[email protected].
4
A/Professor Yizhou Shen, Tel: +86-25-5211 2911. E-mail:
[email protected].
5
Present Addresses
6
†
7
Astronautics, Nanjing 210016, P. R. China
8
‡
9
2nd Road, Huzhou 313000, P. R. China
College of Materials Science and Technology, Nanjing University of Aeronautics and
Department of Materials Chemistry, Qiuzhen School, Huzhou University, 759, East
10
§
11
Nanyang Avenue 50, Singapore 639798
12
Notes
13
The authors declare no competing financial interest.
14
ACKNOWLEDGMENTS
15
J.T., Y.S. and C.Z. acknowledge financial support from the National Natural Science
16
Foundation of China (No. 51671105, 51705244, 11832012). Y.S. and Y.W. thank the
17
support of the Natural Science Foundation of Jiangsu Province (No. BK20170790), and
18
H.C. acknowledges the General Project of Zhejiang provincial department of education
19
(Y201737320). Z.W. and Y.X. thank the Project Funded by the Priority Academic
School of Materials Science and Engineering, Nanyang Technological University,
27
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 28 of 36
1
Program Development of Jiangsu Higher Education Institutions and the NUAA
2
Innovation Program for Graduate Education (kfjj20170608, kfjj20180609).
28
ACS Paragon Plus Environment
Page 29 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
Note and references
2
(1) Meuler, A. J.; McKinley, G. H.; Cohen, R. E. Exploiting Topographical Texture to
3 4 5
Impart Icephobicity. ACS Nano 2010, 4, 7048-7052. (2) Lv, J.; Song, Y.; Jiang, L.; Wang, J. Bio-inspired Strategies for Anti-icing. ACS Nano 2014, 8, 3152-3169.
6
(3) Cancilla, D. A.; Martinez, J.; Van aggelen, G. C. Detection of Aircraft
7
Deicing/antiicing Fluid Additives in a Perched Water Monitoring Well at an
8
International Airport. Environ. Sci. Technol. 1998, 32, 3834-3835.
9
(4) Habibi, H.; Cheng, L.; Zheng, H.; Kappatos, V.; Selcuk, C.; Gan, T. A Dual De-
10
icing System for Wind Turbine Blades Combining High-power Ultrasonic Guided
11
Waves and Low-frequency Forced Vibrations. Renew. Energy 2015, 83, 859-870.
12
(5) Mayer, C.; Ilinca, A.; Fortin, G.; Perron, J. Wind Tunnel Study of Electrothermal
13 14 15
De-icing of Wind Turbine Blades. Int. J. Offshore Polar Eng. 2007, 17,182-188. (6) Liu, F.; Pan, Q. Facile Fabrication of Robust Ice-phobic Polyurethane Sponges. Adv. Mater. Interfaces 2015, 2, 1500219.
16
(7) Ruan, M.; Li, W.; Wang, B.; Deng, B.; Ma, F.; Yu, Z. Preparation and Anti-icing
17
Behavior of Superhydrophobic Surfaces on Aluminum Alloy Substrates. Langmuir
18
2013, 29, 8482-8491.
19
(8) Emelyanenko, A. M.; Boinovich, L. B.; Bezdomnikov, A. A.; Chulkova, E. V.;
20
Emelyanenko, K. A. Reinforced Superhydrophobic Coating on Silicone Rubber for
21
Longstanding Anti-Icing Performance in Severe Conditions. ACS Appl. Mater.
22
Interfaces 2017, 9, 24210-24219.
29
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
1 2
Page 30 of 36
(9) Chen, J.; Luo, Z.; Fan, Q.; Lv, J.; Wang, J. Anti-ice Coating Inspired by Ice Skating. Small 2014, 10, 4693-4699.
3
(10)Wu, X.; Zheng, S.; Bellido-Aguilar, D. A.; Silberschmidt, V. V.; Chen, Z.
4
Transparent Icephobic Coatings Using Bio-based Epoxy Resin. Mater. Des. 2018,
5
140, 516-523.
6
(11)Li, C.; Li, X.; Tao, C.; Ren, L.; Zhao, Y.; Bai, S.; Yuan, X. Amphiphilic
7
Antifogging/anti-icing Coatings Containing POSS-PDMAEMA-b-PSBMA. ACS
8
Appl. Mater. Interfaces 2017, 9, 22959-22969.
9 10
(12)Golovin, K.; Kobaku, S. P. R.; Lee, D. H.; DiLoreto, E. T.; Mabry, J. M.; Tuteja, A. Designing Durable Icephobic Surfaces. Sci. Adv. 2016, 2, 1501496.
11
(13)Shen, Y.; Wang, G.; Zhu, C.; Tao, J.; Lin, Y.; Liu, S.; Jin, M.; Xie, Y. Petal Shaped
12
Nanostructures Planted on Array Micro-patterns for Superhydrophobicity and
13
Anti-icing Applications. Surf. Coat. Tech. 2017, 319, 286-293.
14
(14)Cheng, T.; He, R.; Zhang, Q.; Zhan, X.; Chen, F. Magnetic Particle-based Super-
15
Hydrophobic Coatings with Excellent Anti-icing and Thermoresponsive Deicing
16
Performance. J. Mater. Chem. A 2015, 3, 21637-21646.
17
(15)Wang, Y.; Xue, J.; Wang, Q.; Chen, Q.; Ding, J. Verification of Icephobic/anti-
18
icing Properties of a Superhydrophobic Surface. ACS Appl. Mater. Interfaces 2013,
19
5, 3370-3381.
20
(16)Wang, N.; Xiong, D.; Lu, Y.; Pan, S.; Wang, K.; Deng, Y.; Shi, Y. Design and
21
Fabrication of the Lyophobic Slippery Surface and Its Application in Anti-icing. J.
22
Phys. Chem. C 2016, 120, 11054-11059. 30
ACS Paragon Plus Environment
Page 31 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
(17)Subramanyam. S. B.; Rykaczewski, K.; Varanasi, K. K. Ice Adhesion on
2
Lubricant-impregnated Textured Surfaces. Langmuir 2013, 29, 13414-13418.
3
(18)Kim, P.; Wong, T.; Alvarenga, J. Kreder, M. J.; Adorno-Martinez, W. E.;
4
Aizenberg J. Liquid-infused Nanostructured Surfaces with Extreme Anti-Ice and
5
Anti-frost Performance. ACS Nano 2012, 6, 6569-6577.
6
(19)Chen, J.; Li, K.; Wu, S.;
Liu, J.; Liu, K.; Fan, Q. Durable Anti-icing Coatings
7
Based on Self-sustainable Lubricating Layer. ACS Omega 2017, 2, 2047-2054.
8
(20)Dou, R.; Chen, J.; Zhang, Y.; Wang, X.; Cui, D.; Song, Y.; Jiang, L.; Wang, J.
9
Anti-icing Coating with an Aqueous Lubricating Layer. ACS Appl. Mater.
10
Interfaces 2014, 6, 6998-7003.
11
(21)Rykaczewski, K.; Anand, S.; Subramanyam, S. B.; Varanasi, K. K. Mechanism of
12
Frost Formation on Lubricant-impregnated Surfaces. Langmuir 2013, 29, 5230-
13
5238.
14
(22)Subramanyam, S. B.; Rykaczewski, K.; Varanasi, K. K. Ice Adhesion on
15
Lubricant-impregnated Textured Surfaces. Langmuir 2013, 29, 13414-13418.
16
(23)Jung, S.; Tiwari, M. K.; Doan, N. V.; Poulikakos, D. Mechanism of Supercooled
17
Droplet Freezing on Surfaces. Nat. Commun. 2012, 3, 615.
18
(24)Boinovich, L. B.; Emelyanenko, A. M.; Emelyanenko, K. A.; Maslakov, K. I. Anti-
19
icing Properties of a Superhydrophobic Surface in a Salt Environment: an
20
Unexpected Increase in Freezing Delay Times for Weak Brine Droplets. Phys.
21
Chem. Chem. Phys. 2016, 18, 3131-3136.
31
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 32 of 36
1
(25)Shen, Y.; Wang, G.; Tao, J.; Zhu, C.; Liu, S.; Jin, M.; Xie, Y.; Chen, Z. Anti-icing
2
Performance of Superhydrophobic Texture Surfaces Depending on Reference
3
Environments. Adv. Mater. Interfaces 2017, 4, 1700836.
4
(26)Jiang, C.; Li, W. A Facile Method for Preparations of Micro-nanotextured Co3O4,
5
Films with the Excellent Superhydrophobic and Anti-icing Behavior. Mater. Lett.
6
2014, 122, 133-138.
7
(27)Zheng, S.; Li, C.; Fu, Q.; Hu, W.; Xiang, T.; Wang, Q.; Du, M.; Liu, X.; Chen, Z.
8
Development of Stable Superhydrophobic Coatings on Aluminum Surface for
9
Corrosion-resistant, Self-cleaning, and Anti-icing Applications. Mater. Des. 2016,
10
93, 261-270.
11
(28)Ruan, M.; Zhan, Y.; Wu, Y.; Wang, X.; Li, W.; Chen, Y.; Wei, M.; Wang, X.;
12
Deng. X. Preparation of PTFE/PDMS Superhydrophobic Coating and its Anti-
13
Icing Performance. RSC Adv. 2017, 7, 41339-41344.
14
(29)Peng, C.; Xing, S.; Yuan, Z.; Xiao, J.; Wang, C.; Zeng, J. Preparation and Anti-
15
icing of Superhydrophobic PVDF Coating on a Wind Turbine Blade. Appl. Surf.
16
Sci. 2012, 259, 764-768.
17
(30)Puretskiy, N.; Chanda, J.; Stoychev, G.; Synytska, A.; Ionov, L. Anti‐icing
18
Superhydrophobic Surfaces Based on Core‐shell Fossil Particles. Adv. Mater.
19
Interfaces 2015, 2, 1500124.
20
(31)Yin, X.; Zhang, Y.; Wang, D.; Liu, Z.; Liu, Y.; Pei, X.; Yu, B.; Zhou, F. Integration
21
of Self‐lubrication and Near‐infrared Photothermogenesis for Excellent
22
Anti‐Icing/deicing Performance. Adv. Funct. Mater. 2015, 25, 4237-4245. 32
ACS Paragon Plus Environment
Page 33 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
(32)Sohn, K. S.; Timilsina, S.; Singh, S. P.; Lee, J. W.; Kim, J. S. A
2
Mechanoluminescent
3
CNT/PDMS Hybrid Sensor: Red-Light Emission and a Standardized Strain
4
Quantification. ACS Appl. Mater. Interfaces, 2016, 8, 34777-34783.
ZnS:
Cu/Rhodamine/SiO2/PDMS
and
Piezoresistive
5
(33)Shen, Y.; Tao, J.; Tao, H.; Chen, S.; Pan, L.; Wang, T. Anti-icing Potential of
6
Superhydrophobic Ti6Al4V Surfaces: Ice nucleation and Growth. Langmuir 2015,
7
31, 10799-10806.
8
(34)Gao, R.; Liu, Q.; Wang, J.; Zhang, X.; Yang, W.; Liu, J.; Liu, L. Fabrication of
9
Fibrous Szaibelyite with Hierarchical Structure Superhydrophobic Coating on
10
AZ31 Magnesium Alloy for Corrosion Protection. Chem. Eng. J. 2014, 241, 352-
11
359.
12
(35)Liu, X.; Xu, Y.; Ben, K.; Chen, Z.; Wang, Y.; Guan, Z. Transparent, Durable and
13
Thermally Stable PDMS-derived Superhydrophobic Surfaces. Appl. Surf. Sci. 2015,
14
339, 94-101.
15
(36)Brassard, J.; Sarkar, D. K.; Perron, J. Synthesis of Monodisperse Fluorinated Silica
16
Nanoparticles and their Superhydrophobic Thin Films. ACS Appl. Mater.
17
Interfaces 2011, 3, 3583-3588.
18
(37)Latthe, S. S.; Terashima, C.; Nakata, K.; Sakai, M. Fujishima, A. Development of
19
Sol-gel Processed Semi-transparent and Self-cleaning Superhydrophobic Coatings,
20
J. Mater. Chem. A 2014, 2, 5548-5553.
33
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 34 of 36
1
(38)Koo, S. H.; Lee, S. G.; Bong, H.; Kwark, Y.; Cho, K.; Lim, H. S.; Cho, J. H. Robust
2
Multifunctional Superhydrophobic Organic-inorganic Hybrid Macroporous
3
Coatings and Films. Polymer 2014, 55, 2661-2666.
4
(39)Xu, W.; Song, J.; Sun, J.; Lu, Y.; Yu, Z. Rapid Fabrication of Large-area,
5
Corrosion-Resistant Superhydrophobic Mg Alloy Surfaces. ACS Appl. Mater.
6
Interfaces 2011, 3, 4404-4414.
7
(40)Qu, M.; Ma, X.; He, J.; Feng, J.; Liu, S.; Yao, Y.; Hou, L.; Liu, X. Facile Selective
8
and Diverse Fabrication of Superhydrophobic, Superoleophobic-superhydrophilic
9
and Superamphiphobic Materials from Kaolin. ACS Appl. Mater. Interfaces 2017,
10
9, 1011-1020.
11
(41)Deng, S.; Huang, J.; Chen, Z.; Lai, Y. Controllable Superhydrophobic Coating on
12
Cotton Fabric by UV Induced Thiol-ene Reaction for Wettability Patterning and
13
Device Metallization. Adv. Mater. Interfaces 2017, 4, 1700268.
14
(42)Zhou, H.; Wang, H.; Niu, H.; Zhao, Y.; Xu, Z.; Lin, T. A Waterborne Coating
15
System for Preparing Robust, Self‐healing, Superamphiphobic Surfaces. Adv.
16
Funct. Mater. 2017, 27, 1604261.
17
(43)Wang, N.; Lu, Y.; Xiong, D.; Carmalt, C. J.; Parkin, I. P. Designing Durable and
18
Flexible Superhydrophobic Coatings and its Application in Oil Purification, J.
19
Mater. Chem. A 2016, 4, 4107-4116.
20
(44)Wu, X.; Fu, Q.; Kumar, D.; Ho, J. W. C.; Kanhere, P.; Zhou, H.; Chen, Z.
21
Mechanically Robust Superhydrophobic and Superoleophobic Coatings Derived
22
by Sol-gel Method. Mater. Des. 2016, 89, 1302-1309. 34
ACS Paragon Plus Environment
Page 35 of 36 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Applied Materials & Interfaces
1
(45)Kim, H.; Lee, C.; Kim, M. H.; Kim, J. Drop Impact Characteristics and Structure
2
Effects of Hydrophobic Surfaces with Micro- and/or Nanoscaled Structures.
3
Langmuir 2012, 28, 11250-11257.
4
(46)Choi, J.; Jo, W.; Lee, S. Y.; Jung, Y. S.; Kim, S.; Kim, H. Flexible and Robust
5
Superomniphobic Surfaces Created by Localized Photofluidization of Azopolymer
6
Pillars. ACS Nano 2017, 11, 7821-7828.
7
(47)Lee, W.; Jung, W.; Nagel, S. R.; Odom, T. W. Stretchable Superhydrophobicity
8
from Monolithic, Three-dimensional Hierarchical Wrinkles. Nano Lett. 2016, 16,
9
3774-3779.
10 11
(48)Yao, X.; Hawkins, S. C.; Falzon, B. G. An Advanced Anti-icing/de-icing System Utilizing Highly Aligned Carbon Nanotube Webs. Carbon 2018, 136, 130-138.
12
(49)Heydari, G.; Moghaddam, M. S.; Tuominen, M.; Fielden, M.; Haapanen, J.;
13
Mäkelä, J. M.; Claesson, P. M. Wetting hysteresis induced by temperature changes:
14
Supercooled water on hydrophobic surfaces. J. Colloid Interf. Sci. 2016, 468, 21-
15
33.
16
(50)Heydari, G.; Thormann, E.; Järn, M.; Tyrode, E.; Claesson, P. M. Hydrophobic
17
surfaces: topography effects on wetting by supercooled water and freezing delay.
18
J. Phys. Chem. C 2013, 117, 21752-21762.
19
(51)Fu, Q.; Wu, X.;
Kumar, D.; Ho, J. W. C.; Kanhere, P. D.; Srikanth, N.; Liu, E.;
20
Wilson, P.; Chen, Z. Development of Sol-gel Icephobic Coatings: Effect of Surface
21
Roughness and Surface Energy. ACS Appl. Mater. Interfaces 2014, 6, 20685-20692.
22 35
ACS Paragon Plus Environment
ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 36 of 36
1
TOC Graphic:
2
We designed and fabricated a kind of high-performance superhydrophobic F-
3
SiO2@PDMS coatings, and focused on the evaluations of anti-icing performance of the
4
as-prepared superhydrophobic coatings around the three aspects of dynamic water
5
repellency, icing delay, and ice adhesion.
6