Highly Efficient Blue Emission and Superior Thermal Stability of

Mar 15, 2018 - Engineering Research Center of Nano-Geomaterials of Ministry of Education, Faculty of Materials Science and Chemistry, China University...
0 downloads 11 Views 2MB Size
Subscriber access provided by Kent State University Libraries

Highly Efficient Blue Emission and Superior Thermal Stability of BaAl12O19:Eu2+ Phosphors based on Highly Symmetric Crystal Structure Yi Wei, Ling Cao, Lemin Lv, Guogang Li, Jiarui Hao, Junsong Gao, Chaochin Su, Chun Che Lin, Ho Seong Jang, Peipei Dang, and Jun Lin Chem. Mater., Just Accepted Manuscript • DOI: 10.1021/acs.chemmater.8b00464 • Publication Date (Web): 15 Mar 2018 Downloaded from http://pubs.acs.org on March 16, 2018

Just Accepted “Just Accepted” manuscripts have been peer-reviewed and accepted for publication. They are posted online prior to technical editing, formatting for publication and author proofing. The American Chemical Society provides “Just Accepted” as a service to the research community to expedite the dissemination of scientific material as soon as possible after acceptance. “Just Accepted” manuscripts appear in full in PDF format accompanied by an HTML abstract. “Just Accepted” manuscripts have been fully peer reviewed, but should not be considered the official version of record. They are citable by the Digital Object Identifier (DOI®). “Just Accepted” is an optional service offered to authors. Therefore, the “Just Accepted” Web site may not include all articles that will be published in the journal. After a manuscript is technically edited and formatted, it will be removed from the “Just Accepted” Web site and published as an ASAP article. Note that technical editing may introduce minor changes to the manuscript text and/or graphics which could affect content, and all legal disclaimers and ethical guidelines that apply to the journal pertain. ACS cannot be held responsible for errors or consequences arising from the use of information contained in these “Just Accepted” manuscripts.

is published by the American Chemical Society. 1155 Sixteenth Street N.W., Washington, DC 20036 Published by American Chemical Society. Copyright © American Chemical Society. However, no copyright claim is made to original U.S. Government works, or works produced by employees of any Commonwealth realm Crown government in the course of their duties.

Page 1 of 12 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Chemistry of Materials

Highly Efficient Blue Emission and Superior Thermal Stability of BaAl12O19:Eu2+ Phosphors based on Highly Symmetric Crystal Structure Yi Wei,† Ling Cao,† Lemin Lv,† Guogang Li,*, † Jiarui Hao,† Junsong Gao,† Chaochin Su,& Chun Che Lin,*,& Ho Seong Jang,§ Peipei Dang,‡ and Jun Lin*,‡ †Engineering Research Center of Nano-Geomaterials of Ministry of Education, Faculty of Materials Science and Chemistry, China University of Geosciences, 388 Lumo Road, Wuhan 430074, P. R. China. Email: [email protected] ‡State Key Laboratory of Rare Earth Resource Utilization, Changchun Institute of Applied Chemistry, Chinese Academy of Sciences, Changchun 130022, P. R. China. Email: [email protected] &Institute of Organic and Polymeric Materials, National Taipei University of Technology, Taipei 106, Taiwan. E-mail: [email protected] §Materials Architecturing Research Center, Korea Institute of Science and Technology, 5, Hwarang-ro 14-gil, Seongbukgu, Seoul 02792, Republic of Korea. ABSTRACT: Highly efficient phosphor materials with superior thermal stability are indispensable for phosphor-converted white light-emitting diodes (pc-wLEDs) solid state lighting. In order to obtain a high quality warm white light, near ultra violet (n-UV) chips combined with trichromatic phosphors have be extensively concerned. Among them, the development of efficient blue phosphor remains a challenging task. In view of the close correlation between 5d-4f transitions of rare earth ions and the coordination environment of host lattice, many studies have been dedicated to improving the photoluminescence performances by modifying of the lattice coordination environment including the lattice rigidity and symmetry. In this work, we reported highly efficient blue-emitting Eu2+ -doped BaAl12O19 (BAO) phosphors with excellent thermal stability, which were prepared via the traditional high-temperature solid state reaction routes. According to the XRD Rietveld refinement analysis, BAO owned a highly symmetric layer-structure with two Ba polyhedrons, marking as Ba(1)O9 and Ba(2)O10, respectively. The diffuse reflectance spectra revealed the optical band gap to be 4.07 eV. Due to the suitable optical bandgap, the Eu2+ ions could realize a highly efficient doping in the BAO matrix. The photoluminescence excitation (PLE) spectra for as-prepared BAO:Eu2+ phosphors exhibited a broad absorption band in the region from 250 to 430 nm, matching well with the n-UV LED chip. Under the UV radiation, it is highly luminous (Internal quantum yields, IQYs = 90%) with the peak around 443 nm. Furthermore, the color purity of BAO:Eu2+ phosphors could achieve 92%, ascribing to the narrow full width at half maximum (FWHM = 52 nm), which was even much better than that of commercially available BAM:Eu2+ phosphor (Color purity = 91.34%, FWHM = 51.7 nm). More importantly, the as-prepared BAO:Eu2+ phosphor showed extra high thermal stability when working in the region of 298 K550 K, which was a bit better than that of commercial BAM:Eu2+ phosphors. According to the distortion calculation of Ba crystallographic occupation, the superior thermal stability could be attributed to the highly symmetric crystal structure of BAO host. In view of the excellent luminescence performances of BAO:Eu2+, it is a promising blue-emitting phosphor for n-UV WLED.

 INTRODUCTION Recently, phosphor-converted white light-emitting diodes (pc-WLEDs) lighting have widely integrated into our daily lives due to their high energy efficiency, low energy consumption, reliability, durability, long lifetime, and ecofriendly features.1-6 A typical pc-WLEDs is commonly fabricated by the combination of a blue (460 nm) InGaN chip with a yellowish YAG phosphor (Y3Al5O12:Ce3+).7-11 However, this kind of pc-WLEDs easily suffer from poor color-rendering indices (Ra < 75) and high correlated color temperatures (CCT > 4500 K) due to the absence of red light components at the long wavelength region,12-15 resulting in an

uncomfortable cold white lights. To overcome this defect, an alternative approach to achieve high-quality warm white lighting is to match n-UV (380-420 nm) LED chip with trichromatic (red, blue, and green) phosphors.16 Therefore, highly efficient trichromatic phosphor materials with superior thermal stability are indispensable. Among them, Eu2+ and Ce3+ activated inorganic phosphors that have superb chemical and optical advantages are highly desired for n-UV based WLEDs solid state lighting.6, 17-21 Presently, the study of highefficiency blue emitting phosphor has drawn the attention of many researchers. The most reported one is

ACS Paragon Plus Environment

Chemistry of Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

BaMgAl10O17:Eu2+ (BAM:Eu2+), which was commonly used as commercial blue-emitting phosphors for n-UV pumped WLEDs.22, 23 Many strategies have been employed to improve the luminescence of BAM:Eu2+ phosphor for realizing the high-quality indoor lighting. For example, Seoung et al.24 developed a “thermal-shock method” to obtain more efficient BAM:Eu2+. Liang et al.25 reported a novel method of carbon coating on BAM:Eu2+ phosphor particles through chemical vapor deposition, enhancing emission intensity and oxidation resistance at high temperature. However, those methods are complicated, time-consuming and costly, and thus limit their commercial application. In view of a closely correlation between 5d-4f transitions of rare earth ions and the coordination environment of host lattice, many studies have also dedicated to improving the photoluminescence performances and designing newly highly efficient blueemitting phosphor materials by the chemical modification of host lattice. Yoon et al.26 reported a zero-thermal-quenching Na3–2xSc2(PO4)3:xEu2+ blue-emitting phosphor. Zhi et al.27 obtained a narrow-band blue-emitting NaBa4(AlB4O9)2X3 (X = Cl, Br):Eu2+ phosphors at low synthesized temperature. Jiang et al.28 realized a blue emission in Sr5(PO4)3Cl:Eu2+ phosphor, which owned an excellent color-rendering index (Ra = 94.65). But those phosphors usually suffered the poor absorption around the n-UV region and terrible thermal stability. Accordingly, the development of efficient blue phosphor remains a challenge, and needs to be further focused. Rare-earth activated BaAl12O19 luminescence materials have previously been reported because of a facile synthesis, low cost, excellent optical properties and highly physicalchemical stability.29-34 In this work, we realized a highly efficient blue emission in BaAl12O19 (BAO) by Eu2+ doping, accompanying an excellent thermal stability, which were prepared via the traditional high-temperature solid state route. According to the XRD Rietveld profile refinement, BAO owned a highly symmetric layer-structure with two Ba polyhedrons, marking as Ba(1)O9 and Ba(2)O10, respectively. The diffuse reflectance spectra reveal the optical band gap to be 4.07 eV. Due to the suitable optical band gap, the Eu2+ ions could realize a highly efficient doping in the BAO matrix. The PLE spectra for as-prepared BAO:xEu2+ phosphors exhibit a broad absorption band in the region from 250 nm to 430 nm, matching well with the n-UV LED chip. Under the n-UV radiation, it emits highly luminous blue light with the peak around 443 nm and internal quantum yields (QYs) about 90%. Furthermore, the color purity of BAO:xEu2+ phosphors could achieve 92.4%, ascribing to the narrow FWHM (52 nm), which is even much better than that of commercially available BAM:Eu2+ phosphor (Color purity = 91.34%, FWHM = 51.7 nm). More importantly, the as-prepared BAO:xEu2+ phosphor shows extra high thermal stability when working in the region of 298-550 K, which is a bit better than that of commercial BAM:Eu2+ phosphor. According to the distortion calculation of Ba crystallographic occupation, the superior thermal stability could be attributed to the highly symmetric crystal structure and rigidity of BAO host lattice. In view of the excellent luminescence performances of BAO:xEu2+ phosphor, it is a promising blue-emitting phosphor for n-UV based WLEDs lighting sources.

 EXPERIMENTAL SECTION Materials synthesis. The Ba1-xAl12O19: xEu2+ (0 ≤ x ≤ 50%) powders were made via the traditional high-temperature solid state reaction. The raw materials were BaCO3 (Sigma-Aldrich, 99.95%), Al2O3 (Sigma-Aldrich, 99.99%), Eu2O3 (SigmaAldrich, 99.99%), BaF2 (Aladdin, 99.9%), BaCl2·2H2O (Aladdin, 99%) and BaBr2 (Aladdin, 99%). Simultaneously, BaF2, BaCl2·2H2O and BaBr2 were also used as fluxes. Stoichiometric amounts of the required cationic sources were weighed and ground together for 40 minutes with a small amount of ethanol using an agate mortar and pestle until the mixtures were almost dry. The obtained mixtures were then transferred into aluminum oxide crucibles, and then treated in the horizontal tube furnace at 1400℃ for 15 hours under a reduced atmosphere of H2 (10%)˗N2 (90%). The annealed samples were again ground, forming the resulting phosphor materials. Characterization. The finely ground powders were used in all measurements. The crystal structure and phase purity of the as-prepared samples were characterized by X-ray powder diffractometer (XRD), which were performed on a D8 Focus diffractometer at as canning rate of 1° min-1 in the 2θ range from 5° to 120° with Ni-filtered Cu-Kα (λ = 1.540598 Å). XRD Rietveld profile refinements of the structural models and texture analysis were performed with the use of General Structure Analysis System (GSAS) software. The morphologies of the samples were inspected using a field emission scanning electron microscope (FE-SEM, S-4800, Hitachi). The photoluminescence excitation (PLE) and emission (PL) spectra were measured by fluorescence spectrometer (Fluoromax-4P, Horiba JobinYvon, New Jersey, U.S.A.) equipped with a 450 W xenon lamp as the excitation source, and both excitation and emission spectra were set up to be 1.0 nm with the width of the monochromator slits adjusted as 0.50 nm. The thermal stabilities of luminescence properties were measured by Fluoromax-4P spectrometer connected heating equipment (TAP-02) and using a combined setup consisting of a Xe-lamp, a Hamamatsu MPCD-7000 multichannel photodetector and a computer-controlled heater. The diffuse reflectance spectra (DRS) were measured by UVVisible diffuse reflectance spectroscopy UV-2550PC (Shimadzu Corporation, Japan). The photoluminescence quantum yield (QY) was measured by absolute PL quantum yield measurement system C9920-02 (Hamamatsu photonics K.K., Japan). The photoluminescence decay curves were obtained from a Lecroy Wave Runner 6100 Digital Osilloscope (1 GHz) using a tunable laser (pulse width = 4 ns, gate = 50 ns) as the excitation (Contimuum Sunlite OPO). Solid-state nuclear magnetic resonance(NMR) spectra were obtained with the use of a Bruker DSX 300 MHz NMR spectrometer, equipped with 4 mm double-resonance magic angle-spinning (MAS) probe. X-ray photoelectron spectroscopy (XPS) measurements were carried out on Mg Ka radiation source (Kratos XSAM-800 spectrometer).

 RESULTS AND DISCUSSION Crystal structure and lattice parameters. The phase purity and structure type of as-prepared BAO:xEu2+ (0 ≤ x ≤ 50%) powders were investigated by XRD and Rietveld profile refinements. The refined crystallographic

ACS Paragon Plus Environment

Page 2 of 12

Page 3 of 12 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Chemistry of Materials

Table 1. Crystallographic Parameters Obtained from XRD Rietveld Refinements for BAO: xEu2+(0 ≤ x ≤ 20%) Reliability Factors

Crystallographic Parameter Samples a/b (Å) x = 0% x = 1% x = 5% x = 10% x = 20% Crystal system Space group

Figure 1. The representative Rietveld refinement XRD patterns of BAO:xEu2+ samples: (a) x = 0 and (b) x = 5%. The measured data, fitting data, and their difference are depicted with black crosses, red solid line, and blue solid line, respectively. The blue short vertical lines show the positions of Bragg reflections of the fitting XRD patterns. (c) Shows the typical XRD patterns of BAO:xEu2+ (1 ≤ x ≤ 25%) samples. The standard BaAl12O19 data (ICSD #79359) is shown as a reference. The right inset is the magnified XRD patterns for the 2 Theta region of 35°-37°. (d), (e) and (f) give the cell parameters (a/b, c) and volume (V), respectively, as a function of Eu2+-doped concentration (x).

parameters of a series of BAO:xEu2+ (1 ≤ x ≤ 25%) samples were summarized in Table 1. Three kinds of fluxes (BaF2, BaCl2·2H2O and BaBr2) were chosen to promote the crystallinity of BAO:xEu2+ samples. In the same conditions, the as-prepared samples using BaF2 as flux had the best crystallinity (Figure S1), and the optimal concentration of BaF2 into BAO:xEu2+ was 5%wt (5%wt represents the weight percentage) of as-prepared powders (Figure S2). Figure 1a and 1b successively show the XRD Rietveld refinement results of BAO host and the representative BAO:xEu2+ samples. The refined lattice parameters imply that the two samples all formed hexagonal phase with space group P63/mmc (194), a = b = 5.59488(5) Å, c = 22.8755(1) Å, V = 620.130(11) Å3 for BAO host and a = b = 5.59485(1) Å, c = 22.8737(5) Å, V = 620.076(21) Å3 for BAO:5%Eu2+, respectively, as shown in Table 1. The atom positions, fraction factors, and thermal vibration parameters were refined by convergence and satisfied well the reflection conditions, Rwp = 7.00%, Rp = 5.11% for x = 0, and Rwp = 6.83%, Rp = 4.73% for x = 5% (Table 1). These results indicate the formation of single-phased BAO crystals. Figure 1c shows the XRD patterns of BAO:xEu2+ (1 ≤ x ≤ 25%) samples, which could be well indexed with the standard card of BaAl12O19 (ICSD No. 79359), and there are no impurity phases with the doping of Eu2+ ions (x) from 1% to 25%, and the enlarged diffraction

α/β (°) 620.130(1) 90 620.076(2) 90 620.035(2) 90 619.883(2) 90 619.242(2) 90 V (Å3)

c (Å)

5.59488(5) 22.8755(1) 5.59485(1) 22.8737(5) 5.59464(8) 22.8740(4) 5.59413(9) 22.8725(5) 5.59256(7) 22.8617(4)

γ (°) 120 120 120 120 120

Rp (%) 7.00 7.43 6.83 8.84 7.70

Rwp (%) 5.11 5.22 4.73 6.13 5.27

Hexagonal P63/mmc

peak position of 2θ = 35-37° shift to the larger angle direction, indicating the as-prepared samples are all pure hexagonal phase and the perfect enter into host lattice of Eu2+ ions by replacing Ba2+ ions. However, a impurity peak appeared at about 2θ = 33.5o when the value of x is more than 25%, as shown in Figure S3a, which are assigned to the EuAl12O19 phase. Therefore, the maximum doping concentration of Eu2+ ions is fixed at x = 25%. In addition, the refined cell parameters as a function of x are shown in Figure 1d. Obviously, the lattice parameters (a/b, c, and V) exhibits a monotonous, liner decreasing trend as x increases from 1% to 20%. That’s because of the substitution with the smaller Eu2+ ions (r = 1.3 Å for CN = 9; r =1.35 Å for CN = 10) where CN signifies the coordination numbers. This phenomenon further indicates the successful incorporation of Eu2+ into the for Ba2+ ions (r = 1.47 Å for CN = 9, r = 1.52 Å for CN = 10), lattice by substituting Ba2+, and simultaneously confirms the formation of solid solutions at x < 25%.

Figure 2. Schematic crystal structure of BaAl12O19:Eu2+ along baxis direction, and the coordination polyhedrons of Ba(1) site (Wyck. 2d) and Ba(2) site (Wyck. 4f), and the coordination of Al(1)-Al(5).

According to the refinement results, a schematic spatial view of the BaAl12O19:Eu2+ unit cell is shown in Figure 2. Interestingly, along the b-axis direction, the studied crystal

ACS Paragon Plus Environment

Chemistry of Materials

Figure 3. (a) The typical SEM image of Ba0.9Al12O19:10%Eu2+ sample, and it's mapping images of elements: (b) Ba L-edge, (c) Eu Ledge, (d) Al K-edge and (e) O K-edge

icant impact on their luminescence properties. Figure S4 plots the PLE and PL spectra with changing the type and dosage of fluxes. It can be observed that the spectral profile and position of BAO:xEu2+ samples maintain unchanged, while the peak intensity are obviously different. When using BaF2 as flux, the peak intensity visibly increases, compared to non-flux sample (Figure S4a). However, BaCl2·2H2O and BaBr2 don’t play their role effectively. Meanwhile, the emission intensity clearly increases first and reaches the maximum value at 5%wt of raw materials as increasing the dosage of BaF2 flux (Figure S4b). This consequence is identical to the XRD analysis of different doping content of BaF2. Therefore, the photoluminescence properties are measured at the series of BAO:xEu2+ (1% ≤ x ≤50%) samples prepared using 5%wt BaF2 as flux.

[F(R∝)hν]1/2

exhibits a layered network structure. It contains five kinds of Al sites, marked as Al(1)˗Al(5). Those Al sites could be coordinated with four or six oxygen atoms, specifically, the Al(1) and Al(4) form AlO6 octahedrons, while Al(2), Al(3) and Al(5) are all AlO4 tetrahedrons. AlO4 polyhedrons connect each other with vertexes, AlO6 polyhedrons connect each other also with vertexes, the two connections of AlO4 and AlO6 appeared alternately. These AlO4 tetrahedrons and AlO6 octahedrons construct a rigid three-dimensional network by sharing the vertexes, edges and faces in the BAO lattice. Based on the above structure, there are two Ba sites: the one perches the AlO4 three-dimensional network, marked Ba(1) (Wyck. 2d), the other one occupies the interval of AlO6 layer, marked as Ba(2) (Wyck. 4f). The sites of Ba(1) and Ba(2) are coordinated with 9 O and 10 O atoms, forming the Ba(1)O9 and Ba(2)O10 polyhedrons with sixteen faces, respectively. Due to the slightly larger ions radius of Ba(1)O9 and Ba(2)O10 polyhedrons, it is suitable for accommodating Eu2+ ions, and thus they are inferred to randomly occupy Ba(1) and Ba(2) sites. It is well known that the luminescence intensity is closely related to the crystallinity, size and morphology of phosphor particles. The SEM image of the representative BAO:10%Eu2+ sample is shown in Figure 3a. Clearly, the studied sample presents an irregular approximate spherical morphology with a size range of 0.5-2 µm. Moreover, a slightly agglomeration of these phosphor particles could be observed. Figure 3b also gives the SEM mapping images of BAO:10%Eu2+, which demonstrates that the sample contains Ba, Al, Eu, O elements, and they evenly distribute in the whole sample. Furthermore, the SEM-EDS analysis of BAO:10%Eu2+ demonstrates the average composition (15 points of different positions) of Al/(Ba + Eu) = 11.84: 1, which is very close to the theoretical ratio of Al/Ba = 12:1. This result is consistent with the previous XRD results, which further confirms the formation of pure BaAl12O19 phase (Table S1). Photoluminescence properties of BAO:Eu2+ phosphors The type and dosage of flux not only could change the crystallinity of BAO:xEu2+ phosphors but also have a signif-

Reflection (%)

1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Page 4 of 12

200

Host 2+ 1% Eu 2+ 5% Eu 2+ 10% Eu 2+ 25% Eu 300

400

4.07 eV 2

3

4

5

6

hν (eV)

500

600

700

Wavelength (nm)

Figure 4. Diffuse reflectance spectra of BAO:xEu2+ (0 ≤ x ≤ 25%) samples. The inset shows the relationship of [F(R∝)hv]1/2 vs photon energy hv.

Figure 4 shows the diffuse reflectance spectra of BAO:xEu2+ (0 ≤ x ≤ 25%) samples. According to the theory given by Mott and Davis, the optical band gap of BAO could be calculated by the following equation:35-40

ACS Paragon Plus Environment

Page 5 of 12 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Chemistry of Materials

Figure 5. (a) The photoluminescence excitation (PLE) and emission (PL) spectra of BAO:xEu2+ (1% ≤ x ≤ 25%) samples. (b) The emission peak intensity and wavelength as function of Eu2+ concentration. (c) The luminescence comparison of commercial BaMgAl10O17:Eu2+ (marked as BAM:Eu2+) and the as-prepared BAO:25%Eu2+. (d) XPS of BAO:25%Eu2+. The insert gives the 3d3/2 and 3d5/2 XPS peaks of the Eu element. (e) The CIE chromaticity coordinates diagram for BAM:Eu2+ and BAO:25%Eu2+. (f), (g) The luminescence photos of BAM:Eu2+ and BAO:25%Eu2+ under 365 nm UV light.

[ F ( R∞)hv]1 / 2 = A(hv − Eg ) (1)

F ( R∞) = (1 − R) 2 / 2 R Where A represents the absorption constant, Eg is the optical band gap, hv represents the photon energy, F(R∝) is the absorption, and R is the reflectance (%) coefficient, respectively. The inset of Figure 4 depicts the plots of [F(R∝ )hv]1/2 versus hv of BAO matrix. The calculated Eg value for BAO sample is 4.07 eV, illustrating that this host is a very appropriate matrix for rare earth luminescence. For BAO:xEu2+ samples, there are remarkable absorption in the region from 200-400 nm due to the 4f7→4f65d transitions of Eu2+ ions, which matches well with the n-UV LED chips. According to the results, it could be deduced that the Eu2+ ions

could realize efficient emission in BAO host. Figure 5a presents the typical PLE and PL spectra of BAO:xEu2+ (1% ≤ x ≤ 25%) samples. It can be observed that the PLE spectra show a strong absorption in the range from 250 nm to 430 nm with the peak position at 350 nm, which is corresponding with the results of the diffuse reflectance spectra. Under the excitation wavelength of 350 nm, the BAO:xEu2+ emit bright blue light and its emission spectra consists of a narrow band from 400 nm to 525 nm, and the maximum peak position is around 443 nm. Interestingly, the PL intensity of BAO:xEu2+ (1% ≤ x ≤ 25%) continuously increases with x, reaching a maximum at x = 25% (Figure 5a and 5b). There is no concentration quenching phenomenon in the pure phase range. The quantum yields of BAO:xEu2+ (1%

ACS Paragon Plus Environment

Chemistry of Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

≤ x ≤ 25%) samples present a similar result, and reach the maximum 92% at x = 25%. The possible reason is that the layered network structure and large Ba(1)O9 and Ba(2)O10 crystallographic sites could accommodate more Eu2+ ions into lattice to efficiently emit. However, an obvious decrease in PL intensity appears at x beyond 25% (Figure S5), which is easily attributed to the existence of EuAl12O19 impurity phase (Figure S3a). Furthermore, a slight red shift can also be observed with enhancing the doping content of Eu2+ ions (Figure 5b). The following equation could help explaining the red-shift phenomena:41, 42

r4 1 Dq = Ze2 5 6 R

(2)

Where Dq is the crystal field splitting energy, Z is the anion charge, e is the electron charge, r is the radius of the d wave function, and R is the bond length. When the Ba2+ ion is substituted and occupied by a smaller Eu2+ ion, the distance between the Eu2+ and O2− ion becomes shorter. Because crystal field splitting is proportional to 1/R5, this shorter Eu2+−O2− distance leads to the enhancement of crystal field strength surrounding the Eu2+ ion, and further results in a larger crystal field splitting of Eu2+ 5d energy levels, which makes the lowest 5d state of Eu2+ ion closer to its ground state and finally generates a red shift of the emission spectra of Eu2+ ion. In addition, Figure S6 exhibits luminescence decay lifetimes for BAO:xEu2+ (x = 10%, 20%, 25%) gradually increase from 571 ns to 600 ns with the increase of x value, which also verify the red-shift emission of BAO:xEu2+. To determine the luminescence performance of the studied samples, the commercial BAM:Eu2+ blue phosphor was chosen as comparison. Figure 5c demonstrates the PLE and PL spectra of the optimal BAO:25%Eu2+ and BAM:Eu2+ phosphors upon exciting with 350 nm wavelength UV. Unexpectedly, the BAO:25%Eu2+ has a higher emission intensity (with the integrated intensity about 107%) than BAM:Eu2+ at the same measurement conditions (Figure 5c). In order to clarify the highly luminous blue emission, Figure 5d shows the X-ray photoelectron spectra (XPS) of the representative BAO:25%Eu2+ sample in the binding energy range of 0-1200 eV. The binding energy signal observed around 73, 280, 532, 781 and 1134 eV could be accounted for Al 2p, C 1s, O 1s, Ba 3d and Eu 3d, respectively.43-45 Thus, the XPS analysis further confirms the formation of BaAl12O19 phase and the presences of Eu in the lattice. Especially, the XPS peaks at 1134.6 and 1164 eV originated from the Eu 3d5/2 and Eu 3d3/2, respectively. Although there are still trace amounts Eu3+, the main peak belongs to Eu 3d5/2, namely, meaning that the activator Eu mainly existed in the form of +2 in the BaAl12O19 matrix. This result could reply the high luminescence efficiency of the as-prepared samples. In addition, the BAO:xEu2+ powders possess a narrow FWHM (52 nm), implying a highly pure blue emission with the CIE color coordination (0.1525, 0.0499), which is even better than that of BAM:Eu2+ (0.1443, 0.0614), as shown in Figure 5c and 5e. Their photoluminescence photos under 365 nm UV light in Figure 5f and 5g also support the above situation. The CIE color coordinate, FWHM and QYs of the as-prepared BAO:xEu2+ samples are also summarized in Table S2. In the CIE diagram, the perimeter is formed by plotting all monochromatic color coordinates. The color purity of a

Page 6 of 12

dominant color is the weight average of the emission color coordinate relative to the coordinate of the dominate wavelength and the CIE white illumination coordinate, which can be calculated by the following equation:27, 28 Color purity =

(x -xi )2 + ( y − yi )2 (x d -xi )2 + ( y d − y i )2

× 100%

(3)

Where (x, y) represent the CIE color coordination of asprepared samples and commercial BAM:Eu2+ phosphor, (xi, yi) is the white light source with CIE color coordinate (0.3333, 0.3333) in the reported work, and (xd, yd) is the color coordinate corresponding to the dominant wavelength of the light source. By substituting the coordinates of (x, y), (xi, yi), and (xd, yd) in eqn (3), we can obtain color purity of asprepared BAO:xEu2+ samples and BAM:Eu2+, respectively. The corresponding calculation results are collected in Table S2. It is found that the as-prepared BAO:xEu2+ sample presents the highest color purity of 92.40%, which is better than that of the commercially available BAM:Eu2+ phosphor (the color purity is 91.35%). Generally, these observations demonstrate that the BAO:xEu2+ manifest the better luminescence efficiency, the higher color purity, and the stronger absorption in 250-430 nm than the commercially available blue-emitting BAM:Eu2+ phosphor, which is a promising blue phosphor for n-UV based WLEDs. Controlled photoluminescence tuning is highly desired for rare earth ions activated phosphor materials, which is commonly used to optimize and modify of luminescence properties. Chemical modification of host materials could induce the structural and electronic alterations in local region, and thus generates anisotropic local environments for rare earth ions, which finally shift the energy levels of emission center and tune the spectral profile.6, 39, 41, 46-52 To expound the highly pure blue emission, the Gaussian fitting of emission spectra for BAO:xEu2+ (1% ≤ x ≤ 25%) are plotted in Figure 6a. At x = 1% and 3%, the emission spectra could be fitted to two single peaks at 2.82 and 2.66 eV, respectively; however, when x ≥ 5% the emission spectra are highly symmetrical and only retain a single peak at 2.82 eV. According to the average bond length of Ba(1)-O (2.72 Å) and Ba(2)-O (2.68 Å) (Table 1), the peaks at 2.82 eV and 2.66 eV of Eu2+ ions should be ascribed to the occupation of Ba(1) and Ba(2) sites in BAO lattice, respectively. In addition, Figure 6b reveals that the average Al(2)-O and Al(4)-O distances lengthened with increasing x value. Thus, a possible mechanism is proposed as follows: In the low doping concentration (x ≤ 3%), Eu2+ ions randomly occupy Ba(1) and Ba(2) sites (Figure 6d). When increasing the x, the expansion of Al(2) and Al(4) polyhedron would lead to the neighboring Ba(2) polyhedrons shrinking, and thus the Ba(2) sites could not accommodate the Eu2+ ions (Figure 6c). Finally, in the high doping concentration (x ≥ 5%), Eu2+ ions preferentially occupy Ba(1) sites (Figure 6e), generating a narrow blue emission. To further verify the effect of Al polyhedrons on the occupation of Eu2+ ions, the solid state NMR spectra of BAO:xEu2+ (0 ≤ x ≤ 25%) are measured and collected in Figure 6c. For BAO host (x = 0), there are two main peaks in -25-25 ppm region with the peak position at 8.44 ppm and 50-80 ppm region with the peak position at 73.56 ppm. The two peaks are characteristic peaks of AlO4 and AlO6, respectively. As the value of x increases, the peak

ACS Paragon Plus Environment

Page 7 of 12 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Chemistry of Materials

position of AlO4 polyhedrons moves slightly to large chemical shift direction, and that of AlO6 turns to the small chemical shift direction, meaning the change of distortion of AlO4 and AlO6 polyhedrons. It can be observed that the ratio of IAlO4/IAlO6 (peak intensity) gradually increase when enhancing x value. Moreover, the AlO6 peaks become broader compared to that of AlO4 peaks, illustrating that the distortion degree of AlO6 octahedrons is more remarkable than AlO4 tetrahedrons, which is consistent with the variation of average Al-O distances via Rietveld refinement.

to 500 K monitoring with 350 nm UV light are shown in Figure 7. Figure 7a and 7c give the PL spectra of BAO:1%Eu2+ and BAM:Eu2+ from 298 K to 500 K, respectively. Unsurprisingly, as the temperature raise, their emission intensity all decreased, because of intensified molecular heat movement at the high working temperature commonly exacerbate the non-radiative transitions.57 Unexpectedly, the as-prepared BAO:1%Eu2+ present a very low luminescence quenching behavior, and its PL intensity still maintains 92.1% of the initial intensity measured at 298 K when measured at 473 K (Figure 7e). This result is even a little better than that of BAM:Eu2+ (91.1%) (Figure 7e). Except for the extremely thermal stability, the color stability of BAO:1%Eu2+ was also more superior than BAM:Eu2+. Clearly, it could be seen from Figure 7b and 7d that when raised temperature from 298 K to 498 K, the emission peak and FWHM of BAO:1%Eu2+ almost retain unchanged, while the FWHM of BAM: Eu2+ phosphor gradually broadens resulting in a slight blue-shift emission. Finally, the thermal quenching behavior of BAO:xEu2+ (x = 1%, 5%, 10%, 20%) samples with Eu2+-doped concentration (x) are also investigated. As shown in Figure 7f, their thermal stability gradually decline with increasing x value. A possible reason is that the increasing substitution of Ba2+ ions by Eu2+ ions would weaken the rigidity of BAO lattice, resulting in the degrade of luminescence intensity with temperatures. Fortunately, the as-prepared BAO:xEu2+ (x = 1%, 5%, 10%, 20%) samples also exhibits outstandingly reversible thermal stability. when the heating temperature varies from 500 K to 298 K, the emission intensity nearly returns to the initial intensity. (Figure S7). Generally, the as-prepared BAO:1%Eu2+ manifested excellent thermal stability even better than that of commercial BAM:Eu2+ phosphor, which further shows its promising application in WLED devices. To further explain the temperature-dependent thermal quenching phenomenon, the activation energy for the thermal quenching has been estimated using the Arrhenius equation: I = T

Figure 6. (a) Gaussian fitting of the emission spectra for BAO:xEu2+ (1% ≤ x ≤25%) samples. (b) The calculated average distance of Al(2)-O and Al(4)-O with Rietveld refinement. (c) 27 Al NMR spectra of BAO:xEu2+ (0 ≤ x ≤ 25%). (d) The proposed mechanism of the blue-shift emission for increasing Eu concentration. (e) The preferential site-occupancy of Eu2+ into Ba(1) and Ba(2) site when x ≥ 5%.

Thermal quenching properties of BAO:xEu2+ phosphors The thermal stability of phosphors is an important performance objective in evaluating its potential for WLED application due to its influence on the light output, service life and color rendering index.51-56 The thermal stability can be indexed through two aspects: the quenching intensity and the spectral shape with elevating the heating temperature. The temperature-dependent PL spectra of the representative BAO:1%Eu2+ and BAM:Eu2+ phosphors recorded from 298 K

I0 1+ c exp( −

(4)

Ea ) kT

Where c is a constant, k is Boltzmann’s constant with a value of 8.62 × 10-5 eV·K-1, I0 is the initial emission intensity measured at room temperature, IT represents the emission intensity measured at different temperatures, and Ea is the activation energy for the thermal quenching. Rearranging equation (5) results in: ln( I0 / I -1)= T

Ea kT

(5) the activation energy Ea can be obtained by plotting the ln(I0/IT-1) vs 1/kT curve. Expressly, the thermal stability of phosphor becomes better with the increase of the value of Ea. Seen from the inset of Figure 7f, the calculated Ea of BAO:xEu2+ appears a declining trend with the doped Eu2+ concentration increasing, which could explain the enhancive thermal quenching of the studied samples with x. It is noteworthy that the Ea of as-prepared BAO:xEu2+ (x = 1%, 5%, 10%) are indeed slightly higher than commercial BAM:Eu2+, which could confirm its higher thermal stability than BAM:Eu2+.

ACS Paragon Plus Environment

Chemistry of Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

As mentioned in previous section, the higher rigidity of host lattice, the better thermal stability of phosphor materials commonly could be expected. According to the Rietveld refinement results, we have determined that the crystal structure of BAO host was highly symmetric. Therefore, we speculate that the excellent thermal stability of BAO:xEu2+ (1% ≤ x ≤ 25%) resulted from the high symmetric lattice environment of Ba sites. To prove this inference, we have calculated the distortion of Ba coordinated polyhedrons, and the calculated lattice distortion vs x for different Ba site were illustrated in Figure 8. The equation is as follows: 51, 52, 58-60

di − d av 1 n∑ d av i =1

leading to the gradually decrease of crystal symmetry, which is consistent with the result of Figure 7f that the thermal stability declines with x. So it is reasonable to infer that the thermal stability is related to the lattice symmetry, which would become much stronger with the reduction of distortion. While a high symmetry of lattice means a better rigidity of crystal structure that is viewed as an ideal indicator for efficient photoluminescence and high thermal stability.53 According to the previous reports, Debye temperature (ΘD) is demonstrated to the positive correlation with the rigidity, the function can be described as follows: 8, 54, 61-65

Θ D, i =

n

D=

Page 8 of 12

(6)

Where D represents the lattice distortion, di is the distance from Ba to the ith coordinating O atoms, dav is the average Ba−O distance, and n is the coordination numbers. From Figure 8, the distortion index of Ba(1) site and Ba(2) site apparently increases as the doped Eu2+ concentration raising,

3h 2TN A Ai kBU iso, i

(7)

It is noticeable that a smaller average atomic displacement parameter (Uiso) could result in a higher Debye temperature. In this work, the average Uiso value is calculated from the powder XRD Rietveld refinement for BAO:xEu2+ (x = 1%, 5%, 20%), the corresponding results are listed in Table S3. Evidently, the average Uiso increases as the x value increasing. Therefore, the rigidity gradually decreases with the increase of x value, which also proves the decreasing thermal stability. Therefore, the high thermal stability of blue emission of Eu2+ in BAO should be attributed to the high structure rigidity resulted from the high symmetry of Ba coordinated polyhedrons.

Figure 8. The distortion of Ba(1) and Ba(2) sites in BAO:xEu2+ (1% ≤ x ≤ 25%) with the various Eu2+-doped concentration (x).

Figure 7. (a) and (b) The normal and normalized PL spectra of the representative BAO:1%Eu2+ sample at various temperatures (298 – 498 K) (λex = 350 nm), respectively. (c) and (d) The normal and normalized PL spectra of the BAM:Eu2+ phosphor at various temperatures (298–498 K) (λex = 350 nm), respectively. (e) The thermal stability comparison between BAO:1%Eu2+ and BAM:Eu2+. (f) Temperature-dependent PL intensity of BAO:1%Eu2+, and the inset is the activation energy (Ea) of BAO: xEu2+ (1% ≤ x ≤ 25%) and BAM:Eu2+.

LEDs Applications To evaluate the device performance of the as-prepared BAO:Eu2+ phosphors, we fabricated blue LEDs and white LEDs with the representative blue BAO:20%Eu2+ phosphor combing UV (370 nm) chip and blue BAO:20%Eu2+, green Ba3Si6O12N2:Eu2+ and CaAlSiN3:Eu2+ phosphors combing UV (370 nm) chip, the electroluminescence spectra are shown in Figure 9. Under a voltage 3.15 V and current 20 mA, the blue LEDs present high efficient luminescence with color purity of 87.8% and CIE color coordinate (0.1578, 0.0769). In addition, the warm white with low corresponding color temperature (CCT = 3084 K), high color rendering index (Ra = 92.2) and CIE color coordinate (0.4147, 0.3638) could be garnered. These results suggest that the as-prepared BAO:Eu2+ could be excellent candidate for a blue-emitting phosphor material for application in near-UV LEDs.

ACS Paragon Plus Environment

Page 9 of 12 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Chemistry of Materials

luminescence efficiency, color purity and superior thermal stability under n-UV excitation, which can act as potential blue-emitting phosphors for promising applications in n-UV based white LEDs lighting and display area.

 ASSOCIATED CONTENT Supporting Information The Supporting Information is available free of on the ACS Publications website at DOI: XRD, PLE, PL, Decay curves, Temperature-dependent PL spectra, Refined crystallographic parameters, EDS, CIE Color Coordinates, Emission Peaks and FWHM of BAO:xEu2+ (1% ≤ x ≤ 50%), Fractional Atomic Coordinates and Isotropic Atomic Displacement Parameters (Å2) of BAO: xEu2+ (x = 1%, x = 5%, x = 20%).

 AUTHOR INFORMATION Corresponding Author *[email protected] *[email protected] *[email protected]

Notes The authors declare no competing financial interest.

 ACKNOWLEDGEMENT Figure 9. Electroluminescence spectra of (a) Blue LEDs fabricated by BAO:20%Eu2+ and 370 nm GaN chip. (b) White LEDs fabricated by BAO:20%Eu2+, Ba3Si6O12N2:Eu2+, CaAlSiN3:Eu2+, and 370 nm GaN chip. The insets of (a) and (b) are the photographs of LEDs. The working voltage and driving current are 3.15 V and 20 mA, respectively.

 CONCLUSION In this work, the highly efficient blue-emitting Ba1xAl12O19: xEu2+ (1% ≤ x ≤ 25%) phosphors with excellent thermal stability were successfully synthesized by traditional high temperature solid state route. The structure refinement indicates that the as-prepared samples crystallizes into hexagonal unit cell with the space group P63/mmc (194), two Ba sites occupy 2d and 4f Wyck. positions, forming highly symmetrical Ba(1)O9 and Ba(2)O10, respectively. The asprepared BAO:xEu2+ phosphors exhibit an efficient absorption in the region from 250 to 430 nm, matching well with the nUV LED chip. Under 350 nm UV excitation, they exhibit a highly efficient blue emission with the peak at around 443 nm (IQYs = 89.6% for x = 25%). Moreover, the as-prepared samples present a high color purity (~ 92%) and excellent thermal stability (> 92% of room temperature intensity at 498 K), which is better than that of commercially available BAM:Eu2+ phosphor. The highly pure blue emission is ascribed to the preferential occupation of single Ba(1) sites at a high Eu2+-doping concentration. Because the expansion of Al(2) and Al(4) polyhedron lead to the neighboring Ba(2) polyhedron shrink, and the Ba(2) site could not accommodate the Eu2+ ions. Finally, the extra high thermal stability of BAO:Eu2+ is related to the highly symmetrical lattice environment of Ba sites. Generally, the as-prepared Ba1xAl12O19:xEu2+ (1% ≤ x ≤ 25%) phosphors exhibit high

This work was supported by the National Natural Science Foundation of China (Grant Nos. 51672259, 51672265, 51672265, 51750110511), Engineering Research Center of NanoGeomaterials of Ministry of Education, China University of Geosciences (Wuhan) (No. NGM2016KF002), the National College Students' Innovative Training Program (No. 201710491016, 201710491115, 201710491130), the Ministry of Science and Technology of Taiwan (Contract no. MOST 1042113-M-027-007-MY3), the Key Research Program Of Frontier Sciences, CAS (Grant No. YZDY-SSW-JSC018), and projects for science and technology development plan of Jilin province (20170414003GH). The authors also thank Dr. Yixi Zhuang and Prof. Rongjun Xie from Xiamen University for their kind help in the measurement of the temperature-dependent emission spectra in BaAl12O19:Eu2+ phosphor powders.

 REFERENCES (1) Xia, Z. G.; Liu, Q. L. Progress in Discovery and Structural Design of Color Conversion Phosphors for LEDs. Prog. Mater. Sci. 2016, 84, 59-117. (2) Dai, P. P.; Li, C.; Zhang, X. T.; Xu, J.; Chen, X.; Wang, X. L.; Jia, Y.; Wang, X. J.; Liu, Y. C. A Single Eu2+-Activated High-ColorRendering Oxychloride White-Light Phosphor for White-LightEmitting Diodes. Light: Science & Applications 2016, 5, e16024. (3) Lin, C. C.; Liu, R. S. Advances in Phosphors for LightEmitting Diodes. J. Phys. Chem. Lett. 2011, 2, 1268-1277. (4) Dai, P.; Lee, S. P.; Chan, T. S.; Huang, C. H.; Chiang, Y. W.; Chen, T. M. Sr3Ce(PO4)3:Eu2+: A Broadband Yellow-Emitting Phosphor for Near Ultraviolet-Pumped White Light-Emitting Devices. J. Mater. Chem. C 2016, 4, 1170-1177. (5) Qin, X.; Liu, X. W.; Huang, W.; Bettinelli, M.; Liu, X. G. Lanthanide-Activated Phosphors Based on 4f-5d Optical Transitions: Theoretical and Experimental Aspects. Chem. Rev. 2017, 117, 44884527. (6) Lee, J. W.; Singh, S. P.; Kim, M.; Hong, S. U.; Park, W. B.; Sohn, K. S. Metaheuristics-Assisted Combinatorial Screening of Eu2+-Doped Ca-Sr-Ba-Li-Mg-Al-Si-Ge-N Compositional Space in

ACS Paragon Plus Environment

Chemistry of Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Search of a Narrow-Band Green Emitting Phosphor and Density Functional Theory Calculations. Inorg. Chem. 2017, 56, 9814-9824. (7) George, N. C.; Pell, A. J.; Dantelle, G.; Page, K.; Llobet, A.; Balasubramanian, M.; Pintacuda, G.; Chmelka, B. F.; Seshadri, R. Local Environments of Dilute Activator Ions in the Solid-State Lighting Phosphor Y3–xCexAl5O12. Chem. Mater. 2013, 25, 39793995. (8) Bachmann, V.; Ronda, C.; Meijerink, A. Temperature Quenching of Yellow Ce3+ Luminescence in YAG:Ce. Chem. Mater. 2009, 21, 2077-2084. (9) Oh, J. R.; Cho, S. H.; Lee, Y. H.; Do, Y. R. Lowering Color Temperature of Y3Al5O12:Ce3+ White Light Emitting Diodes Using Reddish Light-Recycling Filter. Electrochem. Solid-State Lett. 2010, 13, J5-J7. (10) Ueda, J.; Dorenbos, P.; Bos, A. J. J.; Meijerink, A.; Tanabe, S. Insight into the Thermal Quenching Mechanism for Y3Al5O12:Ce3+ through Thermoluminescence Excitation Spectroscopy. J. Phys. Chem. C 2015, 119, 25003-25008. (11) Milosevic, O.; Mancic, L.; Rabanal, M. E.; Torralba, J. M.; Yang, B.; Townsend, P. Structural and Luminescence Properties of Gd2O3:Eu3+ and Y3Al5O12:Ce3+ Phosphor Particles Synthesized via Aerosol. J. Electrochem. Soc. 2005, 152, G707-G713. (12) Zhu, Y. W; Huang, L.; Zou, R.; Zhang, J. H.; Yu, J. B.; Wu, M. M.; Wang, J.; Su, Q. Hydrothermal Synthesis, Morphology and Photoluminescent Properties of An Mn4+-Doped Novel Red Fluoride Phosphor Elpasolite K2LiAlF6. J. Mater. Chem. C 2016, 4, 56905695. (13) Zhong, J. Y.; Zhao, W. R.; Zhuang, W. D.; Xiao, W.; Zheng, Y. L.; Du, F.; Wang, L. G. Origin of Spectral Blue Shift of Lu3+Codoped YAG:Ce3+ Phosphor: First-Principles Study. ACS Omega 2017, 2, 5935-5941. (14) Jang, H. S.; Won, Y. H.; Jeon, D. Y. Improvement of Electroluminescent Property of Blue LED Coated with Highly Luminescent Yellow-Emitting Phosphors. Appl. Phys. B 2009, 95, 715-720. (15) Tian, Y.; Wei, Y.; Zhao, Y.; Quan, Z. W.; Li, G. G.; Lin, J. Photoluminescence Tuning of Ca5(PO4)3Cl:Ce3+/Eu2+,Tb3+/Mn2+ Phosphors: Structure Refinement, Site Occupancy, Energy Transfer and Thermal Stability. J. Mater. Chem. C 2016, 4, 1281-1294. (16) Sheu, J. K.; Chang, S. J.; Kuo, C. H.; Su, Y. K.; Wu, L. W.; Lin, Y. C.; Lai, W. C.; Tsai, J. M.; Chi, G. C.; Wu, R. K. White-Light Emission from near UV InGaN-GaN LED Chip Precoated with Blue/Green/Red Phosphors. IEEE Photonics Tech. Lett. 2003, 15, 1820. (17) Strobel, P.; Weiler, V.; Hecht, C.; Schmidt, P. J.; Schnick, W. Luminescence of the Narrow-Band Red Emitting Nitridomagnesosilicate Li2(Ca1–xSrx)2[Mg2Si2N6]:Eu2+ (x = 0-0.06). Chem. Mater. 2017, 29, 1377-1383. (18) Shang, M. M.; Liang, S. S.; Qu, N. R.; Lian, H. Z.; Lin, J. Influence of Anion/Cation Substitution (Sr2+→Ba2+, Al3+→Si4+, N3– →O2–) on Phase Transformation and Luminescence Properties of Ba3Si6O15:Eu2+ Phosphors. Chem. Mater. 2017, 29, 1813-1829. (19) Park, W. B.; Kim, H.; Park, H.; Yoon, C.; Sohn, K. S. The Composite Structure and Two-Peak Emission Behavior of a Ca1.5Ba0.5Si5O3N6:Eu2+ Phosphor. Inorg. Chem. 2016, 55, 2534-2543. (20) Yan, C. P.; Liu, Z. N.; Zhuang, W. D.; Liu, R. H.; Xing, X. R.; Liu, Y. H.; Chen, G. T.; Li, Y. F.; Ma, X. L. YScSi4N6C:Ce3+-A Broad Cyan-Emitting Phosphor to Weaken the Cyan Cavity in FullSpectrum White Light-Emitting Diodes. Inorg. Chem. 2017, 56, 11087-11095. (21) Wang, C. Y.; Takeda, T.; Ten Kate, O. M.; Tansho, M.; Deguchi, K.; Takahashi, K.; Xie, R. J.; Shimizu, T.; Hirosaki, N. CeDoped La3Si6.5Al1.5N9.5O5.5, a Rare Highly Efficient Blue-Emitting Phosphor at Short Wavelength toward High Color Rendering White LED Application. ACS Appl. Mater. Interfaces 2017, 9, 2266522675. (22) Wang, Z. L.; Cheah, K. W.; Tam, H. L.; Gong, M. L. NearUltraviolet Light Excited Deep Blue-Emitting Phosphor for SolidState Lighting. J. Alloys Compd. 2009, 482, 437-439.

Page 10 of 12

(23) Kim, K. B.; Kim, Y. I.; Chun, H. G.; Cho,T. Y.; Jung, J. S.; Kang, J. G. Structural and Optical Properties of BaMgAl10O17:Eu2+ Phosphor. Chem. Mater. 2002, 14, 5045-5052. (24) Lee, S. S.; Kim, H. J.; Byeon, S. H.; Park, J. C.; Kim, D. K. Thermal-Shock-Assisted Solid-State Process for the Production of BaMgAl10O17:Eu Phosphor. Ind. Eng. Chem. Res. 2005, 44, 43004303. (25) Yin, L. J.; Dong, J. T.; Wang, Y. P.; Zhang, B.; Zhou, Z.Y.; Jian, X.; Wu, M. Q.; Xu, X.; van Ommen, J. R.; Hintzen, H. T. Enhanced Optical Performance of BaMgAl10O17:Eu2+Phosphor by a Novel Method of Carbon Coating. J. Phys. Chem. C 2016, 120, 23552361. (26) Kim, Y. H.; Arunkumar, P.; Kim, B. Y.; Unithrattil, S.; Kim, E.; Moon, S. H.; Hyun, J. Y.; Kim, K. H.; Lee, D.; Lee, J. S.; Im, W. B. A Zero-Thermal-Quenching Phosphor. Nat. Mater. 2017, 16, 543550. (27) Lian, Z. P.; Yan, Q. F. Eu2+-Doped NaBa4(AlB4O9)2X3 (X = Cl, Br) Phosphors with Intense Two-Center Blue Emission and High Color Purity for n-UV Pumped White Light-Emitting Diodes. J. Mater. Chem. C 2016, 4, 7959-7965. (28) Schubert, E. F. Light Emitting Diodes, Cambridge University Press, 2006. (29) Deshmukh, A. D.; Valechha, A.; Valechha, D.; Kumar, A.; Peshwe, D. R.; Dhoble, S. J. Effect of Ca2+ and Sr2+ Alkaline Earth Ions on Luminescence Properties of BaAl12O19:Eu Nanophosphor. J. Lumin. 2009, 129, 691-695. (30) Singh, V.; Chakradhar, R. P. S.; Rao, J. L.; Ko, I.; Kwak, H. Y. Luminescence and EPR Studies of Eu2+ Doped BaAl12O19 Blue Light Emitting Phosphors. J. Lumin. 2010, 130, 703-708. (31) Singh, V.; Sivaramaiah, G.; Rao, J. L.; Kim, S. H. Optical and EPR Properties of BaAl12O19:Eu2+, Mn2+ Phosphor Prepared by Facile Solution Combustion Approach. J. Lumin. 2015, 157, 74-81. (32) Liu, B.; Han, B.; Zhang, F.; Wen, Y.; Zhu, G.; Zhang, J.; Wang, Y. H. Photoluminescence Properties of Si–N-Doped BaAl12O19:Mn2+ Phosphors for Three-Dimensional Plasma Display Panels. Mater. Res. Bull. 2012, 47, 156-159. (33) Xie, Y.; Xiao, L. J.; He, M. R.; Chen, Y. J.; Li, W. Z.; Yu, W. K. Effects of Sr2+ on Structure and Luminescent Properties of BaAl12O19:Eu Phosphors. J. Rare Earths 2010, 28, 229-231. (34) Singh, V.; Chakradhar, R. P. S.; Rao, J. L.; Kwak, H. Y. Investigations on Green-Emitting, Mn2+: BaAl12O19 Phosphors Obtained by Solution Combustion Process. J. Mater. Sci. 2011, 46, 3928-3934. (35) Liu, L. L.; Yang, Y.; Jing, Q.; Dong, X. Y.; Yang, Z. H.; Pan, S. L.; Wu, K. K5Ba10(BO3)8F: A New Potassium Barium Borate Fluoride with a Perovskite-Like Structure. J. Phys. Chem. C 2016, 120, 18763-18770. (36) Wang, X. M.; Zhang, X.; Ye, S.; Jing, X. P. A Promising Yellow Phosphor of Ce3+/Li+ Doped CaSiN(2-2δ/3)Oδ for pc-LEDs. Dalton. Trans. 2013, 42, 5167-5173. (37) Deng, T. T.; Song, E. H.; Sun, J.; Wang, L. Y.; Deng, Y.; Ye, S.; Wang, J.; Zhang, Q. Y. The Design and Preparation of the Thermally Stable, Mn4+ Ion Activated, Narrow Band, Red Emitting Fluoride Na3GaF6:Mn4+for Warm WLED Applications. J. Mater. Chem. C 2017, 5, 2910-2918. (38) Tauc, J.; Grigorovici, R.; Vancu, A. Optical Properties and Electronic Structure of Amorphous Gemanium. phys. start. 1966, 15, 627-637. (39) Liu, Y. F.; Silver, J.; Xie, R. J.; Zhang, J. H.; Xu, H. W.; Shao, H. Z.; Jiang, J.; Jiang, H. C. An Excellent Cyan-Emitting Orthosilicate Phosphor for NUV-Pumped White LED Application. J. Mater. Chem. C 2017, 5, 12365-12377. (40) Jørgensen, C. K. Modern Aspects of Ligand Field Theory, North-Holland, Amsterdam, 1971. (41) Hong, S. U.; Singh, S. P.; Pyo, M.; Park, W. B.; Sohn, K. S. Density Functional Theory Calculations for the Band Gap and Formation Energy of Pr4-xCaxSi12O3+xN18-x; a Highly Disordered Compound with Low Symmetry and a Large Cell Size. Phys. Chem. Chem. Phys. 2017, 19, 16702-16712.

ACS Paragon Plus Environment

Page 11 of 12 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Chemistry of Materials

(42) Li, G. G.; Tian, Y.; Zhao, Y.; Lin, J., Recent Progress in Luminescence Tuning of Ce(3+) and Eu(2+)-Activated Phosphors for pc-WLEDs. Chem. Soc. Rev. 2015, 44, 8688-8713. (43) Penke, Y. K.; Anantharaman, G.; Ramkumar, J.; Kar, K. K. Aluminum Substituted Cobalt Ferrite (Co-Al-Fe) Nano Adsorbent for Arsenic Adsorption in Aqueous Systems and Detailed Redox Behavior Study with XPS. ACS Appl. Mater. Interfaces 2017, 9, 11587-11598. (44) Song, X. Y.; Ma, Y.; Ge, X.; Zhou, H. J.; Wang, G. Z.; Zhang, H. M.; Tang, X. X.; Zhang, Y. X. Europium-Based Infinite Coordination Polymer Nanospheres as an Effective Fluorescence Probe for Phosphate Sensing. RSC Adv. 2017, 7, 8661-8669. (45) Senapati, S.; Nanda, K. K. Red Emitting Eu:ZnO Nanorods for Highly Sensitive Fluorescence Intensity Ratio Based Optical Thermometry. J. Mater. Chem. C 2017, 5, 1074-1082. (46) Kang, F. W.; Peng, M. Y.; Lei, D. Y.; Zhang, Q. Y. Recoverable and Unrecoverable Bi3+-Related Photoemissions Induced by Thermal Expansion and Contraction in LuVO4:Bi3+ and ScVO4:Bi3+ Compounds. Chem. Mater. 2016, 28, 7807-7815. (47) Li, L. Y.; Cao, J. K.; Viana, B.; Xu, S. H.; Peng, M. Y. Site Occupancy Preference and Antithermal Quenching of the Bi2+ Deep Red Emission in β-Ca2P2O7:Bi2+. Inorg. Chem. 2017, 56, 6499-6506. (48) Xu, H. B.; Zhuang, W. D.; Wang, L.; Liu, R. H.; Liu, Y. H.; Liu, L. H.; Cho, Y.; Hirosaki, N.; Xie, R. J. Synthesis and Photoluminescence Properties of a Blue-Emitting La3Si8N11O4:Eu2+ Phosphor. Inorg. Chem. 2017, 56, 14170-14177. (49) Zhang, N. M.; Tsai, Y. T.; Fang, M. H.; Ma, C. G.; Lazarowska, A.; Mahlik, S.; Grinberg, M.; Chiang, C. Y.; Zhou, W Z..; Lin, J. G.; Lee, J. F.; Zheng, J. M.; Guo, C. F.; Liu, R. S. Aluminate Red Phosphor in Light-Emitting Diodes: Theoretical Calculations, Charge Varieties, and High-Pressure Luminescence Analysis. ACS Appl. Mater. Interfaces 2017, 9, 23995-24004. (50) Unithrattil, S.; Arunkumar, P.; Kim, Y. H.; Kim, H. J.; Vu, N. H.; Heo, J.; Chung, W. J.; Im, W. B. A Phosphosilicate Compound, NaCa3PSiO8: Structure Solution and Luminescence Properties. Inorg. Chem. 2017, 56, 15130-15137. (51) Chen, M. Y.; Xia, Z. G.; Molokeev, M. S.; Wang, T.; Liu, Q. L. Tuning of Photoluminescence and Local Structures of Substituted Cations in xSr2Ca(PO4)2-(1-x)Ca10Li(PO4)7:Eu2+ Phosphors. Chem. Mater. 2017, 29, 1430-1438 (52) Chen, M. Y.; Xia, Z. G.; Molokeev, M. S.; Lin, C. C.; Su, C. C.; Chuang, Y. C.; Liu, Q. L. Probing Eu2+ Luminescence from Different Crystallographic Sites in Ca10M(PO4)7:Eu2+ (M = Li, Na, and K) with β‑Ca3(PO4)2‑Type Structure. Chem. Mater. 2017, 29, 7563-7570. (53) Yeh, C. W.; Chen, W. T.; Liu, R. S.; Hu, S. F.; Sheu, H. S.; Chen, J. M.; Hintzen, H. T. Origin of Thermal Degradation of Sr2xSi5N8:Eux Phosphors in Air for Light-Emitting Diodes. J. Am. Chem. Soc. 2012, 134, 14108-14117. (54) Chen, W. P. Eu2+ and Eu3+ Co-Activated LaAlO3 Phosphor: Synthesis and Tuned Luminescence. Dalton Trans. 2015, 44, 1773017735. (55) Piao, X. Q.; Machida, K. I.; Horikawa, T.; Hanzawa, H.; Shimomura, Y.; Kijima N. Preparation of CaAlSiN3:Eu2+ Phosphors by the Self-Propagating High-Temperature Synthesis and Their Luminescent Properties. Chem. Mater. 2007, 19, 4592-4599. (56) Im, W. B.; George, N.; Kurzman, J.; Brinkley, S.; Mikhailovsky, A.; Hu, J.; Chmelka, B. F.; DenBaars, S. P.; Seshadri, R. Efficient and Color-Tunable Oxyfluoride Solid Solution Phosphors for Solid-State White Lighting. Adv. Mater. 2011, 23, 2300-2305. (57) Wang, C. Y.; Kate, O. M.; Takeda, T.; Hirosaki, N. Efficient and Thermally Stable Blue-Emitting Ce3+ Doped LaAl(Si6−zAlz)(N10−zOz) (JEM:Ce) Phosphors for White LEDs. J. Mater. Chem. C 2017, 5, 8295-8300. (58) Zhao, M.; Xia, Z. G.; Molokeev, M. S.; Ning, L. X.; Liu, Q. L. Temperature and Eu2+-Doping Induced Phase Selection in NaAlSiO4 Polymorphs and the Controlled Yellow/Blue Emission. Chem. Mater. 2017, 29, 6552-6559.

(59) Baur, W. H. The geometry of polyhedral distortions. Predictive Relationships for the Phosphate Group. Acta Crystallographica Section B Structural Crystallography and Crystal Chemistry 1974, 30, 1195-1215. (60) Brgoch, J.; DenBaars, S. P.; Seshadri, R. Proxies from Ab Initio Calculations for Screening Efficient Ce3+ Phosphor Hosts. J. Phys. Chem. C 2013, 117, 17955-17959. (61) George, N. C.; Birkel, A.; Brgoch, J.; Hong, B. C.; Mikhailovsky, A. A.; Page, K.; Llobet, A.; Seshadri, R. Average and Local Structural Origins of the Optical Properties of the Nitride Phosphor La3-xCexSi6N11 (0 < x ≤ 3). Inorg. Chem. 2013, 52, 1373013741. (62) Willis, B. T. M.; Pryor, A. W. Thermal Vibrations in Crystallography.Cambridge University Press: Cambridge, U. K. 1975. (63) Dalba, G.; Fornasini, P. EXAFS Debye-Waller Factor and Thermal Vibrations of Crystals. J. Synchrotron Radiat. 1997, 4, 243255. (64) Ha, J. M.; Wang, Z. B.; Novitskaya, E.; Hirata, G. A.; Graeve, O. A.; Ong, S. P.; McKittrick, J. An Integrated First Principles and Experimental Investigation of the Relationship between Structural Rigidity and Quantum Efficiency in Phosphors for Solid State Lighting. J. Lumin. 2016, 179, 297-305. (65) Anderson, O. L. A Simplified Method for Calculating the Debye Temperature from Elastic Constants. J Phys. Chem. Solids 1963, 24, 909-917.

ACS Paragon Plus Environment

Chemistry of Materials 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60

Highly efficient blue emission and superior thermal stability were realized in the BaAl12O19:Eu2+ phosphor based on the highly symmetric crystal structure. 281x121mm (72 x 72 DPI)

ACS Paragon Plus Environment

Page 12 of 12