Subscriber access provided by University of Massachusetts Amherst Libraries
Article
Enamine approach for versatile and reversible functionalization on cellulose related porous sponges Liduo Rong, Hongchen Liu, Bijia Wang, Zhiping Mao, Hong Xu, Linping Zhang, Yi Zhong, Jinying Yuan, and Xiaofeng Sui ACS Sustainable Chem. Eng., Just Accepted Manuscript • DOI: 10.1021/ acssuschemeng.8b01369 • Publication Date (Web): 30 May 2018 Downloaded from http://pubs.acs.org on May 30, 2018
Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.
is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.
Page 1 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
1
Enamine approach for versatile and reversible functionalization on
2
cellulose related porous sponges
3
Liduo Rong†, Hongchen Liu†, Bijia Wang†, Zhiping Mao†, Hong Xu†, Linping Zhang†,
4
Yi Zhong†, Jinying Yuan‡, Xiaofeng Sui†, *
5
† Key Lab of Science & Technology of Eco-textile, Ministry of Education, College of
6
Chemistry, Chemical Engineering and Biotechnology, Donghua University, No. 2999
7
North Renmin Road, Shanghai 201620, People’s Republic of China.
8
‡
9 10
Key Lab of Organic Optoelectronics and Molecular Engineering of Ministry of Education, Department of Chemistry, No.1, Tsinghua Yuan Road, Haidian District, Tsinghua University, Beijing, 100084, People’s Republic of China.
11 12
*Corresponding authors:
13
Address: No. 2999 North Renmin Road, Shanghai 201620, People’s Republic of
14
China.
15
Tel.: +86 21 67792605. Fax: +86 21 67792707.
16
E-mail:
[email protected] 17
1
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
18
Page 2 of 22
Abstract
19
A readily modifiable cellulose sponge was prepared from cellulose
20
acetoacetate (CAA). Facile post-modification with primary amino-containing
21
modifiers such as octadecyl amine (ODA), cysteine (CYS), and L-glutamic acid
22
(GLU) could be achieved demonstrating the ease of anchoring a broad selection of
23
functional groups to the surface of the sponges. This post-modification process was
24
systematically characterized by Fourier transform infrared spectroscopy, and X-ray
25
photoelectron spectroscopy, which confirmed the formation of the enamine bonds.
26
Besides, the microstructures and mechanical properties of the sponges were well
27
preserved throughout the post-modification process. The enamine bonds, as one of the
28
dynamic covalent bonds, were easily formed under the mild and neutral conditions
29
and broken exposure to a low pH stimulus. The enamine bonds were used to modify
30
the CAA sponges, which can achieve the versatility and recycling of cellulose porous
31
materials. Therefore, the resulting sponges could serve as a versatile precursor to a
32
broad spectrum of multifunctional porous materials, paving a new way for
33
constructing smart sponges through the post-modification strategy.
34 35 36 37
Key words: Cellulose acetoacetate; Post-modification; Enamine bond; Sponge; Reversible
2
ACS Paragon Plus Environment
Page 3 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
38
INTRODUCTION
39
Functional cellulose porous materials (aerogels or sponges)1-2 have high porosity,
40
large surface areas, and low density; hence, they can be good candidates for diverse
41
applications in catalyst support, thermal insulation, adsorption, etc.3-13 Nevertheless,
42
the performance of porous materials often depend chemical composition on the
43
surface, and these functional cellulose sponges always have a high density of surface
44
specific groups, e.g. alkyl groups,14 amino groups,9 thiol groups,15 to meet particular
45
requirements. For example, hydrophobic materials could be potentially used to adsorb
46
oil from water.16-17 The thiol group as the good heavy metal adsorbent18-19 and catalyst
47
carrier20-21 has been widely studied. By regulating the pH, the carboxyl group could
48
effectively adsorb the protein.22 Thus, it remains important to the optimize the surface
49
properties of the cellulose sponge.
50
To obtain functionalized cellulose sponges, two methods have been developed
51
including either derivatizing the cellulose before preparing the sponge, or
52
post-modification after sponge is formed.23 Xin et.al reported a hierarchically porous
53
cellulose acetate (CA) as the starting monolith as a template-free fabricated,
54
functionalized platform, which could be modified with typical reactive groups such as
55
epoxy, primary amino, and aldehyde.24 However, the modification processes are
56
irreversible and often demand the tedious chemical transformations. Laure and
57
co-workers achieved reversible tethering of end-functionalized polymers onto
58
catechol-based titanium platforms based on a reversible Diels−Alder (DA)
59
cycloaddition reaction,25 which allowed recycle and reuse of the modifiers and the
60
original materials. Therefore, it is desirable to develop a mild, reversible and versatile
61
strategy for post-modification of the cellulose sponge to better preserve their delicate
62
morphological features.
63
The use of mussel-inspired polydopamine (PDA) chemistry to create a versatile
64
nanoplatform capable of further modifications toward various applications has been
65
achieved on ordered mesoporous carbons (OMCs).26 Inspired by the PDA-based
66
platform, we constructed a CAA-based sponge reinforced by cellulose nanofibers 3
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 4 of 22
67
(CNF) and demonstrated that it could be used as a universal precursor for
68
multifunctional cellulose sponges via a post-modification strategy. Cellulose
69
acetoacetate (CAA), as a water-soluble cellulose ester, has received extensive
70
attention and research by both industry and academia.27-28 The acetoacetyl group is
71
susceptible to a series of transformations via the active methylene and carbonyl
72
carbons. A dynamic covalent enamine bond can be formed by reacting the ketone
73
carbonyl carbon with a primary amino group under mild conditions,29-30 and it is
74
reversibly cleaved, restoring the carbonyl upon exposure to a low pH stimulus. The
75
transformations could be performed under mild conditions without catalysis; thus,
76
CAA could be used as the starting materials to develop a mild, facile, and reversible
77
strategy for the post-modification of cellulose sponge materials to better preserve their
78
delicate morphological features. In this work, acetoacetate-containing cellulose
79
sponges reinforced with CNF using APTES could be easily post-modified with the
80
functional molecules containing the primary amino group due to the unreacted
81
acetoacetyl groups on the sponge.
82 83
Scheme 1. (a) Reaction mechanism of the CAA sponge crosslinked with CNF and APTES; (b)
84
Schematic illustration of the reversible surface-modified CAA sponge.
85
EXPERIMENTAL SECTION
86
Materials
87
A cellulose nanofibers (CNF) suspension (solid content = 1 wt%) was provided by
88
Tianjin Haojia Cellulose Co., Ltd. (China) and was subjected to high-pressure 4
ACS Paragon Plus Environment
Page 5 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
89
homogenization (APV-2000 Homogenizer, Germany) before use. The average CNF
90
diameter was under 100 nm. The Wood pulp was supplied by Xinxiang Natural
91
Chemical Co., Ltd. The viscosity-average degree of polymerization was estimated as
92
870
93
cupriethylenediamine
94
1-allyl-3-methylimidazolium chloride (AMIMCl) was purchased from the Center for
95
Green Chemistry and Catalysis (CGCC), LICP, CAS. Octadecyl amine (ODA),
96
cysteine (CYS), L-glutamic acid (GLU), 3-aminopropyltriethoxysilane (APTES),
97
hydrochloric acid (HCl), and tert-butyl acetoacetate (t-BAA, 99%) were supplied by
98
Sinopharm Chemical Reagent Co., Ltd. All other chemicals were of analytical grade
99
and used without further purification.
100
according
to
measurements hydroxide
using solution
an
Ubbelohde
(CUEN).
The
viscometer ionic
in
liquid
Preparation of CAA
101
The synthesis of CAA (degree of substitution (DS) = 0.87, Figure S1) was carried
102
out according to our previous reports.31 In brief, 2.0 g of cellulose was dispersed in 38
103
g of 1-allyl-3-methylimidazolium chloride (AMIMCl) in a three-necked flask, and the
104
mixture was heated to 95 °C and held there until the sample was dissolved completely.
105
Dimethylformamide (DMF) (10.0 mL) was added to the solution as diluent,
106
subsequently, the solution was heated to 110 °C, and tert-butyl acetoacetate (t-BAA,
107
15.6 g, 98.7 mmol) was added dropwise under the protection of nitrogen with stirring
108
for 4 h. After the reaction, the products were precipitated using methanol, then washed
109
and dried for use.
110
Preparation of CAA sponges
111
A CNF suspension (1 wt%) was sonicated for 1 h to achieve a thorough dispersion
112
(TEM image of the CNF is shown in Figure. 1a). To 10.0 g CNF (1 wt%) suspension
113
was added drop-wise a predetermined amount of 10 wt% hydrolyzed APTES solution
114
(0, 0.1, 02, 0.3, 0.6 mL). The mixed suspension was magnetically stirred for 2 h at
115
25 °C, followed by addition of 10 g 1 wt% CAA aqueous solution. Stirring was
116
continued for 30 min. The suspensions were then kept still for gelatinization. After 2 h,
117
the gel was subjected to a bottom-up quick-freeze with liquid nitrogen to yield ice 5
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 6 of 22
118
gels, which were freeze-dried using a Labconco apparatus (FD5-3, Labconco USA) at
119
-55 °C under vacuum. The resulting sponges were further dried and cured for 30 min
120
at 110 °C. The sponges were coded CAA-n, where n% represented the mass ratio of
121
APTES to CAA and CNF.
122
The post-modification of CAA sponges with various amino compounds
123
In 100 mL of ethanol, 0.4 g of ODA was dissolved at 40 °C. Separately, 0.4 g of
124
CYS and GLU were dissolved in 100 mL each of an ethanol/water (1:1 v/v, pH = 8.5)
125
solution at 40 °C, following which, 0.2 g each of the CAA-10 sponges were subjected
126
separately to the above-mentioned different amino compound solutions. The CAA-10
127
mixtures were magnetically stirred at 40 °C for 12 h. After modification, the samples
128
were washed with ethanol and water to remove the physically adsorbed amino
129
compounds on the surface of the sponge. Finally, the samples were freeze-dried. The
130
samples were coded as CAA-ODA, CAA-CYS, and CAA-GLU.
131
Reversible modification of CAA sponges with ODA, CYS, GLU
132
The modified CAA sponges could be easily restored to the original sponges
133
through the dynamic enamine bonds. Specifically, the CAA-ODA, CAA-CYS,
134
CAA-GLU sponges were placed in an acidic ethanol/water solution (pH = 3.0) and
135
the ensuing suspension was stirred at room temperature for 4 h. These experiments
136
were also carried out with the neutral ethanol/water solution (pH = 7.0) as a control.
137
Then, the samples were washed with ethanol and water to remove the physically
138
adsorbed amino-molecules in the sponges. Finally, the samples were freeze-dried. The
139
resulting sample could be repeatedly modified again with ODA, CYS, GLU according
140
to the procedure in above mentioned section and coded as CAA-mODA, CAA-mCYS,
141
CAA-mGLU where m represented the times of the cyclic modifications. The results
142
of the reversible modification process were characterized by FTIR spectroscopy.
143
Characterization
144
1
H NMR spectra were acquired on an Avance 400 MHz (Bruker, USA)
145
spectrometer in the proton noise-decoupling mode with a standard 5 mm probe. The
146
DS of CAA was calculated according to Equation (1). 6
ACS Paragon Plus Environment
Page 7 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
DS =
I × 7 (1) I × 3
147
where I1 is the integration value of the methyls of acetoacetate and I2 is the integration
148
value of the backbone of the anhydroglucose ring of CAA.27, 31
149
Fourier transform infrared (FTIR) spectroscopy analyses were carried out using a
150
PerkinElmer Spectrum Two (USA) equipped with an attenuated total reflectance
151
(ATR) accessory. All spectra were recorded in the 4000–450 cm−1 range and at a
152
resolution of 4 cm−1. The thermal properties of the samples were evaluated by
153
thermogravimetric analysis (TGA) (NETZSCH 209F1, German). Under nitrogen
154
purge, the samples were heated from 30 to 600 °C at a heating rate of 10 °C/min. The
155
morphologies of the samples were observed using a Hitachi TM-1000 scanning
156
electron microscope (Japan). The sponges before and after modification were
157
analysed using X-ray photoelectron spectroscopy (XPS) (Thermo Fisher ESCALAB
158
250Xi, USA) to gain further information about the surface composition. Before XPS
159
analysis, all the samples were pressed into the uniform film to meet the test
160
requirement. The mechanical properties of the sponges were evaluated on a universal
161
testing machine (HY 940F, China) equipped with the special pressure sensing
162
accessories (Transcell, BAB-20MT, three-digit accuracy). The testing procedures
163
(Figure S2) were with a compression speed of 2 mm/min (sample diameter: 20 mm,
164
scale distance 12 mm). The thickness recovery S was defined as the percentage of the
165
original thickness according to Equation (2)32
166 167 168
S(%) = 100 −
(2)
where the εfinal is the strain at the final position when the force detected reached 0 N.
169
The N2 adsorption-desorption isotherms and specific surface areas were
170
characterized by a TriStar II 3020M analyser (Micrometrics instrument corp.). The
171
porosities of the sponges were measured using a previously reported gravimetric
172
method.33 The dynamic water contact angle (WCA) was measured with a DSA30
173
contact angle analyzer (Kruss, German). 7
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
174
RESULTS AND DISCUSSION
175
Synthesis and characterization of the CAA sponges
Page 8 of 22
176
Scheme 1a illustrates the preparation of the CAA sponge via cross-condensation
177
with APTES to form a physically stable gel with three-dimensional network structure.
178
CNF were used as reinforced component (Figure S3). Subsequently, the CAA
179
sponges were post-modified with the amino-containing octadecyl amine (ODA),
180
cysteine (CYS), or L-glutamic acid (GLU), as representative examples, to prove the
181
feasibility of the post-modification strategy. The modification with amino compounds
182
showed reversible pH responsiveness (Scheme 1b).
183
As shown in Scheme 1a, the amount of APTES was controlled to ensure that the
184
CAA sponges have a large number of unreacted acetoacetyl groups (Table S1), that
185
could react with the functional molecules containing primary amino groups including
186
ODA, CYS, and GLU in the post-modification process. The resulting sponge presents
187
a white appearance and has low density (Figure 1b).
188
Figure 1c shows the FTIR spectra of the CAA sponges containing different
189
amounts of APTES. With the increase of APTES, the double carbonyl-characteristic
190
peaks of acetoacetyl at 1700−1760 cm−1 became weaker.30 The peaks at 1650 and
191
1605 cm−1 could be ascribed to the enamine bond,29 and their intensity became
192
stronger (Figure S4a). For the CAA sponge, the typical Si−O−Si bond-stretching
193
adsorption peaks from the siloxane compounds in the 1000–1130 cm−1 region
194
overlapped with the peaks for the C−O bonds of cellulose,34 while the peak at 800
195
cm−1 from the CAA sponges was assigned to the C−O−Si stretching vibration and
196
became increasingly prominent with the increase of APTES.35 As shown in Figure.
197
1d, as more APTES was incorporated the compressive modular of the sponges
198
increased from 14 to 36 KPa. The major contributor to the enhancement of
199
compressive strength is due to higher degree of crosslinking.
200
The thermal stability of the CAA sponges was also studied with TGA. The
201
samples presented a gradient change in thermostability as shown in Figure 1e. The 8
ACS Paragon Plus Environment
Page 9 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
202
maximum rate of thermal decomposition decreased with increasing the content of
203
APTES according to DTG (Figure S4b).36 However, the temperature of the DTG
204
peaks did not change significantly. Besides, the char residue mass fractions
205
significantly increased to 32.0 % with increasing APTES ratios, which could be
206
ascribed to silicon and the low oxygen content in APTES, along with lower
207
decomposition rates that contributed to the improved thermal stability of the
208
crosslinked CAA sponges. As seen from the SEM images of the sponges (Figure S5),
209
little difference was observed in terms of morphology between samples containing
210
varying amounts of APTES. This was as expected since the crosslinking happened on
211
the molecular level.
212
Considering that there was a trade-off between reinforcement and available
213
modification sites, the CAA-10 sponge which still had 1.45 mmol/g remnant
214
acetoacetyl group (Table S1) and reasonably good mechanical strength was chosen
215
for the post modification experiments.
216 217
Figure 1. (a) Transmission electron microscopy (TEM) image of CNF; (b) Photograph of a
218
round sample of the CAA sponge on the leaf; (c) FTIR spectra, (d) compressive stress-strain 9
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
219
curves, and (e) TGA of CAA sponges crosslinked with different APTES amounts.
220
Surface modification with ODA, CYS, and GLU
Page 10 of 22
221
The CAA sponges could be imparted with the new properties through the
222
post-modification process. As shown in Scheme 1b, ODA, CYS, and GLU were used
223
to introduce different specific groups (alkyl, thiol, or carboxyl, respectively) and to
224
functionalize the CAA sponge. After surface modification and pH-cleavage reaction,
225
the sponges were always freeze-dried. The modified sponges were washed with
226
ethanol and subjected to air-drying and vacuum-drying. The results are included as
227
Figure S6 in the supporting information. As can be seen from Figure S6, both
228
air-dried and vacuum-dried samples suffered from deformation and shrinkage to some
229
extent, while the freeze-dried sample could maintain its original shape. Hence,
230
freeze-drying was chosen to prepare the modified CAA sponges in this work.
231
Figure 2a-f shows the FTIR spectra of the original CAA-10 sponge and the
232
CAA-ODA, CAA-CYS, and CAA-GLU sponges. After post-modification with ODA,
233
CYS, and GLU, the intensity of the peak for the acetoacetyl groups at 1700−1760
234
cm−1 on the CAA-10 sponge became lower and even disappeared, and the peak of the
235
enamine bonds at 1650 and 1605 cm−1 became stronger.29-30 These results clearly
236
demonstrate that the alkyl group, thiol group, and carboxyl group were successfully
237
anchored on the skeleton surface of the CAA sponges. Besides, the peaks at
238
2865−2930 cm−1 for the CAA-ODA sponge corresponded to the CH stretching
239
vibration.37 The peak for C=O in the CAA-CYS, and CAA-GLU sponges at
240
approximately 1655 cm−1 overlapped with the peak of the enamine bond as shown in
241
Figure 2d and 2f.
242
10
ACS Paragon Plus Environment
Page 11 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
243 244
Figure 2. FTIR spectra of the ODA(a), CYS(c), GLU(e) modified CAA sponges. FTIR spectra in
245
the range of peaks assignable to acetoacetyl groups and enamine bonds in the ODA(b), CYS(d),
246
GLU(f) modified CAA sponges.
247 248 249
Figure 3. SEM images of the CAA-10 sponges (a, b), CAA-ODA sponges (c, d), CAA-CYS sponges (e, f), and CAA-GLU sponges (g, h).
250
The morphologies and microstructures of the unmodified and modified sponges
251
were observed using SEM (Figure 3). The micro-structures of the CAA-10 sponge
252
exhibited a network structure with pore sizes in the range of 20−60 µm. 11
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 12 of 22
253
Freeze-casting offers a versatile approach to produce highly anisotropic porous
254
materials.38 When the CAA-10 gel was frozen inside molds, the first cores of ice were
255
formed, and the fibers were separated from frozen water. Then, large ice crystals grew
256
along the cooling/freezing direction.39 During this process, the cellulose fibers were
257
confined to the interstitial regions, which caused contraction and aggregation between
258
the ice crystals. After modification with ODA, CYS, and GLU, SEM images showed
259
that the morphological structure of the sponge did not change after treatment with
260
amino-containing modifiers.
261
To further illustrate the surface composition, XPS analyses of the CAA-10 and
262
post-modified sponges were conducted, the results for which are shown in Figure
263
4a-c. In the wide-scan spectra, the characteristic signals of C1s (285 eV), O1s (545
264
eV), N1s (399 eV), Si2s (153 eV), Si2p (100 eV), S2s (233 eV), and S2p (169 eV)
265
were all detected. As shown in Figure 4d-f, the high-resolution spectrum of the N1s
266
peaks can be resolved into peaks at 402.0 eV and 399.3 eV, attributed to the formation
267
of the enamine bond.40 Figure 4d-f clearly demonstrated that the N1s peaks
268
(attributed to enamine Nitrogen) of the amine-modified samples were more intense
269
compared to that of the original CAA-10, suggesting the amino-containing functional
270
molecules were fixed on the surface of the sponge by enamine bonds. The elemental
271
composition of the CAA-10 sponge and post-modified sponges were determined
272
using survey scans from XPS. Table 1 summarizes the elemental composition derived
273
from the XPS survey spectra for the CAA-10 sponge before and after
274
functionalization. The composition of surface elements changed significantly, which
275
confirmed that various functional molecules had been fixed on the surface of the
276
sponges. X-ray photoelectron spectroscopy (XPS) is the most commonly used
277
technique of surface analysis in the nanometer depth.41 After modification by ODA, it
278
was expected that the surface silicon atoms would be covered by the C18 carbon
279
chain of ODA, which could explain the observation that intensity of Si2s was greatly
280
reduced while that of C1s was enhanced.
12
ACS Paragon Plus Environment
Page 13 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
281 282
Figure 4. XPS wide-scan spectra of the CAA-10 sponge compared with the CAA-ODA,
283
CAA-CYS, and CAA-GLU sponges (a-c), and high-resolution N1s spectra of the CAA-10
284
compared with the CAA-ODA, CAA-CYS, CAA-GLU sponges (d-f).
285 286 287
Table 1. Percent elemental concentration for the CAA-10, CAA-ODA, CAA-CYS, and CAA-GLU sponges from XPS survey scan Samples
Element
CAA-10 CAA-ODA CAA-CYS CAA-GLU
Atomic composition (%) O1s N1s
C1s 59.08 73.21 54.98 56.29
35.04 21.3 36.14 37.68
2.06 3.76 3.75 3.42
Si2s
S2p
3.43 1.73 2.34 2.61
2.8 -
288 289
To illustrate influences of the post-modification process on the specific surface 13
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 14 of 22
290
areas and hierarchical porous structures of the CAA-10 sponge, the nitrogen
291
adsorption/desorption isotherms for the CAA sponge and modified sponges are shown
292
in Figure 5a-c. The Brunauer–Emmett–Teller (BET) surface area of the CAA-10
293
sponge was calculated to be 9.076 m2/g. The lack of any distinct peak below 500 Å in
294
the pore size distribution calculated from the Barrett–Joyner–Halenda method (BJH)
295
indicates the lack of micro- or mesoporosity.42 The BET surface areas, bulk densities,
296
and porosities of all samples are summarized in Table 2. The modified sponges had a
297
trend towards a reduction in specific surface areas, and an increase in bulk densities.
298
This may be because during the post-modification and freeze-drying process, the
299
samples had a certain degree of contraction of the porous framework from
300
freeze-drying.
301 302 303 304
Figure 5. N2 adsorption-desorption isotherms of (a) CAA sponges compared with CAA-ODA sponges, (b) CAA-CYS sponges, and (c) CAA-GLU sponges; (d) The compressive stress-strain curves of modified CAA sponges
305 306
Table 2. Physical properties of the CAA-10, CAA-ODA, CAA-CYS, and CAA-GLU sponges 14
ACS Paragon Plus Environment
Page 15 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
Samples 2
BET surface area (m /g) Bulk density (mg/cm3) Porosity (%)
CAA-10
CAA-ODA
CAA-CYS
CAA-GLU
9.0760 14.3 95
8.3782 16.6 92
8.4368 16.7 91
7.3074 16.8 90
307
The compressive stress-strain curves for the CAA-10 sponge and the modified
308
sponges are shown in Figure 5d. The four sponges were compressed to 60% of their
309
original thickness. In general, the modified sponges had comparable compressive
310
stresses and Young’s moduli in comparison with the CAA-10 sponge,indicating the
311
post-modification had no detrimental effects on the mechanical properties of the
312
sponge. The reason for CAA-ODA sponge to have better recovery performance (70%)
313
could be due to the formation of new hydrogen bonding post-deformation was
314
hindered by the long carbon chains.
315
3.3 Reversible surface modification
316
During the post-modification process, the enamine bond was used to immobilize
317
functional molecules on the surface of the CAA sponges. The enamine bond, as a
318
dynamic covalent bond, could be reversibly cleaved and reformed upon exposure to
319
pH stimuli.29, 43 Therefore, this post-modification could be reversible. To verify this
320
assumption, the modified sponges were taken as an example. The FTIR spectra were
321
used to investigate the entire recyclable modification process (Figure 6c, Figure S7).
322
As the original material, the CAA-10 sponge was super-hydrophilic, and the
323
water droplet immediately permeated the sample (< 1s) and caused a little shrinkage
324
of the sponge. The sponge functionalized with ODA displayed durable hydrophobicity
325
with a water contact angle of approximately 145° as shown in Figure 6a. It is worth
326
noting that the reaction of hydrophobic modification not only occurred on the surface
327
of the sponge but also in its interior. This result could be ascribed to the highly porous
328
structure of the CAA sponge, which could promote the rapid diffusion of ODA, and
329
permeation through the sponge skeleton.44 As a proof of concept of the reversible
330
modification, the ODA-modified sponge was immersed in the acid ethanol/water
331
solution (pH = 3.0) for 4 h. The experiment was also carried out with the neutral
332
ethanol/water solution as a control. As shown in Figure 6a, after acid treatments, the 15
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 16 of 22
333
surface of the CAA-ODA sponge was restored to the original hydrophilic
334
characteristics, suggesting the removal of the hydrophobic molecules from the
335
sponges. More importantly, this sponge could be cyclically post-modified with ODA.
336
As shown in Figure 6b, after four cycles, the contact angle remains above 140°. FTIR
337
spectra were used to trace the change of the characteristic peaks during the recycle
338
modification process. As shown in Figure 6c, Figure S7, the peaks of the enamine
339
and acetoacetyl groups transformed to one another throughout the cycle, confirming
340
the reversible nature of the dynamic covalent enamine bonds. In addition, CAA-ODA
341
sponge immersed in the neutral ethanol/water solution showed no change in FTIR
342
spectra indicating that the enamine bond was relatively stable under neutral conditions
343
(Figure 6d).
344
Specifically, the amine-modified sponges were subjected to pH-cleavage
345
followed by re-modification and the compressive stress of the samples prior to and
346
after the re-modification were compared (Figure S8). The results showed that, for all
347
three modified-amines, the change of compressive strength due to the re-modification
348
process were less than 5%. The porosity of all samples is approximately 90%, which
349
has no significant change compared with the CAA-10 sponge. In addition, the SEM
350
images of sponges before and after re-modification showed no obvious difference
351
(Figure S9). These results confirmed the practicability for cyclic use of the sponges.
16
ACS Paragon Plus Environment
Page 17 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
352 353 354 355 356
Figure 6. (a) Evolution of the CAA-10 and CAA-ODA sponge contact angles, (b) contact angles of the recycled CAA sponge, (c) FTIR spectra of the reversibly modified ODA, and (d) FTIR spectra of contrast samples.
CONCLUSIONS
357
In the present study, a functional CAA sponge was successfully prepared by
358
crosslinking CAA and CNF with APTES. Mechanical strength of up to 24 KPa and
359
thermal stability of up to 230 °C could be achieved with an APTES loading of 10%,
360
leaving sufficient unreacted acetoacetate groups to allow the facile post-modification.
361
The
362
amino-containing modifiers ODA, CYS, and GLU via the dynamic covalent enamine
363
bond, to yield cellulose sponges featuring hydrophobic long carbon chain, thiol, and
364
carboxyl moieties, respectively. After post-modification, the sponges still maintained
365
excellent three-dimensional microstructures. In addition, the pH-induced cleavage of
366
the modifiers demonstrated that the post-modification could be reversed. The CAA
367
sponge could be therefore a key intermediate in constructing multifunctional cellulose
368
sponges through a mild and general post-modification strategy.
sponge
was conveniently and efficiently
modified
by the
primary
17
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 18 of 22
369 370 371
Supporting Information
372
Figure S1. 1H NMR spectra of CAA in DMSO-d6. Table S1. The theoretical content
373
of the functional groups on different CAA sponges. Figure S2. Sequential photos of
374
the sponge during the compression process. Figure S3. (a) FTIR spectra, (b)
375
compressive stress-strain curves of the CAA-10 sponge and the CAA-10-N sponge
376
without CNF. Figure S4. (a) FTIR spectra in the range of peaks assignable to
377
acetoacetyl groups and enamine bonds, (b) DTG of CAA sponges crosslinked with
378
different APTES amounts. Figure S5. SEM images of the CAA-0, CAA-5, CAA-10,
379
CAA-15, CAA-30 sponges. Figure S6. Photograph of a round samples of the sponges
380
before and after drying via different methods. Figure S7. FTIR spectra of the
381
reversibly modified CAA-CYS (a), CAA-GLU (b) sponges. Figure S8. The
382
compressive stress for the sponges in the cycling experiments at 60% strain. Figure
383
S9. SEM images of the regenerated CAA-10 sponges (a, b), CAA-2ODA sponges (c,
384
d), CAA-2CYS sponges (e, f), CAA-2GLU sponges (g, h).
385
ACKNOWLEDGEMENTS
386
This work was financially supported by the Fundamental Research Funds for the
387
Central Universities (No. 2232018A3-04 and No. 2232018-02), the National Key
388
R&D Program of China (No. 2016YFC0802802), and the Programme of Introducing
389
Talents of Discipline to Universities (No. 105-07-005735)
390
REFERENCE
391 392 393 394 395 396 397 398
1.
Lavoine, N.; Bergström, L., Nanocellulose-based foams and aerogels: Processing, properties, and
applications. J. Mater. Chem. A. 2017, 5 (31), 16105-16117. 2.
De France, K. J.; Hoare, T.; Cranston, E. D., Review of hydrogels and aerogels containing
nanocellulose. Chem. Mater. 2017, 29 (11), 4609-4631. 3.
Li, Y.; Xu, L.; Xu, B.; Mao, Z.; Xu, H.; Zhong, Y.; Zhang, L.; Wang, B.; Sui, X., Cellulose sponge
supported palladium nanoparticles as recyclable cross-coupling catalysts. ACS Appl. Mater. Interfaces. 2017, 9 (20), 17155-17162. 4.
Nguyen, S. T.; Feng, J.; Ng, S. K.; Wong, J. P.; Tan, V. B.; Duong, H. M., Advanced thermal 18
ACS Paragon Plus Environment
Page 19 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
399 400 401 402 403 404 405 406 407 408 409 410 411 412 413 414 415 416 417 418 419 420 421 422 423 424 425 426 427 428 429 430 431 432 433 434 435 436 437 438 439 440 441 442
insulation and absorption properties of recycled cellulose aerogels. Colloids Surf., A. 2014, 445, 128-134. 5.
Gupta, V.; Carrott, P.; Singh, R.; Chaudhary, M.; Kushwaha, S., Cellulose: A review as natural,
modified and activated carbon adsorbent. Bioresour. Technol. 2016, 216, 1066-1076.
6. Li, Y.; Wang, B.; Sui, X.; Xu, H.; Zhang, L.; Zhong, Y.; Mao, Z., Facile synthesis of microfibrillated cellulose/organosilicon/polydopamine composite sponges with flame retardant properties. Cellulose 2017, 24 (9), 3815-3823. 7.
Wu, Z.; Li, Y.; Zhang, L.; Zhong, Y.; Xu, H.; Mao, Z.; Wang, B.; Sui, X., Thiol–ene click reaction
on cellulose sponge and its application for oil/water separation. RSC Adv. 2017, 7 (33), 20147-20151. 8.
Du, Y.; Cheng, H.; Li, Y.; Wang, B.; Mao, Z.; Xu, H.; Zhang, L.; Zhong, Y.; Yan, X.; Sui, X.,
Temperature-responsive cellulose sponge with switchable pore size: Application as a water flow manipulator. Mater. Lett. 2018, 210, 337-340. 9.
Cheng, H.; Li, Y.; Wang, B.; Mao, Z.; Xu, H.; Zhang, L.; Zhong, Y.; Sui, X., Chemical
crosslinking reinforced flexible cellulose nanofiber-supported cryogel. Cellulose 2018, 25 (1), 573-582. 10. Cheng, H.; Du, Y.; Wang, B.; Mao, Z.; Xu, H.; Zhang, L.; Zhong, Y.; Jiang, W.; Wang, L.; Sui, X., Flexible cellulose-based thermoelectric sponge towards wearable pressure sensor and energy harvesting. Chem. Eng. J. 2017, 338, 1-7. 11. Wu, X.; Shi, Z.; Fu, S.; Chen, J.; Berry, R. M.; Tam, K. C., Strategy for synthesizing porous cellulose nanocrystal supported metal nanocatalysts. ACS Sustainable Chem. Eng. 2016, 4 (11), 5929-5935. 12. Shi, Z.; Gao, H.; Feng, J.; Ding, B.; Cao, X.; Kuga, S.; Wang, Y.; Zhang, L.; Cai, J., In situ synthesis of robust conductive cellulose/polypyrrole composite aerogels and their potential application in nerve regeneration. Angew. Chem., Int. Ed. 2014, 53 (21), 5380-5384. 13. Cai, J.; Liu, S.; Feng, J.; Kimura, S.; Wada, M.; Kuga, S.; Zhang, L., Cellulose–silica nanocomposite aerogels by in situ formation of silica in cellulose gel. Angew. Chem., Int. Ed. 2012, 124 (9), 2118-2121. 14. Sai, H.; Fu, R.; Xing, L.; Xiang, J.; Li, Z.; Li, F.; Zhang, T., Surface modification of bacterial cellulose aerogels’ web-like skeleton for oil/water separation. ACS Appl. Mater. Interfaces. 2015, 7 (13), 7373-7381. 15. Keshipour, S.; Khezerloo, M., Au‐dimercaprol functionalized cellulose aerogel: Synthesis, characterization and catalytic application. Appl. Organomet. Chem. 2018. DOI: 10.1002/aoc.4255. 16. Chen, W.; Zhang, Q.; Uetani, K.; Li, Q.; Lu, P.; Cao, J.; Wang, Q.; Liu, Y.; Li, J.; Quan, Z., Sustainable carbon aerogels derived from nanofibrillated cellulose as high‐performance absorption materials. Adv. Mater. Interfaces. 2016, 3 (10), DOI: 10.1002/admi.201600004. 17. Abraham, E.; Weber, D. E.; Sharon, S.; Lapidot, S.; Shoseyov, O., Multifunctional cellulosic scaffolds from modified cellulose nanocrystals. ACS Appl. Mater. Interfaces. 2017, 9 (3): 2010-2015. 18. Yang, R.; Aubrecht, K. B.; Ma, H.; Wang, R.; Grubbs, R. B.; Hsiao, B. S.; Chu, B., Thiol-modified cellulose nanofibrous composite membranes for chromium (vi) and lead (ii) adsorption. Polymer. 2014, 55 (5), 1167-1176. 19. Kabiri, S.; Tran, D. N.; Cole, M. A.; Losic, D., Functionalized three-dimensional (3d) graphene composite for high efficiency removal of mercury. Environ. Sci.: Water Res. Technol. 2016, 2 (2), 390-402. 20. Rull‐Barrull, J.; d'Halluin, M.; Le Grognec, E.; Felpin, F. X., Harnessing the dual properties of thiol‐grafted cellulose paper for click reactions: A powerful reducing agent and adsorbent for Cu. 19
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
443 444 445 446 447 448 449 450 451 452 453 454 455 456 457 458 459 460 461 462 463 464 465 466 467 468 469 470 471 472 473 474 475 476 477 478 479 480 481 482 483 484 485 486
Page 20 of 22
Angew. Chem., Int. Ed. 2016, 55 (43), 13549-13552. 21. Rull-Barrull, J.; d'Halluin, M.; Le Grognec, E.; Felpin, F.-X., A paper-based biomimetic device for the reduction of Cu (ii) to Cu (i)–application to the sensing of Cu (ii). Chem. Commun. 2016, 52 (39), 6569-6572. 22. Fu, Q.; Wang, X.; Si, Y.; Liu, L.; Yu, J.; Ding, B., Scalable fabrication of electrospun nanofibrous membranes functionalized with citric acid for high-performance protein adsorption. ACS Appl. Mater. Interfaces. 2016, 8 (18), 11819-11829. 23. Tingaut, P.; Zimmermann, T.; Sèbe, G., Cellulose nanocrystals and microfibrillated cellulose as building blocks for the design of hierarchical functional materials. J. Mater. Chem. 2012, 22 (38), 20105-20111. 24. Xin, Y.; Xiong, Q.; Bai, Q.; Miyamoto, M.; Li, C.; Shen, Y.; Uyama, H., A hierarchically porous cellulose monolith: A template-free fabricated, morphology-tunable, and easily functionalizable platform. Carbohydr. Polym. 2017, 157, 429-437. 25. Laure, W.; Fournier, D.; Woisel, P.; Lyskawa, J., Reversible tethering of polymers onto catechol-based titanium platforms. Langmuir. 2017, 33 (14), 3434-3443. 26. Song, Y.; Ye, G.; Wu, F.; Wang, Z.; Liu, S.; Kopec, M.; Wang, Z.; Chen, J.; Wang, J.; Matyjaszewski, K., Bioinspired polydopamine (PDA) chemistry meets ordered mesoporous carbons (OMCs): A benign surface modification strategy for versatile functionalization. Chem. Mater. 2016, 28 (14), 5013-5021. 27. Edgar, K.; Arnold, K.; Blount, W.; Lawniczak, J.; Lowman, D., Synthesis and properties of cellulose acetoacetates. Macromolecules 1995, 28 (12), 4122-4128. 28. Edgar, K. J.; Buchanan, C. M.; Debenham, J. S.; Rundquist, P. A.; Seiler, B. D.; Shelton, M. C.; Tindall, D., Advances in cellulose ester performance and application. Prog. Polym. Sci. 2001, 26 (9), 1605-1688. 29. Sanchez-Sanchez, A.; Fulton, D. A.; Pomposo, J. A., Ph-responsive single-chain polymer nanoparticles utilising dynamic covalent enamine bonds. Chem. Commun. 2014, 50 (15), 1871-1874. 30. Liu, H.; Rong, L.; Wang, B.; Mao, Z.; Xie, R.; Xu, H.; Zhang, L.; Zhong, Y.; Sui, X., Facile synthesis of cellulose derivatives based on cellulose acetoacetate. Carbohydr. Polym. 2017, 170, 117-123. 31. Liu, H.; Sui, X.; Xu, H.; Zhang, L.; Zhong, Y.; Mao, Z., Self‐healing polysaccharide hydrogel based on dynamic covalent enamine bonds. Macromol. Mater. Eng. 2016, 301 (6), 725-732. 32. Zhang, Z.; Sèbe, G.; Rentsch, D.; Zimmermann, T.; Tingaut, P., Ultralightweight and flexible silylated nanocellulose sponges for the selective removal of oil from water. Geographical Research 2014, 26 (8), 2659–2668. 33. Liu, H.; Rong, L.; Wang, B.; Xie, R.; Sui, X.; Xu, H.; Zhang, L.; Zhong, Y.; Mao, Z., Facile fabrication of redox/ph dual stimuli responsive cellulose hydrogel. Carbohydr. Polym. 2017, 176, 299-306. 34. Li, S.; Zhang, S.; Wang, X., Fabrication of superhydrophobic cellulose-based materials through a solution-immersion process. Langmuir. 2008, 24 (10), 5585-90. 35. Dourbash, A.; Motahari, S.; Omranpour, H., Effect of water content on properties of one-step catalyzed silica aerogels via ambient pressure drying. J. Non-Cryst. Solids. 2014, 405 (8), 135-140. 36. Jakab, E.; Varhegyi, G.; Faix, O., Thermal decomposition of polypropylene in the presence of wood-derived materials. J. Anal. Appl. Pyrolysis. 2000, 56 (2), 273-285. 37. Hu, Z.; Berry, R. M.; Pelton, R.; Cranston, E. D., One-pot water-based hydrophobic surface 20
ACS Paragon Plus Environment
Page 21 of 22 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
ACS Sustainable Chemistry & Engineering
487 488 489 490 491 492 493 494 495 496 497 498 499 500 501 502 503
modification of cellulose nanocrystals using plant polyphenols. ACS Sustainable Chem. Eng. 2017, 5 (6), 5018-5026. 38. Deville, S.; Tomsia, A. P., Freezing as a path to build complex composites. Science 2006, 311 (5760), 515-518. 39. Deville, S., Freeze‐casting of porous ceramics: A review of current achievements and issues. Adv. Eng. Mater. 2008, 10 (3), 155-169. 40. Mrówczyński, R.; Bunge, A.; Liebscher, J., Polydopamine—an organocatalyst rather than an innocent polymer. Chemistry 2014, 20 (28), 8647-53. 41. Powell, C. J.; Jablonski, A., Progress in quantitative surface analysis by x-ray photoelectron spectroscopy: Current status and perspectives. J. Electron Spectrosc. Relat. Phenom. 2010, 178 (5), 331-346. 42. Tripathi, A.; Parsons, G. N.; Rojas, O. J.; Khan, S. A., Featherlight, mechanically robust cellulose ester aerogels for environmental remediation. ACS Omega 2017, 2 (8), 4297-4305. 43. Sánchez, D.; Bastida, D.; Burés, J.; Isart, C.; Pineda, O.; Vilarrasa, J., Relative tendency of carbonyl compounds to form enamines. Org. Lett. 2012, 14 (2), 536-539. 44. Liao, Q.; Su, X.; Zhu, W.; Hua, W.; Qian, Z.; Liu, L.; Yao, J., Flexible and durable cellulose aerogels for highly effective oil/water separation. RSC Adv. 2016, 6 (68), 63773-63781.
504 505
21
ACS Paragon Plus Environment
ACS Sustainable Chemistry & Engineering 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
506
Page 22 of 22
TOC
507 508 509 510
Synopsis The CAA sponges could serve as a versatile and reversible precursor, paving a new way for constructing smart sponges through the post-modification strategy.
22
ACS Paragon Plus Environment