Novel Magnetic Properties of Graphene: Presence ... - ACS Publications

The Journal of Physical Chemistry C. Advanced Search .... H. S. S. Ramakrishna Matte, K. S. Subrahmanyam and C. N. R. Rao*. International Centre for ...
0 downloads 0 Views 1MB Size
9982

2009, 113, 9982–9985 Published on Web 05/14/2009

Novel Magnetic Properties of Graphene: Presence of Both Ferromagnetic and Antiferromagnetic Features and Other Aspects H. S. S. Ramakrishna Matte, K. S. Subrahmanyam, and C. N. R. Rao* International Centre for Materials Science, New Chemistry Unit and CSIR Centre of Excellence in Chemistry, Jawaharlal Nehru Centre for AdVanced Scientific Research, Jakkur P. O., Bangalore 560 064, India ReceiVed: April 13, 2009; ReVised Manuscript ReceiVed: May 2, 2009

Investigations of the magnetic properties of graphenes prepared by different methods reveal that dominant ferromagnetic interactions coexist along with antiferromagnetic interactions in all of the samples, somewhat like in frustrated or phase-separated systems. All of the graphene samples exhibit room-temperature magnetic hysteresis. The magnetic properties of the graphene samples depend on the number of layers and the sample area, small values of both favoring larger magnetization. Molecular charge-transfer affects the magnetic properties of graphene, interaction with a donor molecule such as tetrathiafulvalene having greater effect than with an electron-withdrawing molecule such as tetracyanoethylene. The occurrence of intrinsic magnetism in carbon-based materials possessing the sp2 network has been a controversial subject. Although there has been doubt as to whether the ferromagnetic features of some of the graphitic materials was due to magnetic impurities such as iron, there is also evidence for ferromagnetism in highly oriented pyrolytic graphite (HOPG) and related materilas.1 For example, proton irradiated HOPG seems to show room temperature magnetism. It was pointed out sometime ago that edges in graphene ribbons play a crucial role in determining the electronic structure.2 There have been a few studies on the properties of nanographite particles and ribbons which demonstrate the importance of the edge states arising from the nonbonding electrons.3,4 Nanographite particles are reported to exhibit unusual magnetic properties including spin-glass behavior and magnetic switching phenomena, and their properties have been reviewed by Enoki et al.,5-7 and the main message is that edge states as well as adsorbed or intercalated species affect the magnetic properties. Bilayer graphene is predicted to be ferromagnetic.8 Hydrogenated nanographite is also predicted to show spontaneous magnetism.9 Theoretical studies suggest the existence of a ferromagnetically ordered ground state in graphene, specially at the zigzag edges.10 Zigzag edges longer than 3-4 repeat units are predicted to be magnetic, irrespective of whether the edges are regular or irregular.11 Theoretical studies also show the importance of the crystallographic nature of graphene in determining its electronic properties and the possibility of half-metallicity in graphene ribbons.12 We have carried out an experimental study of the magnetic properties of graphene samples prepared by different methods, ensuring that they were devoid of transition metal impurities. We have also investigated the effect of electron donor and acceptor molecules on the magnetic properties of graphene. For this purpose, we have measured the effect of interaction of graphene with tetrathiafulvalane (TTF) and tetracyanoethylene (TCNE). These molecules are known to significantly affect the * To whom correspondence should be addressed. E-mail: cnrrao@ jncasr.ac.in. Fax: (+91) 80-2208 2760.

10.1021/jp903397u CCC: $40.75

electronic properties and Raman spectra of graphene because of charge-transfer.13 Significantly, we find that all of the graphene samples show evidence for ferromagnetism with welldefined hysteresis, along with antiferromagnetic features. Electrondonating TTF markedly affects the magnetic properties of graphene. Graphene samples were prepared by the thermal exfoliation of graphitic oxide (EG),14 conversion of nanodiamond (DG),3,14 and arc evaporation of graphite in hydrogen (HG).15 We also prepared a graphene sample (EG-H) by reducing single-layer graphene oxide with hydrazine hydrate.16 The absence of magnetic transition metal impurities was ensured by employing due care in synthesis as well as specific procedures. Thus, in the case of DG, the nanodiamond was washed with concentrated hydrochloric acid before carrying out the transformation. EPR measurements in the 2.5-300 K range as well as electron energy loss spectra of the samples gave no indication of transition metal impurities. All of the samples were characterized using transmission electron microscopy (TEM), atomic force microscopy (AFM), Raman spectroscopy, and Brunauer-Emmett-Teller (BET) surface areas. Magnetic measurements were performed on 6-8 mg of graphene samples by employing a vibrating sample magnetometer (VSM) in physical property measuring system (Quantum Design, USA). Electron paramagnetic resonance (EPR) spectra were recorded using a Bruker EMX X-band continuous wave (CW) EPR spectrometer. The effect of adsorption of 0.01 and 0.05 M benzene solutions of TTF and TCNE on the magnetic properties of HG was also studied. In Figure 1, we show typical AFM data and Raman spectra in the case of EG and HG. Unlike the HG sample, the EG sample consists of a larger number of layers. From the AFM measurements, the average number of graphene layers was estimated to be 6-7, 4-5, and 2-3 repectively in EG, DG, and HG. Raman spectra show the D-, G-, and 2D bands around 1320, 1570, and 2640 cm-1 and the relative intensity of the defect-related D-band is much higher in HG. The BET surface areas17 of the samples were 826, 781, and 680 m2/g, respectively.  2009 American Chemical Society

Letters

J. Phys. Chem. C, Vol. 113, No. 23, 2009 9983

Figure 1. AFM images and the associated height profiles and Raman spectra of (a) HG and (b) EG samples. The ratio of intensities of the D and G bands in the Raman spectra are given.

Figure 3. Magnetic hysteresis in EG, DG, and HG at 300 K. Inset shows magnetic hysteresis in DG at 5 K.

Figure 2. Temperature variation of magnetization of EG, DG and HG at 500 Oe showing the ZFC and FC data. The insets show the magnetization data at 1 T.

The areas of the graphene flakes in the EG, DG, and HG samples were 65 ( 25 × 103, 40 ( 20 × 103, and 25 ( 15 × 103 nm2, respectively. Of the three graphene samples, HG had the smallest number of graphene layers and the smallest area. The EG-H sample appears to possess even a smaller number of layers close to unity.16 In Figure 2, we show the temperature-dependence of magnetization of EG, DG, and HG measured at 500 Oe. All of the samples show divergence between the field-cooled (FC) and zero-field-cooled (ZFC) data, starting around 300 K. The divergence nearly disappears on the application of 1 T as can be seen from the insets in Figure 2. EG-H also shows a behavior similar EG, DG, and HG. Divergence between the FC and ZFC data in the graphene samples is comparable to that in magnetically frustrated systems such as spin-glasses and superparamagnetic materials. The Curie-Weiss temperatures obtained from the high-temperature inverse susceptibility data were

negative in all these samples, indicating the presence of antiferromagnetic interactions. Interestingly, we observe welldefined maxima in the magnetization at low temperatures, the maxima becoming prominent in the data recorded at 1 T (see insets in Figure 2). Such magnetic anomalies are found when antiferromagnetic correlations compete with ferromagnetic (FM) order. Application of high fields aligns the FM clusters and decreases the divergence between FC and ZFC data as indeed observed. It is possible that the data correspond to a percolation type of situation, where in different types of magnetic states coexist. The FM clusters in such a case would not be associated with a well-defined global ferromagnetic transition temperature. This behavior is similar to that of microporus carbon and some phase-separated members of the rare earth Manganite family, Ln1-xAxMnO3 (Ln ) rare earth, A ) alkaline earth); nanoparticles of antiferromagnetic oxides also show a similar behavior.18 Recent theoretical calculations do indeed predict the presence of antiferromagnetic states in the sheets and ferromagnetic states at the edges of graphene.19 All of the graphene samples show magnetic hysteresis at room temperature (Figure 3). Of the three samples, HG shows the best hysteretic features with saturation. While DG also shows saturation, the value of saturation magnetization, MS, is, however, low compared to that of HG. In Table 1, we list the values of MS, remnant magnetization, MR, and the Curie-Weiss temperature, θp, along with value of magnetization at 100 K

9984

J. Phys. Chem. C, Vol. 113, No. 23, 2009

Letters

TABLE 1: Magnetic Properties of the Graphene Samples M (emu/g) (FC) T)5 T ) 300 K sample (H ) 1T) (H ) 0.3 T) HG DG EG

0.527 0.281 0.258

0.393 0.127 0.007

|θp| 3335 686 230

MS MR (T ) 5 K) (T ) 300 K) 0.69 0.45 0.062

0.053 0.0162 0.0032

(at 3000 Oe) for the three graphene samples studied by us. We see that θp, MR, and MS are highest in the case of HG which also shows a higher value of magnetization than the other samples at all temperatures. We have plotted the values of the various magnetic properties of the samples in Figure 4a to demonstrate how the properties vary as HG > DG > EG. In Figure 4b, we have shown the variation of the average area and the number of layers in these three samples. It is noteworthy that both the area and the number of layers decrease in the order of EG > DG > HG. It is likely that edge effects would be greater in samples with a smaller number of layers as well as small areas. In the case of HG, hydrogenation could have occurred to some extent, thereby favoring ferromagnetism. Since we completed research on the magnetic properties of graphene, we have noticed a report of ferromagnetism in a graphene sample by Wang et al.20 who propose long-range coupling of spin units (defects) to be responsible for ferromagnetism. These workers prepared graphene by partially reducing graphene oxide with hydrazine and annealing the samples at different temperatures in an argon atmosphere. It is noteworthy that the EG-H sample

Figure 4. (a) Comparison of the magnetic properties of EG, DG, and HG. (b) Variation of the number of layers and sample area in the graphene samples.

prepared by us exhibits very large magnetization, much larger than that of HG.21 As mentioned earlier, the graphene samples studied by us did not contain detectable levels of transition metal impurities. The unusual magnetic properties reported here are, therefore, considered to be intrinsic to the graphene samples. Since we find the presence of Antiferromagnetic interactions as well as magnetic hysteresis in our graphene samples, a behavior somewhat like that of frustrated magnetic systems, we carried out ac susceptibility measurements on HG and DG samples in the frequency range from 97 to 9997 Hz. We did not find any frequency-dependent features in the ac susceptibility data in the 3-300 K range. This suggests that observed ferromagnetism is not due to spin-glass behavior. We have carried out EPR investigations in the temperature range from 2.5 to 300 K on the same EG, DG, and HG samples subjected to magnetic measurements. We observe a signal with a line-width of ∆H ≈ 0.7-2.9 mT with a g value that is in the 2.006-2.013 range. The small value of the line-width and the small deviation in the g value from the free-electron value suggest that the spins do not originate from transition-metal impurities but from only carbon-inherited spin species in the graphene sheets. The temperature variation of the EPR intensity is consistent with the magnetization data showing a marked increase at low temperatures. Spin-density measurements were carried on EG, DG, and HG samples taking copper sulfate as a reference and gave values of 2.86 × 10,12 1.48 × 10,13 and 2.46 × 10,14 spins/mg., respectively. Adsorption of benzene solutions of TTF and TCNE has a profound effect on the magnetic properties of graphene. In Figure 5, we show typical results on the effect of adsorbing 0.01 and 0.05 M solutions of TTF on the magnetic properties of HG. The value of the magnetization drastically decreases on adsorption of TTF and TCNE, although the basic trend in the temperature-variation of magnetization remains the same. Thus, the graphene sample continues to show room-temperature hysteresis. On increasing the concentration of TTF or TCNE, the magnetization value decreases progressively. Interestingly, TTF has a greater effect than TCNE, even though the magnitude of adsorption of TCNE on HG is greater. Magnetic hysteresis of HG persists even after adsorption of TTF and TCNE. The value of MS at 300 K decreases on adsorption of TTF and TCNE, the decrease being larger in the case of former. The Curie-Weiss temperature, θp, also decreases markedly on adsorption of these molecules. Thus, θp of HG becomes -485 and -83 K after adsorbing 0.05 M TCNE and TTF respectively (compared to -3340 K for pure HG). Clearly, charge-transfer interaction between graphene and TTF (TCNE)12 is responsible for affecting the magnetic properties. In the literature, there is some evidence to show that adsorption of H2O22 and interaction of acids23 reduce the magnetization of nanographite. Potassium clusters also reduce the magnetization of nanographite.24 In these cases, the reduction in magnetization has been interpreted as being due to the interaction with lonepair orbitals as well as charge-transfer with graphene sheets. The large reversible concentration-dependent effects of adsorbing TTF and TCNE on the magnetic properties of graphene lend additional evidence to the fact that the magnetic properties of the graphene samples observed by us are intrinsic to them. In conclusion, graphene samples with the number of layers in the 2-7 range, prepared by different methods, show prominent ferromagnetic features along with antiferromagnetic characteristics. The behavior is not unlike that in certain other materials such as antiferromagnetic nanoparticles and frustrated magnetic systems, showing magnetic hysteresis below a certain

Letters

J. Phys. Chem. C, Vol. 113, No. 23, 2009 9985 single layer graphene, shows much larger magnetization than HG.21 At present, we are investigating EG-H samples as well as other samples containing primarily single-layer graphene. Acknowledgment. The authors thank Prof. S. V. Bhat, Indian Institute of Science, for EPR measurements. References and Notes

Figure 5. Temperature-variation of the magnetization of HG samples (500 Oe) after adsorption of 0.01 and 0.05 M solutions of TTF. The magnetization data given in the figure are corrected for the weight of adsorbed TTF. Magnetic hysteresis data at 300 K are shown as insets. In the case of 0.05 M TTF-HG, magnetization data at 1 T are shown as an inset. Magnetization data of HG with adsorbed TCNE are similar to those with TTF, except that the decrease in magnetization relative to pure HG is much smaller.

temperature where divergence between ZFC and FC data occurs. It is not possible to exactly pin down the origin of magnetism in the graphene samples although defects, and edge effects, are likely to play a major role.20,25 As pointed out recently, stacking faults and other defects can indeed impart ferromagnetic and antiferromagnetic features in graphene.25 Furthermore, it is to be noted that all inorganic nanoparticles are known to exhibit magnetic hysteresis at room temperature due to surface defects.26 The values of magnetization as well as the other magnetic properties vary from sample to sample. If we consider ferromagnetism to be primarily the result of edge effects, it is not surprising that HG shows the best FM features. Besides the smallest number of layers, this sample has the smallest flakes and therefore more edges. Interestingly, the intensity ratio of the D band with respect to the G band in the Raman spectrum is higher in HG than in EG. It is noteworthy that preliminary studies show that the EG-H sample, probably containing mainly

(1) (a) Hans, K. H.; Spemann, D.; Esquinazi, P.; Holine, R.; Reide, V.; Butz, T. AdV. Mater. 2003, 15, 1719–1722. (b) Makarova, T. Magnetism of carbon-based materials; Nova Publishers: New York, 2003; p 44. (2) Nakada, K.; Fujita, M.; Dresselhaus, G.; Dresselhaus, M. S. Phys. ReV. B 1996, 54, 17954. (3) (a) Andersson, O. E.; Prasad, B. L. V.; Sato, H.; Enoki, T.; Hishiyama, Y.; Kaburagi, Y.; Yoshikawa, M.; Bandow, S. Phys. ReV. B 1998, 58, 16387. (b) Enoki, T.; Kawatsu, N.; Shibayama, Y.; Sato, H.; Kobori, R.; Maruyama, S.; Kaneko, K. Polyhedron 2001, 20, 1311–1315. (4) Wakabayashi, K.; Fujita, M.; Ajiki, H.; Sigrist, M. Phys. ReV. B 1999, 59, 8271. (5) Enoki, T.; Kobayashi, Y. J. Mater. Chem. 2005, 15, 3999–4002. (6) Enoki, T.; Takai, K. Dalton Trans. 2008, 3773-3781. (7) Enoki, T.; Kobayashi, Y.; Fukui, K. Int. ReV. Phys. Chem. 2007, 26, 609–645. (8) Castro, E. V.; Peres, N. M. R.; Stauber, T.; Silva, N. A. P. Phys. ReV. Lett. 2008, 100, 186803. (9) Kusakabe, K.; Maruyama, M. Phys. ReV. B 2003, 67, 092406. (10) (a) Lee, H.; Son, Y. W.; Park, N.; Han, S. W.; Yu, J. J. Phys. ReV. B 2005, 72, 1745431. (b) Harigaya, K. J. Phys.: Condens. Matter 2005, 13, 1295–13002. (11) Bhowmick, S.; Shenoy, V. B. J. Chem. Phys. 2008, 128, 244717. (12) (a) Barone, V.; Hod, O.; Scuseria, G. E. Nano Lett. 2006, 12, 2748– 2754. (b) Son, Y. W.; Cohen, M. L.; Louie, S. G. Nature 2006, 444, 347– 349. (13) (a) Das, B.; Voggu, R.; Rout, C. S.; Rao, C. N. R. Chem. Comm. 2008, 5155-5157. (b) Voggu, R.; Das, B.; Rout, C. S.; Rao, C. N. R. J. Phys.: Condens. Matter 2008, 20, 472204. (14) (a) Subrahmanyam, K. S.; Vivekchand, S. R. C.; Govindaraj, A.; Rao, C. N. R. J. Mater. Chem. 2008, 18, 1517–1523. (b) Rao, C. N. R.; Biswas, K.; Subrahmanyam, K. S.; Govindaraj, A. J. Mater. Chem. 2009, 19, 2457–2469. (15) Subrahmanyam, K. S.; Panchakarla, L. S.; Govindaraj, A.; Rao, C. N. R. J. Phys. Chem. C 2009, 113, 4257–4259. (16) Stankovich, S.; Dikin, D. A.; Piner, R. D; Kohlhaas, K. A.; Kleinhammes, A.; Jia, Y.; Wu, Y.; Nguyen, S. T.; Ruoff, R. S. Carbon 2007, 45, 1558–1565. (17) Ghosh, A.; Subrahmanyam, K. S.; Krishna, K. S.; Datta, S.; Govindaraj, A.; Pati, S. K.; Rao, C. N. R. J. Phys. Chem. C 2008, 112, 15704–15707. (18) (a) Kopelvich, Y.; Dasilva, R. R.; Torres, J. H. S.; Penicaud, A. Phys. ReV. B 2003, 68, 092408. (b) Dho, J.; Kim, W. S.; Hur, N. H. Phys. ReV. Lett. 2002, 89, 027202. (c) Shenoy, V. B.; Rao, C. N. R. Phil. Trans. R. Soc. A 2008, 366, 63–82. (d) Ghosh, M.; Biswas, K.; Sundaresan, A.; Rao, C. N. R. J. Mater. Chem. 2006, 16, 106–111. (19) Dutta, S.; Lakshmi, S.; Pati, S. K. Phys. ReV. B 2008, 77, 073412. (20) Wang, Y.; Huang, Y.; Song, Y.; Zhang, X.; Ma, Y.; Liang, J.; Chen, Y. Nano Lett. 2009, 9, 220–224. (21) We have not given the actual data on EG-H, since we want to be sure that it does not contain any magnetic impurities introduced during synthesis. Detailed studies on EG-H and related samples are in progress. (22) Sata, H.; Kawatsu, N.; Enoki, T.; Endo, M.; Kobori, R.; Maruyama, S.; Kaneko, K. Solid State Commun. 2003, 125, 641–645. (23) Hao, S.; Takai, K.; Kang, F.; Enoki, T. Carbon 2008, 46, 110– 116. (24) Takai, K.; Eto, S.; Inaguma, M.; Enoki, T.; Ogata, H; Tokita, M.; Watanabe, J. Phys. ReV. Lett. 2007, 98, 017203. (25) (a) Yazyev, O. V.; Helm, L. Phys. ReV. B 2007, 75, 125408. (b) Yazyev, O. V. Phys. ReV. Lett. 2008, 101, 037203. (26) Sundaresan, A.; Rao, C. N. R. Nano Today 2009, 4, 96–101.