Dynamic Compression of in Situ Grown Living Polymer Brush: Simulation and Experiment K. Jalili,†,‡ F. Abbasi,‡ and A. Milchev*,†,§ †

Max Planck Institute for Polymer Research, 10 Ackermannweg, 55128 Mainz, Germany Institute of Polymeric Materials, Sahand University of Technology, P.O. Box 51335-1996, Tabriz, Iran § Institute for Physical Chemistry, Bulgarian Academy of Science, 1113 Sofia, Bulgaria ‡

S Supporting Information *

ABSTRACT: A comparative dynamic Monte Carlo simulation study of polydisperse living polymer brushes, created by surface-initiated living polymerization, and conventional polymer monodisperse brush, comprising linear polymer chains, grafted to a planar substrate under good solvent conditions, is presented. The living brush is created by endmonomer (de)polymerization reaction after placing an array of initiators on a grafting plane in contact with a solution of initially nonbonded segments (monomers). At equilibrium, the monomer density profile ϕ(z) of the LPB is found to decline as ϕ(z) ∝ z−α with the distance from the grafting plane z, while the distribution of chain lengths in the brush scales as c(N) ∝ N−τ. The measured values α ≈ 0.64 and τ ≈ 1.70 are very close to those predicted within the framework of the diffusion-limited aggregation theory, α = 2/3 and τ = 7/4. At varying mean degree of polymerization (from ⟨L⟩ = 28 to ⟨L⟩ = 170) and effective grafting density (from σg = 0.0625 to σg = 1.0), we observe a nearly perfect agreement in the force−distance behavior of the simulated LPB with own experimental data obtained from colloidal probe AFM analysis on PNIPAAm brush and with data obtained by Plunkett et al. [Langmuir 2006, 22, 4259] from SFA measurements on the same polymer.

I. INTRODUCTION After the recent advances in the nanostructuring of surfaces, polymers can now be end-grafted on nanometer scale structures.1,2 The recent progress in the production of nanoscale polymer structures has, however, only partially been matched by advances in the experimental methods of measuring the properties of such systems.3 Available contactless methods, for example, optical methods, average the brush properties over areas that are larger than the nanoscale so that fine spatial resolution is lost. To retain sufficient spatial resolution, atomic force microscopy (AFM) is conventionally used.4−7 However, the necessary contact between the AFM tip and the polymer thin layer distorts the layer and thus the object that it intends to study.8 AFM measurements of polymers, tethered on surfaces with various geometries, illustrate a more general and fundamental class of problems, namely, the response of soft matter to external forces. Polymer brushes, that is, densely packed arrays of polymer chains end-attached to an interface, have been studied extensively (for reviews see refs 7 and 9−13) due to their ability to modify surface properties, prevent colloid aggregation, and enhance lubrication or adhesion.7,14−16 When properly designed, polymer brushes in good solvent conditions have been shown to remarkably reduce friction.17 The brush structure and its properties can be controlled by tuning the © 2012 American Chemical Society

grafting density and variation of polymer molecular weight, temperature, and solvent quality.18 Numerous theoretical,19−26 experimental,27−31 and simulational32−45 studies have examined the structure and properties of polymer brushes. There exist, however, sometimes significant differences between the theoretical and the experimental investigations of polymer brushes. So most theories assume strong stretching of polymer chains in the brush, while it is hard for an experimentalist to achieve densities high enough so as to meet this assumption.46 The polydisperse nature of the synthesized brushes poses another significant difference. While it is practically impossible for an experimentalist to produce a perfectly monodisperse polymer brush, to the best of our knowledge, most of the theoretical works so far have not taken into consideration the intrinsic polydispersity of the brushes with a realistic chain length distribution; see, however, the early work of Milner et al.47 The interaction between an AFM tip and a nanodesigned polymer brush bears resemblance to the problems mentioned above. Previous works on the interaction between a uniformly grafted polymer brush and an external object usually neglected Received: August 21, 2012 Revised: October 27, 2012 Published: November 30, 2012 9827

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

monodisperse polymer brush, computing the density ϕ is not possible from the knowledge of the force F aloneinstead, additional information about the brush is needed,65 such as its grafting density, σg, and this information frequently might not be available. Still, for the case of monodisperse polymer brush, a relation between F and ϕ always exists, and it also does not depend on the transversal position of the AFM tip. All of this changes when a polydisperse polymer brush is considered instead. Even for the same brush, identical values of the force F now correspond to different values of the density ϕ (or some other quantity of interest). This hinders a deeper understanding of the polymer brush properties via direct interpretation of AFM results. Thus, the need to understand the response of polydisperse polymer brushes to local external forces is both fundamental and practical. In this article, we first grow the polydisperse living polymer brush (LPB) in situ, monomer by monomer, from a functionalized seed carrying polymerization initiators that is representative for a wider range of realistic systems. We then perform coarse-grained off-lattice Monte Carlo (MC) simulations66,67 of the interaction between the polydisperse living brush and a piston as representative for the AFM tip. The simulations represent roughly 2000−20 000 g/mol chains (30− 260 coarse-grained monomers per chain) over a range of grafting densities. The high grafting densities examined in this study are achievable experimentally by “grafting from” techniques such as atom transfer radical polymerization (ATRP).68,69 Anticipating, we observe good agreement between simulational and experimental force−distance relationships. The outline of the remainder of the paper is as follows. In section II we sketch briefly the basis of the analytical treatment of LPB and the principal properties of living polymer brushes. In sction III we introduce the Monte Carlo model, employed in our study, and elucidate the salient features of the underlying algorithm. The steric repulsion exerted on an impenetrable and semipermeable wall in compression experiments with in situ grown LPB is presented in section V. In this section, we ask what happens when a layer of polydisperse polymer chains, grafted to a planar substrate by special groups, is subjected to external force (such a AFM tip). We also examine the effect of keeping the concentration of single nongrafted monomers in the box constant by using a semipermeable wall so that the mean degree of polymerization in the brush does not change when the wall is moved. In section VI, the comparison between experiment and simulation is presented in more detail in view of our own experimental data obtained from colloidal probe AFM measurements. We briefly discuss the physical significance of the conversion factors for chain conformation sizes and length scales in real application, from the simulation to experiment. Eventually, in section VII, we end this work by a brief summary of our findings.

effects of polydispersity and high grafting density of the tethered chains48−53 even though the properties of living polymers in the bulk have been considered by Flory,54 Wheeler,55 Pfeuty,56 and others. A step toward understanding the role of polydispersity in soft matter outdoor response was done by the investigation of “equilibrium polymers” (EP) as summarized in ref 57. EPs (or living polymers) denote polymer solutions where the chains are dynamic objects with the unique feature of constantly fluctuating lengths. Subject to external perturbation, concentration, or temperature change, they are able to respond via polymerization−depolymerization reactions allowing new thermodynamic and chemical equilibrium to be established. An important example of such constant process of dynamic equilibrium between polymers and their respective building units is that of surfactant molecules forming long flexible cylindrical aggregates, the so-called wormlike giant micelles (GM),57 which break and recombine constantly at random points along the sequence. EPs are intrinsically polydisperse, and their molecular weight distribution (MWD) in equilibrium is expected58,54 to follow an exponential decay with chain length. An efficient way to create polymer brushes is the growth of living polymer chains from active sites on a surface whereby brushes with given polydispersity index and grafting density can be synthesized.59,60 One of the earliest works investigating theoretically the growth of polymer chains from a surface was carried out by Wittmer et al.,61 combining elements of diffusion-limited aggregation (DLA)62 with the theory of polydisperse strongly stretched polymer brushes.19,63 Generalizing the “needle growth” problem,64 they considered the formation of the brush as a particular case of diffusion-limited aggregation without branching (DLAWB). The interaction between a polydisperse grafted layer, commonly referred to as living polymer brush (LPB), and an AFM tip is similar to that of a polymer layer with a particle of mesoscopic size. A theoretical discussion of the latter has already been presented by Subramanian et al.50 Their treatment considered both dense brush (high grafting density) and “mushroom” (low grafting density) regime. For fixed brushes, in which the anchoring points on the surface are immobile, they assumed that when the particle is pushed against the grafted chains, these chains undergo pure compression and do not splay. Under such an assumption, the force of compression (force F divided by cross-sectional area of the compressing particle A) per unit area, F/A, does not depend on the radius of the compressing particle and is identical to the force for a brush pressed by a flat (infinite radius) plate. In the mushroom regime, they allowed the chains to deform and escape compression, and in this case Subramanian et al.50 found that the chains do splay to the side to avoid being compressed. A nanopatterned polydisperse polymer brush, however, is a much more complex system as its distributed correlation length is of the same order as the size of the system. Therefore, the brush can evade to the side, which is impossible for the monodisperse grafted brush, making the nanopatterned polydisperse brush effectively “softer”. The force measured in an AFM experiment is rarely the quantity that one is ultimately interested in. The noteworthy exception to this statement are studies of the chemical nature of the brush surface where the degree of sticking is the soughtafter information.5 In most other cases, the measured force F first has to be converted, or “gauged”, to yield, for example, the brush density ϕ. However, already for a homogeneously

II. THEORETICAL FRAMEWORK A. Analytical Predictions of the Distribution of Chain Length. On a coarse-grained level, systems of living polymers are characterized by the monomer volume fraction ϕ, the energy difference E between saturated and unsaturated bond states, the persistence length lp, and the excluded volume size b of the monomer. For chains that are long compared to persistence length lp, reversibility of the self-assembly process 9828

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

plane in a good solvent, one expects Fchain(N) = τ ln(N) with the exponent τ = 1 − γs where the universal “surface” exponent γs ≈ 0.65 < 1. Hence, one expects to find a weakly singular c(N) ∝ N−τ exp(−μ1N). Thus, in a weakly stretched polymer brush at low grafting density σg, when the living polymers do not overlap strongly, the excluded volume interactions are expected to favor longer chains which can explore broader regions of the living polymer brush. This would lead to a power law MWD (plus exponential cutoff). Therefore, for a self-similar mushroom structure of the living polymer brush with blob size ξ(z) ∝ z the monomer density would scale as ϕ(z) ∝ z−α, α = (3ν − 1)/ν. The chain-end density, like the blob density, ρe(z) ∝ 1/ ξ(z)3 ∝ z−β with β = 3. Since c(N) dN = ρe(z) dz, one readily finds a power-law distribution, c(N) ∝ N−τ with τ = 1 + 2ν ≈ 11/5. In contrast, assuming that the polymer brush may be viewed as a compact layer of concentration blobs ξ(z) ∝ ϕ(z)−ν/(3ν−1), within the Alexander−de Gennes picture of a strongly stretched brush (the so-called strong stretching limit, SSL), the chains are described within the self-consistent field theory approach (SCFT) as classical trajectories, which are strongly stretched at distances, larger than ξ. If scaling holds, one may then use power-law functions to express ϕ(z) ∝ z−α, ρe(z) ∝ z−β, c(N) ∝ N−τ, and z(s) ∝ sν⊥, as in the case of the weak stretching limit. Assuming that in the SSL a living polymer brush may be considered as grown by diffusion-limited aggregation (DLAWB) without branching, one obtains then a set of exponents86 as α = 2/3, β = 2, τ = 7/4, and ν⊥ = 3/4.61 Indeed, one can verify that these theoretical predictions agree well with earlier MC simulation results86 and our present observations (see below) of a dense LPB in equilibrium. Given that the DLAWB model61 pertains to a steady-state process of brush growth under irreversible polymerization in conditions of adiabatically slow influx of free monomers, this result appears somewhat surprising. Even if one could provide some arguments that the structure of a steadily growing “needle forest” under certain conditions may be viewed as close to that of a LPB in dynamic equilibrium, the two cases clearly differ, and this interesting result (whose study is beyond the scope of the present study) certainly needs special investigation. Regarding the force exerted by a polymer brush on a plane at distance D from the grafting surface, the problem was first considered using the Alexander−de Gennes19 model; one assumes that the force is strictly zero for h < D (corresponding to zero osmotic pressure at the outer end of the brush). Using a Flory type argument, one estimates a force−distance relation73

ensures that the molecular weight distribution (MWD) c(N) of the polymeric species is in thermal equilibrium. Polymer brushes are usually created by means of surface-initiated polymerization79 and are characterized by non-negligible polydispersity.80 A large variety of synthetic routes for the generation of polymer brushes include, e.g., ionic,81 ringopening (ROP),82 atom transfer radical (ATRP),83 and reversible addition−fragmentation chain transfer (RAFT)84 polymerization. Most frequently in living polymers one observes a Flory− Schulz molecular weight distribution (MWD) of chain lengths: c(N ) = (1 − pr )pr

N−1

N−1 M0 ⎛ M0 ⎞ = ⎟ ⎜1 − Mn ⎝ Mn ⎠

(2.1)

where c(N) is the fraction of chains with length N, pr ≤ 1 is the probability that a monomer has reacted, M0 is the molecular weight of a monomer, and Mn is the number-averaged molecular weight. Physically, eq 2.1 reflects a case when the reactivity of building units is independent of macromolecular weight. In the case of dilute chains in the bulk, it has been shown that the MWD takes the form of Schulz−Zimm distribution85 γ− 1 ⎛ γγ ⎛ l ⎞ l ⎞ ⎜ ⎟ exp⎜ −γ c(l) = ⎟ Γ(γ ) ⎝ ⟨L⟩ ⎠ ⎝ ⟨L⟩ ⎠

(2.2)

and a mean chain length is given by ⟨L⟩ ∝ ϕα exp(δE)

(2.3)

In eqs 2.2−2.3 one has57 α = δ = (1 + γ)−1 whereby γ ≈ 1.165 in three dimensions. In living polymers the semidilute conditions correspond to the case L* ≪ ⟨L⟩ and ϕ > ϕ*, where L* and ϕ* mark the mean chain length and the density at crossover regime. Eventually, proceeding as in the ideal case, one may recover in the semidilute case a simple exponential expression for the molecular weight distribution c(l) =

⎛ l ⎞ ϕ exp⎜ − ⎟ 2 ⎝ ⟨L⟩ ⎠ ⟨L⟩

(2.4)

with a slightly different expression for the average polymer length ⟨L⟩ ∝ ϕα exp(δE),

δ=

1 2

(2.5)

where α = /2[1 + (γ − 1)/(3ν − 1)] ≈ 0.6. Turning now from living polymers in the bulk to a living polymer brush (LPB), one retains the unique feature that the chains are dynamic objects with constantly fluctuating lengths. Subject to external perturbation, inter alia to pressure through a piston, they are able to respond dynamically via polymerization−depolymerization reactions allowing new thermodynamic equilibrium to be attained. Here we consider a typical case of living ionic polymerization whereby chains grow from initiators, fixed on a grafting plane, by end-monomer-mediated attachment−detachment events whereby the total number of chains remains constant. Making use of scaling considerations,57 one may try to predict the power law exponents that govern LPB structure under various conditions. In the simplest case of dilute nonoverlapping living polymers (mushrooms), tethered to a 1

57

f ̃ (D) =

kBThσg 3/2 ⎡⎛ h ⎞5/4 ⎛ D ⎞7/4 ⎤ ⎢⎜ ⎟ − ⎜ ⎟ ⎥ , ⎝ h ⎠ ⎥⎦ 2a3D ⎢⎣⎝ D ⎠

h>D (2.6)

The first term in eq 2.6 stems from the contribution to free energy due to confinement whereas the second term is due to the energy of stretching. Note that for small relative compression ε = 1 − D/h the force f ̃ scales linear in ε. Here σg is the grafting density, h is the theoretical brush height (thickness), kB is the Boltzmann constant, and T denotes the temperature. Regarding the force of interaction, f, for the geometry of a grafted plane and a spherical body of radius R at distance D between the surfaces can be described by a slightly modified equation74−77 9829

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

Figure 1. (a) Plots of bonded (FENE) and nonbonded (Morse) interactions used in the present model. The shaded area denotes distances where scission−recombination events may take place. (b) Two-dimensional projection of the living polymerization−depolymerization process with corresponding rates of polymerization kp and depolymerization kd: chains consists of successively connected bonds, labeled by pointers. The pointers of end-bonds point to NIL (red particles). The breaking of a saturated bond ibond requires to set the pointers of the two connected bonds ibond and jbond = pointer(ibond) to NIL (yellow particles, 2, 4). Setting pointer(3) = 1 and pointer(1) = 3 connects the end-monomer imon = 1 and the individual reacting monomer jmon = 3.

⎤ 8kBThσg 3/2 ⎡ ⎛ h ⎞5/4 f ⎛ D ⎞7/4 ⎢7⎜ ⎟ + 5⎜ ⎟ − 12⎥ = ⎝h⎠ ⎢⎣ ⎝ D ⎠ ⎥⎦ R 35

spring algorithm for polymer chains (for technical details see ref 89), and this off-lattice scheme is characterized by the bonded and nonbonded interactions shown in Figure 1a. It is clear that in a system of EP where scission and recombination of bonds constantly take place the particular scheme of bookkeeping should be no trivial matter.90 Since selfassembled EP chains are only transient objects, the data structure of the chains can only be based on the individual monomers or, rather, on the saturated or unsaturated bonds of each monomer.57 As sketched in Figure 1b, in the polymerized and depolymerized (recombination and scission) state a reacting monomer 1 is either randomly linked to another reacting monomer 2 through a given bonding potential and thus contributes to the final conformation of the polymer chain, or nonbonded, belonging thus to the fully free single reacting monomers (yellow particles). It is further imposed that in the state in which living polymerization and depolymerization events take place simultaneously (Figure 1b), the polymerizing monomer is located within the region of low intermolecular energy determined by a suitable bonding potential. Note that active chain ends do not react (recombine) with one another. Using the assumption that no branching of chains is permitted, each bond is considered as a pointer, originating at a given monomer and pointing to the respective other bond with which the couple forms a nearest neighbor (brown particles), or to NIL (red particles), if the bond is free (unsaturated). The two possible bonds of each monomer imon are called ibond = imon and ibond = −imon. No specific meaning (or direction) is attached to the sign, and this is merely a convenience for finding the monomer from the bond list: imon = |ibond|. Pointers are taken to couple independently of sign, and the bonds are coupled by means of a pointer list in a completely transitive fashion. In the LPB, only two simple operations are required for polymerization or depolymerization processes. Unsaturated bonds at chain ends point to NIL (nowhere), and only these bonds may recombine (pair) with the unsaturated bond of a free monomer. Therefore, the main difference with respect to EPs is that the monomer may attach or dissociate reversibly only to/from end-monomers of grafted LPB chains (following

(2.7)

where the constant term is included to ensure that the force goes to zero when h = D. Equation 2.7 has been used also by Plunkett et al.72 While the theoretical results, eqs 2.6 and 2.7, have been derived for monodisperse brushes, it is also interesting to examine the effect of polydispersity on the effective mean height of a polymer brush and the ensuing force exerted by the polymer brush on a plane upon compression. As shown by Milner, Witten, and Cates,20 the height of a polydisperse brush within the SSL-SCFT is66 h[σg ] =

12 π2

∫0

Nmax

dn

3

σg − σg(n)

(2.8)

where σg(n) is the grafting density of chains per unit area of length less than n. Therefore, one can estimate that the effective height h(Δ) = h0(1 + Δ/(2N̅ )) (e.g., for a narrow uniform molecular weight distribution) increases as a square root of the variance Δ2, where Mw/Mn = 1 + Δ2/(3N̅ 2). Accordingly, at small compression the repulsive force of the polydisperse brush increases and is always larger than that of a monodisperse polymer brush with chains of length equal to the mean length of the polydisperse brush N̅ . At large compression, the two forces should be identical.78 For a broad distribution c(N), cf. eq 2.2, this effect may also be estimated, and one would expect a quartic force law up to compressions of order h.78

III. METHOD: MODEL AND SIMULATION ASPECTS We use a coarse-grained off-lattice bead−spring model to describe the polymer chains in our two systems: LPB and MPB. As far as for many applications in a biological context rather short grafted chains are used,88 and in order to do a reasonable comparison, we restrict ourselves to the range of ⟨L⟩ = 28−170 and N = 32, 64, and 128 at various grafting densities σg in the cases of LPB and MPB, respectively. A. Living Polymer Brush (LPB). For the off-lattice version presented here we have now harnessed a very efficient bead− 9830

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

where J corresponds to the constant scission energy. Note that UFENE(l = l0) = −J and UFENE near its minimum at l0 is harmonic, with K being the spring constant, and the potential diverges to infinity both when l → lmax and l → lmin = 2l0 − lmax. Following ref 90, we choose the parameters lmax − l0 = l0 − lmin = 0.3 and K/kBT = 20, T being the absolute temperature. The units are such that the Boltzmann constant kB = 1. The nonbonded interactions between brush and free chain segments are described by the Morse potential, r being the distance between the beads

the model definition sketched in Figure 2), and no explicit distinction between the end-monomers, middle monomers, or free monomers is required.

UM(r ) = exp[− 2α(r − rmin)] − 2 exp[−α(r − rmin)] εM (3.2)

with parameters α = 24, rmin = 0.8, and εM/kBT standing for the strength of monomer−monomer interactions. In our present study we take typically εM/kBT = 0.2, which corresponds to good solvent conditions since the Θ-point of the coil−globule transition for a (dilute) solution of polymers described by the model, eqs 3.1 and 3.2, has been estimated66 as kBΘ/εM ≈ 0.62. The model can be simulated fairly efficiently with a dynamic MC algorithm, as described previously.66,91 The trial update involves choosing a monomeric unit at random and attempting to displace it randomly by displacements Δx, Δy, and Δz chosen uniformly from the interval −0.5 ≤ Δx, Δy, Δz ≤ 0.5. The transition probability for the attempted move is calculated from the δU of the potential energies before and after the move as W = exp(−ΔU/kBT). Moves are then accepted according to the Metropolis criterion, if W exceeds a random number uniformly distributed in the interval [0,1) and one Monte Carlo Step (MCS) involves as many attempted moves as there are monomers in the system. In addition, during each MCS as many bonds as there are initiators in the system are chosen at random at the active ends of the grafted chains, and an attempt is made to break them according to the Metropolis algorithm. Attempts are also made to create new bonds between the endmonomers and free monomers within the potential range of UM (i.e., a new bond with energy UFENE). In order to keep the system in equilibrium with the ambient phase of single free monomers and prevent the longer polymer chains from touching the top of the container, we have used a

Figure 2. Schematic representation of the model LPB growth between two parallel plates. Polymer chains grow reversibly from the initiator molecules (red spheres) fixed on the impenetrable bottom wall. They are in thermal equilibrium with a reservoir of free monomers (gold spheres). We suppose that both the scission energy J and the activation barrier are independent of the monomer position (along the chain contour as well as in space) and density. Desorption events occur only at the active chain ends (green spheres) and chains are not allowed to break along the backbone. Branching of chains is forbidden as well. The opposite im(semi)permeable wall is a bare surface at distance z from the grafting plane.

As an example, Figure 3 shows snapshot pictures of LPB corresponding to mean chain length ⟨L⟩ = 32 (left) and ⟨L⟩ = 64 (right) and grafting density σg = 1.0. Each bond is described by a shifted FENE potential ⎡ ⎛ l − l 0 ⎞2 ⎤ UFENE(l) = −K (lmax − l0)2 ln⎢1 − ⎜ ⎟⎥−J ⎢⎣ ⎝ lmax − l0 ⎠ ⎥⎦ (3.1)

Figure 3. Snapshot picture of two LPB with σg = 1.0, ⟨L⟩ = 32 (left part) and σg = 1.0, ⟨L⟩ = 64 (right part) in their unperturbed states. The substrates are highlighted by cyan color and the opposite walls are in green color, while monomers of polydisperse brush belonging to short and long chains are displayed by different colors for more distinction. The ambient free monomers are not displayed for the sake of clarity. Only the shorter chains do sufficiently overlap and, hence, are somewhat stretched by the density gradient. 9831

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

rather low value of the bond energy J = 2.0. The lattice constant s of the square grid of activated initiators is taken as a rule as s = 1 for the case of a dense brush and, as a special case of a loose mushroom-like layer, s = 4. In the z-direction the simulation box is bound by smooth (unstructured) impenetrable walls using the so-called Weeks− Chandler−Andersen (WCA) potential, UWCA(r) (i.e., by the shifted and truncated repulsive branch of the Lennard-Jones potential) (cf. Figure 2)

The second wall is placed originally at a far enough distance from the grafting plane such that it does not affect the chain configurations for the chain length considered in the simulations. We study the system of polymer chains consisting of N monomer with N = 32, 64, and 128 for the highest value of grafting density σg = 1.0. Periodic boundary conditions were applied in the xy direction. The brush was created in a fully stretched configuration and was then equilibrated over times much longer than the longest relaxation time τR of an single chain with excluded-volume interactions to obtain totally independent and relaxed start configuration for compression runs. It is well-known92 that for a chain with N beads and under excluded-volume interactions the largest (Rouse) relaxation time τR is given by, in units of N, τR ≈ 0.25N2.19 in the absence of explicit solvent. In the monodisperse case, we have equilibrated the system for a time τ = 10τRMCS. Same as the LPB system, in the MPB case, each bond is described by FENE potential where a bond of length l has a maximum at lmax = 1.0 (eq 3.1), and the nonbonded interaction between effective monomers is described by a Morse-type potential (eq 3.2).

⎧ ⎡⎛ r ⎞12 ⎛ r ⎞6 ⎤ 0 0 1/6 ⎪ ⎪ 4ε⎢⎝⎜ ⎠⎟ − ⎝⎜ ⎠⎟ ⎥ + ε , for r ≤ 2 r0 r r ⎦ UWCA(r ) = ⎨ ⎣ ⎪ ⎪ 0, for r > 21/6r0 ⎩ (3.3)

which prevents particles from leaving the container. In eq 3.3 we set r0 = 1.0. Thus, while the substrate plane is fixed at z = 0, the top wall can be shifted in vertical direction like a piston to some desirable height Ztop whereby all particles at distances closer than Ztop − r0 to it are subject to repulsive force taken as the derivative of eq 3.3. Typically, boxes of size Lx × Ly × Lz and periodic boundary conditions in x and y directions have been used in the simulations with Lx = Ly = 16 and 32 and 64 ≤ Lz ≤ 256 (all length in units of lmax) for systems from Mt = 4096 up to 32 768 monomers. Before starting to derive statistical averages, the grafted living polymer brush is equilibrated by MC method for a period of 107 MCS (depending of the average chain length ⟨L⟩ this period is varied) whereupon one performs 100 measurement runs, each of length 5 × 107 MCS. In order to calculate the force, resulting from compression of the LPB, the simulation starts with a well-equilibrated in situ grown dense LPB (σg = 1.0) containing chains of, say, ⟨L⟩ = 32 and the upper wall far enough above the top of the LPB so that it is not in contact with the brush. The wall is then gradually pushed down against the brush with different moving rates along a line normal to the grafting surface. After moving the wall to a specified distance from the grafting surface, the position of the wall is held fixed and measurements are carried out. B. Homogeneous Monodisperse Polymer Brush (MPB). In this case we also used the efficient off-lattice Monte Carlo method with the first monomer of each chain being rigidly fixed to grafting sites that are arranged regularly on a square lattice as shown in Figure 4 . The grafting surface is located at z = 0.0, and a second nonadsorbing wall is put at Lz.

IV. EXPERIMENTAL STUDIES Materials. N-Isopropylacrylamide (NIPAAm, Aldrich, 97%) was purified by passing through an inhibitor removal column using a mixture of dichloromethane and hexane (v/v ≈ 1:1) as the solvent and then recrystallized twice from a toluene/hexane solution (50% v/v) and dried under vacuum prior to use. Copper(I) bromide (CuBr, Aldrich, 98%) was purified by stirring in glacial acetic acid, filtering, and washing with ethanol three times, followed by drying in vacuum at room temperature overnight. Copper(II) bromide (Sigma-Aldrich, ≥99%), N,N,N′,N″,N″-pentamethyldiethylenetriamine (PMDETA; 98%, Acros Organics), ethyl 2-bromoisobutyrate (E2Br-iB, 98%, Aldrich), (3-aminopropyl)trimethoxysilane (APTMOS, 99%, Acros), bromoisobutyryl bromide (BIBB, 99%, Aldrich), and anhydrous toluene (Merck) were used as received. Milli-Q water (with a minimum resistivity of 18.2 MΩ·cm) was obtained from a Millipore Direct-Q 5 ultrapure water system. THF for reactions and washings were dried by sodium before use. Double-sided polished silicon wafers (P-doped, (100)-oriented, 10−20 Ω·cm resistivity, 0.56 mm thickness) were supplied by University Wafer Company (Boston, MA) and cut into 5 × 5 mm2 pieces using a Micro Ace Series 3 dicer (Loadpoint Ltd., England). Ultrahigh-purity-grade argon was used in this study. Initiator Synthesis. The ATRP initiator, 2-bromo-2-methyl-N-3[(trimethoxysilyl)propyl]propanamide (BrTMOS), was synthesized using a procedure modified from the literature:93 To a stirred solution of APTMOS (1.79 g, 10 mmol) and triethylamine (1.01 g, 10 mmol) in 50 mL of dried THF, BIBB (3.45 g, 15 mmol) was added dropwise at 0 °C for 2 h under argon. The reaction was heated to room temperature and kept for 12 h with stirring and under argon protection. The precipitate was filtered off using a frit funnel. The product was a yellowish oil after the removal of the solvent. The product was redissolved with CH2Cl2 (20 mL) and washed with 0.01 N HCl (2 × 20 mL) and cold water (2 × 20 mL). The organic phase was dried with anhydrous CaCl2. After the removal of the solvent, the final product was a colorless oil with a yield of 90.5%. 1H NMR (300 MHz, CHCl3): 6.91 (s, 1H, NH), 3.49 (s, 9H, SiOCH3), 3.25 (t, 2H, CH2N), 1.95 (s, 6H, CH3), 1.68 (m, 2H,CH2), 0.67 (t, 2H, SiCH2). 13 C NMR (600 MHz, CHCl3): 171.98, 62.57, 50.29, 42.62, 32.44, 22.52, 7.64. Surface-Initiated Atom Transfer Radical Polymerization (SIATRP). Silicon wafers were sonicated for 5 min in ethanol and water, activated for 30 min at 150 °C in piranha solution (H2O2 (30 wt % in H2O)/H2SO4 (98 wt %), v/v ≈ 3:7) (caution: piranha solutions are strongly oxidizing and should not be allowed to contact organic solvent), thoroughly rinsed with water and ethanol, and dried in a stream of argon. A self-assembled monolayer (SAM) of the ATRP initiator was

Figure 4. Snapshot of a MPB with chain length N = 32 at grafting density σg = 1.0 at equilibrium. Polymer chains are red, substrate atoms are cyan, and upper wall is green. Solvent particles are omitted for clarity. 9832

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

Figure 5. (a) Density profile of LPB, ϕp(z), at different temperatures (in units of kBT) for LPB with total density of the system ϕt = 0.5 at σg = 1.0. (b) Double-logarithmic plot of density profiles at different temperatures, confirming the scaling behavior ϕ(z) ∝ z−α. attached to the silicon wafer by immersion in a 10 mM solution of BrTMOS in dry toluene at room temperature overnight. Next, the wafers were rinsed with anhydrous toluene, sonicated for 1 min in acetone and in a water/tert-butanol mixture (v/v ≈ 1:1), rinsed with water, dried in a stream of argon, and transferred to the appropriate reactors for the polymerizations. SI-ATRP of NIPAAm monomer was carried out at room temperature from a monolayer containing the SAM-Br initiator as follows: A mixture of MeOH/H2O (v/v ≈ 1:1) was degassed through four freeze−pump−thaw cycles before being introduced into the controlled atmosphere glovebox. NIPAAm (5.0 g, 44 mmol), CuBr (40.0 mg, 0.278 mmol), CuBr2 (14 mg, 0.063 mmol), and PMDETA (175 mL, 0.835 mmol) were dissolved in 30 mL of MeOH/H2O inside the glovebox. The solution was then transferred via a cannula into a vial containing silicone wafer with uniform initiator SAM and sacrificial initiator E2Br-iB (10 mL, 0.07 mmol), and then vial was sealed and kept at room temperature for polymerization. After polymerization for a times ranging from 30 to 120 min, the substrate was removed from the vial and rinsed with a copious amount of DI water, followed by sonication in EtOH and then H2O. After drying with a stream of argon, the samples were stored under ultrahighpurity-grade argon. AFM Measurements. Force measurements were carried out with a NanoScope IIIa multimode atomic force microscope (Digital Instruments, Veeco-Bruker, Santa Barbara, CA) equipped with a standard liquid cell on SI-ATRP grown PNIPAAm films in a liquid environment filled with deionized water. One micrometer in diameter SiO2 colloidal probe (Novascan Technologies, Inc., Ames, CA) with a spring constant of 0.050 ± 0.003 N m−1 (determined using the thermal tune method) and a diameter of 1.00 ± 0.006 μm (determined by a scanning a tip array) was used in the experiments. PNIPAAm-coated wafer was placed on liquid cell, degassed DI water was injected into the cell, and then the film was allowed to equilibrate for 1 h. The AFM cantilever was then set on top of the sample and started to move toward the sample surface with Z-ramp size of 2 nm and a dwell time of 100 ms per step. Cantilever deflection was recorded and averaged at each interval until tip−sample forces caused a deflection by 10 nm, after which the cantilever was withdrawn from the surface in the same manner.

after a T-quench from an initial equilibrium state at kBT = 1.0. It should be noted that all profiles are normalized to unity as ∫ z0ϕ(z) dz = 1. Evidently, in logarithmic coordinates (Figure 5b), one observes a power law decay of the density profiles, ϕ(z) ∝ z−α, manifested as a straight line, whereby the observed power α ≈ 0.64 at T = 1.0 is shown to be in good agreement the theoretically expected one α ≈ 2/3.86 The data shown in Figure 5 correspond to equilibrated LPBs whereby the total monomer concentration in the container has been kept constant. We observe the same value of the exponent α when the temperature is further increased. Small deviations from the expected scaling behavior are found only during quenching of LPB chains to lower temperatures (Figure 5b) for the higher z. We believe that this is probably due to single rather long chains which get repelled by the ceiling of the simulation container and bend backward, increasing the local monomer density under the upper plane of the box. The reader may get impression about such effects from the snapshots shown in Figure 6 where we display the variation of the average chain length ⟨L⟩ in a LPB with the total monomer concentration ϕt.

V. SIMULATION RESULTS As far as our main concern in this work is the comparison of experimentally measured compression force of a LPB with data, we mention very briefly some related results obtained from our Monte Carlo simulation. An interesting question thereby is to what extent the structure of the LPB meets theoretical predictions, mentioned in section II. Therefore, in Figure 5a we present the observed density profiles of grafted monomers, ϕ(z), in an equilibrated LPB system at various temperatures

Figure 6. Average chain length ⟨L⟩ for a wide range of total monomer concentration ϕt confirming the scaling eqs 2.3 and 2.5. The three slopes correspond to dilute, semidilute, and concentrated regimes at σg = 1.0. The observed slopes are 1.42, 0.18, and −0.51, respectively. Sample snapshots belonging to each regimes are inserted in the plot. 9833

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

Figure 7. (a) Force−displacement curves for relaxed MPB with grafting density σg = 1.0 and chain length N = 32 during the loading ↓ and unloading ↑ process at kBT = 1.0. The rates of approaching and retraction as unit of MCS−1 are given as parameter. The inset shows a plot of the mean-squared gyration radius component ⟨Rgz2⟩ in direction perpendicular to the grafting surface vs height of the mobile compressing surface (repulsive wall) during loading and unloading. (b) Density profile of MPB, ϕp(z), for different wall positions in the loading experiment.

The measured variation of the mean chain length ⟨L⟩ versus total monomer concentration, along with visual evidence from snapshots taken in the course of compositional variation (Figure 6), suggests the existence of several distinct regimes in terms of ϕt. One may conclude from Figure 5 that the mean chain length of a LPB in a wide range of concentration is governed by a power-law relationship, confirming the scaling eqs 2.3 and 2.5 with exponents that differ from the predicted values for living polymers in bulk. Interestingly, at rather high concentrations the mean length ⟨L⟩ decreases with further growth of ϕt; i.e., the LPB gets more compact as the longest chains are hindered in their growth due to the finite size of the simulation box. Thus, the polymerization process is shifted, and this affects increasingly the many short chains living in the bottom. Clearly, more comprehensive investigation and increased computational efforts are needed to elucidate this aspect of the LPB behavior which we postpone for a separate publication. A. Compression of in Situ Grown LPB. In this section we examine the interaction between a LPB chains immersed in a good solvent and a test surface using coarse-grained off-lattice Monte Carlo simulations. Our purpose is to obtain force− displacement curves for the penetration of such an AFM tip (test surface) into a polydisperse chains of LPB as a function of layer characteristics. To this end, the test surface is represented either as an impenetrable or as semipermeable surface, consisting of a long cylinder of cross-section area A. The interaction between a LPB and a AFM tip can easily be simulated by a slight variation of the algorithms used to study forces between two test surfaces in which one of them bears an end-grafted polymer brush. In the simulations results given below, we assumed a repulsive force between the monomers and the surface,94 taken as a Weeks−Chandler−Andersen potential, i.e., as the repulsive (and shifted) branch of a Lennard-Jones potential. One might also use a Lennard-Jones with an attractive short-range components.95,96 Both of these forces gave qualitatively similar results. For the sake of comparison, we also simulated an equilibrated monodisperse polymer brush (MPB) containing chains of equal length N = 32 at high grafting density σg = 1.0. Originally, the mobile wall is far enough so that it is not in contact with the brush. To simulate the loading and unloading processes of wall, we move it downward at rate RA, and then up at retraction rate RR, measured as distance per time units of MCSteps.

Figure 7a shows the results of the force−displacement curve for an equilibrated high-density MPB at vanishing rates RA = RR = 1.9 × 10−6. The force F is normalized by the area A of contact and describes thus the pressure on the wall. As shown in the main panel of Figure 7a, during the loading from zi = 30 to zf = 10, the tip goes into the sample down to a depth δ = zf − zi, causing deformation of the brush. During the wall retraction, it goes back from zf = 10 to zi = 30. Since the rates of approaching and retraction at well-equilibrated conditions are negligible, the MPB behaves as an elastic material and regains step by step its own shape, exerting equal pressure on the wall. The F vs z curves for the approaching/retracting wall lie on top of each other and are virtually indistinguishable. Therefore, during such an “infinitely” slow loading and unloading one observes no hysteresis in the force−height relationship. In the inset to Figure 7a we plot the mean-squared gyration radius component ⟨Rgz2⟩ in direction perpendicular to the grafting surface as a function of the wall position. Evidently, in logarithmic coordinates these transients appear as straight lines, suggesting that the height of the perturbed MPB changes by a power law, ⟨Rgz2⟩ ∝ zα, whereby the observed power α ≈ 1.96, i.e., h ∝ z for z < 30. In Figure 7b, we show the monomer distribution of the MPB along the z-direction at different piston positions (wall level) during the loading experiments. As can be seen from Figure 7b, the histograms follow indeed the parabolic characteristics of “dead” monodisperse brushes97 in the beginning of the process (nearly unperturbed state) while at stronger compression, for z ≤ 22, the histograms indicate a flat uniform distribution of matter in the compressed MPB. Eventually, one ends up with a rather sharply peaked ϕp(z) (not included for the sake of clarity) near the grafting surface, characterizing a “proximal zone” with density oscillations typical for all fluids “packed” in the vicinity of a hard wall. In the main panel of Figure 8 we compare the pressure of grafted monomers along direction z, normal to the grafting surface for two MPBs with chain lengths N = 64 and N = 128, both at highest grafting density, i.e., σg = 1.0. The density profiles are included for the sake of comparison. It becomes evident from Figure 8 that both simulations demonstrate a qualitatively similar behavior to that of Figure 7. In the inset to Figure 8 one may see the same scaling of mean-squared gyration radius component ⟨Rgz2⟩ in direction perpendicular to the grafting surface as in Figure 7a, whereby the force− 9834

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

The equilibrium profile of such a monodisperse “dead” brush is more compact with a steeper slope near z ≈ ⟨z⟩ than that of the analogous LPB system (as shown in Figure 9) which goes to far larger z. In agreement with the theoretical predictions47 (cf. section II), it is seen from Figure 9 that the weak compression force of the LPB exceeds significantly the one due to MPB. At large compression (z < ⟨z⟩ = 22.75) or small separations, of course, the two force−displacement relations are indistinguishable. The pressure in this limit is exerted by the uniform density of the compressed brush, suggesting that the repulsive force is well approximated by the corresponding osmotic pressure of a nongrafted semidilute solution. Hence, the two interaction forces become identical when the MPB height ⟨z⟩ = 22.75 is much less than the average chain length ⟨L⟩ = 32 of the corresponding LPB case. For small compressions (z ≈ ⟨z⟩ = 22.75), the force− displacement curve of the MPB vanishes abruptly in contrast to the equivalent LPB case (see inset to Figure 9). This important distinction is due to the existence of few much longer chains in the LPB. Therefore, the reactive force of a LPB extends to larger separations, and the simulation predicts a nonvanishing force at z > ⟨z⟩ = 22.75. In order to be as close as possible to real applications of LPB, in which a LPB is subjected to force measurement by either AFM or SFA instruments, we also examined the case of a semipermeable wall (SPW) as opposed to that of completely impenetrable rigid wall (IPW). With a SPW, a complete equilibration of the whole LPB takes place under conditions when the unreacted single monomers may move freely through the wall and enter the volume above it. In this way the monomer concentration under the moving wall is not affected by the wall motion and remains equal to that in the whole volume regardless of the wall position as is the case with an AFM tip. Otherwise, any change in the wall position would have induced a change in the average chain length ⟨L⟩ because of growing ϕt according to eq 2.5 and, therefore, also in the reactive force of the LPB even before the wall gets in touch with the brush. In other words, any variation of an impenetrable wall would produce an essentially different LPB which precludes a meaningful study of the force−wall position relationship at fixed monomer concentration ϕ. In order to avoid inaccuracies and in view of the additional time the monomers need to move through the SPW, we chose in this case the equilibration periods twice longer than in the IPW case with rate in the range 10−8−10−10. The result of such simulation for force−displacement curve in loading experiment is shown in Figure 10, together with the curve for the same LPB, compressed by an IPW of identical area. The average chain length in both cases is ⟨L⟩ = 32, and the grafting density is σg = 1.0. The force exerted by the LPB on the SPW excludes the interaction between nongrafted monomers and the test surface. One can immediately see that the SPW clearly gives a weaker force compared to that with IPW at small compressions. This difference becomes indistinguishable at lower separation or large degrees of compression, and the curves in both cases superimpose perfectly for z ≤ 20 as expected. It is evident from Figure 10 that the force−displacement curves appear as straight lines in logarithmic coordinates, suggesting a power law scaling, F ∝ z−α, where the observed exponent α ≈ 3.4 is shown to describe a dense LPB system in both the SPW and IPW case. Eventually, in Figure 11 we present the effects of tip scan rate on the hysteresis behavior in the force−displacement curve

Figure 8. Comparison between force−displacement curves of two relaxed MPB with grafting density σg = 1.0 and chain length N = 64 and N = 128 in the loading experiment ↓. The density profile (shaded area) is included for comparison. The inset shows the same trend for ⟨Rgz2⟩ as N = 32.

displacement curves again collapse on a single master curve. This behavior is characteristic for large tip AFM experiments.50 Because of the large grafting density and the excluded-volume interactions, the chains are strongly stretched and resemble rods with small probability for the chains to escape compression by moving away from the test surface. In Figure 9, a force−displacement approach curve obtained for LPB system with ⟨L⟩ = 32 is compared to the equivalent

Figure 9. Force−displacement curves of relaxed LPB and MPB in loading experiment for ⟨L⟩ = 32 (LPB) and N = 32 (MPB) at σg = 1.0. The rate of wall displacement is RA = 1.9 × 10−6 for both LPB and MPB.

MPB with length N = 32 of the grafted chains. For both cases the data corresponds to polymer brushes at their highest grafting density, i.e., σg = 1.0. For better interpretation, the resulting brush profiles are also included in the main panel of Figure 9 by the shaded area. It is common to define the layer thickness ⟨z⟩ of a MPB as the first moment of the monomer density profile ϕp(z), i.e., the average distance of a chain monomer from the surface ⟨z⟩ =

2 ∫ zϕp(z) dz

∫ ϕp(z) dz

(5.1) 9835

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

and retraction curves. The values of energy dissipation have been measured experimentally for different systems.100 As can be seen from the Figure 11, by decreasing the scan rate the hysteresis may be completely eliminated when full equilibrium is reached without energy dissipation. The latter shows an elastic behavior of a thin layer in which the material can regains step by step its own shape during the withdrawal process.101 In practice, the sample may lose elasticity in the process of compression so that when the tip is withdrawn, it does not regain immediately its former shape. The load gradually decreases whereas the penetration depth stays the same. Hence, indentation and retraction curves seldom overlap. At a given penetration depth the force of the unloading curve is smaller than the force at loading. This difference between the indentation and the withdrawal force curves appears as a “loading−unloading hysteresis”. The hysteresis may lead to an incorrect determination of displacements, and in particular, because of the hysteresis, the load in the loading curve for a given displacement may appear bigger and finally overcome those of the unloading curve. Experimentally, Hoh and Engel99 have shown that the loading/unloading hysteresis is scan rate (or velocity)-dependent. At high scan rates the separation between the contact lines in indentation and retraction modes is large, and a considerable hysteresis appears. As the scan rate is decreased, the system has more time to recover, and this separation reaches a minimum so that the hysteresis becomes smaller and may vanish.

Figure 10. Comparison between force−displacement curves of relaxed LPB, obtained with both impermeable and semipermeable wall for ⟨L⟩ = 32 at σg = 1.0.

VI. COMPARISON BETWEEN EXPERIMENT AND SIMULATION Here we focus on the comparison of our simulations exclusively with own AFM-based, colloidal probe compression measurements. PNIPAAm brush was grafted on the surface of a selfassembled monolayer containing the initiator, using surfaceinitiated atom transfer radical polymerization (ATRP). Varying the reaction time and monolayer initiator concentration controlled the molecular weight and grafting density, respectively. For details on the synthesis of PNIPAAm brush samples and evaluation of grafting density, see the Supporting Information. AFM measurements were performed on ATRP grown PNIPAAm films in a standard fluid cell containing deionized water as a good solvent at 26 °C, which was below the LCST temperature of PNIPAAm. Experimentally, a surface force apparatus (SFA) was used by Zhu et al.71 and Plunkett et al.72 to measure the force encountered between tethered poly(N-isopropylacrylamide) (PNIPAAm) at, below, and above lower critical solution temperature (LCST) and plain mica surfaces and mica surfaces coated with lipid bilayers. In the SFA technique, the force of interaction between two perpendicular crossed cylinders can be measured as a function of the distance between the two cylindrical surfaces. Plunkett et al.72 coated the surface of one cylinder with terminally anchored PNIPAAm and kept the surface of the other cylinder bare. In our simulation, force was measured between a LPB and a wall, taken as either a hard impenetrable or a semipermeable layer, and compared to experimental data obtained for PNIPAAm under good solvent condition (below LCST) as well as to the simulation results for monodisperse MPB case. This comparison makes sense only when the length of chains in the MPB brush, N, is equal to the mean chain length ⟨L⟩ of the LPB. However, for a living polymer ⟨L⟩ depends essentially on the concentration of free monomers in the container57 and in

Figure 11. Effect of moving velocity of the test wall on the force− displacement curve of LPB with ⟨L⟩ = 32 and σg = 1.0 during the loading process. In the inset a detailed view of the force hysteresis during loading and unloading experiments for a LPB is shown. Results for four incoming and retraction velocities are included, as indicated.

during a loading/unloading experiment. Recently, the response of a compressed monodisperse polymer brush as a function of σg and compression rate RA/RR was studied by Brownian dynamics simulation.98 Our simulations for a LPB system are performed with an average chain length ⟨L⟩ = 32 and grafting density σg = 1.0. The main panel of Figure 11 shows the observed force−displacement curve in loading experiments for different indentation/compression rate. Evidently, as the scan rate gets faster, the final values of the response force at small separations z < 15 grow while the superposition region is shifted to lower compressions. These predictions are found to agree well with experimental interpretations of Hoh and Engel99 in their AFM indentation test even though our approaching rates are about 3 orders of magnitude smaller than in a real AFM indentation experiment. In the inset plots of Figure 11 one may see the hysteresis becomes stronger with increasing loading/unloading rate, which reflects also growing energy dissipation given by the enclosed area of the indentation 9836

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

Figure 12. (a) Normalized force of Plunkett et al.72 for ⟨L⟩exp = 655 plotted vs the distance between untreated mica and a PNIPAM brush polymerized at grafting density 229 Å2/chain and comparing to simulated interaction force for a given grafting density and degree of polymerization, as indicated. (b) Same as (a) but for ⟨L⟩exp = 1830, grafting density 1930 Å2/chain, and simulated interaction force for a different set of grafting density and degree of polymerization, as indicated.

experimentally synthesized grafted layer is in the genuine brush regime. Bearing in the mind that the self-similar character of the conformation of the chains allows for some arbitrariness of the scales, one has to do an explicit mapping of a coarse-grained model of a flexible linear polymer in either grafted or nongrafted form on the real material. The principles of this mapping originate from the assumed general shape of the free energy of a chain f p, when one compares it with the properties of ideal chains in good solvents with an end-to-end distance R. The free energy of a single chain for a regular solution is obtained by inserting the excluded-volume contribution f ep and entropic component f sp into the equation f p = f ep + f sp. The excluded-volume contribution to the free energy of a single chain is obtained by integration over the occupied volume, hereby calculating the average over the all conformations

the case of impenetrable wall will therefore change dynamically with the variation of monomer concentration as the wall is moved with respect to the grafting plane. To prevent this and examine solely the effect of polydispersity at equal length of the chains in both LPB and MPB brush, we use in our simulation also a semipermeable wall that is impenetrable for the grafted polymers yet completely permeable for the single nonpolymerized monomers. These monomers can then move freely through the mobile wall and thus keep the total concentration in the box constant. Figure 12 illustrates the starting point of our analysis: from the data presented by Plunkett et al.72 for a range of end-grafted PNIPAM polymers that were synthesized by living polymerization (ATRP) on a gold flat surface with different grafting density (σgexp) and degree of polymerization (⟨L⟩exp), we can identify a number of choices (σg exp, ⟨L⟩ exp) where a quantitatively precise mapping of the experimental force− displacement curve on the simulated interaction force, for carefully chosen pairs of parameters (σgsim, ⟨L⟩sim), is possible. Here we use subscripts “exp” and “sim” to distinguish the real experimental data from their simulation counterparts, respectively. Thus, apart from suitable adjustment of pair parameters, the length scale of the simulation (i.e., the lattice spacing) s is adjusted to physical units by requiring that ⎛ ⎞exp ⎛ ⎞sim s s ⎜⎜ ⎟ ⎜ ⎟ =⎜ 2 1/2 ⎟ 2 1/2 ⎟ ⎝ 2⟨RF ⟩ ⎠ ⎝ 2⟨RF ⟩ ⎠

f pe =

1 2

∫ kTυe⟨cm2(r)⟩ d3r

(6.2)

where ⟨cm2(r)⟩ is square average local monomer density and υe is excluded-volume interaction parameter. If we choose for the description of the mean local density ⟨cm(r)⟩ a Gaussian function, with a radius of gyration Rg, we obtain f pe

(6.1)

⎛ ⎞3/2 kT 3 ⎟ 2⎜ = υeN ⎜ 2⎟ 2 ⎝ 4πR g ⎠

(6.3)

Eventually, one may choose the ideal state with vanishing excluded-volume forces and coil size in thermal equilibrium R0, where Rg = Rg,0 and R02 = a02N, and replace Rg by R assuming R ∼ Rg. Thus, one may express f ep as

The results of this fitting process for two experimentally calculated values (s/2⟨RF2⟩1/2) = 0.033 and 0.046 (obtained by Plunkett et al.72) are shown in Figure 12. As can be seen from the figure, a good fit over the entire range of separations z is obtained for ⟨L⟩ = 62 and σg = 0.25 in case a and for ⟨L⟩ = 130 and σg = 0.0625 in case b. The corresponding experimental values for ⟨L⟩ and σg are indicated in the figure. It should be noted, from experimental point of view, that all experimentally determined grafting densities are sufficiently high72 so that the excluded-volume interactions make the chains extend away from the substrate and form a brush structure. Therefore, the selected experimental grafting density for the comparison with simulated data at ϕ = 0.5 (which corresponds to semidilute brush regime in the simulation) confirmed that the

f pe =

3 kT 3/2 ⎛ R 0 ⎞ 3 ψ⎜ ⎟ ⎝R⎠ 2

(6.4)

The parameter ψ = (3/2π) is dimensionless and determines the excluded-volume energy associated with a single chain. A further requirement is that one needs an expression to take into account the conformational entropy indicating the elastic force built up on a coil expansion. This equation yields the second part of the free energy, f sp, and is given by 3/2

9837

(υe/a04)R0

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

Figure 13. (a) Normalized force for ⟨L⟩exp = 162 plotted vs the distance between AFM colloidal tip and a PNIPAM brush polymerized at grafting density 98 Å2/chain and comparing to simulated interaction force for a given grafting density and degree of polymerization, as indicated. (b) Same as (a) but for ⟨L⟩exp = 146, grafting density 98 Å2/chain, and simulated interaction force for a different set of grafting density and degree of polymerization, as indicated.

⎛ R ⎞2 f ps ≈ kT ⎜ ⎟ ⎝ R0 ⎠

VII. CONCLUSIONS In the present work we have studied and tried to reproduce the force exerted by a LPB chains on a test surface. Our studies have been carried out by means of an efficient off-lattice Monte Carlo algorithm. To this end comprehensive Monte Carlo simulations of the properties of a LPB made of flexible living polymer chains under good solvent conditions have been carried out. Most of our studies consider moderate and high grafting densities of the chains whereby the ensuing polymer brush may be classified as strongly stretched. An examination of the static properties of such LPB suggests that the observed monomer density profiles reveal power-law decline of the density ϕ(z) with increasing distance z perpendicular to the grafting plane, ϕ(z) ∝ zα with α ≈ 0.64, which is very close to the theoretically predicted value of α = 2/ 3 for diffusion-limited aggregation.61 The probability distribution c(N) of chain lengths N in the strongly polydisperse living polymer brush is also found to follow a power law relationship, c(N) ∝ N−τ, which qualitatively differs from the exponential Flory−Schulz molecular weight distribution typical for living polymers in the bulk. The observed value of τ ≈ 1.70 is again rather close to the value of τ = 7/4, predicted for the case of “needle growth” (diffusion-limited aggregation without branching),61 except for cases of rather short LPBs, grown at high temperature T > 1.0, where the chains do not stretch strongly and an exponential MWD is observed. One may thus conclude that the static properties of a LPB at equilibrium are very different from those of a semidilute or dense solution of living polymers in the bulk and are governed by different laws. One of the main concerns of this work has been the study of the force, exerted by a LPB on a test surface, and the comparison of simulational data with that from our own and other laboratory experiments. We have compared the force− displacement behavior from the set of experiments,72 obtained by SFA analysis on PNIPAAm brush under good solvent condition at temperature below LCST of PNIPAAm (Figure 12), and also our own experimental results obtained by colloidal probe AFM measurements on PNIPAAm brush at same conditions of SFA (Figure 13) with data from the present simulation. Generally, by adjusting the conformational parameter s/2⟨RF2⟩1/2 and the conversion factor from model lattice spacings to realistic nanometer scale, we find an almost

(6.5)

Finally, combination of the eqs 6.4 and 6.5 yields the free energy of a chain as a function of R. One may determine the important relation between RF and the degree of polymerization N by calculating the equilibrium value of R at the minimum of the free energy f p, where df p/d(R/R0) = 0. R0 is the coil size in thermal equilibrium. This leads to the relation R ≃ (νe/a04)1/5R06/5 = (νea02)1/5N3/5. One may identify R with the Flory radius RF, and it can be represented thus as RF = aFN3/5 with aF ≃ (νea02)1/5. The scaling law eq 6.1 is indeed in full accord with experiments (e.g., see ref 94), and it can be used for the translation of experimental findings to results of simulation in the case of various expanded polymer system in a good solvent. Of particular interest, we applied the same criteria in order to map our coarse-grained level simulations of force−displacement curve of a LPB to the experimental results obtained by SFA experiment (see Figure 12) and own colloidal probe AFM analysis on PNIPAAm brush in the good solvent. Since in the case of LPB system, there is only a single factor relating the length scale of the simulation to the real length scale and leads to a mapping process that conserves the chain conformation during translation, it can be expected that the precise description of coarse-grained model for force−displacement curve in Figure 12 is restricted to special cases. As an example, Figure 12 presents the force−displacement behavior in a AFM analysis for the pairs (⟨L⟩ = 162, σg = 98 Å2/chain)exp and (⟨L⟩ = 146, σg = 98 Å2/chain)exp. All force data are normalized by the colloidal tip radius Rtip. As can be seen from Figure 12, we find the closest corresponding translated pairs in simulation data as (⟨L⟩ = 98, σg = 1.0)sim and (⟨L⟩ = 72, σg = 1.0)sim. The inset in Figure 13a shows that for very small compressions the semilog plot of the force−displacement curve deviates somewhat from the coarse-grained model, and near z ≈ 900 Å the simulation curve ⟨L⟩sim = 98 slightly underestimates the experimental data. As shown in the inset to Figure 12b, in the case of lower degree of polymerization, ⟨L⟩sim = 72, the same deviation is also observed for lower separations while the underestimation is slightly decreased. 9838

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

(21) Milner, S. T.; Witten, T. A.; Cates, M. E. Europhys. Lett. 1988, 5 (5), 413. (22) Halperin, A.; Zhulina, E. B. Macromolecules 1991, 24 (19), 5393. (23) Biesheuvel, P. M. J. Colloid Interface Sci. 2004, 275 (1), 97. (24) Biesheuvel, P. M.; de Vos, W. M.; Amoskov, V. M. Macromolecules 2008, 41 (16), 6254. (25) de Gennes, P. G. Macromolecules 1980, 13 (5), 1069. (26) Wijmans, C. M.; Scheutjens, J. M. H. M.; Zhulina, E. B. Macromolecules 1992, 25 (10), 2657. (27) Auroy, P.; Mir, Y.; Auvray, L. Phys. Rev. Lett. 1992, 69 (1), 93. (28) Cho, J.-H. J.; Smith, G. S.; Hamilton, W. A.; Mulder, D. J.; Kuhl, T. L.; Mays, J. Rev. Sci. Instrum. 2008, 79 (10), 103908. (29) Smith, G. S.; Kuhl, T. L.; Hamilton, W. A.; Mulder, D. J.; Satija, S. Physica B: Condens. Matter 2006, 385−386 (Part 1), 700. (30) de Vos, W. M.; Biesheuvel, P. M.; de Keizer, A.; Kleijn, J. M.; Cohen Stuart, M. A. Langmuir 2008, 24 (13), 6575. (31) de Vos, W. M.; Biesheuvel, P. M.; de Keizer, A.; Kleijn, J. M.; Cohen Stuart, M. A. Langmuir 2009, 25 (16), 9252. (32) Grest, G. S. J. Chem. Phys. 1996, 105 (13), 5532. (33) Murat, M.; Grest, G. S. Macromolecules 1989, 22 (10), 4054. (34) Lai, P. Y.; Zhulina, E. B. Macromolecules 1992, 25 (20), 5201. (35) Lai, P.-Y.; Binder, K. J. Chem. Phys. 1992, 97 (1), 586. (36) Lai, P.-Y.; Binder, K. J. Chem. Phys. 1993, 98 (3), 2366. (37) Neelov, I. M.; Binder, K. Macromol. Theory Simul. 1995, 4 (1), 119. (38) Neelov, I. M.; Borisov, O. V.; Binder, K. Macromol. Theory Simul. 1998, 7 (1), 141. (39) Neelov, I. M.; Borisov, O. V.; Binder, K. J. Chem. Phys. 1998, 108 (16), 6973. (40) He, G.-L.; Merlitz, H.; Sommer, J.-U.; Wu, C.-X. Macromolecules 2007, 40 (18), 6721. (41) Coluzza, I.; Hansen, J.-P. Phys. Rev. Lett. 2008, 100, 016104. (42) Seidel, C.; Netz, R. R. Macromolecules 2000, 33 (2), 634. (43) Kreer, T.; Metzger, S.; Muller, M.; Binder, K.; Baschnagel, J. J. Chem. Phys. 2004, 120 (8), 40124023. (44) Dimitrov, D. I.; Milchev, A.; Binder, K. J. Chem. Phys. 2006, 125 (3), 034905. (45) Dimitrov, D. I.; Milchev, A.; Binder, K. J. Chem. Phys. 2007, 127 (8), 084905. (46) Milner, S. T. Science 1991, 251, 905. (47) Milner, S. T. Europhys. Lett. 1988, 7, 695. (48) Jeon, S. I.; Lee, J. H.; Andrade, J. D.; Gennes, P. G. D. J. Colloid Interface Sci. 1991, 142, 149−158. (49) Jeon, S. I.; Andrade, J. D. J. Colloid Interface Sci. 1991, 142, 159− 166. (50) Subramanian, G.; Williams, D. R. M.; Pincus, P. A. Macromolecules 1996, 29, 4045−4050. (51) McCoy, J. D.; Curro, J. G. J. Chem. Phys. 2005, 122, 164905. (52) Steels, B. M.; Koska, J.; Haynes, C. A. J. Chromatogr., B 2000, 743, 41−56. (53) Pang, P.; Koska, J.; Coad, B. R.; Brooks, D. E.; Haynes, C. A. Biotechnol. Bioeng. 2005, 90, 1−13. (54) Flory, P. J. Principles of Polymer Chemistry; Cornell University Press: Ithaca, NY, 1953. (55) Wheeler, J. C.; Pfeuty, P. Phys. Rev. Lett. 1981, 46, 1409. (56) Pfeuty, P.; Wheeler, J. C. Phys. Lett. 1981, A84, 493. (57) Wittmer, J. P.; Milchev, A.; Cates, M. E. J. Chem. Phys. 1998, 109, 834. (58) Cates, M. E.; Candau, S. J. J. Phys.: Condens. Matter 1990, 6869. (59) Vidal, A.; Guyot, A.; Kennedy, J. P. Polym. Bull. (Berlin) 1982, 6, 401−407. (60) Advincula, R. C., Brittain, W. J., Caster, K. C., Rühe, J., Eds.; Polymer Brushes: Synthesis, Characterization, Applications; Wiley-VCH: Weinheim, 2004. (61) Wittmer, J. P.; Cates, M. E.; Johner, A.; Turner, M. S. Europhys. Lett. 1996, 33, 397. (62) Witten, T. A.; Sander, L. M. Phys. Rev. B 1983, 27, 5686. (63) Guiselin, O. Europhys. Lett. 1992, 17, 225.

perfect agreement. Small deviations between simulation results and experiment are only found for weak compression where in the case of SFA measurements the simulation slightly overestimates the data and in the case of AFM experiments the simulation slightly underestimates them. It is clear, however, that more work is needed until full understanding of the properties of living polymer brushes, obtained by ATRP is achieved. Especially interesting and unexplored is the problem of LPBs, grown on curved surfaces, including the corresponding force−distance relationship which we see as our next target for research.



ASSOCIATED CONTENT

S Supporting Information *

Full details of the experimental characterization used in this study. This material is available free of charge via the Internet at http://pubs.acs.org.



AUTHOR INFORMATION

Corresponding Author

*E-mail [email protected]. Notes

The authors declare no competing financial interest.



ACKNOWLEDGMENTS K. Jalili and A. Milchev are indebted to the Max-Planck Institute for Polymer Research in Mainz, Germany, for hospitality and support during their work on the problem. A.M. gratefully acknowledges financial support by CECAM nano SMSM.



REFERENCES

(1) Dyer, D. J. Adv. Funct. Mater. 2003, 13, 667. (2) Gates, B. D.; Xu, Q.; Stewart, M.; Ryan, D.; Willson, C. G.; Whitesides, G. M. Chem. Rev. 2005, 105, 1171. (3) Kawaguchi, M.; Takahashi, A. Adv. Colloid Interface Sci. 1992, 37, 219. (4) Binnig, G.; Quate, C. F. Phys. Rev. Lett. 1986, 56, 930. (5) Magonov, S. N.; Reneker, D. H. Annu. Rev. Mater. Sci. 1997, 27, 175. (6) Garca, R.; Pérez, R. Surf. Sci. Rep. 2002, 47, 197. (7) Kaholek, M.; Lee, W.-K.; LaMattina, B.; Caster, K. C.; Zauscher, S. In Polymer Brushes; Advincula, R. C., Brittain, W. J., Caster, K. C., Rühe, J., Eds.; Wiley-VCH: Weinheim, Germany, 2004; p 381. (8) Wilder, K.; Quate, C. F.; Singh, B.; Alvis, R.; Arnold, W. H. J. Vac. Sci. Technol., B 1996, 14, 4004. (9) Halperin, A.; Tirrell, M.; Lodge, T. Adv. Polym. Sci. 1992, 100, 31. (10) Klein, J. Annu. Rev. Mater. Sci. 1996, 26, 581. (11) Szleifer, I.; Carignano, M. A. Adv. Chem. Phys. 1996, 94, 165. (12) Grest, G. S. Adv. Polym. Sci. 1999, 138, 149. (13) Binder, K.; Kreer, T.; Milchev, A. Soft Matter 2011, 7, 5669. (14) Napper, D. H. Polymeric Stabilization of Colloidal Dispersions; Academic Press: London, 1983. (15) Hamilton, W. A.; Smith, G. S.; Alcantar, N. A.; Majewski, J.; Toomey, R. G.; Kuhl., T. L. J. Polym. Sci., Part B: Polym. Phys. 2004, 42 (17), 3290. (16) Pastorino, C.; Binder, K.; Kreer, T.; Muller, M. J. Chem. Phys. 2006, 124 (6), 064902. (17) Klein, J.; Kumacheva, E.; Mahalu, D.; Perahia, D.; Fetters, L. J. Nature 1994, 370 (6491), 634. (18) Auroy, P.; Auvray, L.; Léger, L. Phys. Rev. Lett. 1991, 66 (6), 719. (19) Alexander, S. J. Phys. (Paris) 1977, 38, 983. (20) Milner, S. T.; Witten, T. A.; Cates, M. E. Macromolecules 1988, 21 (8), 2610. 9839

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840

Macromolecules

Article

(64) Meakin, P. Phys. Rev. A 1986, 33, 3371. Krug, J.; Kassner, K.; Meakin, P.; Family, F. Europhys. Lett. 1993, 24, 527. (65) Murat, M.; Grest, G. S. Macromolecules 1996, 29, 8282−8284. (66) Milchev, A.; Paul, W.; Binder, K. J. Chem. Phys. 1993, 99, 4786. (67) Milchev, A.; Binder, K. Macromol. Theory Simul. 1994, 3, 915. (68) von Werne, T.; Patten, T. E. J. Am. Chem. Soc. 2001, 123 (31), 7497−7505. (69) Ell, J. R.; Mulder, D. E.; Faller, R.; Patten, T. E.; Kuhl, T. L. Macromolecules 2009, 42 (24), 95239527. (70) Deutsch, H. P.; Binder, K. J. Chem. Phys. 1991, 94, 2294. (71) Zhu, X.; Yan, C.; Winnik, F. M.; Leckband, D. E. Langmuir 2007, 23, 162. (72) Plunkett, K. N.; Zhu, X.; Moor, J. S.; Leckband, D. E. Langmuir 2006, 22, 4259. (73) Butt, H.-J.; Capella, B.; Kappl, M. Surf. Sci. Rep. 2005, 59, 1− 152. (74) Block, S.; Helm, C. J. Phys. Chem. B 2008, 112, 9318−9327. (75) Wang, J.; Butt, H. J. Phys. Chem. B 2008, 112, 2001−2007. (76) Mendez, S.; Andrzejewski, B. P.; Canavan, H. E.; Keller, D. J.; McCoy, J. D.; Lopez, G. P.; Curro, J. G. Langmuir 2009, 25, 10624− 10632. (77) Kutnyanszky, E.; Julius Vancso, G. Eur. Polym. J. 2012, 48, 8− 15. (78) Milner, S. T.; Witten, T. A.; Cates, M. E. Macromolecules 1989, 22, 853−861. (79) Olivier, A.; Meyer, F.; Raquez, J.-M.; Damman, P.; Dubois, P. Prog. Polym. Sci. 2012, 37, 157. (80) Ruths, M.; Johannsmann, D.; Rühe, J.; Knoll, W. Macromolecules 2000, 33, 3860. (81) Sakellariou, G.; Park, M.; Advincula, R.; Mays, J. W.; Hadjichhristidis, N. J. Polym. Sci., Part A 2006, 44, 769. (82) Voccia, S.; Bech, L.; Gilbert, B.; Jerome, R.; Jerome, C. Langmuir 2004, 20, 10670. (83) Frustrup, C. J.; Jankova, K.; Hvilsted, S. Soft Matter 2009, 5, 4623. (84) Chiefari, J.; Chong, Y. K.; Ercole, F.; Krstina, J.; Jeffery, J.; Le, T. P. T.; Mayadunne, R. T. A.; Meijs, G. F.; Moad, C. L.; Moad, G.; Rizzardo, E.; Thang, S. H. Macromolecules 1998, 31, 5559. (85) Grosberg, A. Y.; Khokhlov, A. R. Statistical Physics of Macromolecules; AIP Press: New York, 1994. (86) Milchev, A.; Wittmer, J. P.; Landau, D. P. J. Chem. Phys. 2000, 112, 1606. (87) Milchev, A.; Rouault, Y.; Landau, D. P. Phys. Rev. E 1997, 56, 1946. (88) Semal, S.; Vou, M.; de Ruijter, M. J.; Dehuit, J.; de Coninck, J. J. Phys. Chem. B 1999, 103, 4854. (89) Gerroff, I.; Milchev, A.; Paul, W.; Binder, K. J. Chem. Phys. 1993, 98, 6526. (90) Milchev, A.; Wittmer, J. P.; Landau, D. P. Phys. Rev. E 2000, 61, 2959. (91) Milchev, A.; Binder, K. Macromolecules 1996, 29, 343. (92) Gurler, M. T.; Crabb, C. C.; Dahlin, D. M.; Kovac, J. Macromolecules 1983, 16, 398. (93) Sun, Y. B.; Ding, X. B.; Zheng, Z. H.; Cheng, X.; Hu, X. H.; Peng, Y. X. Eur. Polym. J. 2007, 43, 762. (94) Murat, M.; Grest, G. S. Phys. Rev. Lett. 1989, 63, 1074. (95) Grest, G. S.; Murat, M. Macromolecules 1993, 26, 3108. (96) Grest, G. S. Macromolecules 1994, 27, 418. (97) Winehold, J. D.; Kumar, S. K. J. Chem. Phys. 1994, 101, 4312. (98) Carlsson, T.; Kamerlin, N.; Arteca, G. A.; Elvingson, C. Phys. Chem. Chem. Phys. 2011, 13, 16084−16094. (99) Hoh, J. H.; Engel, A. Langmuir 1993, 9, 3310. (100) Trevethan, T.; Kantorovich, L. Nanotechnology 2006, 17, S205. (101) Lee, C.; Wei, X.; Kysar, J. W.; Hone, J. Science 2008, 321, 385. (102) Strobl, G. R. The Physics of Polymers: Concepts for Understanding Their Structures and Behavior; Springer-Verlag: New York, 1996.

9840

dx.doi.org/10.1021/ma301743r | Macromolecules 2012, 45, 9827−9840