Hierarchically Bicontinuous Porous Copper as Advanced 3D Skeleton

structure is beneficial for stable and reversible Li plating/stripping. 38-40. From this point of view, .... 3D hierarchically bicontinuous porous cop...
0 downloads 7 Views 4MB Size
Subscriber access provided by UNIVERSITY OF TOLEDO LIBRARIES

Energy, Environmental, and Catalysis Applications

Hierarchically Bicontinuous Porous Copper as Advanced 3D Skeleton for Stable Lithium Storage Xi Ke, Yifeng Cheng, Jun Liu, Liying Liu, Naiguang Wang, Jianping Liu, Chunyi Zhi, Zhicong Shi, and Zaiping Guo ACS Appl. Mater. Interfaces, Just Accepted Manuscript • DOI: 10.1021/acsami.8b01978 • Publication Date (Web): 30 Mar 2018 Downloaded from http://pubs.acs.org on March 30, 2018

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

Hierarchically Bicontinuous Porous Copper as Advanced 3D Skeleton for Stable Lithium Storage ⊥



Xi Ke† , Yifeng Cheng† , Jun Liu†, Liying Liu†, Naiguang Wang†, Jianping Liu†, Chunyi Zhi#, Zhicong Shi†* and Zaiping Guo§* †

Guangdong Provincial Key Laboratory of Functional Soft Condensed Matter, Smart Energy

Research Centre, School of Materials and Energy, Guangdong University of Technology, Guangzhou 510006, China #

Department of Materials Science and Engineering, City University of Hong Kong, 83 Tat Chee

Avenue, Hong Kong SAR, China §

Institute for Superconducting and Electronic Materials, Australian Institute for Innovative

Materials, University of Wollongong, Innovation Campus, North Wollongong, NSW 2500, Australia Keywords: Lithium metal anodes; 3D skeletons; Hierarchically bicontinuous; Polystyrene microspheres; Electrodeposition

ACS Paragon Plus Environment

1

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 2 of 30

Abstract: Rechargeable lithium metal anodes (LMAs) with long cycling life have been regarded as the “Holy Grail” for high-energy-density lithium metal secondary batteries. The skeleton plays an important role in determining the performance of LMAs. Commercially available copper foam (CF) is not normally regarded as a suitable skeleton for stable lithium storage owing to their relatively inappropriate large pore size and relatively low specific surface area. Herein, for the first time, we revisit CF and address these issues by rationally designing a highly porous copper (HPC) architecture grown on CF substrate (HPC/CF) as a 3D hierarchically bicontinuous porous skeleton through a novel approach combining self-assembly of polystyrene microspheres, electrodeposition of copper, and a thermal annealing treatment. In comparison with the CF skeleton, the HPC/CF skeleton exhibits a significantly improved Li plating/stripping behavior with high coulombic efficiency (CE) and superior Li dendrite growth suppression. The 3D HPC/CF-based LMAs can run for 620 h without short-circuiting in a symmetric Li/Li@Cu cell at 0.5 mA cm-2, and the Li@Cu/LiFePO4 full cell exhibits a high reversible capacity of 115 mAh g-1 with a high CE of 99.7% at 2 C for 500 cycles. These results demonstrate the effectiveness of the design strategy of 3D hierarchically bicontinuous porous skeletons for developing stable and safe LMAs.

1. Introduction The development of power sources with high energy density has become more and more important in recent years with the exploding demands for portable electronics, electric vehicles, and grid-scale energy storage. Currently, rechargeable lithium-ion batteries (LIBs) have been regarded as the state-of-the-art energy-storage devices, owing to their high energy density, high specific power, and long cycle life.1-3 Unfortunately, the energy density of LIBs is now

ACS Paragon Plus Environment

2

Page 3 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

approaching their theoretical limits owing to the relatively low capacity of the cathode and anode materials. In this context, lithium metal batteries (LMBs), such as Li-sulfur (Li-S)4-5 and Li-air (Li-O2)6-7 batteries, have attracted considerable attention since Li metal anodes (LMAs) possesses a number of advantageous characteristics, including extremely high theoretical specific capacity (3860 mAh g-1), the lowest known negative electrochemical potential (-3.04 V versus the standard hydrogen electrode) and low density (0.534 g cm-3).8-11 Its widespread application has been severely impeded, however, by the problems of lithium dendrite growth,12-13 which may lead to serious safety concerns, and low coulombic efficiency (CE) during repeated Li plating/stripping processes, all of which stem from fundamental issues concerning the intrinsic reactivity of Li metal with the electrolyte at low potentials14 and non-uniform lithium plating,15 as well as the poor mechanical stability of the solid-electrolyte interphase (SEI).16-17 In order to address these issues for LMAs, a large number of strategies, such as adding electrolyte additives,18-21 construction of artificial SEI film on Li metal,22-25 inhibition of space charge layer formation,26-27 regulation of Li metal nucleation,28-30 reducing effective current density,31-33 and designing stable hosts34-36 have been developed to stabilize the lithium plating and suppress the lithium dendrite growth. Alternatively, it is also very effective to employ largesurface-area conductive scaffolds with micro-/nano-structures as 3D porous skeletons for LMAs applications. For example, graphitized carbon fibers37 and copper skeletons38-40 with 3D porous structures have been demonstrated to effectively accommodate lithium and address the issue of Li dendrite growth. It is thus generally concluded that the porous conductive architecture can be employed as candidate 3D skeletons under conditions of large pore volume, proper pore size in the submicron range, and high electroactive surface area, since a 3D skeleton with such a pore structure is beneficial for stable and reversible Li plating/stripping.38-40 From this point of view,

ACS Paragon Plus Environment

3

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 30

commercially available metal foam skeleton, such as copper foam (CF) and nickel foam (NF), are not normally regarded as suitable 3D porous skeletons for LMAs, owing to their inappropriately large pore size and relatively low surface area. Previous studies have shown that the CF or NF skeletons exhibit relatively low CE and short cycle life, with a high tendency towards lithium dendrite growth and dead lithium formation.38-39,

41

Nevertheless, the metal

foams still stand a chance of acting as skeletons in LMAs configuration through rationally constructing their pore structures so as to effectively enlarge their electroactive surface areas to lower the local current density and delay the growth of lithium dendrites during Li plating/stripping. Colloidal crystals are one promising class of materials formed through self-assembly from monodisperse colloidal building blocks, such as polystyrene (PS) and silica microspheres, which have long been used as effective templates for the fabrication of a wide range of advanced porous materials at low cost and on a large scale.42 Normally, the 3D colloidal crystal template technique is employed in the fabrication of porous materials with long-range-ordered porosity and well-defined pore size, namely, an inverse opal structure in most cases, which generally involves a three-step procedure, including first self-assembling of colloidal microspheres into a colloidal crystal, then infiltrating or depositing functional materials into the interstitial void spaces in the colloidal crystal template, and finally removing the colloidal crystal template.43-44 The fabrication of such porous materials is usually carried out on flat solid substrates, however, such as ordinary glass slides,43 indium-doped tin oxide (ITO) glass,45 and gold-coated silicon wafers,46 and the self-assembly of colloidal crystal templates on porous curved substrates with irregular surfaces such as metal foams has rarely been reported. Herein, we extend the colloidal crystal template technique to assist in the fabrication of 3D highly porous copper (HPC)

ACS Paragon Plus Environment

4

Page 5 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

Figure 1. Schematic illustration of the fabrication procedure for the 3D HPC/CF composite.

frameworks grown on commercially available CF substrates (HPC/CF) via a four-step procedure (Figure 1). Specifically, synthetic PS microspheres are first self-assembled on a CF substrate (PS/CF). Secondly, the copper electrodeposition process is carried out on the as-prepared PS/CF substrate to yield a copper-deposited PS/CF substrate. Thirdly, the copper-deposited PS/CF substrate is washed with chloroform to remove the colloidal crystal template to produce a relatively ordered porous copper structure on the CF substrate. Finally, the obtained samples are subjected to a thermal annealing treatment to simultaneously coarsen the copper ligaments and enlarge the pore size, in order to create a HPC film that seamlessly integrated with the CF substrate (HPC/CF). The as-fabricated HPC/CF composite fulfills the aforementioned criteria required for a potential 3D porous skeletons for high performance LMAs, considering that such a 3D hierarchically bicontinuous porous copper architecture may provide a proper pore structure as well as intrinsically superior electrical conductivity. 2. Experimental section

ACS Paragon Plus Environment

5

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 6 of 30

2.1. Synthesis of polystyrene (PS) microspheres Briefly, 100 mL water, 5 mg sodium dodecyl sulfate, 32 g styrene (previously extracted three times with 0.1 M NaOH and three times with distilled water), and 0.1 g α-methylacrylic acid were added into a 500 mL three-necked round-bottom flask with a magnetic stir bar and a N2 inlet. The mixture was purged with N2 for 30 min with magnetic stirring. After the temperature was raised to 80°C, 0.1 g potassium persulfate dissolved in 3 mL water was rapidly added to the mixture. The mixture was then kept stirring for 8 h under N2 atmosphere. Finally, the suspension was diluted to 3 wt.% PS microspheres. The average diameter of the PS microspheres was about 500 nm (Figure S1). 2.2. Fabrication of 3D HPC/CF skeletons Copper foam (CF) substrates were cut into 1×5 cm2 pieces and washed successively in acetone, ethanol, and distilled water for 30 min. The clean CF substrates were then immersed in a dilute hydrochloric acid solution for 30 min to remove the native oxide on the copper surface. The pretreated CF substrates were then immersed in the monodispersed PS microsphere solution at 70°C for 2 h. After the self-assembly process, the CF substrates modified with the PS colloidal crystal template were used as the working electrodes for copper electrodeposition in a three electrode system, with two Pt mesh electrodes and a saturated calomel electrode (SCE) as the counter and the reference electrode, respectively. The electrolyte was an aqueous solution of CuSO4 (16 g L-1) and H2SO4 (0.12 g L-1). The electrodeposition process was carried out in galvanostatic mode at a current density of 12 mA cm-2 for 60 min at room temperature. After copper electrodeposition, the electrodes were rinsed with chloroform in order to first remove the PS microspheres. Finally, the electrodes were annealed successively at 120°C for 30 min, 300°C

ACS Paragon Plus Environment

6

Page 7 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

for 1 h, and 450°C for 2 h in a 5% H2/Ar mixture. The as-prepared 3D HPC/CF composites were cut into square discs (0.8 cm2) as skeletons for LMAs after vacuum drying. The areal weights of the as-obtained CF and HPC/CF skeletons were 63.1 and 75.9 mg cm-2, respectively. 2.3. Characterization and electrochemical measurements The crystal structures of the samples were analyzed by X-ray diffraction (XRD, Rigaku D/max2200/PC) using a Cu Kα radiation source at a wavelength of 0.1541 nm. The samples at different fabrication stages and the LMAs were characterized by field-emission scanning electron microscopy (FESEM, JEOL, JSM-6700F). Specifically, for the ex-situ characterization of the LMAs, the coin cell batteries containing them were first disassembled in a glove box to obtain the LMAs, which were rinsed with 1,3-dioxolane/dimethoxyethane (DOL/DME) solvents to remove residual electrolyte and lithium salt, and then dried in a glove box. Finally, the LMAs were sealed in a plastic box in the glove box to avoid air exposure during transfer to the vacuum chamber of the SEM. The electrochemical performance of the 3D HPC/CF and the CF skeletons for lithium storage was characterized in CR2032-type coin cells, which were assembled in an argon-filled glove box. The coin cells were composed of a HPC/CF or a CF skeleton as the working electrode, a Celgard separator, and a Li foil as the counter/reference electrode. The electrolyte was 1 M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) in DOL/DME (1:1 by volume) with LiNO3 as additive. The coulombic efficiency (CE) was measured at 1, 1.5, 2, and 3 mA cm-2 on a LAND electrochemical testing system under ambient conditions. The coin cells were initially cycled at 0−1 V (vs. Li+/Li) at 50 µA for 5 cycles in order to remove the surface impurities and stabilize the solid-electrolyte interphase (SEI). Then, 1 mAh cm-2 of Li metal was plated onto the HPC/CF

ACS Paragon Plus Environment

7

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 8 of 30

or the CF skeleton and then charged to 1.0 V (vs. Li+/Li) to strip the Li metal at 1, 1.5, 2, and 3 mA cm-2 for each cycle. The CEs were calculated based on the ratio of the stripped to the plated amounts of Li. Symmetric cells were used to analyze the cycling stability and cycle life of the LMAs on 3D HPC/CF and CF skeletons. For long-term galvanostatic charge/discharge measurements, 3 mAh cm-2 of Li was initially plated on the skeletons at 0.5 mA cm-2, and the cells were then charged and discharged at 0.5, 1, and 1.5 mA cm-2 for 1 mAh cm-2 in each half cycle. Electrochemical impedance spectra (EIS) measurements were conducted using an electrochemical workstation (Solartron 1287/1260) in the frequency range of 100 kHz to 0.1 Hz after selected cycles. Furthermore, LiFePO4 was employed as the cathode material for full cell characterization. LiFePO4 powder was mixed with Super-P and polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP) solvent to form a slurry, which was pasted onto carbon-coated aluminum foil to prepare the cathode. The 3D HPC/CF or the CF skeletons were initially assembled into a half cell with Li foil as the counter electrode. After plating 2 mAh cm-2 of Li metal into the skeletons, the LMAs in the copper skeletons were unloaded from the half cells and reassembled against the LiFePO4 cathode in a full cell with the same electrolyte composition as that in half cells. 3. Results and Discussion Figure S2 and Figure 2 display typical digital photographs and the corresponding SEM images of the samples at different stages during the fabrication procedure for the HPC/CF composite, respectively. It can be observed from Figure 2a that the pretreated CF substrate is composed of a network of 3D interconnected ligaments with diameters of 60-90 µm and highly porous structures, while the corresponding higher magnification SEM image (Figure 2b) shows that a ligament consists of a number of irregularly shaped micro-sized granules. After the self-

ACS Paragon Plus Environment

8

Page 9 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

Figure 2. SEM images of the CF at low (a) and high (b) magnification, top-view SEM image of PS colloidal crystal template-modified CF substrate (c), and SEM images at different magnifications (d-f) of the 3D HPC/CF composite.

assembly process for the PS microspheres on the CF, the copper ligament surface is covered by close-packed arrays of PS microspheres (Figure 2c), which are employed as the template for the subsequent copper electrodeposition carried out in galvanostatic mode. Figure S3 displays a typical chronopotentiometric polarization curve for the galvanostatic copper electrodeposition on the PS colloidal crystal-covered CF substrate at a current density of 12 mA cm-2. After a sequential process including copper electrodeposition, PS colloidal crystal leaching, and a thermal annealing treatment, the HPC structures were firmly grown on the CF substrate, which

ACS Paragon Plus Environment

9

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 10 of 30

clearly results in an increase in the copper ligament size up to about 100-150 µm (Figure 2d). The higher magnification SEM image (Figure 2e) reveals that a large number of porous copper granules with various sizes ranging from 5 to 25 µm were grown on the original CF ligament. Furthermore, it can be observed from Figure 2f that a bicontinuous network of copper ligaments and void pores was formed in these granules through this fabrication route. The sizes of the ligaments and pores are in the submicron range, which may be determined by the size of the PS microspheres. The energy dispersive X-ray spectroscopy (EDX) and corresponding elemental mapping results for the HPC/CF composite confirm the presence of Cu (Figure S4). X-ray diffraction (XRD) measurements were employed to further characterize the crystal phase of the HPC/CF composite. For comparison, the XRD pattern of the CF substrate was also collected. As shown in Figure S5, the XRD pattern of the HPC/CF composite was consistent with that of the CF substrate. The peaks appearing at 2θ values of 43.7°, 50.8°, and 74.4° can be indexed to the diffraction from the (111), (200), and (220) planes of cubic copper (JCPDS card no. 04-0836), respectively. Such results confirm that the as-prepared HPC structures were made of metallic copper. According to mercury porosimetry measurements, the CF and the HPC/CF have a pore area of 0.023 and 0.05 m2/g, respectively (Figure S6a-b). The increase in specific surface area of the HPC/CF compared to the CF can be attributed to the presence of the HPC structures with high submicron porosity. In addition, the cumulative pore volume of the HPC/CF composite was determined to be 0.5216 cm3 g-1 (Figure S6c). As such, a 3D hierarchically bicontinuous porous copper architecture was successfully constructed through the PS colloidal crystal templateassisted copper electrodeposition on the commercially available CF substrate. Ideally, such a facile and low-cost fabrication procedure could be extended to the preparation of other types of 3D hierarchically porous metallic structures, which may be examined in our further studies.

ACS Paragon Plus Environment

10

Page 11 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

Figure 3. Low (a, c, e) and high magnification (b, d, f) SEM images showing the morphological evolution of HPC structures on the CF substrate at the initial stage (a, b), and after annealing successively at 120°C for 30 min (c, d) and 300°C for 1 h (e, f).

It was found that the thermal annealing step in the fabrication procedure plays an important role in the formation of the bicontinuous porous structure of the HPC granules. In order to understand the effect of the annealing treatment on the morphology and structural evolution of the HPC, we characterized the samples at different stages to observe the morphological evolution of the electrodeposited copper structures, as shown in Figure 3. It can be seen that, after the copper electrodeposition and the following rinsing with chloroform, a large number of honeycomb-like copper microspheres with various sizes are distributed on the surfaces of the pristine copper ligaments (Figure 3a), and the uniformly distributed pores in these microspheres

ACS Paragon Plus Environment

11

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 12 of 30

with a size of about 500 nm are apparently produced by the leaching of the PS microspheres with chloroform after copper electrodeposition (Figure 3b). After heating to 120°C for 30 min, the sizes of the copper ligaments and pores start to increase (Figure 3c and d). The quasi-ordered porous structures on the copper microsphere surface began to become randomly bicontinuous porous structures. After further annealing at 300°C for 1 h, the ligament coarsening becomes more apparent and the ligament surfaces become very smooth, as shown in Figure 3e and f. The final annealing step at 450°C for 2 h employed to remove the possible residual PS has little effect on the morphology of the copper structures (data not shown). It is revealed that the surface morphology of the electrodeposited copper structures is transformed from the quasi-ordered honeycomb-like morphology to the bicontinuous sponge-like morphology after this annealing stage. Therefore, it is demonstrated from the above results that the thermal annealing treatment, which coarsens the copper ligaments and enlarges the pore size, is a very essential step for the formation of HPC structures. It is suggested in a previous report that the coarsening of the porous metals, which involves ligament pinch-off and the formation of void bubbles, results from a surface-diffusion-controlled solid-state Rayleigh instability, which controls the change in topology of the porous material.47 In this study, the surface diffusion of copper atoms may be activated during the thermal annealing process. The protocol presented here would provide a new avenue for the rational design of other porous metallic structures for many applications. Figure 4 displays a top-view of the surface morphology evolution of the pristine skeletons and t h e p l at e d Li m e t a l a f t er d i ff e r e n t c yc l e s . T h e e l ec t ro l yt e w a s 1 M l i t h i u m bis(trifluoromethanesulfonyl)imide (LiTFSI) in DOL/DME (1:1 by volume) with 1 wt% LiNO3 as the additive. This DOL/DME ether-based electrolyte is commonly used in lithium metal sulfur batteries, and LiNO3 is employed to form a stable SEI on the lithium metal surface. In addition,

ACS Paragon Plus Environment

12

Page 13 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

Figure 4. SEM images of the surface morphology of Li metal electrodeposited on the CF and the 3D HPC/CF skeletons with a current density of 1.5 mA cm-2 for a capacity of 1 mAh cm-2 of Li. SEM images under different magnifications of the pristine CF skeleton (a, e), and the 10th (b, f), the 80th (c, g), and the 180th (d, h) Li plating, respectively. SEM images under different magnifications of the pristine 3D HPC/CF skeleton (i, m), and the 10th (j, n), the 80th (k, o), and the 180th (l, p) Li plating, respectively.

the morphology of lithium metal deposits in this electrolyte is inclined to be spherical which is convenient for particle size analysis from SEM images.40 For the CF skeleton, the lowmagnification SEM images (Figure 4a-d) show that the metallic Li rapidly filled the pores of the CF with increasing cycle numbers, while the magnified SEM images (Figure 4e-h) reveal that the Li metal deposits were composed of mossy and dendritic structures which were mainly loosely stacked in the pores of the skeletons. The rapid growth of Li metal into the pore spaces of

ACS Paragon Plus Environment

13

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 14 of 30

the CF (Figure S7b) was possibly caused by the faster deposition rate of Li metal on the curved ridge regions of the copper ligament (indicated by the blue arrows in Figure S7a) compared to the smooth surface regions of the copper ligament (indicated by the red arrows in Figure S7a), which can be attributed to the intensified current density distribution and the greater Li ion flux on the curved ridge area compared to the smooth surface.40 In contrast, Li plating on the 3D HPC/CF skeleton leads to a distinct change in surface morphology evolution. The lowmagnification SEM images (Figure 4i-l) show that the original macroporosity of the skeleton is maintained after cycling, indicating that the Li metal was well accommodated in the pores of the 3D HPC structures, while the magnified SEM images (Figure 4m-p) show that the Cu skeleton was covered with a homogeneous, dense and smooth Li layer without any Li dendrites, which was further verified by the cross-sectional SEM images of the fresh and cycled HPC/CF skeletons (Figure S8). A similar trend in the surface morphology evolution was also observed for the Li plating at the current densities of 1.0 and 2.0 mA cm-2 (Figures. S9, S10). The above results indicate that the 3D HPC/CF skeleton with hierarchically bicontinuous porosity can effectively suppress the growth of the Li dendrites, which can be attributed to these two synergistic factors: first, its increased specific surface area can not only provide more sites, but also reduce the local current density for Li plating, significantly retarding the growth of Li dendrites; second, its higher curvature in the HPC structures can induce more Li nucleation and growth in the pores owing to the tip effect, greatly suppressing the growth of Li dendrites.40 Based on the above results and previous reports,9, 48 the Li plating behavior on the CF and the 3D HPC/CF skeletons can be schematically illustrated in Figure 5. Specifically, for the CF skeleton, Li metal first forms small Li islands on the copper skeleton in the nucleation step, with most of the islands distributed on the curved ridges due to the intensified current density distribution and

ACS Paragon Plus Environment

14

Page 15 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

Figure 5. Schematic diagram of the Li plating stages on the CF (top) and the 3D HPC/CF (bottom) skeletons.

greater Li ion flux. As the plating progresses, a Li metal layer grows on the copper skeleton surface, with massive Li dendrites growing from the ridge area into the pore space, caused by the above-mentioned tip effect on the curved ridge area. In contrast, for the 3D HPC/CF skeleton, owing to the existence of numerous highly curved submicron-size copper ligaments in the HPC granules, Li metal preferentially nucleates and grows in the HPC structures due to the tip effect. As the plating progresses, Li metal was well accomodated into the HPC structures, thus effectively suppressing the growth of Li dendrites. The electrochemical performance in an actual LMB is an important index for the application prospects of the as-prepared 3D HPC/CF skeletons. CEs at different current densities (1, 1.5, 2, and 3 mA cm-2) were measured and the results are shown in Figure 6. At a current density of 1.0

ACS Paragon Plus Environment

15

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 16 of 30

Figure 6. CEs of LMAs on the 3D HPC/CF and the CF skeletons at different current densities of 1 mA cm-2 (a), 1.5 mA cm-2 (b), 2 mA cm-2 (c), and 3 mA cm-2 (d). The amount of Li plating in each cycle was fixed at 1.0 mAh cm-2.

mA cm-2, the HPC/CF-based electrode maintained a high CE of 98% over 270 cycles, while that of the CF-based electrode decreased markedly to below 70% after 160 cycles (Figure 6a). As the current density was increased to 1.5, 2, and 3 mA cm-2, the HPC/CF-based Cu/Li cell exhibited highly stable CEs at 96% over 200 cycles, at 95% over 150 cycles, and at 94% over 100 cycles, respectively, whereas the CF-based Cu/Li cell showed a rapid decrease in its CEs after 120 cycles, 60 cycles, and 40 cycles, respectively (Figure 6b-d). The rapid decline in the CEs, accompanied by large oscillations, can be ascribed to uncontrollable growth of dendritic and mossy Li, which results in the continuous growth of the SEI layer, consuming much of the Li. Such results reveal that the hybridization of the 3D HPC architecture on the CF substrate effectively improves the cycling performance of the Li metal plating/stripping. It is worth noting

ACS Paragon Plus Environment

16

Page 17 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

that the cycling performance of the as-prepared 3D HPC/CF skeletons in LMAs also significantly outperforms recently reported 3D copper skeletons, for example, a 3D skeleton with a jungle-like porous copper layer composed of Cu submicron fibers grown on copper foil exhibits a stable CE of about 97% at 0.5 mA cm-2 over 50 cycles,38 and another highly porous 3D skeleton, which was derived from chemical dealloying of commercially available Cu-Zn alloy foil, shows a stable CE of about 97% at 1.0 mA cm-2 for 140 cycles.39 Figure 7a and b show the voltage profiles of the Li plating/stripping on the CF and the 3D HPC/CF skeletons at a current density of 1.5 mA cm-2 for a total of 1 mAh cm-2 of Li metal. It is shown that the charge/discharge curves of the 3D HPC/CF skeletons are nearly overlapping, except for the first cycle, whereas the amount of stripped Li was significantly reduced after cycling for the CF skeleton, which is in line with the results shown in Figure 6b. Moreover, as displayed in the insets of Figure 7a and b, the 3D HPC/CF skeleton exhibits smaller voltage hysteresis, which is defined as the voltage difference between the discharge and charge processes, than the CF skeleton, indicating reduced interfacial resistance in the 3D HPC/CF skeleton. Furthermore, the long-term cycling stability of the 3D HPC/CF and the CF skeletons was characterized by testing a symmetric Li/Li cell containing a Li foil counter/reference electrode and a Li@Cu working electrode. The 3DHPC/CF and CF skeletons were initially plated with 3 mAh cm-2 of Li metal, and then cycled at a current density of 0.5 mA cm-2 and a cycling capacity of 1 mAh cm-2. As can be observed from the voltage-time profiles of the Li plating/stripping (Figure 7c), the LMA on the CF skeleton shows random voltage oscillations after cycling for 160 h, which could be attributed to the polarization resulting from the continuous formation of a SEI layer, and then a sudden voltage drop after cycling for 340 h, which could possibly be caused by a dendrite-induced short circuit of the cell. In comparison, the Li plating/stripping for

ACS Paragon Plus Environment

17

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 18 of 30

Figure 7. Voltage profiles of Li plating/stripping on the CF (a) and the 3D HPC/CF (b) skeletons at a current density of 1.5 mA cm-2 for a total of 1 mAh cm-2 of Li, with the insets showing enlargements of the low voltage range. Voltage-time profiles of the Li plating/stripping with a cycling capacity of 1 mAh cm-2 at 0.5 mA cm-2 in symmetric Li/Li@Cu cells with the 3D HPC/CF and the CF skeletons (c). Cycling performances of the LMAs with 3D HPC/CF and CF skeletons in a full cell with a LiFePO4 cathode at 2 C (d).

the LMA on the 3D HPC/CF skeleton exhibits greatly improved cycling stability without notable voltage fluctuation. There appears to be no sign of a short circuit after cycling for 620 h,

ACS Paragon Plus Environment

18

Page 19 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

suggesting that the growth of Li dendrites has been effectively suppressed. The corresponding voltage hysteresis curves (Figure S11) also clearly show the voltage fluctuation phenomenon and the short circuit event during the cycling. Specifically, at a current density of 0.5 mA cm-2, Li plating/stripping on the CF-based LMA leads to a continuously oscillating voltage hysteresis above 50 mV, and then there is a sharp drop to about 17 mV after 80 cycles indicating a short circuit, whereas the Li plating/stripping on the 3D HPC/CF-based LMA leads to a very stable voltage hysteresis below 27 mV during the whole of the cycling. As is well known, the voltage hysteresis is mainly affected by the charge transfer resistance, interfacial properties, and current density.22-23 The decrease in the voltage hysteresis on the 3D HPC/CF-based LMA may result from the increased specific surface area of the 3D HPC/CF skeleton, which can reduce the charge transfer resistance, offer a larger interfacial area, and lower the local current density. Electrochemical impedance spectroscopy (EIS) measurements of the two types of skeletons were further performed to investigate the interfacial properties. It is shown in Figure 8 that the values of the SEI resistance (RSEI) and the charge transfer resistance (Rct) (Figure 8d) of the 3D HPC/CF skeleton are always smaller than those for the CF skeleton, and these resistances decrease with cycling, which reveals that the HPC structure can stabilize the electrode/electrolyte interface. Additionally, the long-term cycling at larger current densities of 1.0 and 1.5 mA cm-2 of the 3D HPC/CF skeleton also results in a smaller and much more stable voltage hysteresis than for the CF skeleton (Figure S12). Furthermore, in order to evaluate the potential practical application of the as-prepared 3D HPC/CF skeleton, full cells were assembled with the 3D HPC/CF or the CF skeletons, on which 2 mAh cm-2 of Li metal was pre-plated as the anode, and LiFePO4 as the cathode. Figure 7d shows the cycling performance of the LMA with the 3D HPC/CF and the CF as the skeletons at 2 C for 500 cycles, it can be observed that the LMA

ACS Paragon Plus Environment

19

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 20 of 30

Figure 8. EIS curves for selected cycles of the CF (a) and the 3D HPC/CF (b) skeletons at a current density of 1.5 mA cm-2 for a total of 1 mAh cm-2 of Li; the corresponding equivalent circuit model used to fit the experimental results (c) and the fitting results for the circuit elements (d).

based on the 3D HPC/CF skeleton exhibits greatly enhanced cycling performance compared to

ACS Paragon Plus Environment

20

Page 21 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

the LMA using the CF skeleton. The reversible capacity of the 3D HPC/CF skeleton-based LMA could be retained at 115 mAh g-1 with a high CE of 99.7%, revealing a capacity retention of 71.1%, whereas that of the CF skeleton based LMA remained at 102.5 mAh g-1 after 300 cycles with a CE of 99.4%, corresponding to a capacity retention of 67.7%, and then abruptly decreased to only 7.6 mAh g-1 after 500 cycles with a CE of 92.8%. The significantly enhanced electrochemical performance of the 3D HPC/CF, in comparison to that of the CF skeleton, indicates good application prospects for 3D HPC/CF skeletons in practical LMBs. 4. Conclusion In summary, we have demonstrated a novel fabrication approach for constructing HPC frameworks on the commercially available CF substrate to produce a 3D hierarchically bicontinuous porous copper skeleton (HPC/CF) by a protocol combining self-assembly of PS microspheres, Cu electrodeposition, and thermal annealing. The thermal annealing treatment plays an essential role in the surface morphology and structural evolution of the HPC structures. The engineering of the structure of the CF skeleton by integrating the HPC frameworks provides a 3D hierarchically bicontinuous porous copper skeleton with an increased specific surface area, which can not only provide a larger interfacial area, but also reduce the charge transfer resistance and reduce the local current density during Li plating/stripping. Additionally, Li metal preferentially nucleates and grows in the HPC frameworks due to the tip effect, which effectively suppresses the growth of Li dendrites, leading to high electrochemical performance of the LMAs. The cells with the 3D HPC/CF skeletons delivered enhanced CEs, and thus presented superior Li plating/stripping cycling performance. The 3D HPC/CF-based LMAs can run for 620 h without short-circuiting in a symmetric Li/Li@Cu cell at a current density of 0.5 mA cm-2. Furthermore, the Li@Cu/LiFePO4 full cell exhibits superior capacity retention with a high CE of 99.7% at 2 C

ACS Paragon Plus Environment

21

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 22 of 30

for 500 cycles, revealing the potential practical applications of the 3D HPC/CF skeletons in LMBs. This work paves the way for engineering the structure of the commercially available CF in order to significantly improve its electrochemical performance for application in LMAs and provides insight into the rational design of 3D hierarchically bicontinuous porous skeletons for highly efficient and safe LMAs for next-generation high-energy-density LMBs.

Supporting Information Additional optical, SEM, EDX, XRD characterizations; mercury porosimetry measurement, and additional electrochemical tests.

Corresponding Author * [email protected] (Z. Shi); [email protected] (Z. Guo) Author Contributions The manuscript was written through contributions of all authors. All authors have given approval to the final version of the manuscript. ⊥These authors contributed equally.

Notes The authors declare no competing financial interest.

Acknowledgment

ACS Paragon Plus Environment

22

Page 23 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

This work was supported by the National Natural Science Foundation of China (Nos. 21673051 and 51604086), the Guangdong Science and Technology Department (Nos. 2016A010104015 and 2017B010119003), the Guangzhou Science & Innovative Committee (Nos. 201604030037 and 201704030011), the “One-hundred Talents plan” (No. 220418056), the “One-hundred Young Talents plan” (No. 220413126), and the Youth Foundation of Guangdong University of Technology (No. 252151038). The authors also appreciate Dan Liu and Qinghai Li from Dynavolt Renewable Energy Technology Co., Ltd. for helpful discussion.

References 1.

Wang, S. B.; Guan, B. Y.; Yu, L.; Lou, X. W. Rational Design of Three-Layered

TiO2@Carbon@MoS2 Hierarchical Nanotubes for Enhanced Lithium Storage. Adv. Mater. 2017, 29, 1702724. 2.

Wang, S. T.; Quan, W.; Zhu, Z.; Yang, Y.; Liu, Q.; Ren, Y.; Zhang, X. Y.; Xu, R.; Hong,

Y.; Zhang, Z. T.; Amine, K.; Tang, Z. L.; Lu, J.; Li, J. Lithium Titanate Hydrates with Superfast and Stable Cycling in Lithium Ion Batteries. Nat. Commun. 2017, 8, 627. 3.

Chae, S.; Kim, N.; Ma, J.; Cho, J.; Ko, M. One-to-One Comparison of Graphite-Blended

Negative Electrodes Using Silicon Nanolayer-Embedded Graphite versus Commercial Benchmarking Materials for High-Energy Lithium-Ion Batteries. Adv. Energy Mater. 2017, 7, 1700071. 4.

Wang, H. Q.; Zhang, W. C.; Liu, H. K.; Guo, Z. P. A Strategy for Configuration of an

Integrated Flexible Sulfur Cathode for High-Performance Lithium-Sulfur Batteries. Angew. Chem. Int. Ed. 2016, 55, 3992-3996.

ACS Paragon Plus Environment

23

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

5.

Page 24 of 30

Hou, T. Z.; Xu, W. T.; Chen, X.; Peng, H. J.; Huang, J. Q.; Zhang, Q. Lithium Bond

Chemistry in Lithium-Sulfur Batteries. Angew. Chem. Int. Ed. 2017, 56, 8178-8182. 6.

Aurbach, D.; McCloskey, B. D.; Nazar, L. F.; Bruce, P. G. Advances in Understanding

Mechanisms Underpinning Lithium-Air Batteries. Nat. Energy 2016, 1, 16128. 7.

Lu, J.; Lee, Y. J.; Luo, X. Y.; Lau, K. C.; Asadi, M.; Wang, H. H.; Brombosz, S.; Wen, J.

G.; Zhai, D. Y.; Chen, Z. H.; Miller, D. J.; Jeong, Y. S.; Park, J. B.; Fang, Z. Z.; Kumar, B.; Salehi-Khojin, A.; Sun, Y. K.; Curtiss, L. A.; Amine, K. A Lithium-Oxygen Battery Based on Lithium Superoxide. Nature 2016, 529, 377-382. 8.

Xu, W.; Wang, J. L.; Ding, F.; Chen, X. L.; Nasybutin, E.; Zhang, Y. H.; Zhang, J. G.

Lithium Metal Anodes for Rechargeable Batteries. Energy Environ. Sci. 2014, 7, 513-537. 9.

Tikekar, M. D.; Choudhury, S.; Tu, Z. Y.; Archer, L. A. Design Principles for

Electrolytes and Interfaces for Stable Lithium-Metal Batteries. Nat. Energy 2016, 1, 16114. 10.

Cheng, X. B.; Zhang, R.; Zhao, C. Z.; Zhang, Q. Toward Safe Lithium Metal Anode in

Rechargeable Batteries: A Review. Chem. Rev. 2017, 117, 10403-10473. 11.

Yang, C. P.; Fu, K.; Zhang, Y.; Hitz, E.; Hu, L. B. Protected Lithium-Metal Anodes in

Batteries: From Liquid to Solid. Adv. Mater. 2017, 29, 1701169. 12.

Jana, A.; Garcia, R. E. Lithium Dendrite Growth Mechanisms in Liquid Electrolytes.

Nano Energy 2017, 41, 552-565. 13.

Rong, G. L.; Zhang, X. Y.; Zhao, W.; Qiu, Y. C.; Liu, M. N.; Ye, F. M.; Xu, Y.; Chen, J.

F.; Hou, Y.; Li, W. F.; Duan, W. H.; Zhang, Y. G. Liquid-Phase Electrochemical Scanning Electron Microscopy for In Situ Investigation of Lithium Dendrite Growth and Dissolution. Adv. Mater. 2017, 29, 1606187.

ACS Paragon Plus Environment

24

Page 25 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

14.

Camacho-Forero, L. E.; Balbuena, P. B. Elucidating Electrolyte Decomposition under

Electron-Rich Environments at the Lithium-Metal Anode. Phy. Chem. Chem. Phys. 2017, 19, 30861-30873. 15.

Cheng, J. H.; Assegie, A. A.; Huang, C. J.; Lin, M. H.; Tripathi, A. M.; Wang, C. C.;

Tang, M. T.; Song, Y. F.; Su, W. N.; Hwang, B. J. Visualization of Lithium Plating and Stripping via in Operando Transmission X-ray Microscopy. J. Phys. Chem. C 2017, 121, 77617766. 16.

Cheng, X. B.; Zhang, R.; Zhao, C. Z.; Wei, F.; Zhang, J. G.; Zhang, Q. A Review of

Solid Electrolyte Interphases on Lithium Metal Anode. Adv. Sci. 2016, 3, 1500213. 17.

Li, Y. Z.; Li, Y. B.; Pei, A.; Yan, K.; Sun, Y. M.; Wu, C. L.; Joubert, L. M.; Chin, R.;

Koh, A. L.; Yu, Y.; Perrino, J.; Butz, B.; Chu, S.; Cui, Y. Atomic Structure of Sensitive Battery Materials and Interfaces Revealed by Cryo-Electron Microscopy. Science 2017, 358, 506-510. 18.

Lu, Y. Y.; Tu, Z. Y.; Archer, L. A. Stable Lithium Electrodeposition in Liquid and

Nanoporous Solid Electrolytes. Nat. Mater. 2014, 13, 961-969. 19.

Zhang, X. Q.; Cheng, X. B.; Chen, X.; Yan, C.; Zhang, Q. Fluoroethylene Carbonate

Additives to Render Uniform Li Deposits in Lithium Metal Batteries. Adv. Funct. Mater. 2017, 27, 1605989. 20.

Zheng, J. M.; Engelhard, M. H.; Mei, D. H.; Jiao, S. H.; Polzin, B. J.; Zhang, J. G.; Xu,

W. Electrolyte Additive Enabled Fast Charging and Stable Cycling Lithium Metal Batteries. Nat. Energy 2017, 2, 17012. 21.

Cheng, X. B.; Zhao, M. Q.; Chen, C.; Pentecost, A.; Maleski, K.; Mathis, T.; Zhang, X.

Q.; Zhang, Q.; Jiang, J. J.; Gogotsi, Y. Nanodiamonds Suppress the Growth of Lithium Dendrites. Nat. Commun. 2017, 8, 336.

ACS Paragon Plus Environment

25

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

22.

Page 26 of 30

Zheng, G. Y.; Lee, S. W.; Liang, Z.; Lee, H. W.; Yan, K.; Yao, H. B.; Wang, H. T.; Li,

W. Y.; Chu, S.; Cui, Y. Interconnected Hollow Carbon Nanospheres for Stable Lithium Metal Anodes. Nat. Nanotechnol. 2014, 9, 618-623. 23.

Yan, K.; Lee, H. W.; Gao, T.; Zheng, G. Y.; Yao, H. B.; Wang, H. T.; Lu, Z. D.; Zhou,

Y.; Liang, Z.; Liu, Z. F.; Chu, S.; Cui, Y. Ultrathin Two-Dimensional Atomic Crystals as Stable Interfacial Layer for Improvement of Lithium Metal Anode. Nano Lett. 2014, 14, 6016-6022. 24.

Li, N. W.; Yin, Y. X.; Yang, C. P.; Guo, Y. G. An Artificial Solid Electrolyte Interphase

Layer for Stable Lithium Metal Anodes. Adv. Mater. 2016, 28, 1853-1858. 25.

Ma, L.; Kim, M. S.; Archer, L. A. Stable Artificial Solid Electrolyte Interphases for

Lithium Batteries. Chem. Mater. 2017, 29, 4181-4189. 26.

Lu, Y. Y.; Tikekar, M.; Mohanty, R.; Hendrickson, K.; Ma, L.; Archer, L. A. Stable

Cycling of Lithium Metal Batteries Using High Transference Number Electrolytes. Adv. Energy Mater. 2015, 5, 1402073. 27.

Tu, Z. Y.; Kambe, Y.; Lu, Y. Y.; Archer, L. A. Nanoporous Polymer-Ceramic Composite

Electrolytes for Lithium Metal Batteries. Adv. Energy Mater. 2014, 4, 1300654. 28.

Yan, K.; Lu, Z. D.; Lee, H. W.; Xiong, F.; Hsu, P. C.; Li, Y. Z.; Zhao, J.; Chu, S.; Cui, Y.

Selective Deposition and Stable Encapsulation of Lithium through Heterogeneous Seeded Growth. Nat. Energy 2016, 1, 16010. 29.

Zhang, R.; Chen, X. R.; Chen, X.; Cheng, X. B.; Zhang, X. Q.; Yan, C.; Zhang, Q.

Lithiophilic Sites in Doped Graphene Guide Uniform Lithium Nucleation for Dendrite-Free Lithium Metal Anodes. Angew. Chem. Int. Ed. 2017, 56, 7764-7768.

ACS Paragon Plus Environment

26

Page 27 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

30.

Yang, C. P.; Yao, Y. G.; He, S. M.; Xie, H.; Hitz, E.; Hu, L. B. Ultrafine Silver

Nanoparticles for Seeded Lithium Deposition toward Stable Lithium Metal Anode. Adv. Mater. 2017, 29, 1702714. 31.

Cheng, X. B.; Peng, H. J.; Huang, J. Q.; Wei, F.; Zhang, Q. Dendrite-Free

Nanostructured Anode: Entrapment of Lithium in a 3D Fibrous Matrix for Ultra-Stable LithiumSulfur Batteries. Small 2014, 10, 4257-4263. 32.

Cheng, X. B.; Peng, H. J.; Huang, J. Q.; Zhang, R.; Zhao, C. Z.; Zhang, Q. Dual-Phase

Lithium Metal Anode Containing a Polysulfide-Induced Solid Electrolyte Interphase and Nanostructured Graphene Framework for Lithium-Sulfur Batteries. ACS Nano 2015, 9, 63736382. 33.

Zhang, R.; Cheng, X. B.; Zhao, C. Z.; Peng, H. J.; Shi, J. L.; Huang, J. Q.; Wang, J. F.;

Wei, F.; Zhang, Q. Conductive Nanostructured Scaffolds Render Low Local Current Density to Inhibit Lithium Dendrite Growth. Adv. Mater. 2016, 28, 2155-2162. 34.

Lin, D. C.; Liu, Y. Y.; Liang, Z.; Lee, H. W.; Sun, J.; Wang, H. T.; Yan, K.; Xie, J.; Cui,

Y. Layered Reduced Graphene Oxide with Nanoscale Interlayer Gaps as a Stable Host for Lithium Metal Anodes. Nat. Nanotechnol. 2016, 11, 626-632. 35.

Liu, Y. Y.; Lin, D. C.; Liang, Z.; Zhao, J.; Yan, K.; Cui, Y. Lithium-Coated Polymeric

Matrix as a Minimum Volume-Change and Dendrite-Free Lithium Metal Anode. Nat. Commun. 2016, 7, 10992. 36.

Liang, Z.; Lin, D. C.; Zhao, J.; Lu, Z. D.; Liu, Y. Y.; Liu, C.; Lu, Y. Y.; Wang, H. T.;

Yan, K.; Tao, X. Y.; Cui, Y. Composite Lithium Metal Anode by Melt Infusion of Lithium into a 3D Conducting Scaffold with Lithiophilic Coating. Proc. Natl. Acad. Sci. U. S. A. 2016, 113, 2862-2867.

ACS Paragon Plus Environment

27

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

37.

Page 28 of 30

Zuo, T. T.; Wu, X. W.; Yang, C. P.; Yin, Y. X.; Ye, H.; Li, N. W.; Guo, Y. G.

Graphitized Carbon Fibers as Multifunctional 3D Current Collectors for High Areal Capacity Li Anodes. Adv. Mater. 2017, 29, 1700389. 38.

Yang, C. P.; Yin, Y. X.; Zhang, S. F.; Li, N. W.; Guo, Y. G. Accommodating Lithium

into 3D Current Collectors with a Submicron Skeleton towards Long-Life Lithium Metal Anodes. Nat. Commun. 2015, 6, 8058. 39.

Yun, Q. B.; He, Y. B.; Lv, W.; Zhao, Y.; Li, B. H.; Kang, F. Y.; Yang, Q. H. Chemical

Dealloying Derived 3D Porous Current Collector for Li Metal Anodes. Adv. Mater. 2016, 28, 6932-6939. 40.

Wang, S. H.; Yin, Y. X.; Zuo, T. T.; Dong, W.; Li, J. Y.; Shi, J. L.; Zhang, C. H.; Li, N.

W.; Li, C. J.; Guo, Y. G. Stable Li Metal Anodes via Regulating Lithium Plating/Stripping in Vertically Aligned Microchannels. Adv. Mater. 2017, 29, 1703729. 41.

Xie, K. Y.; Wei, W. F.; Yuan, K.; Lu, W.; Guo, M.; Li, Z. H.; Song, Q.; Liu, X. R.; Wang,

J. G.; Shen, C. Toward Dendrite-Free Lithium Deposition via Structural and Interfacial Synergistic Effects of 3D Graphene@Ni Scaffold. ACS Appl. Mater. Interfaces 2016, 8, 2609126097. 42.

Vogel, N.; Retsch, M.; Fustin, C. A.; del Campo, A.; Jonas, U. Advances in Colloidal

Assembly: The Design of Structure and Hierarchy in Two and Three Dimensions. Chem. Rev. 2015, 115, 6265-6311. 43.

Wu, Y. N.; Li, F. T.; Zhu, W.; Cui, J. C.; Tao, C. A.; Lin, C. X.; Hannam, P. M.; Li, G. T.

Metal-Organic Frameworks with a Three-Dimensional Ordered Macroporous Structure: Dynamic Photonic Materials. Angew. Chem. Int. Ed. 2011, 50, 12518-12522.

ACS Paragon Plus Environment

28

Page 29 of 30 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

ACS Applied Materials & Interfaces

44.

Barako, M. T.; Sood, A.; Zhang, C.; Wang, J. J.; Kodama, T.; Asheghi, M.; Zheng, X. L.;

Braun, P. V.; Goodson, K. E. Quasi-ballistic Electronic Thermal Conduction in Metal Inverse Opals. Nano Lett. 2016, 16, 2754-2761. 45.

Liu, J. C.; Wan, L.; Zhang, M. B.; Jiang, K. J.; Song, K.; Wang, J. X.; Ikeda, T.; Jiang, L.

Electrowetting-Induced Morphological Evolution of Metal-Organic Inverse Opals toward a Water-Lithography Approach. Adv. Funct. Mater. 2017, 27, 1605221. 46.

Zhang, H. G.; Yu, X. D.; Braun, P. V. Three-Dimensional Bicontinuous Ultrafast-Charge

and -Discharge Bulk Battery Electrodes. Nat. Nanotechnol. 2011, 6, 277-281. 47.

Erlebacher, J. Mechanism of Coarsening and Bubble Formation in High-Genus

Nanoporous Metals. Phys. Rev. Lett. 2011, 106, 225504. 48.

Pei, A.; Zheng, G. Y.; Shi, F. F.; Li, Y. Z.; Cui, Y. Nanoscale Nucleation and Growth of

Electrodeposited Lithium Metal. Nano Lett. 2017, 17, 1132-1139.

ACS Paragon Plus Environment

29

ACS Applied Materials & Interfaces 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 30 of 30

TOC

ACS Paragon Plus Environment

30