Evolution of Nitrogen-Related Defects in Graphitic Carbon Nitride

6 days ago - Defects play a pivotal role in the device performance of a photocatalytic, light emitting or photovoltaic system. Herein, graphitic carbo...
26 downloads 18 Views 4MB Size
Subscriber access provided by Eastern Michigan University | Bruce T. Halle Library

C: Physical Processes in Nanomaterials and Nanostructures

Evolution of Nitrogen-Related Defects in Graphitic Carbon Nitride Nanosheets Probed by Positron Annihilation and Photoluminescence Spectroscopy Biswajit Choudhury, Kamal Kumar Paul, Dirtha Sanyal, Anil Hazarika, and Pravat Kumar Giri J. Phys. Chem. C, Just Accepted Manuscript • DOI: 10.1021/acs.jpcc.8b01388 • Publication Date (Web): 06 Apr 2018 Downloaded from http://pubs.acs.org on April 8, 2018

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Evolution of Nitrogen-Related Defects in Graphitic Carbon Nitride Nanosheets Probed by Positron Annihilation and Photoluminescence Spectroscopy Biswajit Choudhury1*, Kamal Kumar Paul2, Dirtha Sanyal3,4, Anil Hazarika5, P. K. Giri2 1

Physical Sciences Division, Institute of Advanced Study in Science and Technology, Paschim Boragaon, Guwahati 781035, India 2

Department of Physics, Indian Institute of Technology Guwahati, Guwahati 781039, India 3 4

Variable Energy Cyclotron Center, 1/AF Bidhanngar, Kolkata 700064, India

Homi Bhabha National Institute, Training School Complex, Anushakti Nagar, Mumbai 400094, India

5

Department of Electronics and Communication Engineering, Tezpur University, Tezpur 784028, India

*Corresponding Author: [email protected] , [email protected] , Phone: +918486912412

1

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 44

ABSTRACT: Defects play a pivotal role in the device performance of a photocatalytic, light emitting or photovoltaic system. Herein, graphitic carbon nitride (g-C3N4) nanosheets are prepared at different calcination temperatures, and the evolution of defects in the system is studied by positron annihilation spectroscopy (PAS) and photoluminescence (PL) spectroscopy. Steady-state PL spectra show that free and defect bound excitonic emissions peaked at 2.78 eV, 2.58 eV and 2.38 eV are dominant with above bandgap excitation. Time-resolved PL studies reveal a significant enhancement of excitonic lifetime from 17.4 ns for free exciton to 27.4 ns in case of defect bound exciton. We provide a direct correlation between the defects observed by PAS with that of the excitonic lifetime found from the PL studies. Below bandgap excitation activates defect emission and it is characterized by a short carrier lifetime (~0.14 ns). Excitation power-dependent PL study with 405 nm laser shows progressive red-shift and narrowing of the emission line. We have interpreted the different PL features with defect band-filling of exciton, interplanar, intraplanar, interchain exciton migration, etc. These results are significant for tuning the optoelectronic properties of g-C3N4 nanosheets and exploiting its applications in various emerging areas.

2

ACS Paragon Plus Environment

Page 3 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

1. INTRODUCTION 1

Carbon nitride with graphene-like layered structures has drawn full attention for water splitting

2

reaction and in the decontamination of aqueous organic pollutants under visible light.1-4 The

3

system has a bandgap of 2.7 eV and builds up of s-heptazine units with tertiary nitrogen bridging

4

the nearest heptazine structures.1,3 Graphitic carbon nitride (g-C3N4) can be synthesized by

5

simple thermal condensation method from low-cost precursors, viz., thiourea,5 melamine,6

6

cyanamide,7 urea,3,8, etc. Temperature has a direct influence on the degree of condensation and

7

packing between layers, which otherwise influences the π conjugation in the sp2 bonded

8

framework.9 The high calcination temperature is known to reduce the interlayer distance in C3N4.

9

Compactness of the layers has an impact on the spectral red-shift in absorption and

10

photoluminescence. Wu et al. with density functional calculation studied the effect of interlayer

11

electron coupling on the optical properties of C3N4.10 In another study, Chen et al. reported that

12

the steric interactions of the lone pair electrons on adjacent nitrogen atom could tune the visible

13

light absorption in C3N4.11 C3N4 emits strong blue light under UV excitation.12 Its strong

14

excitonic emission in the visible region, thermal resistance, and tunable bandgap makes C3N4 a

15

popular choice for light-emitting diodes, luminescence-based bio, and chemosensor.13-16 Excitons

16

generated in the heptazine unit of C3N4 are reported to undergo facile migration along π stacking

17

direction in C3N4.17 Long distance exciton transport is necessary for photovoltaic and light

18

emitting diode applications.18-19 C3N4 quantum dots incorporated into polymer cells show

19

superior solar cell performance wherein the π conjugated system of C3N4 acts as charge transport

20

medium in the hybrid solar cell.19 Cui et al. observed sufficiently long excitonic lifetime in

21

phenyl modified graphitic carbon nitride and its possible requirements for advanced optical

22

super-resolution techniques.20 3

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 44

23

Defects are inevitable in C3N4 as its structure evolves through the formation of several

24

intermediates, such as cyanuric acid, melon, etc.21 The various uncondensed defects in C3N4 are

25

–NH2/NH, cyano/cyanide (C≡N, -NCN-) and oxygenated functional groups (-OH, -COOH).21,22

26

Besides, intrinsic defect such as N and carbon vacancies are also generated in C3N4 in the

27

thermal condensation process.23-25 Dong et al. observed efficient N2 fixation ability of N

28

deficient carbon nitride.23 Similarly, Tay suggested positive attributes of a defect in enhancing

29

photocatalytic H2 production in C3N4.24 With surface photovoltage spectroscopy (SPV), Wu and

30

his team measured the presence of NH/-NH2 related shallow and deep trap states in the bandgap

31

of C3N4.26 It was speculated that these defects are detrimental to the efficient production of H2.

32

In the present study, we aim to understand the specific nature and evolution of defects in

33

C3N4 as a function of its calcination temperature by using positron annihilation spectroscopy

34

(PAS) and photoluminescence (PL) spectroscopy techniques. We investigate the influence of

35

structural defects on the excitonic emission in C3N4. A detailed understanding of the nature of

36

defects in C3N4 and its impact on the excitonic luminescence and decay processes is necessary

37

before the implementation of this material in optoelectronics, photovoltaics, and solar cell

38

applications. Here, we employ steady-state and time-resolved spectroscopy techniques to identify

39

the free excitonic, bound excitonic and defect-related emissions and their decay dynamics. C3N4

40

are grown at different calcination temperatures. To the best of our knowledge and understanding,

41

for the first time, we have employed PAS to identify the nature of defects in C3N4 nanosheets

42

and provided a direct correlation between results of PAS and PL. PAS is a unique nuclear solid-

43

state technique to study the electron density and electron momentum distribution and in

44

particular, vacancy-type defects in the material.27-28 Free and defect bound excitonic emission

45

and trap state related luminescence and the associated carrier lifetime in C3N4 are studied with 4

ACS Paragon Plus Environment

Page 5 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

46

photoexcitation energies above and below the optical bandgap of the samples. Our results show

47

that defect bound excitons have sufficiently longer lifetime than that of the free excitons.

48 49

2. EXPERIMENTAL

50

2.1.

Preparation of graphitic carbon nitride (g-C3N4) at various temperatures

51

Graphitic carbon nitride was synthesized by thermal condensation method. Typically, urea was

52

taken in a beaker and heated in a reaction hood till it was scorched. The dried powder was

53

crushed in a mortar to get fine white powder. The powder was taken in a crucible covered with a

54

lid and heated in a tube furnace at 420 oC for 2 h. The final product was whitish yellow which

55

was again finely ground and kept in a sample vial. Similarly, calcination of dried urea was

56

performed at 470 oC, 520 oC, 570 oC, respectively.

57

2.2.

Materials Characterisation

58

X-ray diffraction (XRD) was performed in a Bruker D8 Advance X-ray diffractometer (0.154 nm

59

Cu Kα radiation, 40 kV, 40 mA) for the diffraction range 2θ~10-35o. Low and high-resolution

60

transmission electron microscope (TEM) images were collected in FEI Technai G2 20 S-Twin.

61

The operating voltage was 200 kV, and the spectral resolution was 2.4 Å. Fourier transform

62

infrared (FTIR) spectroscopy data were recorded in a Perkin Elmer, Spectrum BX

63

spectrophotometer. TGA was performed in a Perkin Elmer TGA 4000 series. The measurement

64

was performed under N2 flow at a heating rate of 10 oC/min. Diffuse reflectance spectra (DRS)

65

of the samples were collected in a Shimadzu UV–visible spectrometer (Model 2450) with BaSO4

66

as the standard reference. Steady-state photoluminescence spectra of the samples were monitored

67

in Fluoromax-4, Horiba Scientific spectrometer with an excitation and emission slit width of 2

68

nm. Laser power dependent PL studies were performed using a 405 nm (3.06 eV) diode laser 5

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 6 of 44

69

(Cube, coherent) equipped with cooled charge-coupled (CCD) detector (Princeton instruments,

70

PIXIS 100B). Time-resolved photoluminescence (TRPL) spectra were recorded using a

71

picosecond time-resolved luminescence spectrometer (Edinburgh Instruments, model: FSP920).

72

The chemical compositions of the samples were evaluated with X-ray photoelectron

73

spectroscopy (XPS) PHI X-tool automated photoelectron spectrometer (ULVAC-PHI, Japan).

74

The source was Al Kα X-ray beam source (1486.6 eV), and the recorded beam current was 20

75

mA. In XPS measurement, adventitious carbon (AdC) C 1s signal at 284.8 eV is considered as

76

binding energy (B.E.) reference.29,30 Au 4f signal might be considered as a B.E. reference peak

77

for carbon materials to reduce the error (0.1±0.2) while considering C 1s as reference.29,30

78

However, correct referencing of Au 4f signal for B.E. correction is not properly resolved and

79

thus, C 1s referencing is considered as widely adopted method for B.E. correction.29 Therefore,

80

in consensus with the report,30 we have considered C 1s at 284.8 eV for binding energy (B.E.)

81

corrections of different elements in C3N4. Defects were identified with positron annihilation

82

spectroscopy (PAS). In the present study, coincidence Doppler broadening (CDB) experiments

83

with two identical HPGe detectors of 12 % efficiency (Type, PGC 1216sp of DSG, Germany)

84

having energy resolution of 1.15 at 514 keV of 85Sr was used in coincidence. A 10 µCi22 NaCl

85

source encapsulated in a 1.5 micron-thin nickel foil was used as a positron source. The details of

86

the experimental set-up were mentioned elsewhere.31 The total counts under the CDB 511 keV

87

spectra of about 107 had been recorded in a dual ADC-based multiparameter data acquisition

88

system (MPA-3 of FAST ComTec., Germany). The CDB spectra had been analyzed by

89

constructing the area normalized ratio-curve method.

90 91 6

ACS Paragon Plus Environment

Page 7 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

92

The Journal of Physical Chemistry

3. Results and discussion

93

Figure 1 shows the XRD pattern of g-C3N4 processed at different temperatures. For all the

94

samples we have observed two diffraction peaks corresponding to (002) (2θ = 27o) and (100)

95

crystallographic planes (2θ = 12.6o).3 The shifting of (002) peak to higher diffraction angle with

96

calcination temperature is shown in the inset of Figure 1. Calculated d-spacing results for the

97

(002) and (100) planes at various calcination temperatures are inserted in Table S1. A reduction

98

in the d-spacing with calcination temperature for (002) plane indicates tight packing of layers

99

along the π-stacking direction of aromatic g-CN units. A reduced stacking distance will increase

100

the repulsion of the lone pair on aromatic as well as on bridging N atoms, favouring buckling of

101

nanosheets at higher calcination temperatures.32,33 As for the (100) peak, the d-spacing slightly

102

increases with calcination temperature. An increase in d-spacing indicates a larger intraplanar

103

distance of s-heptazine unit resulting from steric repulsion of lone pair electrons present on

104

neighbouring nitrogen atoms in s-heptazine unit.32,34

105 106 107

Figure 1 XRD pattern of C3N4 synthesized at different calcination temperatures. Inset shows the expanded view of (002) peak revealing clear peak shift. 7

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 44

108

Figure 2 displays TEM images of C3N4 grown at the different calcination temperature. As seen in

109

the low-resolution TEM images of CN420, CN470, CN520, and CN570 in Figure 2a, 2c, 2e and

110

2g, the as-grown C3N4 nanosheets at different temperatures acquire corrugated morphology with

111

porous structures. The corrugation in the nanosheets is believed to result from the repulsion of

112

lone pair electrons on bridging nitrogen in the s-heptazine unit of the adjacent layers.35 The pore-

113

like features can be well visualized in the high-resolution images of the samples (Figure 2b, 2d,

114

2f, and 2h). High-resolution images show that the nanosheets contain tightly packed layers with

115

approximately ~10-18 layers in the condensed thick structures of the nanosheets. FTIR spectra

116

(see in Figure S1, supporting information) of the samples reveal different types of C-N bonding

117

or presence of uncondensed CN, -CNH in the system. The broad absorption band between 3700-

118

3000 cm-1 comes from –NH vibration, -OH vibration, etc.36,37 The fingerprint region (1705-800

119

cm-1) of g-C3N4 contains several absorption bands. These bands are associated with symmetric,

120

asymmetric, bending vibration of aromatic and bridging C-N (or C=N) bonds in the s-heptazine

121

units of C3N4.38,39 Thermogravimetric analysis (TGA) of C3N4 prepared at different calcination

122

temperatures are shown in Figure S2 (supporting information). For CN420, there is 7 % weight

123

loss till temperature reaches 200 oC, and from 200-450 oC the weight loss is 2 %. In case of

124

CN470, CN520 and CN570 the total weight loss is 6 %, 3.5 %, and 0.5 %, respectively, till

125

temperature reaches 470 oC. The initial weight loss up to 200 oC is due to the removal of

126

adsorbed water and the final weight loss is due to the decomposition of intermediates, such as

127

cyanuric acid, ammeline, and ammelide, formed during the condensation of C3N4.40 The total

128

weight loss for the samples is very low, which indicates that C3N4 is the stable species with

129

fewer impurities. The rapid weight loss above 470 oC is due to the removal of the nitrogenated

8

ACS Paragon Plus Environment

Page 9 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

130

impurities and gases.41 Above 650 oC there is more than 95 % weight loss which is due to the

131

decomposition of C3N4.40

132 133 134

Figure 2 Low- and high- resolution TEM images of: (a-b) CN420, (c-d) CN470, (e-f) CN520 and (g-h) CN570.

135

The chemical composition of as-prepared C3N4 nanosheets is studied with X-ray

136

photoelectron spectroscopy (XPS). The C 1s XPS spectrum for CN520 is shown in Figure 3a,

137

and those of other samples are shown in Figure S3. In CN520, C 1s peak at 288.1 eV can be

138

assigned to sp2 hybridized N-C=N in aromatic s-heptazine ring, and the shoulder peak at 284.7

139

eV is arising from the adventitious carbon.5,42,43 The weak C 1s peak at 286.2 eV is probably

140

occurring due to the presence of nitrogen-related defects in the graphitic carbon nitride system

141

and attributed to N-CH=N bonding structure in the system.43 The high-resolution N 1s spectrum

142

for CN520 is deconvoluted into three components with peaks centered at 398.4 eV, 400.1 eV,

143

and 404.1 eV, respectively (Figure 3b). N 1s spectra for rest of the samples are included in

144

Figure S3. The dominant peak at 398.4 eV can be ascribed to two coordinated N atom (N2C in C-

145

N=C in aromatic ring), and the shoulder peak at 400.1 eV is attributed to three coordinated N 9

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 10 of 44

146

atom (N3C, tertiary nitrogen N-(C3) groups).5,23 The additional minor peak at 404.1 eV can be

147

assigned to cyano group or π-excitation.37 We measured the peak-area ratio of N2C to N3C for

148

C3N4 calcined at different temperatures. It is seen that N2C/N3C ratio changes as 2.14 (CN420),

149

2.36 (CN470), 0.83 (CN520) and 0.92 (CN570). A lower value of N2C/N3C indicates the presence

150

of nitrogen-vacancy at the N2C site, and from the measured values it is evident that CN520

151

experiences higher nitrogen loses at the two coordinated sites (N2C).25, 42,43 This implies a higher

152

density of nitrogen-vacancy defects in CN520.

153

154

Figure 3 Core level (a) C 1s and (b) N 1s peak XPS spectrum of CN520

155

To support our prediction from XPS that CN520 contains higher nitrogen-related vacancy

156

centers, we have employed positron annihilation spectroscopy (PAS) technique. PAS is a

157

powerful tool to identify vacancy-type defects in a material.

10

ACS Paragon Plus Environment

Page 11 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

158 159 160 161

Figure 4 (a) Ratio of area normalized CDB spectra of calcined C3N4 with respect to area normalized CDB spectra of 420 oC calcined C3N4. (b) Doppler broadening shape parameter, Sparameter, for differently calcined C3N4 samples.

162

We have considered coincidence Doppler broadening (CDB) method to determine the

163

nature of defects in C3N4.44 Figure 4a represents the ratio of area normalized CDB spectra of

164

calcined (470, 520 and 570 oC) C3N4 samples concerning the area normalized CDB spectra of

165

C3N4 calcined at 420 oC. It is clear from the Figure 4a that due to calcination at a higher

166

temperature, i.e., 520 oC and 570 oC, the ratio curve shows a broad dip in the momentum value

167

p L ~ 10×10-3 m 0c . The dip around p L = 10×10-3 m 0c represents more open volume defects in the

168

sample since the core electron wave functions are localized and do not span inside the available

169

volumes.31 One can identify the core electrons with which positrons are less annihilating by

170

estimating the kinetic energy of the electrons corresponding to the p L ~ 10×10-3 m 0c . Positrons

171

are almost thermalized before annihilation and using Virial theorem approximation (in the atom

172

the expectation value of the kinetic energy of an electron, is equal to the binding energy of the

173

electron), one can calculate the E kin using p L = (2m 0 E kin ) 2 .45 The calculated kinetic energy

174

corresponds to p L ~ 10×10-3 m 0c ~ 26 eV. In C3N4 nanosheets the core electron near to this value

175

is the only 2s electron of the nitrogen atom (~37 eV). This shows that due to calcination at 520

1

11

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 12 of 44

176

0

177

nitrogen-vacancy is less in case of 420 0C and 470 0C calcined samples.

178

The Doppler broadening shape parameter, S-parameter has been calculated for all the calcined

179

C3N4 samples. The S-parameter of the Doppler broadening of the positron annihilation gamma-

180

ray line profile N(E) vs. E is defined as the ratio of the counts in the central area

181

(511 keV − E ≤ 0.85 keV)

182

parameter represents the fraction of positrons annihilating with the “low” momentum electrons to

183

the “higher” momentum electrons. An increase of S-parameter indicates the increase of defects

184

in the system.31,45 Figure 4b depicts an enlargement of S-parameter due to calcination at 520 0C

185

and 570 0C sample. It is also clear from Figure 4b that the maximum defects can be generated in

186

the sample calcined at 520 0C, which is in agreement with the ratio curve analysis.

C, a large density of nitrogen vacancies has been created in the C3N4 sample, but the density of

(

and the counts in the total area 511 keV − E ≤ 4.25 keV ) . Thus S-

187

Figure 5a shows the Kubelka-Munk absorption plots of g-C3N4 prepared at different

188

calcination temperatures. The corresponding reflectance plot of the samples is shown in Figure

189

S4a. The samples show two absorption bands centered at 277 nm and 378 nm. These bands are

190

attributable to π-π* transition of the aromatic sp2 C=N unit and n-π* transition involving

191

nonbonding electrons on N atom in aromatic sp2 (C=N) and bridging sp3 (C-N).46,47 The bandgap

192

of the samples is determined from the plot of [F(R)hv]1/2 vs. hν (Figure 5b,Table S1). The

193

bandgap in C3N4 is a measure of indirect optical transition from Г to M in the Brillouin zone.48 It

194

is seen from table S1 that the bandgap of the samples decreases with an increase in calcination

195

temperature up to 520 °C. Up to this temperature the bandgap variation follows the trend 2.83 eV

196

(CN420), 2.75 eV (CN470) and 2.73 eV (CN520). The bandgap again increases to 2.85 eV in

197

CN570. The decrease in the bandgap can be attributed to the presence of intermediate defect 12

ACS Paragon Plus Environment

Page 13 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

198

states, such as uncondensed NH/NH2, or structural defects such as nitrogen vacancies.24,26 The

199

enlargement in the bandgap in completely grown CN570 is attributable to quantum confinement

200

effect. The intermediate defect states constitute the Urbach energy (Eu) tail below the optical

201

bandgap of the samples.

202 203 204

Figure 5 (a) Kubelka-Munk absorption plots, and (b) Tauc plots for the band gap calculation for C3N4 samples calcined at different temperatures.

205

We have determined Urbach energy for each sample from the slope of the linear fitting

206

between lnF(R) vs. hν.49 The measured values of Eu for different samples are included in Table

207

S1. There is an inverse relationship between Eg and Eu (Figure S4b). The samples with higher

208

bandgap have lower Eu and vice-versa. A higher Urbach energy value indicates the presence of

209

intermediate defect states in the samples. These defect states are mostly nitrogen-related as

210

manifested by the results of PAS. The overall trend of variation of S-parameter and the variation

211

in the bandgap with calcination temperature is more or less correlated, although not quite

212

matched. This is expected since positron probes only defects. However, for determining the

213

bandgap, defect is one of the many parameters. There are other parameters which might

13

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 14 of 44

214

influence the bandgap modification in C3N4. These include interlayer electron-electron coupling,

215

conjugation of π electron system, interlayer periodicity, etc.10,50, 51

216 217

Figure 6a shows the steady-state PL spectra of as-grown C3N4 nanosheets under an optical excitation energy 3.35 eV, well above the samples bandgap.

218 219 220 221

Figure 6 (a) PL spectra of C3N4 nanosheets grown at different temperatures under an excitation energy of 3.35 eV. The inset shows a magnified view of the PL spectrum of CN420. (b) PL spectra of CN520 obtained under different excitation energies.

222

The spectrum has a maximum emission in the blue region and a low energy tail extending down

223

to 1.8 eV. The blue emission is due to exciton generated in the s-heptazine ring.52 The excitonic

224

emission is red-shifted by ~0.08 eV as the calcination temperature increases from 420-470 °C

225

(Figure S5, supporting information). No change in the position of emission energy is monitored

226

at 520 °C and 570 °C. The observed spectral red-shift might be corroborated by the structural

227

changes in the as-grown C3N4. The changes include degree of condensation of the layers during

228

growth of C3N4, extrinsic and intrinsic defect formation, such as –NH/-NH2 surface

229

decomposition, an aromatic ring and bridging N defect formation, etc.43,46,53 Growth temperature

230

also affects the line-width of an excitonic emission. There is an increment in full-width at half 14

ACS Paragon Plus Environment

Page 15 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

231

maximum (FWHM) by ~0.1 eV on increasing the calcination temperature from 420-470 0C, as

232

seen in Figure S5. Above 470 0C and up to 570 0C, there is a marginal increase in the PL line-

233

width. The structural changes might also be responsible for the broader distribution of emission

234

centers, resulting in the broadening of emission peak.14,54 DFT based theoretical study has also

235

reported that PL properties of C3N4 exhibit extensive modifications in the presence of defects.

236

This has resulted in a synergetic effect of interlayer periodicity and formation of structural

237

defects.50 Since interlayer distance diminishes with increasing calcination temperature (as

238

revealed from the XRD analysis), possible exciton-exciton coupling and scattering might also

239

contribute to the broadening of the PL peak.55 We have also measured the impact of excitation

240

energy variation on the excitonic emission of C3N4. Figure 6b shows the PL spectra of CN520

241

under excitation energies of 3.35 eV, 3.54 eV, 3.75 eV, 4.00 eV and 4.27 eV. There is a

242

monotonic decrease in PL intensity with increasing excitation energy, which may be due to a

243

decrease in intensity of excitation light (a Xenon lamp) at higher energy (from near visible to

244

UV).56 Note that the position of the blue PL band is almost unchanged irrespective of the

245

incident excitation energy. Non-dependence of emission energy on excitation energy suggests

246

that excitonic emission occurs from the same excited π* state irrespective of probing energy.57

247

The emission spectrum of C3N4 (Figure 6) has a low energy tail emission

248

alongside the strong excitonic emission. To extract different emissive components from the

249

broad PL spectrum, we have deconvoluted the PL spectrum of CN520 with three Gaussian

250

peaks. The peaks are centered at 2.78 eV, 2.58 eV, and 2.38 eV, respectively (Figure 7a). In

251

conformity with the bandgap values determined for the absorption spectra and in agreement with

252

literature report, we infer that the intense emission peak at 2.78 eV is the excitonic peak.52 Other

253

emission peaks at 2.58 eV and 2.38 eV are lower than the measured bandgap of the samples. 15

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 16 of 44

254

Therefore, these emissions cannot be related to the free excitonic emission. We speculate that

255

these excitonic emissions are associated with structural defects in C3N4 nanosheets.

256 257 258 259 260 261

Figure 7 (a) Decovoluted (Gaussian) PL spectrum of CN520 under excitation of 3.35 eV. (b) TRPL (logarithmic plot) spectra of CN520 excited at 3.30 eV and monitored at 2.78 eV, 2.58 eV and 2.38 eV emission energies. (c) Plot showing a relation of S-parameter (left Y-axis) and average bound excitonic lifetime (τav at 2.38 eV) (right Y-axis) as a function of calcination temperature, which demonstrates a direct correlation between the S-parameter and τav.

262

263

For a detailed understanding of the associated PL decay, we have recorded the TRPL spectra for

264

different samples at the deconvoluted emission energies. TRPL spectra for CN520 at emission

265

energies 2.78 eV, 2.58 eV and 2.38 eV are obtained under excitation energy of 3.3 eV, and the

266

results are shown in Figure 7b. The decay profile is recorded for 0-200 ns time scale and the

267

amplitudes and lifetime components are listed in Table 1. It is found that the excitonic emission

268

at 2.78 eV has an average lifetime of 17.4 ns, whereas for the 2.58 eV and 2.38 eV emission

269

peaks the lifetimes are extended to 25.2 ns and 27.4 ns, respectively. Therefore, this extended 16

ACS Paragon Plus Environment

Page 17 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

270

carrier lifetime may be due to the involvement of bound excitons in the transition. The TRPL

271

spectra for the other samples are shown in Figure S6. From the PAS analysis, we have found that

272

S-parameter measures the nitrogen-vacancy defects in the system. Higher the S-parameter,

273

higher is the concentration of defects in the system. Figure 7c shows a comparison of the average

274

lifetime (τav) obtained for different samples for the bound excitonic emission. It is seen that

275

CN520 which has the highest defect content (the highest S-parameter) also possesses the longest

276

average PL lifetime for bound excitonic emission. Thus, a direct correlation between the vacancy

277

type defects and the excitonic lifetime established through this data allows us to unambiguously

278

identify the corresponding emissions as bound excitonic emissions in C3N4.

279 280

Table 1. TRPL Data of CN520 Excited at 3.3 eV and Monitored at 2.78 eV, 2.58 eV and 2.38 eV

Emission Energy. Sample

Emission (eV)

Lifetime (ns)

τ 1 (a1 )

CN520

τ 2 (a 2 )

τ av (ns) τ 3 (a 3 )

2.78 eV

1.1 (0.22)

5.0 (0.53)

23.6 (0.25)

17.4 ns

2.58 eV

1.9 (0.29)

7.0 (0.46)

33.6 (0.25)

25.2 ns

2.38 eV

1.8 (0.25)

6.9 (0.48)

36.0 (0.22)

27.4 ns

281

282

From the three components ( τ1 , τ 2 , τ3 ) of the excitonic lifetime in Table 1 for CN520, it

283

is clear that τ1 component does not change much for the three emission peaks. It is τ 2 and mostly

284

the τ3 component, which shows a large difference from that of free excitonic emission. It is seen

285

that the excitonic emission has an average lifetime of 17.4 ns, whereas for the 2.58 eV and 2.38

286

eV emission peaks the lifetimes are extended to 25.2 ns and 27.4 ns, respectively.

287

Now we elaborate on the origin of different lifetime components ( τ1 , τ 2 , τ3 ) for free 17

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 18 of 44

288

excitonic emission at 2.78 eV. Figure 8 gives a schematic view of different pathways of exciton

289

migration.

290 291 292 293 294

Figure 8 Schematic shows exciton migration in (a) π-stacking direction (interplanar), and (b) intraplanar migration (1) and intrachain (2) migration. Free excitons (F-exciton), when attached to nitrogen related defects (N-defects) create bound excitons (DB-exciton). Exciton migration is prohibited if C-H or N-H moiety terminates the heptazine link.

295

After photoexcitation, excitons that are confined to the aromatic ring undergo fast recombination

296

and gives rise to the fast decay component ( τ1 ). Excitons generated in the s-heptazine might also

297

migrate in the extended s-heptazine rings of C3N4 following different pathways. Excitons might

298

undergo facile interplanar migration along a π-stacking direction (Figure 8a) and transport from

299

one layer to another giving rise to the long exciton lifetimes ( τ 2 and τ 3 ).17 The other possible 18

ACS Paragon Plus Environment

Page 19 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

300

pathways of exciton migration that could result in the long excitonic lifetime could be as

301

depicted in Figure 8b. In interplanar migration, exciton moves between two connected s-

302

heptazine units with different symmetry planes. In intrachain migration exciton moves along the

303

s-heptazine chains through bridging N atom giving long excitonic lifetime, however, considering

304

its migration is not interrupted by the presence of N-H bonds or C-H bonds. Thus, we have

305

considered interplanar, intraplanar and intrachain migration as the possible pathways for

306

migration that could result in the long components of the free excitonic lifetime ( τ 2 and τ 3 ).

307

However, reports show that exciton migration follows an exponential decrease with stacking

308

distance.52 Table S1 shows that interplanar (or pi-stacking) distance of adjacent layers in C3N4

309

are separated by ~3.2 A . However, for intraplanar migration or migration along the heptazine

310

chains the exciton sitting on the nearest s-heptazine are separated by ~6.9 A (Table S1).

311

Therefore, exciton coupling and migration are supposed to be weak in this direction. Therefore,

312

we can predict that intraplanar and intrachain exciton migration can be responsible for the

313

τ 2 component. However, it is the interplanar or π-stacking direction which is sought to be the

314

most suitable pathway for long transport of exciton in C3N4 giving the longest τ3 component. If

315

we compare the different components ( τ1 , τ 2 , τ3 ) of lifetime for free excitonic (2.78 eV) and

316

bound excitonic emission (2.58 eV and 2.38 eV), we can easily interpret that it is the

317

τ3 component which is quite long in case of bound exciton emission compared to free emission.

318

Excitons bound to defect are relaxed for a longer period in the defect states before it finds a

319

recombination center. In this way, the defect bound excitons show high fluorescence stability

320

over the longer timescale.

0

0

19

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 20 of 44

321

To understand the response of the defect bound excitons to laser power excitation, we

322

have taken PL spectra of CN520 under diode-pumped solid-state laser. Figure 9a shows the

323

normalized PL spectra of CN520 under excitation of 3.06 eV (405 nm).

324 325 326 327 328

Figure 9 Normalized PL spectra of CN520 for different excitation power (intensity). The samples are excited with a solid-state laser of energy 3.06 eV. (b) Changes in emission energy (left Y-axis), full width at half maximum (FWHM) (right Y-axis) with laser power. The inset shows the PL emission intensity as a function of excitation laser power.

329

The emission spectra are recorded under laser power of 5 mW, 10 mW, 15 mW, 20 mW

330

and 25 mW. The un-normalized PL spectrum is shown in Figure S7. The emission intensity,

331

position and line-width display clear dependence on incident laser power, as shown in Figure 9b.

332

First, we will emphasize the changes in emission intensity with probing laser power. As shown

333

in the inset of Figure 9b, the emission intensity increases slightly on increasing the laser power

334

from 5 mW to 10 mW. There is a significant enhancement in PL intensity at a laser power of 15

335

mW. However, saturation of PL intensity occurs at higher excitation power (>15 mW). From the

336

previous study, it is understood that the emission intensity (IPL) of a sample exhibits a linear

337

variation with incident laser power following the relation, I PL ∞Lα , where L is excitation power

338

and α is power factor.58 In case of free excitonic emission, the emission intensity scales linearly

339

with laser power, whereas for bound excitonic emission the intensity varies linearly at low 20

ACS Paragon Plus Environment

Page 21 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

340

excitation power and deviates from linearity and saturates at high laser power.59 Therefore, we

341

might speculate that the non-linear intensity variation and saturation is resulted by these defect

342

bound excitons of C3N4. The position of emission energy is unchanged for the laser power of 5

343

mW and 10 mW (Figure 9b). There is a red-shift by ~0.5 eV when the laser power is set at 15

344

mW. On increasing the laser power from 15 mW to 20 mW, there is a shift of ~0.1 eV, and in

345

between 15 mW to 25 mW the shifting is ~0.2 eV. A similar trend is observed for FWHM

346

variation with laser power. Several factors have been associated with the red-shift of PL band

347

including laser heating effect, defect level population with photoexcited carriers, bandgap

348

renormalization, energy transfer, etc.58,60 Laser heating effect is prominent in nanoparticles

349

where heat conduction among nanoparticles is poor, and the heating effect is localized on a

350

single nanoparticle.61 However, in C3N4, having a conjugated 2D network, the heat energy might

351

go easy transfer throughout the system and therefore, localized heating effect as such may not be

352

prominent. Moreover, laser-induced local heating is known to cause spectral red-shift and

353

quenching in emission intensity by enhancing electron-phonon interaction and increasing non-

354

radiative recombination centers.62,63 No such spectral features have been observed in the PL

355

spectra. Therefore, laser heating is not the principal reason for the changes observed in emission

356

profile. The observed changes in PL feature can be associated with defect level population with

357

carriers.64 Since the system is excited with 3.06 eV laser, which is above the bandgap of the

358

samples, bound excitons are generated in the system. The number density of such excitons shows

359

dependence on incident laser power. At incident laser power of 5 mW and 10 mW, less number

360

of excitons could occupy the defect states near the conduction band edge. As laser power is

361

increased to 15 mW, large numbers of excitons could fill up the defect spaces distributed near

362

the band edge. Exciton distribution is expected to be non-uniform, and the number of radiative 21

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 22 of 44

363

recombination centers participating in luminescence appeared to be very high giving the spectral

364

broadness or increase in FWHM (Figure 9b). However, when the laser power is increased to 15

365

mW and 20 mW, the upper-level population saturates, and the excitons start to fill-up underlying

366

defect levels. Many of the excitons undergo exciton-exciton scattering and decay non-

367

radiatively. Only those excitons which can occupy the defect levels contribute to luminescence.

368

In the lower lying defect levels the exciton distribution appears to be uniform, and since the

369

number of radiative emission centers in these states seems to be less, the emission spectra attain

370

a narrow and symmetric feature.

371

C3N4 displays defect related sub-bandgap emission when the samples are photoexcited

372

with energies below the optical bandgap. In C3N4 the types of defects are nitrogen related, and

373

these could be cyano (C≡N), NH2, nitrogen vacancy, etc. PAS has characterized presence of

374

these nitrogen related defects. Figure 10a shows the normalized PL spectra of the samples

375

excited at 2.69 eV, 2.61 eV, 2.53 eV, 2.45 eV and 2.38 eV. Unlike above bandgap (BG)

376

photoexcitation where there is a band-to-band optical transition, photoexcitation below BG

377

triggers band to defect (D) transition, viz. π→D or LP→D. A broad asymmetric PL band

378

covering 2.1-2.55 eV spectral range is seen under excitation of 2.69 eV. As the photoexcitation

379

energy is decreased, the PL band becomes narrower and is gradually shifted towards lower

380

energy side. There is a red-shift of PL band by 0.3 eV when the excitation energy is changed

381

from 2.69 eV to 2.38 eV. The red-shift indicates that the trapped charge carriers jump from

382

different defect states to recombine with the holes. Moreover, the asymmetric and broad PL band

383

attains

384

Broadening/narrowing of PL band and its asymmetric/symmetric characteristics depend on the

385

filling up of empty defect levels with photoexcited charge carriers. At higher excitation energy

narrow

and

symmetric

features

as

the

excitation

energy

is

decreased.

22

ACS Paragon Plus Environment

Page 23 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

386

the defect levels near the conduction band-edge are filled up with charge carriers (shown in

387

schematic in Figure 10b).

388 389 390 391 392 393

Figure 10 (a) Photoluminescence spectra of CN520 at different excitation energy. The excitations are below the optical bandgap of the grown nanosheets. (b) Schematic showing below bandgap excitation and emissions due to carrier trapped in different defect states. Different band states in the valence band and conduction band, nitrogen lone pair (LP) state and nitrogen-related defect states are shown. (c) TRPL spectrum (logarithmic plot) of CN520 excited at 2.45 eV.

394

395

When the initial defect levels are filled up, the remaining charge carriers hop to its underlying

396

defect levels. Inhomogeneous distribution of charge carriers in these states might have resulted in

397

a broad PL band at an excitation of 2.69 eV. The narrowing and symmetric feature of PL band at

398

lower excitation energy indicates homogenous carrier distribution in the underlying defect levels.

399

TRPL data is recorded for CN520 with excitation at 2.45 eV and monitored at the emission

400

energy of 2.24 eV (Figure 10c). The three components of carrier lifetime are very short in case of

401

defect emissions (Table S2). Unlike the case of free and bound excitonic emission having an

402

average lifetime of 17.4 ns and 27.4 ns, the average lifetime of defect emissions is very short of

403

the order of 0.14 ns. From the analyzed results of PL under above and below band gap excitation,

404

we might infer that nitrogen related defects could extend the lifetime of free exciton when we

405

choose the excitation energy above the bandgap. Below bandgap excitation releases free carriers, 23

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 24 of 44

406

which are excited directly to the trapped centers underlying the bandgap of C3N4. The defect-

407

related PL band has low stability and decays with a very short lifetime.

4. Conclusions

408

409

In

summary,

we

employed

positron

annihilation,

steady-state

and

time-resolved

410

photoluminescence spectroscopy to probe the evolution of nitrogen-related defects in C3N4 with

411

calcination temperature. After photoexcitation, the excitonic emission in the intraplanar,

412

interplanar or intrachain direction gives rise to the shorter and longer decay components.

413

Excitons bound to nitrogen-related defect states decay with a lifetime of 27.4 ns, which is longer

414

than the free excitonic emission decay of 17.4 ns. Defect emission shows dependence on

415

excitation energy, and the lifetime of defect emission is only 0.14 ns. We have also demonstrated

416

laser power dependent excitonic emission in C3N4 with above bandgap excitation. The spectral

417

red-shift is mostly resulted by the band filling effect in which exciton readily fills up the

418

nitrogen-related defect states. This study provides a direct correlation between the defects

419

monitored by the PAS and PL and establishes the significant role of nitrogen-vacancy defects in

420

controlling the bound excitonic lifetime in C4N4 nanosheets. These results are significant for

421

tuning the optical properties of C3N4 nanosheets for ensuing applications in optoelectronics,

422

energy, and environment.

423

424

ASSOCIATED CONTENT

425

Figures of XPS, FTIR, TGA, Time-resolved PL, laser power dependent PL are included in the

426

Supporting Information. 24

ACS Paragon Plus Environment

Page 25 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

427

ACKNOWLEDGMENTS

428

The authors would like to thank central instruments facility (CIF) IIT Guwahati for providing

429

various characterisation facilities. BC would like to thank Department of Science and

430

Technology (DST), Govt. of India for providing DST Inspire faculty award (IFA15/MS-62) to

431

pursue this work. We thank Prof. M. Fujii, Kobe University, for the XPS measurement.

432 433

References

434 435

(1) Wang, X.; Maeda, K.; Thomas, A.; Takanabe, K.; Xin, W.; Carlsson, J.M.; Domen, K.;

436

Antonietti, M. A Metal Free Polymeric Photocatalyst for Hydrogen Production From Water

437

Under Visible Light. Nature Mater. 2009, 8, 76-80.

438

(2) Wang,X.; Maeda,K.; Chen,X.; Takanabe,K.; Domen,K.; Hou,Y.; Fu,X.; Antonietti, M.

439

Polymer Semiconductors for Artificial Photosynthesis: Hydrogen Evolution by Mesoporous

440

Graphitic Carbon Nitride with Visible Light, J. Am. Chem. Soc. 2009, 131, 1680-1681.

441

(3) Choudhury, B.; Giri, P.K. Isotype Heterostucture of Bulk and Nanosheets of Graphitic

442

Carbon Nitride for Efficient Visible Light Photodegradation of Methylene Blue. RSC Adv. 2016,

443

6, 24976-24984.

444

(4) Zheng, Q.; Durkin, D.P.; Elenewski, J.E.; Sun, Y.; Banek, N.A.; Hua, L.; Chen, H.; Wagner,

445

M.J.; Zhang, W.; Shuai, D. Visible-Light-Responsive Graphitic Carbon Nitride: Rational Design

446

and Photocatalytic Applications for Water Treatment. Environ. Sci. Technol. 2016, 50, 12938–

447

12948.

25

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 26 of 44

448

(5) Xu J.; Wang,Y.; Zhu, Y. Nanoporous Graphitic Carbon Nitride with Enhanced Photocatalytic

449

Performance. Langmuir 2013, 29, 10566−10572.

450

(6) Yan, S.C.; Li, Z.S.; Zou, Z.G. Photodegradation Performance of g-C3N4 Fabricated by

451

Directly Heating Melamine. Langmuir 2009, 25, 10397–10401.

452

(7) Fan, X.; Xing, Z.; Shu, Z.; Zhang, L.; Wang, L.; Shi, J. Improved Photocatalytic Activity of g-

453

C3N4 derived from Cynamide-Urea Solution. RSC Adv. 2015, 5, 8323-8328.

454

(8) Rajender, G.; Choudhury, B.; Giri, P.K. In-situ Decoration of Plasmonic Au Nanoparticles on

455

Graphene Quantum Dots-Graphitic Carbon Nitride Hybrid and Evaluation of its Visible Light

456

Photocatalytic Performance. Nanotechnology 2017, 28, 395703.

457

(9) Ho, W.; Zhang, Z.; Xu, M.; Zhang, X.; Wang, X.; Huang, Y. Enhanced Visible-Light Driven

458

Photocatalytic Removal of NO: Effect on Layer Distortion on g-C3N4 by H2 heating. Appl.

459

Catal., B 2015, 179, 106-112.

460

(10) Wu, F.; Liu, Y.; Yu, G.; Shen, D.; Wang, Y.; Kan, E. Visible-Light-Absorption in Graphitic

461

C3N4 Bilayer: Enhanced by Interlayer Coupling. J. Phys. Chem. Lett. 2012, 3, 3330−3334.

462

(11) Chen, Y.; Wang, B.; Lin, S.; Zhang, Y.; Wang, X. Activation of n→π* Transitions in Two

463

Dimensional Conjugated Polymers for Visible Light Photocatalysis, J. Phys. Chem. C 2014, 118,

464

29981–29989.

465

(12) Zhang, Y.; Pan, Q.; Chai, G.; Liang, M.;Dong, G.; Zhang, Q.; Qiu, J. Synthesis and

466

Luminescence Mechanism of Multicolour-Emitting g-C3N4 Nanopowders by Low Temperature

467

Thermal Condensation of Melamine. Sci. Rep. 2013, 3, 1943.

468

(13) Xu, J.; Shalom, M.; Piersimoni, F.; Antonietti, M.; Neher, D.; Brenner, T. Color-Tunable

469

Photoluminescence and NIR Electroluminescence in Carbon Nitride Thin Films and Light-

470

Emitting Diodes. Adv. Opt. Mater. 2015, 3, 913-917. 26

ACS Paragon Plus Environment

Page 27 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

471

(14) Gan, Z.; Shan, Y.; Chen, J.; Gui, Q.; Zhang, Q.; Nie, S. The Origins of the Broadband

472

Photoluminescence from Carbon Nitrides and Applications to White Light Emitting. Nano Res.

473

2016, 9, 1801-1812.

474

(15) Lee, E. Z.; Lee, S. U.; Heo, N.-S.; Stucky, G. D.; Jun, Y.-S.; Hong, W. H. A Fluorescent

475

Sensor for Selective Detection of Cyanide Using Mesoporous Graphitic Carbon (IV) Nitride.

476

Chem. Commun. 2012, 48, 3942 − 3944.

477

(16) Xiang, M.H.; Liu, J.W.; Li, N.; Tang, H.; Yu, R.Q.; Jiang, J.H. A Fluorescent Graphitic

478

Carbon Nitride Nanosheet Biosensor For Highly Sensitive, Label-Free Detection of Alkaline

479

Phosphatise. Nanoscale. 2016, 8, 4727-4732.

480

(17) Merschjann, C; Tschierlei, S; Tyborski, T; Kailasam, K; Orthmann, S; Hollmann, D;

481

Niedrig, T S; Thomas, A; Lochbrunner S. Complementing Graphenes: 1D Interplanar charge

482

Transport in Polymeric Graphitic Carbon Nitrides. Adv. Mater. 2015, 27, 7993.

483

(18) Burlakov, V.M.; Kawata, K.; Assender, H.E.; Briggs, G.A.D.; Ruseckas, A.; Samuel,

484

I.D.W.Discrete Hopping Model of Exciton Transport in Disordered Media. Phys. Rev. B 2005,

485

72, 075206.

27

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 28 of 44

486

(19) Chen, X.; Liu, Q.; Wu, Q.; Du, P.; Zhu, J.; Dai, S.; Yang, S. Incorporating Graphitic Carbon

487

Nitride (g-C3N4) Quantum Dots into Bulk-Heterojunction Polymer Solar Cells Leads to

488

Efficiency Enhancement. Adv. Funct. Mater. 2016, 26, 1719-1728.

489

(20) Cui, Q.; Xu, J.; Wang, X.; Li, L.; Antonietti, M.; Shalom, M. Phenyl-Modified Carbon

490

Nitride Quantum Dots with Distinct Photoluminescence Behavior. Angew. Chem., Int. Ed. 2016,

491

55, 3672-3676.

492

(21) Lau, V.W.-h; Yu, V.W.-z; Ehrat, F.; Botari, T.; Moudrakovski, I.; Simon, T.; Duppel, V.;

493

Medina, E.; Stolarczyk, J.; Feldmann, J., et al. Urea-Modified Carbon Nitrides: Enhancing

494

Photocatalytic Hydrogen Evolution by Rational Defect Engineering. Adv. Energy Mater. 2017, 7,

495

1602251.

496

(22) Wu, W.; Zhang, J.; Fan, W.; Li, Z.; Wang, L.; Li, X.; Wang, Y.; Wang, R.; Zheng, J.; Wu,

497

M., et al. Remedying Defects in Carbon Nitride To Improve Both Photooxidation and H2

498

Generation Efficiencies. ACS Catalysis 2016, 6, 3365-3371.

499

(23) Dong, G.; Ho, W.; Wang, C. Selective Photocatalytic N2 Fixation Dependent on g-C3N4

500

Induced by Nitrogen Vacancies. J. Mater. Chem. A 2015, 3, 23435-23441.

501

(24) Tay, Q.; Kanhere, P.; Ng, C.F.; Chen, S.; Chakraborty, S.; Cheng, A.; Huan, H.; Sum, T.C.;

502

Ahuja, R.; Chen, Z. Defect Engineered g-C3N4 for Efficient Visible Light Photocatalytic

503

Hydrogen Production. Chem. Mater.2015, 27, 4930-4933.

504

(25) Li, S.; Dong, G.; Hailili, R.; Yang, L.; Li, Y.; Wang, F.; Zeng, Y.; Wang, C. Effective

505

Photocatalytic H2O2 Production Under Visible Light Irradiation at g-C3N4 Modulated by Carbon

506

Vacancies. Appl. Catal., B 2016, 190, 26-35.

28

ACS Paragon Plus Environment

Page 29 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

507

(26) Wu, P.; Wang, J.; Zhao, J.; Guo, L.; Osterloh, F.E. Structural Defects in g-C3N4 Limit

508

Visible Light Driven Hydrogen Evolution and Photovoltage. J. Mater. Chem. A 2014, 2, 20338-

509

20344.

510

(27) Hautojärvi, P.; Corbel, C. Positron Spectroscopy of Solids; IOS Press: Amsterdam, 1995.

511

(28) Dutta, S.; Chattopadhyay, S.; Sarkar, A.; Chakrabarti, M.; Sanyal, D.; Jana, D. Role of

512

Defects in Tailoring Structural, Electrical and Optical Properties of ZnO. Prog. Mater.Sci. 2009,

513

54, 89-136.

514

(29) Greczynski, G.; Hultman, L. C1s Peak of Adventitious Carbon Aligns to the Vacuum

515

Level: Dire Consequences for Material’s Bonding Assignment by Photoelectron Spectroscopy,

516

ChemPhysChem 2017, 18, 1507-1512.

517

(30) https://xpssimplified.com/elements/carbon.php

518

(

519

Polycrystalline ZnO During Annealing Below 300 0C as Studied by In-situ Positron Annihilation

520

Spectroscopy. J. Mater. Sci. 2017, 52, 7615-7623.

521

(32) Tyborski,T.; Merschjann, C.; Orthmann,S.;Yang,F.; Steiner,; M-Ch Lux, Niedrig, Th

522

Schedel, Crystal Structure of Polymeric Carbon Nitride and the Determination of its Process-

523

Temperature-Induced Modifications. J. Phys.: Condens. Matter 2013, 25, 395402.

524

(33) Guo, Q.; Zhang, Y.; Zhang, H.S.; Liu, Y.; Zhao, Y.J.; Qiu, J.; Dong, G. 3D Foam Strutted

525

Graphene Carbon Nitride With Highly Stable Optoelectronic Properties, Adv. Funct. Mater.

526

2017, 27, 1703711.

31) Luitel, H.; Sanyal,D.; Gogurla, N.; Sarkar, A. Defect Generation and Recovery in

29

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

527

(34) Dai, H.; Gao, X.; Liu, E.; Yang, Y.; Hou, W.; Kang, L.; Fan, J.; Hu, X. Synthesis and

528

Characterisation of Graphitic Carbon Nitride Sub-Microscpheres Using Microwave Method

529

Under Mild Condition. Diamond Relat. Mater. 2013, 38, 109-117.

530

(35) Gracia, J.; Kroll, P. Corrugated Layered Heptazine-Based Carbon Nitride: The Lowest

531

Energy Modifications Of C3N4 Ground State. J. Mater. Chem. 2013, 19, 3013–3019.

532

(36) Lan, H.; Li, L.; An, X.; Liu, F.; Chen, C.; Liu, H.; Qu, J. Microstructure of Carbon Nitride

533

Affecting Synergetic Photocatalytic Activity: Hydrogen Bonds vs. Structural Defects, Appl.

534

Catal., B 2017, 204, 49-57.

535

(37) Qiu, P.; Chen, H.; Xu, C.; Zhou, N.; Jiang, F.; Wang, X.; Fu, Y. Fabrication of an Exfoliated

536

Graphitic Carbon Nitride as a Highly Active Visible Light Photocatalyst. J. Mater. Chem. A 2015,3,

537

24237-24244.

538

(38) Yu, Y.; Zhou, Q.; Wang, J. The Ultra-Rapid Synthesis of 2D Graphitic Carbon Nitride

539

Nanosheets via Direct Microwave Heating for Field Emission. Chem. Commun. 2016, 52, 3396-

540

3399.

Page 30 of 44

541

(39) Panasiuk, Y.V.; Raevskaya, A.E.; Stroyuk, O.L.; Lytvyn, P.M.; Kuchmiy, S.Y. Preparation 542

and Optical Properties of Highly Luminescent Colloidal Single-Layer Carbon Nitride. RSC Adv. 543

2015, 5, 46843-46849. 544

(40) Xu, J.; Li,Y.; Peng,S.; Lu, G.; Li, S. Eosin Y-sensitized Graphitic Carbon Nitride Fabricated

545

By Heating Urea For Visible Light Photocatalytic Hydrogen Evolution: The Effiect Of The

546

Pyrolysis Temperature of Urea. Phys. Chem. Chem. Phys. 2013, 15, 7657-7665.

30

ACS Paragon Plus Environment

Page 31 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

547

(41) Schmidt, C.L.; Jansen, M. New Directions in Carbonitride Research: Synthesis Of Resin-

548

Like Dense-Packed C3N4 Using a Hydrogen-Free Precursor. J. Mater. Chem. 2010, 20, 4183–

549

4192.

550

(42) Niu, P.; Liu, G.; Cheng, H.M. Nitrogen Vacancy Promoted Photocatalytic Activity of

551

Graphitic Carbon Nitride, J. Phys. Chem. C 2012, 116, 11013-11018.

552

(43) Niu, P.; Yin, L.C.; Yang, Y.Q.; Liu, G.; Cheng, H.M. Increasing the Visible Light

553

Absorption of Graphitic Carbon Nitride (melon) Photocatalysts by Homogenous Self-

554

Modifications with Nitrogen Vacancies. Adv. Mater. 2014, 26, 8046-8052.

555

(44) Guin, S.N.; Banerjee,S.; Sanyal,D.; Pati, S.K.; Biswas, K. Origin of the Order-Disorder

556

Transition and the Associated Anomalous Change of Thermopower in AgBiS2 Nanocrystals: A

557

Combined Experimental and Theoretical Study. Inorg. Chem. 2016, 55, 6323-6331.

558

(45) Myler, U.; Simpson, P.J. Survey of Elemental Specificity in Positron Annihilation Peak

559

Shapes. Phys. Rev. B 1997, 56, 14303.

560

(46) Bian, J.; Huang, C.; Zhang, R.Q. Graphitic Carbon Nitride Film: An Emerging Star for

561

Catalytic and Optoelectronic Applications. ChemSusChem. 2016, 9, 2723-2735.

562

(47) Butchosa, C.; Guiglion, P.; Zwijnenburg, M.A.Carbon Nitride Photocatalysts for Water

563

Splitting: A Computational Persepective. J. Phys. Chem. C 2014, 118, 24833–24842.

564

(48) Xu, Y.; Gao, S.P. Band Gap of C3N4 in the GW Approximation. Int. J. Hydrogen Energy

565

2012, 37, 11072-11080.

566

(49) Choudhury, B.; Choudhury, A. Oxygen Defect Dependent Variation of Band gap, Urbach

567

Energy and Luminescence Property of Anatase, Anatase-Rutile Mixed Phase and of Rutile

568

Phases of TiO2 Nanoparticles, Phys. E 2014, 56, 364-371. 31

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 32 of 44

569

(50) Guo, Q.; Zhang, Y.; Qiu, J.; Dong, G. Engineering the Electronic Structure and Optical

570

Properties of g-C3N4 By Non Metal Ion Doping, J. Mater. Chem. C 2016, 4, 6839-6847.

571

(51) Dong, G.; Zhang, Y.; Pan, Q.; Qiu, J. A Fantastic Graphitic Carbon Nitride Material:

572

Electronic Structure, Photocatalytic and Photoelectronic Properties, J. Photochem. Photobiol., C

573

2014, 20, 33-50.

574

(52) Merschjann, C.; Tyborski, T.; Orthmann, S.; Yang, F.; Schwarzburg, K.; Lublow, M.; Lux-

575

Steiner, M.C.; Niedrig, S.T. Photophysics of Polymeric Carbon Nitride: An Optical

576

Quasimonomer. Phys. Rev. B 2013, 87, 205204.

577

(53) Yuan, Y.; Zhang, L.; Xing, J.; Utama, M.; Lu, X.; Du, K.; Li, Y.; Hu, X.; Wang, S.; Genc.

578

A., et al. High Yield Synthesis And Optical Properties of g-C3N4. Nanoscale 2015, 7, 12343-

579

12350.

580

(54) Zhang, H.; Yu, A. Photophysics and Photocatalysis of Carbon Nitrides Synthesized at

581

Different Temperatures. J. Phys. Chem. C 2014, 118, 11628-11635.

582

(55) Kose, M.E. Evaluation of Excitonic Coupling And Charge Transport Integrals in P3HT

583

Nanocrystals, J. Phys. Chem. C 2011, 115, 13076–13082.

584

(56) https://www.hamamatsu.com/resources/pdf/etd/Xe-HgXe_TLS1016E.pdf

585

(57) Bian, J.; Li. J.;Kalytchuk, S.; Wang, Y.; Li, Q.; Lau, T.C.; Niehaus, T.A.; Rogach, A.L.;

586

Zhang, R.Q. Efficient Emission Facilitated by Multiple Energy Level Transitions in Uniform

587

Graphitic Carbon Nitride Films, ChemPhysChem 2015,16, 954-959.

588

32

ACS Paragon Plus Environment

Page 33 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

589

(58) Yan, H.; Yang, Y.; Fu, Z.; Yang, B.; Zuo, J.; Fu, S. Excitation-Power Dependence of the

590

Near-Band-Edge Photoluminescence of ZnO Inverse Opals and Nanocrystal films, J. Lumin.

591

2008, 128, 245-249.

592

(59) Tongay, S.; Suh, J.; Ataca, C.; Fan, W.; Luce, A.; Kang, J.S.; Liu, J.; Ko, C.;

593

Raghunathanan, R.; Zhou, J., et al. Defects Activated Photoluminescence in Two Dimensional

594

Semiconductors: Interplay Between Bound, Charged and Free Excitons, Sci. Rep. 2013, 3, 2657.

595

(60) Wang, H.; Ji, Z.; Qu, S.; Wang, G.; Jiang, Y.; Liu, B.; Xu, X.; Mino, H. Influence of

596

Excitation Power and Temperature on Photoluminescence in InGaN/GaN Multiple Quantum

597

Wells, Opt. Express 2012, 20, 3932-3940.

598

(61) Verma, P.;Irmer, G.; Monecke, J. Laser Power Dependence of the Photoluminescence From

599

CdSxSe1-x Nanoparticles in Glass, J. Phys. : Condens. Matter 2000, 12, 1097-1110.

600

(62) Guo, J.; Xu, J.; Zhuang, X.; Wang, Y.; Zhou, H.; Shan, Z.; Ren, P.; Guo, P.; Zhang, Q.;

601

Wan, Q., et al. Laser Photoluminescence Red Shift of ZnTe Nanostructure: The Effect of Twin

602

Structure, Chem. Phys. Lett. 2013, 576, 26-30.

603

(63) Ikhmayies, S.J.; Bitar, R.N.A.; Dependence of Photoluminescence of CdS:In Thin Films on

604

Excitation Power of the Laser, J. Lumin. 2014, 149, 240-244.

605

(64) Dang, G.T.; Kanbe, H.; Kawaharamura, T.; Taniwaki, M. Pulsed Laser Excitation Power

606

Dependence of Photoluminescence Peak Energies in Bulk ZnO. J. Appl. Phys. 2011, 110,

607

083508.

608 609 610 611 33

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

612

Page 34 of 44

TOC GRAPHIC

613

614

34

ACS Paragon Plus Environment

Page 35 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Figure 1 XRD pattern of C3N4 synthesized at different calcination temperatures. Inset shows the expanded view of (002) peak revealing clear peak shift. 72x65mm (600 x 600 DPI)

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 2 Low- and high- resolution TEM images of: (a-b) CN420, (c-d) CN470, (e-f) CN520 and (g-h) CN570. 71x34mm (300 x 300 DPI)

ACS Paragon Plus Environment

Page 36 of 44

Page 37 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Figure 3 Core level (a) C 1s and (b) N 1s peak XPS spectrum of CN520 54x20mm (300 x 300 DPI)

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 4 (a) Ratio of area normalized CDB spectra of calcined C3N4 with respect to area normalized CDB spectra of 420 oC calcined C3N4. (b) Doppler broadening shape parameter, S-parameter, for differently calcined C3N4 samples. 53x20mm (300 x 300 DPI)

ACS Paragon Plus Environment

Page 38 of 44

Page 39 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Figure 5 (a) Kubelka-Munk absorption plots, and (b) Tauc plots for the band gap calculation for C3N4 samples calcined at different temperatures. 40x18mm (300 x 300 DPI)

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 6 (a) PL spectra of C3N4 nanosheets grown at different temperatures under an excitation energy of 3.35 eV. The inset shows a magnified view of the PL spectrum of CN420. (b) PL spectra of CN520 obtained under different excitation energies. 62x24mm (600 x 600 DPI)

ACS Paragon Plus Environment

Page 40 of 44

Page 41 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Figure 7 (a) Decovoluted (Gaussian) PL spectrum of CN520 under excitation of 3.35 eV. (b) TRPL (logarithmic plot) spectra of CN520 excited at 3.30 eV and monitored at 2.78 eV, 2.58 eV and 2.38 eV emission energies. (c) Plot showing a relation of S-parameter (left Y-axis) and average bound excitonic lifetime (tav at 2.38 eV) (right Y-axis) as a function of calcination temperature, which demonstrates a direct correlation between the S-parameter and tav. 80x42mm (600 x 600 DPI)

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 8 Schematic shows exciton migration in (a) π-stacking direction (interplanar), and (b) intraplanar migration (1) and intrachain (2) migration. Free excitons (F-exciton), when attached to nitrogen related defects (N-defects) create bound excitons (DB-exciton). Exciton migration is prohibited if C-H or N-H moiety terminates the heptazine link. 129x126mm (300 x 300 DPI)

ACS Paragon Plus Environment

Page 42 of 44

Page 43 of 44 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

The Journal of Physical Chemistry

Figure 9 Normalized PL spectra of CN520 for different excitation power (intensity). The samples are excited with a solid-state laser of energy 3.06 eV. (b) Changes in emission energy (left Y-axis), full width at half maximum (FWHM) (right Y-axis) with laser power. The inset shows the PL emission intensity as a function of excitation laser power. 52x19mm (600 x 600 DPI)

ACS Paragon Plus Environment

The Journal of Physical Chemistry 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Figure 10 (a) Photoluminescence spectra of CN520 at different excitation energy. The excitations are below the optical bandgap of the grown nanosheets. (b) Schematic showing below bandgap excitation and emissions due to carrier trapped in different defect states. Different band states in the valence band and conduction band, nitrogen lone pair (LP) state and nitrogen-related defect states are shown. (c) TRPL spectrum (logarithmic plot) of CN520 excited at 2.45 eV. 60x20mm (300 x 300 DPI)

ACS Paragon Plus Environment

Page 44 of 44