Tuning the K concentration in the tunnels of #-MnO to increase the content of oxygen vacancy for ozone elimination Guoxiang Zhu, Jinguo Zhu, Wenlu Li, Wenqing Yao, Ruilong Zong, Yongfa Zhu, and Qianfan Zhang Environ. Sci. Technol., Just Accepted Manuscript • DOI: 10.1021/acs.est.8b01594 • Publication Date (Web): 03 Jul 2018 Downloaded from http://pubs.acs.org on July 3, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 29
Environmental Science & Technology
1
Tuning the K+ concentration in the tunnels of α-MnO2 to increase the content of oxygen
2
vacancy for ozone elimination
3
Guoxiang Zhua, Jinguo Zhub, Wenlu Lia, Wenqing Yaoa, Ruilong Zonga, Yongfa Zhua* and Qianfan Zhangb*
4 5
a Department of Chemistry, Tsinghua University, Beijing 100084, China
6
b School of Materials Science and Engineering, Beihang University, Beijing 100191, China
7
1
ACS Paragon Plus Environment
Environmental Science & Technology
8
ABSTRACT
9
α-MnO2 is a promising material for ozone catalytic decomposition and the oxygen vacancy is
10
often regarded as the active site for ozone adsorption and decomposition. Here, α-MnO2 nanowire
11
with tunable K+ concentration was prepared through a hydrothermal process in KOH solution. High
12
concentration K+ in the tunnel can expand crystal cell and break the charge balance, leading to a
13
lower average oxidation state (AOS) of Mn, which means abundant oxygen vacancy. DFT
14
calculation has also proven that the samples with higher K+ concentration exhibit lower formation
15
energy for oxygen vacancy. Due to the enormous active oxygen vacancies existing in the α-MnO2
16
nanowire, the lifetime of the catalyst (corresponding to 100 % ozone removal rate, 25 ºC) is
17
increased from 3 h to 15 h. The FT-IR results confirmed that the accumulation of intermediate
18
oxygen species on the catalyst surface is the main reason why it is deactivated after long time
19
reaction. In this work, the performance of the catalyst has been improved because the abundant
20
active oxygen vacancies are fabricated by the electrostatic interaction between oxygen atoms inside
21
the tunnels and the introduced K+, which offers us a new perspective to design a high efficiency
22
catalyst and may promote manganese oxide for practical ozone elimination.
23
2
ACS Paragon Plus Environment
Page 2 of 29
Page 3 of 29
24
Environmental Science & Technology
TOC Art
25 26
3
ACS Paragon Plus Environment
Environmental Science & Technology
27
1. INTRODUCTION
28
In recent years, ozone is given increased attention as a common air pollutant due to the potential
29
impact on public health and our living environment. A long-term exposure to even low level of ozone
30
would cause serious health problems, including cardiopulmonary disease,1 respiratory disease2 and
31
cardiovascular disease.3, 4 Generally, ozone is formed near the ground in the photochemical reaction
32
referring to volatile organic compounds (VOCs), NOx and carbon monoxide.5 However, household
33
electrostatic equipments6 and ultraviolet disinfection equipments7 also cannot be ignored for indoor
34
ozone production. Besides, ozonation and plasma process also cause serious ozone pollution in
35
factory. Apart from the hazard of ozone, the indoor residual ozone also leads to the formation of
36
VOCs by the ozone-surface reaction with building materials and indoor furnishing,8-10 and the
37
produced compounds may form the secondary organic aerosol (SOA).11, 12 Thus, the Occupational
38
Safety and Health Administration (OSHA, US) stipulates the maximum allowable exposure to ozone
39
in the terms of eight-hour is 0.10 ppm.13 The regulations of Chinese indoor air quality standard’
40
(GB/T 18883 - 2002) also require that the indoor ozone concentration should not exceed 0.08 ppm.
41
Therefore, the research on the ozone elimination is significant for environmental protection and
42
public health.
43
Various methods have been applied for ozone removal, such as plants purification,14
44
adsorption,15 thermal decomposition and catalytic decomposition.16-19 Compared with other methods,
45
the catalytic decomposition has been recognized as a promising approach, due to its higher efficiency,
46
safety and lower cost. The catalyst for ozone elimination can be divided into noble metal,20, 21
47
transitional metal oxide16-19,
48
large-scale application, the research about ozone catalytic decomposition mainly focus on
22, 23
and noble-transitional compounds. Considering the cost and
4
ACS Paragon Plus Environment
Page 4 of 29
Page 5 of 29
Environmental Science & Technology
49
transitional metal oxide, especially manganese oxide. Jia et al.24 compared the activity of
50
α, β and γ−MnO2 for ozone removal and observed the highest ozone removal rate with α−MnO2.
51
They found that the catalytic performance of manganese oxide strongly depends on the density of
52
oxygen vacancies. In our previous study, surface oxygen vacancy was proved to be the active site for
53
ozone adsorption and further decomposition.19 The formation of oxygen vacancy would change the
54
original charge distribution, resulting in a lower ozone adsorption energy and better catalytic
55
activity.25 For example, Wang et al.26 reported that an cryptomelane-type manganese oxide (OMS-2)
56
catalyst synthesized with MnAc2 as Mn2+ precursor could form abundant Mn3+, leading to a higher
57
catalytic performance. Ma et al.18 also reported that a higher catalytic performance could be obtained
58
in transition mental doped OMS-2, resulting in the abundant oxygen vacancies. Therefore, the
59
enhancement of oxygen vacancy is regarded as an effective strategy to improve the catalytic
60
performance.
61
α−MnO2 is consisted of 2 × 2 edge-share MnO6 octahedral chains, which corner-connected to
62
form 0.46 × 0.46 nm tunnels. Abundant MnO6 edges exposes in the structure, leading to easy release
63
of lattice oxygen.27 Manganese is located in the framework and the guest cation, such as Li+, Na+, K+,
64
NH4+, is filled in the tunnels to stabilized the structure. Because of the unique tunnel structure,
65
various cations, especially potassium ion, can be introduced into the tunnels to tailor its chemical and
66
physical properties. For example, Yuan et al.28 reported that the presence of potassium ions inside the
67
tunnels of α−MnO2 would increase its electronic conductivity. Tseng et al.29 pointed out that
68
magnetic properties of α−MnO2 nanotube is closely connected with the K+ doping concentration.
69
Hou et al.30 also demonstrated that K+-doped OMS-2 nanowire has better catalytic activity for
70
benzene oxidation. Generally, these cations are located in the center of tunnels and the charge on the 5
ACS Paragon Plus Environment
Environmental Science & Technology
71
cations would be balanced by substitution of Mn3+ for some of the Mn4+.31 So, oxygen vacancies are
72
easy to form at the MnO6 edges and a higher ozone removal rate is expected when the K+ entered
73
into the tunnels. Herein, we developed a simply post-processing method to prepare K-rich α-MnO2
74
nanowire for ozone catalytic decomposition. The effect of K+ concentration in the tunnels of α-MnO2
75
on the performance for ozone removal has been studied theoretically and experimentally.
76
2. EXPERIMENTAL SECTION
77
Preparation of K-rich MnO2
78
α-MnO2 nanowires were synthesized by a hydrothermal process using KMnO4 and MnSO4.
79
Specifically, 3.042 g MnSO4·H2O and 1.896 g KMnO4 (Mn7+ : Mn2+ = 2 : 3) were added into 80 mL
80
deionized (DI) water with constant stir for 20 mins to form a suspension. Subsequently, the
81
suspension was transformed into 100 mL Teflon-lined stainless steel autoclave and heated at 150 °C
82
for 12 h. The products were collected by centrifugation, then washed with DI water and dried at
83
80 °C for 10 h. The obtained nanowire was identified as MnO2. The K+ concentration was tuned by a
84
hydrothermal process in KOH solution as illustrated in Figure 1. 1.0 g synthesized nanowire was
85
added in 80 mL KOH solution accompanied with ultrasonic dispersion for 20 mins, and then
86
transformed into 100 mL Teflon-lined stainless steel autoclave and heated at 150 °C for several hours.
87
Then the collected products were washed with DI water until the filtrate was neutral (PH ≈ 7).
88
Finally, the K-rich MnO2 nanowire was obtained after drying at 80 °C for 10 h.
6
ACS Paragon Plus Environment
Page 6 of 29
Page 7 of 29
Environmental Science & Technology
89 90
91
Figure 1. Schematic illustration of the preparation of K-rich α-MnO2.
Catalyst Characterization.
92
X-ray diffraction (XRD) patterns of the samples were obtained by a Rigaku D/max-2400 X-ray
93
diffractometer with Cu Kα (λ = 1. 5406 Å) radiation at 40 kV and 150 mA. Morphologies of the
94
samples were captured by a Field Emission Gun Scanning Electron Microscopy (FESEM, Hitachi
95
SU-8010) and a transmission electron microscopy (TEM, Hitachi 7700) with an accelerating voltage
96
of 100 kV. High resolution transmission electron microscopy (HRTEM) images were obtained by a
97
JEM 2100F field emission transmission electron microscope at an accelerating voltage of 200 kV.
98
The element composition and distribution were recorded by ICP-MS (iCAPQ, Thermo Fisher
99
SCientific) and an energy dispersive (EDS) detector in Hitachi SU-8010 and JEM 2100F. X-ray
100
photoelectron spectroscopy (XPS) was conducted in a PHI Quantera SXMTM system and the binding
101
energy was calibrated with the signal for adventitious carbon at 284.8 eV. Fourier transform infrared
102
(FT-IR) spectra and in situ diffused Fourier transform infrared spectroscopy (DFTIR) was recorded
103
by Bruker V70 spectrometer. Thermogravimetric analysis (TGA) was carried out in a TGA/DSC1
104
STARe system (METTLER TOLEDO). Temperature programmed desorption (TPD) was carried out
105
on a Cat-Lab (BEL Japen, Inc.) eqiupped with an online QIC-200 quadrupole mass (Inprocess
106
Instruments, GAM 200) as a detector.
107
Catalytic Activity. 7
ACS Paragon Plus Environment
Environmental Science & Technology
Page 8 of 29
108
The performance of catalytic ozone decomposition was evaluated in a continuous fixed bed
109
reactor (11 mm inner diameter) at room temperature (25 ºC). 0.1 g catalyst was used for each test
110
with the space velocity of 5.4 × 105 mL·g-1·h-1. The total gas flow through the reactor was kept at
111
900 mL/min and the inlet ozone concentration maintained at 50 ± 1 ppm. The relative humidity was
112
measured by a hygronom (605-H1 Testo) and controlled by tuning the gas flow through a humidifier
113
without changing the total gas flowrate. An ozonator (model 1000BT-12, Shanghai Enaly
114
Mechanical and Electrical Technology Company) was applied to generate ozone by arc discharge in
115
O2 stream, where the O2 flow and the discharge voltage can be tuned. The generated ozone mixed
116
adequately with air in a mixing drum and then transported to the reactor. The inlet and outlet ozone
117
concentration were measured by an ozone detector (model 202, 2B Technologies). The ozone
118
removal rate can be calculated from the following equation:
119
Ozone removal rate = 100 % × (Cin - Cout)/Cin.
120
where Cin and Cout are inlet and outlet ozone concentration respectively.
121
3. RESULTS AND DISCUSSION
122
3.1 The Characterization of Structure and Morphology.
123 8
ACS Paragon Plus Environment
(1)
Page 9 of 29
Environmental Science & Technology
124
Figure 2. XRD patterns of α-MnO2 before and after treated in 1M KOH solution (a); the enlarged
125
view of the α-MnO2 (200) peak (b).
126
The structure of α-MnO2 nanowire before and after the treatment in KOH solution were
127
analyzed by XRD as shown in Figure 2a. All the obtained samples have the same peaks,
128
corresponding to a pure tetragonal cryptomelane type MnO2 (JCPDS No. 29-1020), which means the
129
crystalline phase is well maintained during the treatment.32 In order to confirm the influence of the
130
post-processing on the composition of the samples, the bulk contents of K and Mn were detected by
131
ICP-MS (Table 1). After hydrothermal treatment in 1 M KOH solution for 4 h, the K/Mn molar ratio
132
is increased from 13.44 % to 20.75 %. The K/Mn molar ratio on the catalyst surface has also been
133
measured by XPS and the treatment can increase the ratio from 13.46 % to 22.89 % compared with
134
pure MnO2, as shown in Figure S3. The same results can also be obtained by the EDS equipped in
135
FESEM and HRTEM, indicating that the K+ content has been indeed enhanced.
136
In the α-MnO2 crystal structure, the crystal radii of K+ (1.65 Å) is significantly larger than that
137
of Mn3+ (high spin, 0.785 Å; low spin, 0.72 Å) and Mn4+ (0.67 Å), suggesting that K+ entered into
138
the 2 × 2 tunnels of α-MnO2 rather than the octahedral framework.18 Further observation of XRD
139
spectra shows that all the peaks gradually shift to lower angles with the extension of hydrothermal
140
time and the trend is more clearly for (200) peak (Figure 2b), which means the tunnel is expanded.28,
141
29, 33
142
maintained a pure cryptomelane structure and possess of high crystallinity. However, the lattice
143
spacing of (200) plane has increased from 0.476 nm to 0.489 nm after treated, corresponding to the
144
expansion of the tunnel structure. In addition, the mapping images (Figure S4) suggest that the K and
145
Mn is well distributed in the nanowire before and after hydrothermal treatment. Therefore, it can be
High-resolution TEM (HRTEM) images (Figure 3c, f) indicate that MnO2 and KOH-4h
9
ACS Paragon Plus Environment
Environmental Science & Technology
Page 10 of 29
146
concluded that abundant K+ were entered into the tunnel structure and well dispersed in the
147
hydrothermal process.
148
Table 1. Atomic ratio of K/Mn, BET surface areas, and AOS of Mn of the manganese oxide samples. Atomic ratio of K/Mn Sample
BET surface areas AOS of Mn
ICP-MS
FESEM-EDS
[m2/g]
MnO2
13.44
11.45
61.00
3.76
KOH-2h
19.24
16.19
52.50
3.49
KOH-4h
20.75
16.93
52.43
3.43
KOH-6h
23.18
17.16
51.94
3.37
149
The morphologies of as-prepared samples were investigated by FESEM and TEM. As shown in
150
Figure 3a, b, the as-synthesized MnO2 presents a typical nanowire morphology with a diameter in the
151
range of 20-40 nm and a length for about 2-5 µm. However, after hydrothermal treatment in 1 M
152
KOH solution for 4 h, the original isolated nanowire arranges along the diameter direction and forms
153
a bunchy structure. TEM images (Figure 3d, e) also confirmed that the length of KOH-4h bundle has
154
no obvious change but the width is beyond 60 nm. As shown in FT-IR spectra (Figure 4a), the peaks
155
value at 3430 cm-1 and 1630 cm-1, attributed to the surface absorbed water and hydroxyl groups
156
respectively,34 become larger with longer treatment time, suggesting abundant surface hydroxyl
157
groups is formed during the post-processing. Hu et al.35 pointed out that abundant surface hydroxyl
158
groups are produced from the hydroxylation of the surface oxides to balance the overall charge after
159
K+ entered into the tunnels of α-MnO2 nanowire. Therefore, the existing of abundant surface
160
hydroxyl groups means a higher K+ content in the tunnels. From Figure S5, it can also be found that
161
the bundled trend become serious with increased hydrothermal time. Table 1 also has shown that the
162
treatment in KOH solution leads to the decrease of surface area from 61 m2/g to 51.91 m2/g, 10
ACS Paragon Plus Environment
Page 11 of 29
Environmental Science & Technology
163
corresponding to the change in morphology. Besides, the bundled extent of treated samples reduces
164
partly after calcination at 300 ºC for 2 h, while the crystal structure has no obvious difference (Figure
165
S7, 8). Hence, it can be concluded that the bunchy structure is formed with the help of the abundant
166
surface hydroxyl groups, which induce hydrogen bond interaction among isolated nanowires. The
167
bunchy structure also reconfirms the enhancement of K+ concentration in the treated samples.
168 169
Figure 3. FESEM images of α-MnO2 (a) and KOH-4h (d); TEM images of α-MnO2 (b) and
170
KOH-4h (e); HRTEM images of α-MnO2 (c) and KOH-4h (f).
171
The evolution of oxygen from the samples was investigated by temperature programmed
172
desorption (TPD-MS) as shown in Figure 4b. The desorption process can be divided into four parts.
173
The peaks lower than 200 ºC corresponds to the physical absorbed water molecule.36 The peak
174
between 200 ºC and 400 ºC is assigned as the desorption of surface hydroxyl radical. For KOH-4h,
175
the peak at 233 ºC shift to 278 ºC, suggesting the existence of a stronger bond between surface 11
ACS Paragon Plus Environment
Environmental Science & Technology
176
hydroxyl radical and KOH-4h. The peaks between 400 ºC to 650 ºC is assigned as the release of the
177
lattice oxygen close to the surface19 and the crystalline phase will completely transform to Mn2O3
178
while the temperature rises to 800 ºC. Compared with MnO2, the peaks of KOH-4h at 475 ºC and
179
586 ºC shift to 531 ºC and 617 ºC respectively and the peak area has an obvious decrease, indicating
180
that a large amount of lattice oxygen is more stable after treated in KOH solution.33 As shown in
181
Figure 4c, the TGA curve under N2 atmosphere has been recorded to characterize the thermostability.
182
After the treatment in KOH solution, the weight loss from 45 ºC to 800 ºC is reduced from 11.65 %
183
to 9.97 %, as a result of the higher K+ content in KOH-4h. Interestingly, the weight loss between 400
184
ºC to 650 ºC decreases form 5.72 % to 3.26 % while the ratio between 650 ºC to 800 ºC increases
185
from 3.44 % to 4.53 %, corresponding to the TPD-MS results, suggesting a more stable structure is
186
indeed induced by increasing K+ concentration in tunnels. Based on the elaborate analysis of the
187
crystal structure of cryptomelane type MnO2 (Figure S9), it can be found that the increase of K+
188
concentration in the tunnels can induce the electrostatic interaction between K+ and the lattice
189
oxygen with a sp3 hybridization [O (sp3)] to form a balanced force distribution, which leads to a
190
higher temperature for the evolution of oxygen.
191
Considering the vital impact of Mn-O bond on the catalytic activity, the average oxidation state
192
(AOS) of surface Mn atom was analyzed via XPS. As shown in Figure S11, the signals of Mn, O and
193
K can be found in all the samples. After treated in KOH solution, the charge on the tunnel cation (K+)
194
is balanced by substitution of Mn3+ for some of the Mn4+ in the framework.31 Further observation
195
(Figure 4d) has shown that the binding energy difference (∆ܧ௦ ) between the two peaks of Mn 3s
196
varies with the increase of K+ content and the AOS of surface Mn has been estimated via the
197
following formula37,
38
: AOS=8.956-1.126∆ܧ௦ . After treated in KOH solution, the AOS of Mn 12
ACS Paragon Plus Environment
Page 12 of 29
Page 13 of 29
Environmental Science & Technology
198
gradually decreases from 3.76 to 3.37 with the extension of treatment time, meaning a lower average
199
coordination number and higher oxygen vacancy content. In addition, the decrease of AOS means
200
that Jahn-Teller (JT) distortion can occur to lower the system’s ground state37, which has the same
201
conclusion with XRD results.
202 203
Figure 4. The FTIR spectra (a), the TPD-MS profiles (b), TGA curve (c) and Mn 3s XPS spectra (d)
204
of the samples.
205
3.2 Performance of Ozone Removal
206 13
ACS Paragon Plus Environment
Environmental Science & Technology
207 208
Figure 5. The ozone removal rate of the samples treated with different concentration KOH solution
209
(a) and the samples treated for different time in 1M KOH solution (b); The ozone removal rate of the
210
samples treated with different alkali solution for 4h (c); The ozone removal rate of the samples
211
treated with different potassium salt solution for 4h (d); The ozone removal rate on KOH-4h at
212
different RH (e); The ozone removal rate on KOH-4h at alternate humidity condition (f); All the
213
reaction was carried out at 25 ºC.
214
Based on the characterized analysis, K+ entered into the tunnels of α-MnO2 with the treatment,
215
which can generate abundant oxygen vacancy for ozone decomposition. Therefore, a higher ozone
216
removal rate is expected for α-MnO2 with higher K+ content. As shown in Figure 5a, the ozone
217
removal rate of the samples treated in different concentration KOH solution have been evaluated. For
218
α-MnO2 without treatment, the ozone removal rate begins to decrease while the reaction runs for 3 h
219
in the gas flow with 50 ppm ozone and it decreases to 25 % when the reaction maintained for 12 h.
220
The bunchy structure in the treated samples, with a smaller surface area, provides a poor activity if 14
ACS Paragon Plus Environment
Page 14 of 29
Page 15 of 29
Environmental Science & Technology
221
the density of active site has no obvious increase. However, when the as-synthesized nanowire was
222
treated in 0.25 M KOH solution for 4 h, the time possessed of 100 % ozone removal rate increased
223
from 3 h to 10 h and it could extend to 15 h if the concentration of KOH solution keeps at 1.00 M. It
224
indicates that the treatment in KOH solution has indeed improved the catalytic performance for
225
ozone removal. The atomic K/Mn ratio detected by EDS detector equipped in FESEM also shows
226
there is a positive correlation between the catalytic performance and the K+ content, suggesting that
227
the increase of K+ content in the tunnels is beneficial for ozone decomposition. The performance of
228
the catalyst is also affected by hydrothermal time. The optimal catalytic activity can be obtained
229
when α-MnO2 nanowire is treated in 1.00 M KOH solution for 4 h (Figure 5b). However, if the
230
hydrothermal time or the concentration of KOH solution continuously increased, the increase of K+
231
content will be slow (Figure S12a, b) and the effect of bunchy structure on the surface area will be
232
obvious, leading to an almost unchanged catalytic activity.
233
In order to further confirm the reason why the ozone removal rate has been improved, the
234
α-MnO2 nanowire was treated in different alkali and kali salt solution respectively. As can be seen in
235
Figure 5c, the samples treated in LiOH, NaOH or NH3·H2O solution are all possessed of a lower
236
performance compared with untreated MnO2, indicating that it is K+ content in the tunnels rather
237
than surface hydroxyl group that improves the ozone removal rate. When the α-MnO2 nanowire was
238
treated in KNO3, K2SO4 and CH3COOK solution respectively (the K+ concentration keeps at 1M),
239
the activity for ozone removal has different levels of increase except for the sample treated in KNO3
240
solution (seeing Figure 5d), suggesting ozone decomposition is also effected by the anion absorbed
241
on the surface. High-resolution XPS spectra of KNO3-4h, K2SO4-4h, CH3COOK-4h also has
242
confirmed the existence of absorbed anions on the surface of the samples (Figure S14). Besides, the 15
ACS Paragon Plus Environment
Environmental Science & Technology
243
atomic K/Mn ratio has been further analyzed by the EDS detector, as shown in Figure S12c. The
244
samples treated in different kali salt solution are possessed of various K+ content (Figure S12d),
245
resulting in different catalytic performance for ozone removal. It can be concluded that the anion in
246
the solution will affect the ability of K+ entering the α-MnO2 tunnel structure, leading to various
247
content of oxygen vacancy. In general, the ozone catalytic decomposition can be facilitated by
248
increasing the K+ content in the tunnels and it is also influenced by the corresponding anion in the
249
solution.
250
The catalyst is easy to be deactivated in humid environment.17, 39 As can be seen in Figure 5e,
251
when the relative humidity (RH, 25 °C) increases from 22 % to 30 %, the ozone removal rate at 15 h
252
decreases from 99 % to 78 % and the removal rate continues to decreasing with further increase of
253
RH, suggesting that the performance of the catalysts is also sensitive to the humidity of the gas flow.
254
In the high humidity gas flow, a large amount of surface hydroxyl group would form under the
255
combined action of water vapor and ozone molecule. The hydrogen bond interaction between surface
256
hydroxyl group and water molecule would adverse to the ozone uptake on the catalyst.40 For
257
KOH-4h, due to the abundant hydroxyl group on the surface, a strong hydrogen bond interaction has
258
already exist in the initial stage of the reaction, resulting in a dramatically decrease of ozone removal
259
rate at the beginning (Figure S16). For untreated MnO2, the inherent surface hydroxyl group is finite,
260
so the ozone removal rate decreased gradually. However, KOH-4h is possessed of higher activity at
261
12 h than MnO2, which suggests more active sites existing in KOH-4h. As can be seen in Figure 5f,
262
the ozone removal rate has been evaluated at alternate humidity conditions. When the catalyst was
263
placed into the wet gas flow (50 % RH), the ozone removal rate has a sharp decrease due to the
264
competitive adsorption of water molecule. However, once the relative humidity was decreased, the 16
ACS Paragon Plus Environment
Page 16 of 29
Page 17 of 29
Environmental Science & Technology
265
ozone removal rate recover to 100 % quickly, indicating that the deactivation resulting from water
266
molecule is temporary and the catalytic activity in the dry gas flow has not been affected by surface
267
hydroxyl group. When the relative humidity of the gas flow was increased to 50 % again, the ozone
268
removal rate decreases to the level of the latest cycle quickly and then continues at a slower rate,
269
suggesting the increase of the surface hydroxyl group can exacerbate the competitive adsorption
270
which leads to a lower performance for ozone removal.
271
3.3 The Formation Energy of Oxygen Vacancy
272 273
Figure 6. The calculation results of oxygen vacancy formation energies at specific sites with varied
274
K content.
275
The process of oxygen vacancy formation often plays a key role in catalytic activity.41, 42 In
276
order to deeply understand the effect of K+ in the tunnels on the formation of oxygen vacancy, the
277
first-principles calculations are performed based on density functional theory as implemented in the
278
VASP code. The elaborated calculation method can be found in the Supporting Information. As
279
shown in Figure S9, in the framework of α-MnO2, each oxygen atom is coordinate with three 17
ACS Paragon Plus Environment
Environmental Science & Technology
280
manganese atoms.
281
three nearby Mn atoms to form the sp2 hybridization [O (sp2)], while other half locate out of plane to
282
form the sp3 hybridization [O (sp3)] with nearest manganese atoms. The oxygen vacancy formation
283
energy (Eform) at two specified sites (inset of Figure 6), with sp2 and sp3 hybridization respectively,
284
has been simulated in the absence or presence of different K+ concentration in the tunnels to present
285
us a tendency of oxygen vacancy formation energies. As shown in Figure 6, the oxygen vacancy
286
formation energy at the sp2 site dramatically decreases from 3.001 eV to 2.018 eV after 1 K+ is
287
constructed in the tunnel structure, and the formation energy keeps decreasing with the increase of
288
K+ concentration, corresponding to Hou’s results.30 The results indicate that the filled K+ can lead to
289
the electrostatic interaction between K+ and the lattice oxygen which is beneficial to the formation of
290
active oxygen vacancy. Besides, the effect of K+ is closely related to the distance between K+ and the
291
oxygen site. However, different results were obtained at the specific sp3 oxygen site. Without K+ in
292
the tunnels, the sp3 oxygen atom is faced with an asymmetrical force distribution which exhibits
293
lower Eform. However, when two K+ is constructed in the neighborhood of the specified oxygen atom,
294
a symmetrical force distribution forms, leading to a significant increase of oxygen vacancy formation
295
energies at sp3 oxygen atoms. So, the Eform first decreases and then increases with the growth of K+
296
content. Overall, the formation energy of oxygen vacancy is smaller at sp3 oxygen site, indicating
297
that the oxygen vacancy preferentially forms at sp3 oxygen site, corresponding to our former works.19
298
Therefore, tuning the K+ concentration in the tunnels appropriately will be an effective method to
299
enhance the content of oxygen vacancy.
300
3.4 The Schematic of Ozone Decomposition and Catalyst Regeneration.
Among them, half of the oxygen atom locate roughly in the same plane with the
18
ACS Paragon Plus Environment
Page 18 of 29
Page 19 of 29
Environmental Science & Technology
301 302
Figure 7. The schematic of ozone catalytic decomposition on the K-rich MnO2 (a); FT-IR spectra of
303
KOH-4h after reaction for different time (b); FT-IR spectra of MnO2 after reaction in different gas
304
flow (c); The TPD-MS profiles of KOH-4h before and after reaction (d); In situ DFTIR spectra of the
305
sample after reaction (e); High-resolution XPS spectra of KOH-4h before and after reaction (f).
306
The oxygen vacancy mechanism24, 43, 44 is generally accepted and our previous works also have
307
elaborated the effect of oxygen vacancy on the ozone decomposition.19 Firstly, one of the oxygen
308
atoms in the ozone molecule inserts into the surface oxygen vacancy and electrons transform from
309
Mn atom to ozone molecule, leading to the decomposition of ozone molecule into oxygen molecule
310
and oxygen species (O2-). Then, another ozone molecule reacts with the oxygen species and forms an
311
oxygen molecule and peroxide species (O22-). Finally, the peroxide species transforms into oxygen
312
molecule and the oxygen vacancy recovers. As shown in Figure 7a, the hydrothermal treatment in
313
KOH solution will induce the formation of oxygen vacancy. The more oxygen vacancy form, the
314
more active sites for ozone decomposition exist, resulting in a higher performance for ozone 19
ACS Paragon Plus Environment
Environmental Science & Technology
315
removal.
316 317
Figure 8. The FT-IR spectra of KOH-4h before reaction, KOH-4h after reaction and regenerated
318
KOH-4h (a); The ozone removal rate of the KOH-4h and regenerated KOH-4h (b).
319
However, the catalytic performance decreases with the reaction on, so the reason why the
320
catalyst deactivates is important for designing more effective catalyst. As can be seen in Figure 7b,
321
only the peaks around 3430 cm-1 and 1630 cm-1 can be found in the FT-IR spectra of fresh KOH-4h.
322
However, a new peak appears at 1380 cm-1 after the catalytic reaction, suggesting the surface
323
composition has changed in the process.45, 46 And the intensity of that peak increases with the extend
324
of the reaction time, indicating the peak at 1380 cm-1 results from the accumulation of intermediate
325
species. To further confirm the intermediate species, pure O2 was taken as the source gas to evaluate
326
the activity of KOH-4h and the FT-IR spectra of treated KOH-4h was shown in Figure 7c. The peak
327
appears whether the source gas is O2 or air, indicating that the intermediate species belongs to
328
surface oxygen species. The results of TPD-MS (Figure 7d) show that an oxygen desorption peaks
329
appear at 364 ºC, suggesting the intermediate species indeed belongs to oxygen species. To further
330
understand the thermostability of the intermediate oxygen species, in situ DFTIR has been carried
331
out. As shown in Figure 7e, the peak at 1380 cm-1 always exist even the temperature increased to 200 20
ACS Paragon Plus Environment
Page 20 of 29
Page 21 of 29
Environmental Science & Technology
332
ºC, suggesting that the intermediate oxygen species is relatively stable. However, Jia et al.24 reported
333
that the peroxide significantly decomposes at temperature less than 100 ºC from Raman spectrum.24
334
So, we speculate that the peroxide species (O22-)43, 47, 48 would evolve into a relatively stable oxygen
335
species, corresponding to the peak at 1380 cm-1, leading to the deactivation of the catalyst. The same
336
results can be obtained through the increase of the content of surface adsorbed oxygen (Figure S18)
337
and the AOS of Mn atom (Figure 7f). Therefore, the higher performance of KOH-4h results from the
338
abundant oxygen vacancy induced by K+, but the accumulation of intermediate oxygen species
339
causes the inactivation of the catalyst.
340
To reuse the catalyst, the deactivated KOH-4h has been calcinated in Ar atmosphere at 400 ºC
341
for 2 h to remove the accumulation oxygen species. As shown in figure 8a, the peak at 1380 cm-1
342
disappear after the deactivated KOH-4h has been calcinated. At the same times, the performance also
343
recovers partly (figure 8b), indicating that calcination in Ar atmosphere is an effective method to
344
regenerate the catalyst.
345 346
3.5 Implications and Future Direction of the Research.
347
In this work, the K+ content in the tunnel structure of α-MnO2 nanowire is increased dramatically
348
via a simply post-processing with KOH solution, generating abundant oxygen vacancy which leads
349
to a higher performance for ozone removal. Theoretical results show that the increase of K+ content
350
in the tunnels can decrease the formation energy of oxygen vacancy, which is beneficial for the
351
formation of oxygen vacancy in the crystal lattice. Experimental data also shows the AOS of Mn
352
decreases as the K+ content in the tunnels increases, meaning the formation of abundant oxygen
353
vacancy. The existence of active oxygen vacancy accelerates the decomposition of ozone. The K+ 21
ACS Paragon Plus Environment
Environmental Science & Technology
354
content can be controlled by adjusting KOH concentration and hydrothermal conditions. When the
355
as-synthesized α-MnO2 nanowire is treated in 1 M KOH solution for 4 h, the time possessed of 100 %
356
ozone removal rate at high space velocity (5.4 × 105 mL·g-1·h-1) can be increased from 3 h to 15 h.
357
In addition, the deactivation in high humidity is temporary and the activity would recover once the
358
humidity decrease. So, a high performance for ozone decomposition can be obtained by adding a
359
dehumidifier before the reactor. More importantly, the deactivated catalyst can be regenerated by
360
calcination in Ar atmosphere, which is significant for practical application.
361
Here, abundant active surface oxygen vacancy was fabricated by the electrostatic interaction
362
between oxygen atoms inside of the tunnels and introduced K+, which offer us a new perspective to
363
improve the catalytic performance for ozone removal. However, the results of FT-IR spectra show
364
peroxide species (O22-) can accumulate on the surface of the catalyst and evolve into a relatively
365
stable oxygen species, causing a decrease of the ozone removal rate. Therefore, the accumulation of
366
intermediate oxygen species is a key factor limiting ozone decomposition efficiently and sustainably
367
and need to be further researched.
22
ACS Paragon Plus Environment
Page 22 of 29
Page 23 of 29
Environmental Science & Technology
368
4. ASSOCIATED CONTENT
369
Supporting Information Available. Materials characterization methods, DFT calculation method
370
and other supplementary date are provided in the Supporting Information. The detail information
371
about the calculation in this study can be provided by contacting the corresponding author Qianfan
372
Zhang (
[email protected]). These materials are available free of charge via the Internet at
373
http://pubs.acs.org.
374 375
AUTHOR INFORMATION
376
Corresponding Author
377
a* Email:
[email protected] 378
b* Email:
[email protected] 379
Note
380
The authors declare no competing financial interest.
381 382
ACKNOWLEDGEMENTS
383
This work was partly supported by Chinese National Science Foundation (21437003, 21673126,
384
21621003, 21761142017) and Collaborative Innovation Center for Regional Environmental Quality.
385
23
ACS Paragon Plus Environment
Environmental Science & Technology
386
REFERENCE
387
1.
388
Short-term effects of various ozone metrics on cardiopulmonary function in chronic obstructive pulmonary disease
389
patients: Results from a panel study in Beijing, China. Environ. Pollut. 2018, 232, 358-366.
390
2.
391
low-pollution region. J. Occup. Environ. Med. 2017, 59, (7), 624-630.
392
3.
393
White, R. H.; Curriero, F. C., Health benefits from large-scale ozone reduction in the United States. Environ. Health
394
Perspect. 2012, 120, (10), 1404-1410.
395
4.
396
A.; Schwartz, J.; Mittleman, M.; Stone, P.; Horton, E.; Gold, D. R., Opposing effects of particle pollution, ozone,
397
and ambient temperature on arterial blood pressure. Environ. Health Perspect. 2012, 120, (2), 241-246.
398
5.
399
Johnson, B. J.; Tarasick, D.; Leblanc, T.; McDermid, I. S.; Jaffe, D.; Gao, R.; Stith, J.; Ryerson, T.; Aikin, K.;
400
Campos, T.; Weinheimer, A.; Avery, M. A., Increasing springtime ozone mixing ratios in the free troposphere over
401
western North America. Nature 2010, 463, 344.
402
6.
403
office equipment: A review of reported data and information needs. Atmos. Environ. 2008, 42, (7), 1371-1388.
404
7.
405
129-166.
406
8.
407
from carpets. Atmos. Environ. 2017, 148, 42-48.
Li, H.; Wu, S.; Pan, L.; Xu, J.; Shan, J.; Yang, X.; Dong, W.; Deng, F.; Chen, Y.; Shima, M.; Guo, X.,
Magzamen, S.; Moore, B. F.; Yost, M. G.; Fenske, R. A.; Karr, C. J., Ozone-related respiratory morbidity in a
Berman, J. D.; Fann, N.; Hollingsworth, J. W.; Pinkerton, K. E.; Rom, W. N.; Szema, A. M.; Breysse, P. N.;
Hoffmann, B.; Luttmann-Gibson, H.; Cohen, A.; Zanobetti, A.; de Souza, C.; Foley, C.; Suh, H. H.; Coull, B.
Cooper, O. R.; Parrish, D. D.; Stohl, A.; Trainer, M.; Nédélec, P.; Thouret, V.; Cammas, J. P.; Oltmans, S. J.;
Destaillats, H.; Maddalena, R. L.; Singer, B. C.; Hodgson, A. T.; McKone, T. E., Indoor pollutants emitted by
Dhandapani, B.; Oyama, S. T., Gas phase ozone decomposition catalysts. Appl. Catal., B 1997, 11, (2),
Abbass, O. A.; Sailor, D. J.; Gall, E. T., Effect of fiber material on ozone removal and carbonyl production
24
ACS Paragon Plus Environment
Page 24 of 29
Page 25 of 29
Environmental Science & Technology
408
9.
409
to the chemical erosion of squalene interfaces during ozonolysis. Environ. Sci. Technol. 2017, 51, (23),
410
13740-13748.
411
10. Weschler, C. J.; Nazaroff, W. W., Growth of organic films on indoor surfaces. Indoor Air 2017, 27, (6),
412
1101-1112.
413
11. Fadeyi, M. O.; Weschler, C. J.; Tham, K. W.; Wu, W. Y.; Sultan, Z. M., Impact of human presence on
414
secondary organic aerosols derived from ozone-initiated chemistry in a simulated office environment. Environ. Sci.
415
Technol. 2013, 47, (8), 3933-3941.
416
12. Waring, M. S.; Siegel, J. A., Indoor secondary organic aerosol formation initiated from reactions between
417
ozone and surface-sorbed d-limonene. Environ. Sci. Technol. 2013, 47, (12), 6341-6348.
418
13. Lian, Z.; Ma, J.; He, H., Decomposition of high-level ozone under high humidity over Mn–Fe catalyst: The
419
influence of iron precursors. Catal. Commun. 2015, 59, 156-160.
420
14. Abbass, O. A.; Sailor, D. J.; Gall, E. T., Effectiveness of indoor plants for passive removal of indoor ozone.
421
Build. Environ. 2017, 119, 62-70.
422
15. Yang, S.; Zhu, Z.; Wei, F.; Yang, X., Carbon nanotubes/activated carbon fiber based air filter media for
423
simultaneous removal of particulate matter and ozone. Build. Environ. 2017, 125, 60-66.
424
16. Gopi, T.; Swetha, G.; Chandra Shekar, S.; Ramakrishna, C.; Saini, B.; Krishna, R.; Rao, P. V. L., Catalytic
425
decomposition of ozone on nanostructured potassium and proton containing δ-MnO2 catalysts. Catal. Commun.
426
2017, 92, 51-55.
427
17. Gong, S.; Chen, J.; Wu, X.; Han, N.; Chen, Y., In-situ synthesis of Cu2O/reduced graphene oxide composite as
428
effective catalyst for ozone decomposition. Catal. Commun. 2018, 106, 25-29.
429
18. Ma, J.; Wang, C.; He, H., Transition metal doped cryptomelane-type manganese oxide catalysts for ozone
Heine, N.; Houle, F. A.; Wilson, K. R., Connecting the elementary reaction pathways of criegee intermediates
25
ACS Paragon Plus Environment
Environmental Science & Technology
430
decomposition. Appl. Catal., B 2017, 201, 503-510.
431
19. Zhu, G.; Zhu, J.; Jiang, W.; Zhang, Z.; Wang, J.; Zhu, Y.; Zhang, Q., Surface oxygen vacancy induced α-MnO2
432
nanofiber for highly efficient ozone elimination. Appl. Catal., B 2017, 209, 729-737.
433
20. Nikolov, P.; Genov, K.; Konova, P.; Milenova, K.; Batakliev, T.; Georgiev, V.; Kumar, N.; Sarker, D. K.;
434
Pishev, D.; Rakovsky, S., Ozone decomposition on Ag/SiO2 and Ag/clinoptilolite catalysts at ambient temperature.
435
J. Hazard. Mater. 2010, 184, (1), 16-19.
436
21. Hao, Z.; Cheng, D.; Guo, Y.; Liang, Y., Supported gold catalysts used for ozone decomposition and
437
simultaneous elimination of ozone and carbon monoxide at ambient temperature. Appl. Catal., B 2001, 33, (3),
438
217-222.
439
22. Tang, W.-X.; Liu, H.-D.; Wu, X.-F.; Chen, Y.-F., Higher oxidation state responsible for ozone decomposition at
440
room temperature over manganese and cobalt oxides: Effect of calcination temperature. Ozone: Sci. Eng. 2014, 36,
441
(5), 502-512.
442
23. Mehandjiev, D.; Naydenov, A.; Ivanov, G., Ozone decomposition, benzene and CO oxidation over
443
NiMnO3-ilmenite and NiMn2O4-spinel catalysts. Appl. Catal., A 2001, 206, (1), 13-18.
444
24. Jia, J.; Zhang, P.; Chen, L., Catalytic decomposition of gaseous ozone over manganese dioxides with different
445
crystal structures. Appl. Catal., B 2016, 189, 210-218.
446
25. Li, L.; Feng, X.; Nie, Y.; Chen, S.; Shi, F.; Xiong, K.; Ding, W.; Qi, X.; Hu, J.; Wei, Z.; Wan, L.-J.; Xia, M.,
447
Insight into the effect of oxygen vacancy concentration on the catalytic performance of MnO2. ACS Catal. 2015, 5,
448
(8), 4825-4832.
449
26. Wang, C.; Ma, J.; Liu, F.; He, H.; Zhang, R., The effects of Mn2+ precursors on the structure and ozone
450
decomposition activity of cryptomelane-type manganese oxide (OMS-2) Catalysts. J. Phys. Chem. C 2015, 119, (40),
451
23119-23126. 26
ACS Paragon Plus Environment
Page 26 of 29
Page 27 of 29
Environmental Science & Technology
452
27. Saputra, E.; Muhammad, S.; Sun, H.; Ang, H. M.; Tadé, M. O.; Wang, S., Different crystallographic
453
one-dimensional MnO2 nanomaterials and their superior performance in catalytic phenol degradation. Environ. Sci.
454
Technol. 2013, 47, (11), 5882-5887.
455
28. Yuan, Y.; Zhan, C.; He, K.; Chen, H.; Yao, W.; Sharifi-Asl, S.; Song, B.; Yang, Z.; Nie, A.; Luo, X.; Wang, H.;
456
Wood, S. M.; Amine, K.; Islam, M. S.; Lu, J.; Shahbazian-Yassar, R., The influence of large cations on the
457
electrochemical properties of tunnel-structured metal oxides. Nat. Commun.2016, 7, 13374.
458
29. Tseng, L.-T.; Lu, Y.; Fan, H. M.; Wang, Y.; Luo, X.; Liu, T.; Munroe, P.; Li, S.; Yi, J., Magnetic properties in
459
α-MnO2 doped with alkaline elements. Sci. Rep. 2015, 5, 9094.
460
30. Hou, J.; Liu, L.; Li, Y.; Mao, M.; Lv, H.; Zhao, X., Tuning the K+ Concentration in the tunnel of OMS-2
461
nanorods leads to a significant enhancement of the catalytic activity for benzene oxidation. Environ. Sci. Technol.
462
2013, 47, (23), 13730-13736.
463
31. Li, L.; King, D. L., Synthesis and characterization of silver hollandite and its application in emission control.
464
Chem. Mater. 2005, 17, (17), 4335-4343.
465
32. Meng, Y.; Song, W.; Huang, H.; Ren, Z.; Chen, S.-Y.; Suib, S. L., Structure–property relationship of
466
bifunctional MnO2 nanostructures: Highly efficient, ultra-stable electrochemical water oxidation and oxygen
467
reduction reaction catalysts identified in alkaline media. J. Am. Chem. Soc. 2014, 136, (32), 11452-11464.
468
33. Luo, J.; Zhu, H. T.; Liang, J. K.; Rao, G. H.; Li, J. B.; Du, Z. M., Tuning magnetic properties of α-MnO2
469
nanotubes by K+ doping. J. Phys. Chem. C 2010, 114, (19), 8782-8786.
470
34. Rong, S.; Zhang, P.; Yang, Y.; Zhu, L.; Wang, J.; Liu, F., MnO2 framework for instantaneous mineralization of
471
carcinogenic airborne formaldehyde at room temperature. ACS Catal. 2017, 7, (2), 1057-1067.
472
35. Hu, B.; Chen, C.-h.; Frueh, S. J.; Jin, L.; Joesten, R.; Suib, S. L., Removal of aqueous phenol by adsorption
473
and oxidation with doped hydrophobic cryptomelane-type manganese oxide (K−OMS-2) nanofibers. J. Phys. Chem. 27
ACS Paragon Plus Environment
Environmental Science & Technology
474
C 2010, 114, (21), 9835-9844.
475
36. Luo, J.; Zhang, Q.; Garcia-Martinez, J.; Suib, S. L., Adsorptive and acidic properties, reversible lattice oxygen
476
evolution, and catalytic mechanism of cryptomelane-type manganese oxides as oxidation catalysts. J. Am. Chem.
477
Soc. 2008, 130, (10), 3198-3207.
478
37. Yang, Y.; Huang, J.; Wang, S.; Deng, S.; Wang, B.; Yu, G., Catalytic removal of gaseous unintentional POPs
479
on manganese oxide octahedral molecular sieves. Appl. Catal., B 2013, 142-143, 568-578.
480
38. Peng, X.; Guo, Y.; Yin, Q.; Wu, J.; Zhao, J.; Wang, C.; Tao, S.; Chu, W.; Wu, C.; Xie, Y., Double-exchange
481
effect in two-dimensional MnO2 nanomaterials. J. Am. Chem. Soc. 2017, 139, (14), 5242-5248.
482
39. Liu, Y.; Zhang, P., Removing surface hydroxyl groups of Ce-modified MnO2 to significantly improve its
483
stability for gaseous ozone decomposition. J. Phys. Chem. C 2017, 121, (42), 23488-23497.
484
40. Chen, H.; Stanier, C. O.; Young, M. A.; Grassian, V. H., A kinetic study of ozone decomposition on
485
illuminated oxide surfaces. J. Phys. Chem. A 2011, 115, (43), 11979-11987.
486
41. Tompsett, D. A.; Parker, S. C.; Islam, M. S., Rutile (β-)MnO2 surfaces and vacancy formation for high
487
electrochemical and catalytic performance. J. Am. Chem. Soc. 2014, 136, (4), 1418-1426.
488
42. Tompsett, D. A.; Parker, S. C.; Islam, M. S., Surface properties of α-MnO2: Relevance to catalytic and
489
supercapacitor behaviour. J. Mater. Chem. A 2014, 2, (37), 15509-15518.
490
43. Li, W.; Gibbs, G. V.; Oyama, S. T., Mechanism of ozone decomposition on a manganese oxide catalyst. 1. in
491
situ Raman spectroscopy and ab initio molecular orbital calculations. J. Am. Chem. Soc. 1998, 120, (35),
492
9041-9046.
493
44. Knoops, H. C. M.; Elam, J. W.; Libera, J. A.; Kessels, W. M. M., Surface loss in ozone-based atomic layer
494
deposition processes. Chem. Mater. 2011, 23, (9), 2381-2387.
495
45. Roscoe, J. M.; Abbatt, J. P. D., Diffuse reflectance FTIR study of the interaction of alumina surfaces with 28
ACS Paragon Plus Environment
Page 28 of 29
Page 29 of 29
Environmental Science & Technology
496
ozone and water vapor. J. Phys. Chem. A 2005, 109, (40), 9028-9034.
497
46. Yang, L.; Hu, C.; Nie, Y.; Qu, J., Catalytic ozonation of selected pharmaceuticals over mesoporous
498
alumina-supported manganese oxide. Environ. Sci. Technol. 2009, 43, (7), 2525-2529.
499
47. Xi, Y.; Reed, C.; Lee, Y.-K.; Oyama, S. T., Acetone oxidation using ozone on manganese oxide catalysts. J.
500
Phys. Chem. B 2005, 109, (37), 17587-17596.
501
48. Jing, X.-L.; Chen, Q.-C.; He, C.; Zhu, X.-Q.; Weng, W.-Z.; Xia, W.-S.; Wan, H.-L., Mechanistic aspects of
502
photo-induced formation of peroxide ions on the surface of cubic Ln2O3 (Ln = Nd, Sm, Gd) under oxygen. Phys.
503
Chem. Chem. Phys. 2012, 14, (19), 6898-6904.
504
29
ACS Paragon Plus Environment